High-strength free-cutting copper alloy and preparation method thereof

By adding Al, Mn, Fe and Bi to the copper alloy and using P, La, and Ce elements to refine the grains, the problems of low deformation, plasticity and brittle cracking of aluminum brass materials at room temperature are solved, and high strength is achieved. Easy-to-cut and environmentally friendly copper alloy material to meet the needs of high-precision turning.

CN118880107APending Publication Date: 2024-11-01JINTIAN COPPER GROUP CORP NINGBO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411302691.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing aluminum brass materials have low deformation and are prone to brittle cracking at room temperature. The brittleness of the material increases after adding easy-to-cut elements, which affects processing and use. Bismuth elements are more prone to brittle cracking problems as alternatives.

Method used

By adding Al, Mn, and Fe elements to the copper alloy to form a strengthened wear-resistant phase, combining Bi elements to improve cutting performance, and refining grains and improving Bi particle distribution through P, La, and Ce elements, controlling the phase structure to improve deformation Plastic and brittle crack resistance.

Benefits of technology

It realizes high-strength, easy to cut and not easy to brittle crack, meets the requirements of high-precision turning, reduces the risk of brittle crack in hot and cold processing, and has good mechanical properties and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880107A_ABST
    Figure CN118880107A_ABST
Patent Text Reader

Abstract

The invention relates to a high-strength free-cutting copper alloy and a preparation method thereof. The high-strength free-cutting copper alloy comprises the following components in percentage by weight: 65-70% of Cu; 4.0 to 7.0% of Al; 2.0 to 3.0% of Mn; 2.0 to 3.0% of Fe; 0.4 to 1.0 percent of Bi; less than 0.01% of Pb; the balance is Zn and other inevitable impurities; the phase structure of the copper alloy comprises a matrix beta phase, an alpha phase distributed at the grain boundary of the beta phase and Bi particles distributed in the grain boundary, the beta phase accounts for 75-95%, the average grain size of the beta phase is smaller than 100 micrometers, the alpha phase accounts for 5-20%, the average grain size of the alpha phase is smaller than 20 micrometers, the average grain size of the Bi particles is smaller than 15 micrometers, and the distribution number of the Bi particles is larger than 8000 / mm < 2 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal processing, and in particular to a high-strength free-cutting copper alloy and a preparation method thereof. Background Art

[0002] Aluminum brass is a high-strength, high-wear-resistant material that is widely used in the production of gear rings, turbines, gears, bushing shafts, etc. As current industrial products have higher requirements for material processing accuracy and efficiency, the material must have both high strength and good cutting performance.

[0003] Brass products currently mainly improve their cutting performance by adding free-cutting elements. However, due to the material characteristics of aluminum brass, although it has good deformation plasticity under high temperature conditions, its deformation plasticity is very low at room temperature. After adding free-cutting elements, the brittleness of the material will increase further, affecting normal processing and use. At the same time, considering environmental factors, the current more mature brass products mainly add bismuth elements to replace harmful lead elements as free-cutting elements to further improve the cutting performance of the material. However, after adding bismuth elements, the material is prone to brittle cracking, and compared with lead, bismuth is more prone to brittle cracking under cold and hot processing conditions.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The first object of the present invention is to provide a high-strength free-cutting copper alloy to address one of the deficiencies of the current technology, so that the brass product is easy to cut and not prone to brittle cracking.

[0006] The second object of the present invention is to provide a method for preparing a high-strength free-cutting copper alloy.

[0007] To achieve the above-mentioned invention object, the technical scheme of the present invention is: a high-strength free-cutting copper alloy, wherein the copper alloy components include by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; Pb < 0.01%; the balance is Zn and other inevitable impurities; the phase structure of the copper alloy includes a matrix β phase, an α phase distributed at the β phase grain boundary, and Bi particles distributed in the grain boundary, the β phase accounts for 75-95%, the average size of the β phase grains is < 100 μm, the α phase accounts for 5-20%, the average size of the α phase grains is < 20 μm, the average size of the Bi particles is < 15 μm, and the number of Bi particles distributed is > 8000 / mm 2 .

[0008] Through the above technical scheme, Cu and Zn are used as matrix elements in the alloy, and Al, Mn and Fe elements are added to form a certain number of Al-Fe and Al-Mn strengthening wear-resistant phases to ensure that the material has high strength and high wear resistance. Among them, the zinc equivalents of Al, Mn and Fe elements are approximately +6, +0.5 and +0.9 respectively. After adding the above elements, the zinc content in the material matrix is ​​approximately further increased, thereby ensuring that the material forms a large amount of β phase under hot working conditions, further increasing the high-temperature deformation plasticity of the material, and satisfying the material extrusion processing under low-temperature heating conditions. Still has good deformation plasticity. Since the present invention adds Bi elements to improve cutting performance, the melting point of Bi elements is only 271.3°C, so the material is not conducive to improving the cutting performance in an environment where the processing temperature is too high, and at the same time, the brittleness of the material will be further increased, affecting normal processing and use. By controlling the phase structure in the finished alloy, the matrix is ​​made into β phase, which increases the deformation plasticity, and at the same time, a small amount of α phase is formed at the β phase interface, combined with the dispersed distribution of Bi particles at the grain boundary, the brittleness of the material is improved, and a high-strength and easy-to-cut copper alloy that is not easy to crack is obtained.

[0009] Furthermore, the Bi particles are in the form of particles or thin films. The Bi particles in the form of particles or thin films are evenly distributed at the grain boundaries, achieving an easy-to-cut effect.

[0010] Furthermore, the average size of the β-phase grains is 5 to 25 μm, the average size of the α-phase grains is 1 to 10 μm, the average size of the Bi particles is 0.5 to 5 μm, and the number of Bi particles distributed is 8,000 to 20,000 per mm. 2 The above-mentioned size and distribution are the preferred dimensions of copper alloys. Within this range, the copper alloy has high strength, is easy to cut, is not prone to brittle cracking, and has good processing performance.

[0011] Furthermore, the copper alloy components include by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; P: 0.05-0.2%; Pb < 0.01%; the balance is Zn and other inevitable impurities, and the phase structure of the copper alloy also contains Cu3P phase. The addition of P element improves the melt fluidity during the smelting process and reduces the poor fluidity problem caused by the viscosity of the melt due to the addition of Mn element. At the same time, the trace element P forms Cu3P phase with the Cu matrix, which promotes the improvement of the cutting performance of the material. The addition of P element also has a certain inhibitory effect on the aggregation of Bi element, improves the morphology and size control of Bi particles, and reduces the distribution and aggregation of Bi element in thin film morphology, thereby improving the cutting performance of the material and reducing the risk of brittle cracking under hot and cold processing.

[0012] A high-strength free-cutting copper alloy, the copper alloy components include by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; P: 0.05-0.2%; La+Ce: 0.03-0.15%; Pb < 0.01%; the balance is Zn and other inevitable impurities. Al, Mn and Fe elements are added to the brass matrix to form a certain amount of Al-Fe and Al-Mn strengthening wear-resistant phases to ensure that the material has high strength and high wear resistance, and then La, Ce and P elements are directly introduced during the smelting process to form trace phases such as Cu3P with the matrix, refine the grains, curb the aggregation of Bi elements, improve the matrix and Bi particle morphology and size, thereby improving the material cutting performance and reducing the risk of brittle cracking under hot and cold processing.

[0013] Furthermore, the phase structure of the copper alloy includes a matrix β phase, an α phase distributed at the β phase grain boundary, and Bi particles distributed at the grain boundary, the β phase accounts for 75-95%, the average size of the β phase grains is less than 100 μm, the α phase accounts for 5-20%, the average size of the α phase grains is less than 20 μm, the average size of the Bi particles is less than 15 μm, and the number of Bi particles distributed is greater than 8000 / mm 2 . The addition of La and Ce elements can further improve the comprehensive performance of the material. On the one hand, it can refine the grains, improve the granular dispersion of Bi particles, and improve the cutting performance; on the other hand, it can improve the uniformity of the cast grains, thereby ensuring that the material obtains uniform and stable mechanical properties and organizational properties. After grain refinement, the strength and plasticity of the material can be further improved; the uniform mechanical properties can effectively control the residual stress distribution formed during the material processing process, and improve the stretching and straightening effects of the finished product.

[0014] Furthermore, the copper alloy has a tensile strength of 750-1100 MPa, a yield strength of 650-1000 MPa, axial and circumferential residual stress values ​​of ≤100 MPa, and a cutting index of ≥70%. The copper alloy obtained by the scheme of the present invention has high strength, is easy to cut, and is not prone to brittle cracking.

[0015] Furthermore, the high-strength free-cutting copper alloy of the present application is used in industrial piping components, appliances in contact with liquids or gases, pressure vessels and joints, automotive parts, or electrical product parts;

[0016] Preferably, it is used in gear rings, turbines, gears, and bushing shafts.

[0017] The present invention also provides a preparation method of a high-strength free-cutting copper alloy, comprising the following steps: smelting → casting → extrusion → primary annealing → stretching → secondary annealing; batching and smelting according to component requirements; then flowing the smelted copper liquid into a casting device for casting to produce an ingot, then heating and extruding the ingot, first annealing the extruded blank, stretching the annealed blank, and then subjecting the finished product to secondary low-temperature annealing to obtain the copper alloy.

[0018] Through the above technical scheme, the raw materials or recycled materials are alloyed by smelting, and gas and slag are removed; casting transforms the molten copper into a suitable solid state; the hot processing method of extrusion changes the structure and performance of the material; the primary annealing is a recrystallization treatment, which makes part of the β phase in the material matrix precipitate and transform into the α phase, increases the material processing deformation plasticity, and is beneficial to the subsequent stretching processing; after annealing, the blank is stretched as a finished product to change the shape, size and mechanical properties of the material; the secondary annealing is a low-temperature annealing of the finished product, which plays a role in eliminating stress, stabilizing size, shape and performance, and uniformly refining the grains, so that the final copper alloy has high strength, is easy to cut, and is not easy to crack.

[0019] Furthermore, the smelting temperature is controlled at 950-1200°C;

[0020] Preferably, a semi-continuous casting method is adopted, the temperature of the molten copper entering the casting equipment is controlled to be 1120-1200°C, the stable casting speed is 3.0-5.0 m / h, cooling and electromagnetic stirring are performed, and the average cooling rate of the ingot after it leaves the crystallizer is controlled to be less than 15°C / min;

[0021] Preferably, the extrusion heating temperature is 450-650°C, the heating and heat preservation time is 20-60min, and the extrusion ratio is 100-400:1;

[0022] Preferably, the primary annealing temperature is 400-550°C, and the holding time is 0.5-8h;

[0023] Preferably, the stretching processing rate is 2 to 10%;

[0024] Preferably, the secondary annealing holding temperature is 250-400° C., and the holding time is 1-12 hours;

[0025] More preferably, the secondary annealing holding temperature is 280-360°C.

[0026] The beneficial effects of the present invention are as follows: the present invention adopts the Cu-Zn brass system, adds Al, Mn, and Fe elements to the alloy to form a certain amount of Al-Fe and Al-Mn strengthening wear-resistant phases to ensure that the material has high strength and high wear resistance, adds Bi elements instead of Pb to improve cutting performance, combines the addition of P and La+Ce elements to refine the grains, and further improves the dispersion distribution of the grain boundary phase, so that the obtained copper alloy is an alloy material with β phase as the matrix, α phase as the grain boundary phase and dispersed Bi particles, and the final obtained material has both high strength and good cutting performance, does not contain harmful Pb elements, and is environmentally friendly. The copper alloy of the present invention meets the requirements of high-precision turning, solves the problem of brittle cracking of the material after adding bismuth elements, and ensures that the mechanical properties of the material meet the use conditions. The tensile strength of the copper alloy is 750-1100MPa, the yield strength is 650-1000MPa, the axial and circumferential residual stress values ​​are ≤100MPa, and the cutting index is ≥70%. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0028] Figure 1 This is a metallographic microscope photo of the finished rod of Example 1 of the present invention magnified 500 times, in which the white color is the α phase, which is distributed in the grain boundaries of the matrix β phase;

[0029] Figure 2 This is a metallographic microscope photo of the finished rod of Comparative Example 1 of the present invention magnified 500 times;

[0030] Figure 3 This is a metallographic microscope photo of the Bi distribution of the finished rod of Example 1 of the present invention, magnified 500 times, in which the black particles are Bi particles;

[0031] Figure 4 This is a metallographic microscope photograph of Bi distribution of the finished rod of Comparative Example 1 of the present invention, magnified 500 times, wherein the black particles are Bi particles. DETAILED DESCRIPTION

[0032] The terms used herein are only for describing specific embodiments and are not intended to limit the present invention. Unless the context otherwise clearly indicates the opposite, the singular form used herein is also intended to include the plural form. It should also be understood that the term "comprising" does not specifically refer to a certain characteristic, field, integer, step, action, element and / or component, but excludes the existence or addition of other characteristics, fields, integers, steps, actions, elements, components and / or groups.

[0033] If a part is described as being "on" another part, it may be directly on the other part or there may be other parts therebetween. When a part is described as being "directly on" another part, there may be no other parts therebetween.

[0034] Although not otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those commonly understood by those skilled in the art. Terms with definitions in dictionaries should be interpreted as having the same meaning as those disclosed in the relevant technical literature and this article, and should not be interpreted in an idealized or overly formal sense.

[0035] The high-strength free-cutting copper alloy and the preparation method thereof of the present invention are described below in conjunction with the accompanying drawings. However, the present invention can be implemented in various different ways and is not limited to the embodiments described herein.

[0036] According to an embodiment of the present invention, the high-strength free-cutting copper alloy components include, by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; Pb < 0.01%; the balance is Zn and other inevitable impurities; the phase structure of the copper alloy includes a matrix β phase, an α phase distributed at the β phase grain boundary, and Bi particles distributed at the grain boundary, the β phase accounts for 75-95%, the average size of the β phase grains is < 100 μm, the α phase accounts for 5-20%, the average size of the α phase grains is < 20 μm, the average size of the Bi particles is < 15 μm, and the number of Bi particles distributed is > 8000 / mm 2 .

[0037] According to an embodiment of the present invention, the high-strength free-cutting copper alloy components may include, by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; P: 0.05-0.2%; Pb < 0.01%; the remainder is Zn and other inevitable impurities; the phase structure of the copper alloy includes a matrix β phase, an α phase distributed at the β phase grain boundary, and Bi particles distributed at the grain boundary, the β phase accounts for 75-95%, the average size of the β phase grains is < 100 μm, the α phase accounts for 5-20%, the average size of the α phase grains is < 20 μm, the average size of the Bi particles is < 15 μm, and the number of Bi particles distributed is > 8000 / mm 2 .

[0038] According to an embodiment of the present invention, the high-strength free-cutting copper alloy components may include, by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; P: 0.05-0.2%; La+Ce: 0.03-0.15%; Pb<0.01%; the remainder is Zn and other inevitable impurities; the phase structure of the copper alloy includes a matrix β phase, an α phase distributed at the β phase grain boundary, and Bi particles distributed at the grain boundary, the β phase accounts for 75-95%, the average size of the β phase grains is <100μm, the α phase accounts for 5-20%, the average size of the α phase grains is <20μm, the average size of the Bi particles is <15μm, and the number of Bi particles distributed is >8000 / mm 2 .

[0039] According to an embodiment of the present invention, the high-strength free-cutting copper alloy may include the following components by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; P: 0.05-0.2%; La+Ce: 0.03-0.15%; Pb<0.01%; the remainder is Zn and other inevitable impurities.

[0040] First, the reasons for limiting the copper alloy composition will be described.

[0041] The content of the main alloy element Cu is controlled at 65-70%. The lower limit of 65% ensures that the material has good plastic processing performance at room temperature. If the Cu content is further reduced, although the high-temperature processing plasticity of the material can be further increased, the cold deformation plasticity of the material is extremely low at room temperature, and effective stretching and straightening cannot be performed. Controlling the upper limit of 70% can control the industrial production cost on the one hand, and ensure that the material has good hot deformation performance on the other hand. If the Cu content is further increased, the extrusion deformation plasticity of the material is greatly reduced, so the required extrusion temperature is increased. High temperature conditions are not conducive to the good cutting effect of the Bi element, and will promote the brittle cracking of the material.

[0042] The addition of Al, Mn and Fe elements in the alloy should not be too high. If excessive Al is added, it will promote the formation of γ phase. Although the γ phase will further increase the hardness of the material, it will drastically reduce the plasticity. If excessive Mn is added, the viscosity of the melt will increase significantly during the smelting process, which is not conducive to uniform flow, and the casting performance and quality of the material cannot meet the use requirements. If excessive Fe is added, a large amount of Fe-rich phase will be formed, and the cutting performance and plasticity of the material will be greatly reduced.

[0043] The purpose of adding Bi to the alloy is to replace the conventional Pb element to ensure that the material has good cutting performance. Bi is distributed in the grain boundary in the form of particles or films to achieve the effect of easy chip breaking. If the Bi element content is added excessively, the Bi element aggregation in the film morphology will increase, and the cutting performance will be difficult to further improve. Instead, the tendency of brittle cracking during the material casting and processing process will increase significantly.

[0044] The addition of P element in the alloy is mainly to improve the fluidity of the melt during the smelting process and reduce the poor fluidity problem caused by the viscosity of the melt due to the addition of Mn element. At the same time, trace P element forms Cu3P phase with Cu matrix, which promotes the cutting performance of the material to a certain extent. Similarly, the addition of P element has a certain inhibitory effect on the aggregation of Bi element, improves the morphology and size control of Bi particles, reduces the distribution and aggregation of Bi element in thin film morphology, thereby improving the cutting performance of the material and reducing the risk of brittle cracking under hot and cold processing. If the amount of P element added is too low, the improvement effect may not be obvious. If the amount of P element added is too high, it may cause serious burning loss and may also have a counterproductive effect.

[0045] The addition of La and Ce elements in the alloy can further improve the comprehensive performance of the material. On the one hand, it can play a role in refining the grains, improve the granular dispersion distribution of Bi particles, and improve the cutting performance; on the other hand, it can improve the uniformity of the cast grains, thereby ensuring that the material obtains uniform and stable mechanical properties and organizational properties. After grain refinement, the strength and plasticity of the material can be further improved; the uniform mechanical properties can effectively control the residual stress distribution formed during the material processing process, and improve the stretching and straightening effects of the finished product. If the amount of La and Ce elements added is too high, the cost may be high and it may also have a counterproductive effect. If the amount of La and Ce elements added is too low, the improvement effect may not be obvious.

[0046] The balance is Zn element and inevitable impurities. Zn element is a basic component element of brass alloy, and forms an alloy matrix together with Cu element. The content of impurity elements is low and will not affect the effect of the present invention.

[0047] Then the influence of the phase composition of copper alloys is explained.

[0048] The phase structure of the copper alloy includes a matrix β phase, an α phase distributed in the β phase grain boundary, and Bi particles distributed in the grain boundary, wherein the β phase accounts for 75-95%, the average size of the β phase grains is less than 100 μm, the α phase accounts for 5-20%, the average size of the α phase grains is less than 20 μm, the average size of the Bi particles is less than 15 μm, and the number of Bi particles distributed is greater than 8000 / mm 2 The proportion and size of the phase composition strictly affect the strength and cutting performance of the material, while the composition and distribution of the matrix phase and grain boundary phase also affect the brittle fracture.

[0049] Preferably, the average size of the β-phase grains is 5 to 25 μm, the average size of the α-phase grains is 1 to 10 μm, the average size of the Bi particles is 0.5 to 5 μm, and the number of Bi particles distributed is 8,000 to 20,000 per mm 2 .

[0050] The phase structure of the high-strength free-cutting copper alloy according to an embodiment of the present invention may further include a Cu3P phase formed by a P element and a Cu matrix.

[0051] In the high-strength free-cutting copper alloy according to an embodiment of the present invention, the Bi particles distributed in the grain boundaries are in the form of particles or films.

[0052] The characteristics of copper alloys will be described below.

[0053] The copper alloy of the present invention is used in industrial piping components, appliances in contact with liquids or gases, pressure vessels and joints, automotive parts or electrical product parts; it is particularly suitable for use in gear rings, turbines, gears, and bushing shafts. To this end, the copper alloy has a tensile strength of 750 to 1100 MPa, a yield strength of 650 to 1000 MPa, axial and circumferential residual stress values ​​of ≤100 MPa, and a cutting index of ≥70%. The material has both high strength and good cutting performance.

[0054] The preparation method of copper alloy is given.

[0055] According to an embodiment of the present invention, a method for preparing a high-strength free-cutting copper alloy comprises the following steps: smelting → casting → extrusion → primary annealing → stretching → secondary annealing; batching and smelting according to the component requirements; then the smelted copper liquid flows into the casting equipment for casting to produce ingots, then the ingots are heated and extruded, the extruded billet is first annealed, the annealed billet is stretched, and after the finished product is stretched, a secondary low-temperature annealing is performed to obtain the copper alloy. Specifically, the copper alloy components may include, by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; Pb < 0.01%; the remainder is Zn and other inevitable impurities.

[0056] Specifically, the copper alloy may further include P: 0.05-0.2%; or P: 0.05-0.2% and La+Ce: 0.03-0.15%. The requirements for the alloy composition have been stated above, so the description is omitted here.

[0057] First, in the smelting process, the raw materials or recycled materials are added to the medium frequency furnace in turn according to the composition requirements and heated up. The smelting temperature is controlled at 950-1200℃. The upper limit of the temperature is controlled at 1200℃ to avoid serious burning of elements such as Al, Zn, and P. Since Cu and Al release a lot of heat during the fusion process, if the temperature is set too high, the exothermic reaction will be more intense, causing the local temperature of the molten pool to be higher, resulting in intense volatilization of Zn elements and serious burning of P elements.

[0058] Secondly, in the casting process, semi-continuous casting is adopted, the temperature of the molten copper entering the casting equipment is controlled to be 1120-1200℃, the stable casting speed is 3.0-5.0m / h, cooling and electromagnetic stirring are performed, and the average cooling speed of the ingot after leaving the crystallizer is controlled to be less than 15℃ / min. The casting is performed to obtain 100-300mm Ф ingots and is completed according to the requirements.

[0059] The temperature of molten copper flowing into the casting equipment is controlled to be no less than 1120℃ to ensure good melt fluidity and uniform melt distribution during solidification. The temperature of molten copper flowing into the crystallizer is controlled to be no more than 1200℃ to avoid the formation of shrinkage, shrinkage holes and other casting defects.

[0060] Control the casting speed within the range of 3.0-5.0m / h. If the casting speed is too slow, it is easy to cause the solidification liquid point to be too high, increase the friction between the ingot and the crystallizer, and the surface quality of the ingot is difficult to meet the use requirements, which is not conducive to ensuring the quality of the subsequent extrusion process. If the casting speed is too fast, on the one hand, the solidification and cooling effect of the material is reduced. Due to the characteristics of the material, it is very easy to have lateral expansion stress cracks. If the casting speed is further increased, insufficient cooling will occur and "holes" will occur.

[0061] The cooling combined with electromagnetic stirring process is used to improve the size and distribution of β-phase grains and Bi particles in the ingot. Specifically, the casting is carried out in a crystallizer and cooled by cooling water. Cooling water inlet temperature: 5-25°C; cooling water outlet temperature: 10-40°C; secondary cooling is eliminated, and an electromagnetic stirring process is used, with a frequency of 10-50Hz and a current of 50-150A, to control the average cooling rate of the ingot after it leaves the crystallizer, effectively controlling the average size of β-phase grains to <100μm, the average size of Bi particles to less than 15μm, and the number of Bi particles distributed to >8000 / mm 2 . By controlling the size of the matrix β phase to be small and evenly distributed, the Bi particles distributed in the grain boundaries can be better guaranteed to be more dispersed. At the same time, the electromagnetic stirring process promotes the refinement of Bi particles to avoid aggregation and growth, thereby improving the subsequent extrusion quality and the cutting performance of the product. If Bi aggregates and distributes in a large area of ​​film, the risk of extrusion cracking will increase. At the same time, if the number of Bi particles per unit area is too small, the cutting performance of the material cannot meet the use requirements. The average cooling rate of the ingot after it leaves the crystallizer is less than 15℃ / min to avoid stress cracking of the ingot caused by excessive cooling.

[0062] Next, the ingot is heated and extruded, and the ingot is placed in a heating furnace for heat treatment. The extrusion heating temperature is 450-650°C, and the heating and heat preservation time is 20-60 minutes. In the extrusion process, the upper limit of the extrusion temperature is controlled to 650°C, and the heating and heat preservation time is controlled not to exceed 60 minutes. The purpose is to avoid the fusion and aggregation of Bi due to excessively high temperature or too long high-temperature heat preservation time, thereby increasing the risk of extrusion thermal cracking. The lower limit of the temperature is controlled to 450°C and the heating and heat preservation time is controlled to be not less than 20 minutes, in order to ensure that the ingot is fully heated and the high-temperature plasticity meets the extrusion conditions required by the present invention.

[0063] The extrusion ratio is controlled at 100 to 400:1. If the extrusion ratio is too small, the thermal deformation of the material is insufficient, the cast structure and coarse grains are retained, and the extrusion plasticity and strength cannot meet the processing and use conditions. If the extrusion ratio is too large, the heating temperature required for the ingot is higher, and the heating temperature needs to exceed the upper limit requirement of the present invention. If the heating temperature is not increased, the force required for ingot extrusion increases significantly, and transverse periodic cracks are prone to appear on the surface of the extruded billet.

[0064] Next, the extruded billet is annealed, that is, heat treatment annealing. The ingot is placed in an annealing furnace for heat treatment. The annealing holding temperature is 400-550℃, and the holding time is 0.5-8h. After annealing, the billet is pickled. Under this temperature range, part of the β phase in the material matrix can be precipitated and transformed into the α phase. The precipitated α phase is distributed on the β phase grain boundary. The α phase is a soft and tough phase, which can effectively block the expansion of stress cracks. At the same time, it also increases the plasticity of the material during processing and deformation at room temperature, which is beneficial to the subsequent stretching processing and provides sufficient processing and deformation space, so as to obtain higher strength. The heat treatment temperature of this process should not be too high. If the temperature is too high, Bi will fuse and aggregate, the number of Bi particles distributed per unit area will be greatly reduced, and the cutting performance of the material will be greatly reduced.

[0065] Next, the finished product of the primary annealing is stretched, and the annealed blank is stretched to a finished product, and the stretching processing rate is controlled at 2 to 10%. The mechanical properties of the material are further improved through stretching hardening. Based on the material characteristics, the processing rate should not be too high to avoid tensile deformation and cracking.

[0066] Next, the finished stretched product is subjected to a low-temperature secondary annealing process. The finished stretched rod is subjected to a low-temperature annealing treatment. The holding temperature is 250-400°C and the holding time is 1-12 hours. The purpose is to eliminate the residual stress of the finished rod, slightly increase the plasticity of the rod, and achieve axial and circumferential residual stress values ​​within 100MPa, which is beneficial to the subsequent straightening process. At the same time, when the rod is used in downstream industries for mechanical turning, controlling lower residual stress is beneficial to ensuring the dimensional accuracy of the turned parts, avoiding deformation caused by stress release of the turned parts after completion, thereby changing the dimensional tolerance. The annealing temperature should not be too high. If the stretched blank of the present invention is subjected to annealing heat treatment above 400°C, the Bi morphology and distribution inside the material will deteriorate. If the annealing temperature is low, the stress elimination is not thorough.

[0067] After the secondary annealing process, the finished product can be straightened according to actual needs, and after passing the inspection, it can be packaged and stored to obtain the bar material.

[0068] Thus, the properties of the finished product of the present invention are obtained: tensile strength: 750-1100MPa, yield strength: 650-1000MPa, axial and circumferential residual stress values ​​≤100MPa, average size of β phase grains: 5-25μm; β phase ratio: 75-95%; average size of α phase grains: 1-10μm; α phase ratio: 5-20%; average size of Bi particles: 0.5-5μm; Bi distribution: 8000-20000 / mm 2 ; Cutting index ≥ 70%, the material has both high strength and good cutting performance.

[0069] Example 1

[0070] The preparation steps of high strength free-cutting copper alloy are as follows:

[0071] 1) Melting: According to the composition requirements, the raw materials or recycled materials are added into the melting equipment in turn and heated up. The melting temperature is 1120℃.

[0072] 2) Casting: semi-continuous casting is used to produce ingots. The temperature of molten copper when it flows into the crystallizer is 1140℃; stable casting speed is 4m / h; cooling water inlet temperature is 5~20℃; cooling water outlet temperature is 10~35℃; secondary cooling is cancelled, and electromagnetic stirring process is adopted, frequency is 35Hz, current is 60A, and the average cooling speed of the ingot after it leaves the crystallizer is controlled to be less than 15℃ / min; Ф200mm ingot is obtained by casting, and sawing is completed.

[0073] 3) Extrusion: The ingot is placed in a heating device for heating, the extrusion heating temperature is 580°C, the heating and holding time is 40 min, the extrusion ratio is 260:1, and a 12.4 mm Φ billet is obtained by extrusion.

[0074] 4) Primary annealing: Place the extruded billet in the annealing equipment for heat treatment. Annealing holding temperature: 480°C; holding time: 3h; after annealing, the billet is pickled.

[0075] 5) Stretching: The annealed blank is stretched to obtain a finished product with a stretching processing rate of 6.3% to obtain a 12mm Ø finished product bar.

[0076] 6) Secondary annealing: The finished product is subjected to low-temperature annealing after stretching. Annealing temperature: 340°C; holding time: 5h.

[0077] 7) Straightening: Straighten the finished bars and pack them for storage after passing the inspection.

[0078] Example 2

[0079] The preparation steps of high strength free-cutting copper alloy are as follows:

[0080] 1) Melting: According to the composition requirements, the raw materials or recycled materials are added into the melting equipment in turn and heated up. The melting temperature is 1050℃.

[0081] 2) Casting: semi-continuous casting is used to produce ingots. The temperature of molten copper when it flows into the crystallizer is 1120℃; stable casting speed is 4m / h; cooling water inlet temperature is 5~20℃; cooling water outlet temperature is 10~35℃; secondary cooling is cancelled, and electromagnetic stirring process is adopted, frequency: 35Hz, current: 80A, and the average cooling speed of the ingot after it leaves the crystallizer is controlled to be less than 15℃ / min; Ф200mm ingot is obtained by casting, and sawing is completed.

[0082] 3) Extrusion: The ingot is placed in a heating device for heating, the extrusion heating temperature is 530°C, the heating and holding time is 50 min, the extrusion ratio is 260:1, and a 12.4 mm Φ billet is obtained by extrusion.

[0083] 4) Primary annealing: Place the extruded billet in the annealing equipment for heat treatment. Annealing holding temperature: 430°C; holding time: 6h; after annealing, the billet is pickled.

[0084] 5) Stretching: The annealed blank is stretched to obtain a finished product with a stretching processing rate of 6.3% to obtain a 12mm Ø finished product bar.

[0085] 6) Secondary annealing: The finished product is subjected to low-temperature annealing after stretching. Annealing temperature: 300°C; holding time: 6h.

[0086] 7) Straightening: Straighten the finished bars and pack them for storage after passing the inspection.

[0087] Example 3

[0088] The preparation steps of high strength free-cutting copper alloy are as follows:

[0089] 1) Melting: According to the composition requirements, the raw materials or recycled materials are added into the melting equipment in turn and heated up. The melting temperature is 1160℃.

[0090] 2) Casting: semi-continuous casting is used to produce ingots. The temperature of molten copper when it flows into the crystallizer is 1170℃; stable casting speed is 3m / h; cooling water inlet temperature is 5~15℃; cooling water outlet temperature is 10~30℃; secondary cooling is cancelled, and electromagnetic stirring process is adopted, frequency is 35Hz, current is 120A, and the average cooling speed of the ingot after it leaves the crystallizer is controlled to be less than 15℃ / min; Ф250mm ingot is obtained by casting, and sawing is completed.

[0091] 3) Extrusion: The ingot is placed in a heating device for heating, the extrusion heating temperature is 600°C, the heating and holding time is 40 min, the extrusion ratio is 295:1, and a 10.3 mm Ø billet is obtained by extrusion.

[0092] 4) Primary annealing: Place the extruded billet in the annealing equipment for heat treatment. Annealing holding temperature: 490°C; holding time: 4h; after annealing, the billet is pickled.

[0093] 5) Stretching: The annealed blank is stretched to obtain a finished product with a stretching processing rate of 5.7% to obtain a 10 mm Ø finished product bar.

[0094] 6) Secondary annealing: The finished product is subjected to low-temperature annealing after stretching. Annealing temperature: 320°C; holding time: 4h.

[0095] 7) Straightening: Straighten the finished bars and pack them for storage after passing the inspection.

[0096] Example 4

[0097] The preparation steps of high strength free-cutting copper alloy are as follows:

[0098] 1) Melting: According to the composition requirements, the raw materials or recycled materials are added into the melting equipment in turn and heated up. The melting temperature is 1170℃.

[0099] 2) Casting: semi-continuous casting is used to produce ingots. The temperature of molten copper when it flows into the crystallizer is 1190℃; stable casting speed is 3.5m / h; cooling water inlet temperature is 5~15℃; cooling water outlet temperature is 10~30℃; secondary cooling is cancelled, and electromagnetic stirring process is adopted, frequency: 45Hz, current: 130A, and the average cooling speed of the ingot after it leaves the crystallizer is controlled to be less than 15℃ / min; Ф250mm ingot is obtained by casting, and sawing is completed.

[0100] 3) Extrusion: The ingot is placed in a heating device for heating, the extrusion heating temperature is 620°C, the heating and holding time is 45 min, the extrusion ratio is 295:1, and a 10.3 mm Ø billet is obtained by extrusion.

[0101] 4) Primary annealing: Place the extruded billet in the annealing equipment for heat treatment. Annealing holding temperature: 520°C; holding time: 4h; after annealing, the billet is pickled.

[0102] 5) Stretching: The annealed blank is stretched to obtain a finished product with a stretching processing rate of 5.7% to obtain a 10 mm Ø finished product bar.

[0103] 6) Secondary annealing: The finished product is subjected to low-temperature annealing after stretching. Annealing temperature: 360°C; holding time: 3h.

[0104] 7) Straightening: Straighten the finished bars and pack them for storage after passing the inspection.

[0105] Comparative Example 1

[0106] 1) Melting: According to the composition requirements, the raw materials or recycled materials are added into the melting equipment in turn and heated up. The melting temperature is 1200℃.

[0107] 2) Casting: semi-continuous casting is used to produce ingots. The temperature of molten copper when it flows into the crystallizer is 1140℃; the stable casting speed is 4m / h; the ingot with a diameter of 150mm is obtained by casting and sawing is completed.

[0108] 3) Extrusion: The ingot is placed in a heating device for heating, the extrusion heating temperature is 600°C, the heating and holding time is 80 min, the extrusion ratio is 76:1, and a 12.2 mm Ø blank is obtained by double-hole extrusion.

[0109] 4) Finished product drawing: The annealed billet is subjected to finished product drawing, and the drawing process obtains a 12mm finished product specification bar.

[0110] 5) Finished product annealing: The finished product is stretched and subjected to low-temperature annealing. Annealing temperature: 400°C; holding time: 6h.

[0111] 6) Straightening: Straighten the finished bars and pack them for storage after passing the inspection.

[0112] Comparative Example 2

[0113] 1) Melting: According to the composition requirements, the raw materials or recycled materials are added into the melting equipment in turn and heated up. The melting temperature is 1250℃.

[0114] 2) Casting: semi-continuous casting is used to produce ingots. The temperature of molten copper when it flows into the crystallizer is 1200℃; the stable casting speed is 4.5m / h; the ingot with a diameter of 200mm is obtained by casting and sawing is completed.

[0115] 3) Extrusion: The ingot is placed in a heating device for heating, the extrusion heating temperature is 620°C, the heating and holding time is 70 min, the extrusion ratio is 132:1, and a 12.3 mm Ø blank is obtained by double-hole extrusion.

[0116] 4) Finished product drawing: The annealed billet is subjected to finished product drawing, and the drawing process obtains a 12mm finished product specification bar.

[0117] 5) Finished product annealing: The finished product is stretched and subjected to low-temperature annealing. Annealing temperature: 300°C; holding time: 5h.

[0118] 6) Straightening: Straighten the finished bars and pack them for storage after passing the inspection.

[0119] The present invention provides 4 embodiments and 2 comparative examples. The specific components are shown in Table 1. The testing method standards of the materials obtained in each embodiment and comparative example are as follows:

[0120] 1) Tensile and yield strength test: GB / T 228.1-2010 Tensile tests on metallic materials Part 1: Room temperature tensile test method.

[0121] 2) Metallographic microscopic test: YS / T 449-2002 Microstructure inspection method for copper and copper alloy castings and processed products.

[0122] 3) Cutting index test: The cutting performance test method in Appendix B of YS-T 647-2007 "Copper-Zinc-Bismuth-Tellurium Alloy Rod" was used for evaluation, and the cutting index of C36000 (HPb63-3) was set to 100%.

[0123] 4) Residual stress test: ASTM E915-21 Standard practice for calibration and verification of X-ray diffractometers for residual stress measurements.

[0124] The specific mechanical properties and cutting index of the materials are shown in Table 2, and the specific microstructure properties of the materials are shown in Table 3. The specific metallographic structure photos of the bars are shown in Figure 1-4 .

[0125] Table 1. Examples and Comparative Examples Composition Unit: wt%

[0126] Cu Al Mn Fe Bi P La+Ce Zn Example 1 67.56 5.22 2.57 2.49 0.78 0.09 0.10 Remain Example 2 65.75 4.29 2.23 2.15 0.96 0.12 0.12 Remain Example 3 68.23 5.74 2.46 2.34 0.67 0.08 0.08 Remain Example 4 69.04 6.48 2.74 2.88 0.50 0.06 0.05 Remain Comparative Example 1 67.67 5.20 2.64 2.42 0.75 / / Remain Comparative Example 2 65.59 5.16 3.06 3.27 / / / Remain

[0127] Table 2. Mechanical properties and cutting index of finished rods of Examples and Comparative Examples

[0128]

[0129] Table 3. Microstructure and properties of finished rods of examples and comparative examples

[0130]

[0131]

[0132] Figure 1 The middle white is the α phase, which is distributed in the grain boundaries of the matrix β phase; Figure 2 There is basically no (white) α phase precipitation, and the overall plasticity of the material is not as good as that of the embodiment; Figure 3 The black particles are Bi particles, which are small in size and have a large number per unit area; Figure 4 The black particles are Bi particles, which are large in size and have a small number per unit area.

[0133] Comparative Example 1 adopts a conventional production process, and elements such as P, La, and Ce are not added. At the same time, the casting process adopts a conventional method. Therefore, if the ingot is subsequently extruded using a high extrusion ratio method, hot brittle cracking is very likely to occur, and a small extrusion ratio extrusion method must be used, resulting in insufficient grain crushing of the finished product, larger β phase size and Bi particle size, and significantly lower Bi distribution amount than the embodiment, which indirectly causes the cutting performance of Comparative Example 1 to be inferior to that of the embodiment.

[0134] At the same time, after extrusion, the comparative example 1 is directly stretched to the finished product by conventional process without intermediate annealing. Therefore, a large amount of β phase is retained in the extruded structure of the comparative example 1, and the overall plasticity of the material is extremely low. The subsequent drawing processing rate should not be too large. At the same time, in order to ensure a good straightening effect, the temperature required for annealing the finished product is higher, and the material softening is more serious. The particle size and morphology of the finished product Bi of the comparative example 1 are not as good as those of the embodiment, which indirectly increases the brittleness of the material and reduces the strength. The above factors lead to the overall strength performance of the finished product of the comparative example 1 not being as good as that of the embodiment.

[0135] Comparative Example 2 is a common aluminum brass product. Since it does not contain easy-cutting elements, the material cutting performance is not as good as that of the embodiment. At the same time, it is produced by conventional processes, and basically no α phase is precipitated in the material matrix. After annealing and straightening of the finished product, the residual stress value is large, which is much higher than that of the embodiment. Therefore, after high-speed turning, the precision and dimensional tolerance control level of the machined parts of the product of Comparative Example 2 are not as good as those of the embodiment.

[0136] The present invention can be implemented in various ways and is not limited to the above-mentioned embodiments and / or examples. A person skilled in the art can understand that the present invention can be implemented in other specific ways without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above-mentioned embodiments and / or examples are exemplary and are not intended to limit the present invention.

Claims

1. A high-strength free-cutting copper alloy, characterized in that: The copper alloy components include, by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; Pb < 0.01%; the balance is Zn and other inevitable impurities; The phase structure of the copper alloy includes a matrix β phase, an α phase distributed at the β phase grain boundary, and Bi particles distributed at the grain boundary, the β phase accounts for 75-95%, the average size of the β phase grains is less than 100 μm, the α phase accounts for 5-20%, the average size of the α phase grains is less than 20 μm, the average size of the Bi particles is less than 15 μm, and the number of Bi particles distributed is greater than 8000 / mm 2 .

2. The high-strength free-cutting copper alloy according to claim 1, characterized in that: The Bi particles are in the form of particles or thin films.

3. The high-strength free-cutting copper alloy according to claim 2, characterized in that: The average size of the β-phase grains is 5 to 25 μm, the average size of the α-phase grains is 1 to 10 μm, the average size of the Bi particles is 0.5 to 5 μm, and the number of Bi particles distributed is 8,000 to 20,000 per mm 2 .

4. The high-strength free-cutting copper alloy according to claim 3, characterized in that: The copper alloy components include, by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; P: 0.05-0.2%; Pb < 0.01%; the remainder is Zn and other inevitable impurities, and the phase structure of the copper alloy also contains Cu3P phase.

5. A high-strength free-cutting copper alloy, characterized in that: The copper alloy components include, by weight percentage: Cu: 65-70%; Al: 4.0-7.0%; Mn: 2.0-3.0%; Fe: 2.0-3.0%; Bi: 0.4-1.0%; P: 0.05-0.2%; La+Ce: 0.03-0.15%; Pb<0.01%; the remainder is Zn and other inevitable impurities.

6. The high-strength free-cutting copper alloy according to claim 5, characterized in that: The phase structure of the copper alloy includes a matrix β phase, an α phase distributed at the β phase grain boundary, and Bi particles distributed at the grain boundary, the β phase accounts for 75-95%, the average size of the β phase grains is less than 100 μm, the α phase accounts for 5-20%, the average size of the α phase grains is less than 20 μm, the average size of the Bi particles is less than 15 μm, and the number of Bi particles distributed is greater than 8000 / mm 2 .

7. The high-strength free-cutting copper alloy according to any one of claims 1 to 6, characterized in that: The copper alloy has a tensile strength of 750-1100 MPa, a yield strength of 650-1000 MPa, axial and circumferential residual stress values ​​of ≤100 MPa, and a cutting index of ≥70%.

8. The high-strength free-cutting copper alloy according to any one of claims 1 to 6, characterized in that: The copper alloy is used for industrial piping members, equipment in contact with liquid or gas, pressure vessels and joints, automobile parts, or electric product parts.

9. The high-strength free-cutting copper alloy according to claim 8, characterized in that: The copper alloy is used in gear rings, turbines, gears, and bushing shafts.

10. A method for preparing a high-strength free-cutting copper alloy, characterized in that: The preparation method is a preparation method of the high-strength free-cutting copper alloy according to any one of claims 1 to 9, comprising the following steps: smelting → casting → extrusion → primary annealing → stretching → secondary annealing; The ingredients are mixed and smelted according to the component requirements; the smelted copper liquid is then flowed into a casting device for casting to produce an ingot, and the ingot is then heated and extruded, the extruded billet is first annealed, the annealed billet is stretched, and the finished product is stretched and then subjected to a secondary low-temperature annealing to obtain the copper alloy; Preferably, the smelting temperature is controlled at 950-1200°C; Preferably, the casting step adopts a semi-continuous casting method, controls the temperature of the molten copper entering the casting equipment to be 1120-1200°C, the stable casting speed is 3.0-5.0 m / h, cools and performs electromagnetic stirring, and controls the average cooling speed of the ingot after it leaves the crystallizer to be less than 15°C / min; Preferably, the extrusion heating temperature is 450-650°C, the heating and heat preservation time is 20-60min, and the extrusion ratio is 100-400:1; Preferably, the primary annealing temperature is 400-550°C, and the holding time is 0.5-8h; Preferably, the stretching processing rate is 2 to 10%; Preferably, the secondary annealing holding temperature is 250-400° C., and the holding time is 1-12 hours; More preferably, the secondary annealing holding temperature is 280-360°C.