Thick steel plate for high-fatigue belleville spring and manufacturing method of thick steel plate
Through the full process high-purity-low segregation control technology and narrow component design, combined with low segregation continuous casting and high-temperature normalization treatment, the problems of segregation and plate shape difference in the production of disc spring steel plates are solved, and high-quality and low segregation are achieved The production of disc spring steel plates with a degree of improvement, which improves the production efficiency and fatigue life of disc springs.
Patent Information
- Application Number
- CN202410888817.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-04
AI Technical Summary
In the prior art, there are problems such as serious segregation, poor plate shape, low material yield, high energy consumption in the production process, and unstable quality in particular, steel plates with large width and thickness are difficult to meet high strength. and high toughness requirements.
Using the full process high-purity-low segregation control technology, the C, Si, Mn, and Cr element content is controlled through narrow components, and combined with the medium-frequency furnace and vacuum degassing process, low segregation continuous casting and high-temperature normalization treatment are carried out, and combined with rolling The process produces 15-40mm thick disc spring steel plate with low segregation resolution and flat plate shape.
The low segregation, flatness and high quality of the steel plate are achieved, the dimensional accuracy and production efficiency of the disc spring are improved, the production cost is reduced, and the fatigue life of the disc spring is extended.
Smart Images

Figure CN118880167A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metallurgy, and in particular to a spring steel plate and a manufacturing method thereof. Background Art
[0002] Disc springs are conical disc-shaped in appearance. Compared with traditional springs, they have shorter strokes, smaller space requirements, easier assembly and maintenance, and higher economic applicability. They are widely used in various industrial engineering fields such as brakes, buffer shock absorbers, bearing preload safety overload devices, clamping devices, etc. They are also used in some special fields such as the nuclear industry, aerospace industry, and military industry. Spring manufacturers mainly purchase disc spring steel plates, and then stamp or machine the steel plates into hollow annular spring parts according to their own processes and needs, and then produce disc spring parts through processes such as heat treatment and fine milling.
[0003] At present, standard disc spring parts (thickness <15mm) on the market are stamped into rings with steel strips or flat steel, and then further processed. Another type is medium and large disc spring parts with a thickness of more than 15mm, which use die-cast blanks, which are heated and forged into round steels of different sizes for multiple times. After the round steel is annealed, it is stamped into rings with a large stamping machine. Due to the variety of inner and outer diameter sizes of disc spring parts, the disc spring steel used as raw materials has many specifications and small quantities, resulting in a low yield rate of raw materials. In addition, the production process control of the blanks is unstable, the dimensional accuracy of the forged round steel fluctuates greatly, and the utilization rate of stamping and subsequent finishing is low. At present, the maximum deviation of the inner and outer diameter dimensions of medium and large disc spring ring parts after stamping in forged round steel production is 10mm, the thickness allowance is 5mm, the disc spring fine milling processing is large, time-consuming, labor-intensive, and costly. In addition, disc springs have high requirements for fatigue life, high dimensional accuracy, and high requirements for material purity and decarburization layer. For blanks produced by medium-frequency furnaces or small ingots, the material purity control fluctuates greatly, and the quality of disc spring ring parts is unstable.
[0004] Chinese patent document CN111349846A discloses a method for producing high-strength and high-toughness spring flat steel and patent document CN109161803A discloses a 1550MPa-grade spring flat steel and its production method. The width of the spring flat steel produced by the above methods is ≤150mm, while the outer diameter of large-size disc springs is usually 300-1000mm, which does not meet the use requirements. The continuous rolling of thick steel plates has a high utilization rate of size specifications, but the spring steel plates belong to medium-high carbon alloy steel plates, and the center segregation and center looseness of the slabs are serious, resulting in a large difference in the heat-treated surface and core structure of the spring steel, and a low service life. Moreover, when the width of the steel plate is greater than 2000mm, the spring steel plate has large internal stress after rolling, severe buckling, and high strength after rolling, making the disc spring difficult to form.
[0005] At present, domestic steel enterprises rarely produce low segregation spring steel plates with width > 1600mm and thickness > 15mm. In view of the above situation, it is expected to obtain a stable, efficient and high-quality thick steel plate for disc springs. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the current shortcomings of severe segregation and poor plate shape of wide and thick steel plates, optimize the element composition, realize the production of low-segregation continuous casting slabs, and use medium and thick plate rolling mills to produce 15-40mm thick disc spring steel plates with low segregation, flat plate shape and stable quality, replacing the high production energy consumption and low cost-effective die casting-forging process to produce spring steel plates.
[0007] The technical solution adopted by the present invention to solve the above problems is: a thick steel plate for high fatigue disc spring and its manufacturing method, the steel plate production thickness is 15-40mm, the steel plate segregation band width is ≤80 microns, the straightness is ≤3mm / m, the thickness difference between the same plate is less than 0.3mm, and the hardness is ≤252HBW. The chemical composition of the steel plate is calculated by mass percentage, C: 0.48% to 0.52%, Si: 0.15% to 0.27%, Mn: 0.70% to 0.90%, Cr: 0.90% to 1.10%, V: 0.10 to 0.15%, P: ≤0.015%, S: ≤0.003%, H≤0.0001%, N+H+O≤0.0065%, and the balance is Fe and unavoidable impurity elements.
[0008] The component design of the present invention is specifically described below:
[0009] C and Mn are both elements that can improve the strength and hardness of steel plates, but excessive C and Mn contents are prone to segregation and lead to uneven structure. The present invention controls the narrow composition, with the contents of C: 0.48% to 0.52% and Mn: 0.70% to 0.90%.
[0010] Si: It is a deoxidizing element in steel, which improves the strength and hardness of steel by solid solution strengthening. When the Si content is lower than 0.10%, the deoxidation effect is poor. When the Si content is higher, the silicate inclusions in the molten steel increase and the purity decreases. The Si content of the present invention is controlled to be 0.15-0.27%.
[0011] Cr: It is the main element for improving the strength and hardness of spring steel. However, excessive Cr will reduce the toughness of the material and bring in more Ti, which is easy to produce sharp and hard oxides during smelting, affecting the fatigue life of the disc spring. The present invention controls its content to 0.90% to 1.10%.
[0012] V: can disperse and precipitate V (C, N), significantly improving the strength and hardness of steel, but the cost is relatively high. The present invention controls its content to 0.10-0.15%.
[0013] H: harmful gas element. A high H content is prone to produce white spots, which expands microcracks in the steel plate and causes processing cracking. The present invention strictly controls the H content to be no more than 0.00010%.
[0014] O, N: harmful gas elements, high content, easy to produce hard and sharp inclusions, seriously reducing the fatigue life of the spring. The present invention strictly controls the O content to be no higher than 0.0010% and the N content to be no higher than 0.0040% through LF refining and RH vacuum process.
[0015] The present invention provides a method for manufacturing a thick steel plate for a high fatigue disc spring, and the specific process steps are as follows:
[0016] (1) High-purity molten steel smelting: molten iron is sequentially pretreated - converter smelting - LF refining - RH vacuum degassing. After pretreatment, the S content of molten iron is not more than 0.002%. Deep dephosphorization smelting method is adopted during converter steelmaking, and slag is retained to reduce phosphorus reversion. LF adopts high-basicity white slag refining and steel slag mixing technology during steel tapping to effectively reduce the P and S content. In addition, the fluctuation range of Si and Mn alloy elements and the content of harmful elements of P and S are strictly controlled, requiring residual elements Ti: ≤0.003%; Sb: ≤0.003%, Sn: ≤0.005%, As: ≤0.007%, and the argon flow rate is high at the beginning and low at the end to ensure uniform stirring of the molten steel while avoiding secondary oxidation. Increase the high vacuum time during RH vacuum degassing, which is not less than 20 minutes, and the total time is not less than 45 minutes. Guarantee molten steel P: ≤0.015%, S: ≤0.003%, H: ≤0.0001%, O: ≤0.0010%, N: ≤0.0040%.
[0017] (2) Low segregation continuous casting: non-oxidation protection continuous casting, automatic slag detection, low superheat-constant casting speed process. The light reduction in continuous casting is 4-7mm, and the small-large-small distribution method is adopted to reduce the liquid level fluctuation and increase the removal effect of non-metallic inclusions. The cooling rate is controlled in the second cooling section of continuous casting so that the light reduction section acts on the solid phase ratio of the slab in the range of 0.5-0.9 to improve the center segregation of the continuous casting slab. Continuous casting slabs with a thickness of 150mm and a width of 1800-2800mm are produced. The low-multiple quality center segregation of the slab is C0.5, the center looseness is 0.5, and there are no other defects.
[0018] (3) Hydrogen expansion and slow cooling: After the continuous casting slab comes off the line, it enters the slow cooling pit at high temperature to expand hydrogen and slowly cools to below 200°C to promote the diffusion of hydrogen in the slab.
[0019] (4) Rolling: The ingot is heated at high temperature in the furnace to fully dissolve and diffuse the segregated components of the slab, and the heating and insulation temperature is ≥1210℃. After leaving the heating furnace, it is descaled by high-pressure water, and then rolled to optimize the plate shape. The starting rolling temperature is set to be greater than 1050℃, and the first 2-3 passes are rolled with high deformation reduction rate, the maximum pass reduction rate is greater than 25%, and the last pass reduction rate is not more than 10%.
[0020] (5) High temperature normalizing: In order to further reduce the segregation of the steel plate and improve the uniformity of the steel plate structure, high temperature diffusion normalizing is adopted. The temperature is 920±10℃ and the furnace time is 2.5~3.0min / mm.
[0021] (6) Tempering: Tempering heat treatment is carried out in a roller hearth continuous furnace, with a tempering temperature of 740±10℃ and a holding time of 3.5~4.5min / mm. Before entering the tempering furnace, the steel plate needs to be shot blasted to remove the surface oxide scale; after tempering, it needs to be straightened with heat to ensure that the straightness of the steel plate is ≤3mm / m.
[0022] The present invention has the following characteristics or advantages:
[0023] The present invention adopts the full-process high purity-low segregation control technology, through the narrow composition control of C, Si, Mn, Cr, adding an appropriate amount of V, improving the strength of the steel plate of the present invention while reducing the element segregation tendency. The refining-vacuum degassing process can reduce the content of harmful elements such as P, S, O, N, and H. The constant pulling speed-low superheat-precision light pressure reduction process is improved to reduce the center segregation of the slab, ensuring low center segregation C0.5 level, center looseness 0.5 level, and no other defects.
[0024] The present invention adopts the combined technology of high temperature heating of the blank and high temperature normalizing to further improve the center segregation of the steel plate, so as to achieve a segregation bandwidth of the steel plate of no more than 80 μm. In addition, the continuous furnace high temperature tempering process is adopted to achieve stress relief and structural uniformity transformation of the spring thick steel plate, which is convenient for the later disc spring cutting and processing.
[0025] The present invention rolls wide and thick steel plates with high-quality continuous casting slabs and adopts optimized plate shape controlled rolling technology, aiming to produce spring steel plates with high thickness accuracy and flat plate shape, reducing the turning and milling allowances during the processing of disc spring rings, greatly improving the yield rate and reducing production costs.
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] The manufacturing method of the thick steel plate for high fatigue disc springs of the present invention optimizes the component design, realizes the production of low segregation continuous casting slabs, changes the traditional casting plus forging stamping forming medium and large disc spring ring production process, can overcome the technical difficulties of low purity and unstable quality of the traditional process, and greatly improves the dimensional accuracy and production efficiency of the thick steel plate for disc springs. The straightness of the thick steel plate for disc springs produced is ≤3mm / m, the thickness difference is 0.3mm, and the hardness is ≤252HBW. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The near surface structure of disc spring steel is 100×;
[0029] Figure 2 The disc spring steel core structure is 100×, Figure 1 The organization shown is consistent, and the surface and core organizations are uniform. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0031] Embodiment 1
[0032] Production steps of thick steel plates for butterfly springs:
[0033] 1. After the molten iron and clean scrap steel are smelted in a converter to remove harmful elements P, the molten steel is smelted in a LF refining furnace for 45 minutes. After desulfurization and alloy composition adjustment, the molten steel is vacuum degassed for 25 minutes in RH vacuum treatment and refining to further reduce the content of harmful gas elements in the molten steel. The final molten steel composition before continuous casting is C: 0.50%, Si: 0.27%, Mn: 0.83%, P: 0.01%, S: 0.0005%, Cr: 1.0%, V: 0.12%, H: 0.6ppm, O: 12ppm, N: 24ppm, and the remainder is Fe and impurity elements
[0034] 2. Molten steel is continuously cast into slabs with a thickness of 150mm*1900mm by a straight arc continuous casting machine. Non-oxidation protection casting is adopted during continuous casting, the superheat is controlled at 10-20℃, the constant pulling speed is 1.2m / min, and the light pressing technology is adopted. The slab has a low center segregation of C0.5, a center looseness of 0.5, and no center cracks, corner cracks, or triangular cracks. After the continuous casting slab is off the line at high temperature, it is slowly cooled and hydrogen expanded.
[0035] 3. The continuous casting billet is transferred to the 3500mm rolling plant and heated by a walking furnace. The temperature of the continuous casting billet soaking section is 1220℃ and the soaking time is 2 hours. The continuous casting billet rolling temperature is 1050℃. The single pass reduction rate of the first three rolling passes is ≥15%, the maximum reduction rate is 25%, and the last pass reduction rate is 9.8%. Finally, it is rolled into a steel plate with a thickness of 9.75mm, a width of 1900mm, and a length of 19000mm.
[0036] 4. After the hot-rolled steel plate is cooled to room temperature, it enters the roller-hearth continuous furnace for high-temperature normalizing at 920°C. After the normalized steel plate is air-cooled, it is subjected to tempering heat treatment at 740°C and a holding time of 4.0 min / mm. After tempering, the steel plate is air-cooled out of the furnace. After the steel plate is cooled, it is shot blasted for rust removal. The steel plate also needs to be straightened in a straightening machine, and the final straightness of the steel plate is 3mm / m.
[0037] Embodiment 2
[0038] Production steps of thick steel plates for butterfly springs:
[0039] 1. After the molten iron and clean scrap steel are smelted in a converter to remove harmful elements P, the molten steel is smelted in a LF refining furnace for 45 minutes. After desulfurization and alloy composition adjustment, the molten steel is vacuum degassed for 25 minutes in RH vacuum treatment and refining to further reduce the content of harmful gas elements in the molten steel. The final molten steel composition before continuous casting is C: 0.50%, Si: 0.27%, Mn: 0.84%, P: 0.01%, S: 0.0005%, Cr: 1.0%, V: 0.12%, H: 0.5ppm, O: 12ppm, N: 25ppm, and the remainder is Fe and impurity elements
[0040] 2. Molten steel is continuously cast into slabs with a thickness of 150mm*2800mm by a straight arc continuous casting machine. Non-oxidation protection casting is adopted during continuous casting, the superheat is controlled at 10-20℃, the constant pulling speed is 0.5m / min, and the light pressing technology is adopted. The slab has a low center segregation of C0.5, a center looseness of 0.5 level, and no center cracks, corner cracks, or triangular cracks. After the continuous casting slab is off the line at high temperature, it is slowly cooled and hydrogen expanded.
[0041] 3. The continuous casting billet is transferred to the 4300mm rolling plant and heated by a walking furnace. The temperature of the continuous casting billet soaking section is 1250℃ and the soaking time is 2 hours. The continuous casting billet starting rolling temperature is 1050℃, the final rolling temperature is 860℃, the single pass reduction rate of the first 3 passes is ≥15%, the maximum pass reduction rate is 30%, and the last pass reduction rate is 8%. Finally, it is rolled into a steel plate with a thickness of 36mm, a width of 2800mm, and a length of 15000mm.
[0042] 4. After the hot-rolled steel plate is cooled to room temperature, it enters the roller-bottom continuous furnace for normalizing at 920°C. After the normalized steel plate is air-cooled, it is subjected to tempering heat treatment at 740°C and a holding time of 4.0 min / mm. After tempering, the steel plate is air-cooled out of the furnace. After the steel plate is cooled, it is shot blasted for rust removal. The steel plate also needs to be straightened in a straightening machine, and the final straightness of the steel plate is 2 mm / m.
[0043] Table 1 Inclusions (DIN 50602 standard M method) and decarburized layer test results of the example
[0044] hardness Straightness Thickness difference Inclusion Index Embodiment 1 231HBW 3mm / m 0.2mm 3.2 Embodiment 2 220HBW 2mm / m 0.3mm 3.2
[0045] The disc spring rings produced in the above embodiments are sent to customers for processing into disc springs and then subjected to fatigue life tests. The fatigue test of a single disc spring produced in Embodiments 1 and 2 is greater than 2 million times, and the test of a combination of 10 disc springs is ≥ 700,000 times, far exceeding the purchase requirement of 130,000 times. This shows that the disc spring rings produced by the present invention are of excellent quality.
[0046] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.
Claims
1. A thick steel plate for high fatigue butterfly spring, characterized in that: The chemical composition of the steel plate is calculated by mass percentage as follows: C: 0.48%-0.52%, Si: 0.15%-0.27%, Mn: 0.70%-0.90%, Cr: 0.90%-1.10%, V: 0.10-0.15%, P: ≤0.015%, S: ≤0.003%, H: ≤0.0001%, N+H+O: ≤0.0065%, and the remainder is Fe and unavoidable impurity elements.
2. The steel plate according to claim 1, characterized in that: The production thickness of the steel plate is 15-40 mm and the width is 1800-2800 mm.
3. The steel plate according to claim 1, characterized in that: The segregation band width of the steel plate is ≤80 microns, the straightness is ≤3 mm / m, the thickness difference between the same plate is ≤0.3 mm, and the hardness is ≤252 HBW.
4. A method for manufacturing the steel plate according to claim 1, characterized in that: The steps include, 1. High-purity molten steel smelting: the molten iron is sequentially subjected to pretreatment, converter smelting, LF furnace refining, and vacuum degassing. The S content of the molten iron after pretreatment is ≤0.002%. Deep dephosphorization is performed during converter smelting, and slag is retained for tapping to reduce rephosphorization. LF furnace refining uses high-basicity white slag refining and two-thirds of refined slag is taken during tapping to control the increase in P and S content. In addition, the fluctuation of Si and Mn alloy elements is controlled, and the residual elements Ti: ≤0.003%; Sb: ≤0.003%, Sn: ≤0.005%, As: ≤0.007%. The molten steel is stirred with argon gas. The argon gas flow rate in the early stage of smelting is: 300-600L, and the argon gas flow rate in the later stage of smelting is: 100-150L. The high vacuum treatment time is increased during vacuum degassing, and the high vacuum holding time is not less than 20min, and the total time is not less than 45min.
2. Low segregation continuous casting: The whole process is non-oxidation protection continuous casting, automatic slag detection is adopted, low superheat: below 20℃, constant casting speed process, light pressure reduction is implemented in the range of 0.5-0.9 solid phase ratio of continuous casting billet, and the light pressure reduction is 4-7mm; 150mm thick continuous casting slab is produced, the low-multiple mass center segregation of the slab is C0.5 level, the center looseness is 0.5 level, and there are no other defects; 3. Hydrogen expansion and slow cooling: After the continuous casting slab comes off the line, it is put into the slow cooling pit at high temperature to expand hydrogen, and the pit is cooled to below 200℃ to promote the diffusion of hydrogen; 4. Rolling: The ingot is heated at high temperature in the furnace to fully dissolve and diffuse the segregated components of the slab. After being removed from the heating furnace and descaled, rolling is carried out. The starting rolling temperature is greater than 1050°C. The first 2-3 passes are rolled with high deformation reduction rate, the maximum pass reduction rate is greater than 25%, and the last pass reduction rate is not more than 10%. After rolling, 2-4 passes of hot straightening are carried out; 5. High temperature normalizing: high temperature diffusion normalizing is adopted, the heating temperature is 920±10℃, the furnace time is 2.5~3.0min / mm, and air cooling is adopted; 6. Tempering: The tempering temperature is 740±10℃, the tempering time in the furnace is 3.5~4.5min / mm, air cooling after taking out of the furnace, and shot blasting after tempering.
5. The method according to claim 4, characterized in that: Step 1: During the whole process of molten steel smelting, P is controlled to be ≤0.015%, S to be ≤0.003%, H to be ≤0.0001%, O to be ≤0.0010%, and N to be ≤0.0040%.
6. The method according to claim 4, characterized in that: Step 2: The width of the continuous casting slab is 1800-2800mm. The light reduction in the continuous casting range is distributed according to 2-4-2mm. The second cooling section of the continuous casting adopts atomized water spray to control the cooling rate, so that the light reduction section acts on the slab solid phase ratio in the range of 0.5-0.9 to improve the center segregation of the continuous casting slab.
7. The method according to claim 4, characterized in that: Step 4: The continuous casting slab is heated and kept at a temperature of ≥1210°C to accelerate the diffusion of segregation elements in the steel and fully dissolve V (C, N) in the slab.
8. The method according to claim 4, characterized in that: Step 6: The steel plate is tempered in a roller hearth continuous furnace. Before entering the furnace, the steel plate is shot blasted to remove the surface oxide scale. After tempering, it is straightened with heat to ensure that the straightness of the steel plate is ≤3mm / m.
Citation Information
Patent Citations
High-tenacity high-speed steel and production technique thereof
CN105648325A
Ultra-thick alloy die steel plate produced by continuous casting billets and manufacturing method of ultra-thick alloy die steel plate
CN110396648A
Manufacturing method of 50CrVA hot-rolled spring wide steel plate
CN111876664A
42SiCrV6 spring steel for large-wire-diameter hot coiling spring on large excavator
CN114959486A
Free-cutting pre-hardened die steel plate with thickness of 201-300mm and manufacturing method thereof
CN116770169A