600MPa-grade hot-dip aluminum-silicon high-reaming complex-phase steel and preparation method thereof
Through the preparation method of composite steel with aluminum-silicon plating, the problems of reducing zinc resources and short-term alloying in hot-dip galvanizing technology of composite steel are solved, and high-strength, good pore reaming performance and moldability are achieved. The structure is ferrite, bainite, martensite and pearlite, and the surface is aluminum-silicon plating, which improves bainite transformation and mechanical properties.
Patent Information
- Application Number
- CN202410861846.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-06-28
Smart Images

Figure BDA0004919314560000071 
Figure BDA0004919314560000072 
Figure BDA0004919314560000073
Abstract
Description
Technical Field
[0001] The invention belongs to the field of automobile steel manufacturing, and particularly relates to a 600MPa-grade hot-dip aluminum-silicon high-hole expansion complex phase steel and a preparation method thereof. Background Art
[0002] The fuel consumption of a car is closely related to the weight of the car body. Studies have shown that for every 10% reduction in the weight of a car, fuel consumption will be reduced by 6% to 10% and emissions will be reduced by 4%. According to the fifth edition of the Advanced High Strength Steel Application Guide released by the World Steel Association, advanced high strength steel generally refers to high strength steel with a strength of more than 550MPa. As a typical representative of advanced high strength steel, complex phase steel has a microstructure of ferrite and bainite, which may contain martensite and austenite. Due to its good stamping and flanging performance and good strength and plasticity, it has been widely used in the automotive industry. Through the combined effect of martensite, bainite and precipitation strengthening, complex phase steel has the characteristics of high strength and good flanging performance, which is suitable for roll forming in the forming process of automotive parts and has broad market prospects. In addition to good mechanical properties and application performance, many car bodies require structural parts to have good surface quality. At present, the surface coating of complex phase steel is mainly hot-dip galvanizing. However, with the decreasing zinc resources and increasing prices, a new hot-dip method matching the heat treatment system is urgently needed to meet the future market demand for complex phase steel with good surface quality and mechanical properties.
[0003] The Chinese authorized patent with publication number CN111945075B discloses a 590MPa grade alloyed hot-dip galvanized DH steel with high hole expansion performance and its preparation method. It adopts a component system design of C, Mn, Si+Al, and adds 0.02-0.6% Al element to the steel to inhibit the decomposition of residual austenite and the precipitation of carbides, but the addition of Al will affect the difficulty of continuous casting in the steelmaking process. At the same time, it also adopts alloying galvanizing to obtain the coating, wherein the alloying temperature is between 470 and 530°C, and the alloying holding time is 5 to 60s. The alloying process is high temperature and short time, which is not conducive to the full progress of bainite phase transformation and may affect the hole expansion performance of the steel plate.
[0004] The Chinese authorized patent with publication number CN103667948B discloses a complex phase steel and its preparation method. The invention adopts the composition design of C, Mn, Si+Al, and adds Cr element to increase the hardenability of steel and refine the structure. At the same time, the steel plate performance obtained by smelting and hot rolling is 430-590MPa yield strength, 600-700MPa tensile strength, 20-35% elongation, and more than 80% hole expansion rate, but the invention involves cold rolling and coating. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a 600MPa-grade complex phase steel plate with an aluminum-silicon coating. By ingeniously designing the component combination process and reasonably controlling the aluminum-silicon liquid, and adopting a novel hot coating process to match the heat treatment process, the obtained new complex phase steel has a tensile strength of more than 600MPa, a yield strength of 400-550MPa, an elongation of more than 20%, and a hole expansion value of more than 90%, thereby achieving good strength, plasticity and formability of the steel plate, while taking into account the excellent hole expansion performance of the aluminum-silicon coated complex phase steel.
[0006] The object of the invention is achieved in this way:
[0007] The invention provides a 600MPa grade complex phase steel plate with an aluminum silicon coating, comprising a substrate and a coating. The chemical composition of the substrate comprises, by weight percentage, the following: C: 0.08%-0.12%, Si: 1.0%-2.0%, Mn: 0.2%-0.5%, Cr: 0.1-0.4%, Mo: 0.05-0.2%, P≤0.02%, S≤0.005%, Ti: 0.01-0.03%, Nb: 0.01-0.03%, and the balance is Fe and unavoidable impurities.
[0008] Furthermore, the chemical composition of the coating includes the following components by weight percentage: Al content is 88-93%, and Si content is 7-12%.
[0009] Furthermore, in the substrate, Mn+Cr=0.5% to 0.8%.
[0010] Furthermore, in the substrate, Mo / Cr=1 / 3 to 2 / 3.
[0011] Furthermore, the steel plate has a tensile strength of 600 MPa or more, a yield strength of 400-550 MPa, an elongation of ≥20%, and a hole expansion rate of ≥90%.
[0012] Furthermore, the steel plate microstructure includes ferrite, bainite, pearlite and martensite. According to the plane area method, the ferrite content is 35% to 61%, the bainite content is 20% to 35%, the pearlite content is 6% to 12%, and the martensite content is between 12% and 25%.
[0013] The reasons for the alloy design of the present invention are as follows:
[0014] C: The C element is a traditional and economical strengthening element for low carbon steel. However, if the C content is too high, it will inhibit the bainite phase transformation, increase the hardness difference of each phase in the steel plate structure, and lead to a decrease in the hole expansion performance of the steel plate. At the same time, it will bring difficulties to smelting and welding. If the C content is too low, it is difficult to make the steel plate reach 600MPa. Therefore, this application controls the C content to about 0.1%, and the optimal range is 0.08-0.12%.
[0015] Si: Si mainly plays the role of strengthening ferrite, which is beneficial to reducing the hardness difference of each phase, and further beneficial to the hole expansion performance of the steel plate. Therefore, in the present invention, the content of Si element is controlled to 1.0% to 2.0%.
[0016] Mn: Mn is a strengthening element of the steel plate, which improves the strength of the steel plate. At the same time, this element is also an austenite stabilizing element, which can improve the hardenability of the steel plate. If the content of this element is too low, it will affect the strength of the steel plate, and if the content is too high, segregation will occur, which will deteriorate the performance of the steel plate. Therefore, the present invention requires that the content of this element be controlled within 0.2% to 0.5%.
[0017] Cr: Cr is similar to Mn in that it can strengthen the steel plate by solid solution. It is also a stabilizing element of austenite, which can significantly delay the transformation of pearlite and bainite, and significantly improve the hardenability of steel. In addition, since the C content in the present invention is fixed at about 0.1%, in order to achieve a steel plate strength of 600MPa, the present invention requires that the Cr element content be controlled at 0.1-0.4%. At the same time, if the Mn+Cr content is too low, the steel plate strength may be insufficient, and if it is too high, the hole expansion performance may be reduced. Therefore, the Mn+Cr content is also required to be between 0.5% and 0.8%.
[0018] Mo: Mo element in the steel plate mainly plays the role of improving the hardenability of the steel plate and inhibiting the occurrence of ferrite and bainite phase transformation. Generally, Mo element and Cr are added together to achieve better results. If the content of this element is too low, the hardenability of the steel plate will be insufficient, and if it is too high, the cost of the steel plate will be significantly increased. Therefore, the present invention requires that the content of Mo element be controlled at 0.05% to 0.2%, and that its content is 1 / 3 to 2 / 3 of that of Cr.
[0019] Ti: Ti can capture free N atoms in steel and play a role in fixing N. At the same time, TiN can precipitate during the solidification process and play a role in pinning grain boundaries. Ti(C,N) precipitates during the hot rolling stage and plays a role in pinning the original austenite grain boundaries and refining the original austenite grains. At the same time, a small amount of Ti precipitates during the continuous annealing stage, which plays a role in strengthening ferrite and bainite, but adding too much Ti has limited effect and increases the composition. Therefore, in the present invention, the Ti element content is controlled to 0.01% to 0.03%.
[0020] Nb: Nb plays a significant role in grain refinement, phase transformation behavior, C enrichment in austenite and martensite nucleation. Nb combines with C and N to form fine carbonitrides, which prevent grain growth and have a significant strengthening effect. Therefore, the present application controls the Mn element content to 0.01-0.03%.
[0021] P: P is a harmful element in steel. The lower its content, the better. However, too low a requirement will increase the difficulty of steelmaking and increase the smelting cost. Therefore, in the present invention, the content of P is controlled to P≤0.02%.
[0022] S: S is a harmful element in steel, and the lower its content, the better. Too low a content of this element will also seriously increase the difficulty of steelmaking and increase the cost, so in the present invention, the content of S is controlled to S≤0.005%.
[0023] The second technical solution of the present invention is to provide a method for preparing 600MPa grade hot-dip aluminum-silicon high-hole expansion complex phase steel, comprising the following steps: smelting, hot rolling, pickling, cold rolling, continuous stripping of aluminum-silicon, and finishing. The specific steps are as follows:
[0024] Smelting: Smelting is carried out through a converter to obtain an alloy composition within the above range.
[0025] Hot rolling: ① The heating temperature is between 1200 and 1250℃, and the holding time is ≧100min. The limited temperature and time can ensure that Ti atoms precipitate with N and C elements in the steel to form Ti(C, N), so that the N element in the steel can be effectively fixed. At the same time, the precipitation of Ti(C, N) can play a role in pinning the original austenite grain boundaries and refining the original austenite grains. ② The starting rolling temperature is between 1100 and 1150℃, and the final rolling temperature is above 900℃ to ensure the rolling temperature in the recrystallization zone and promote the dynamic recrystallization behavior of the original austenite grains in the hot rolling stage. ③ The coiling temperature is between 560 and 700℃ to prevent the coiling temperature from being too low and increase the difficulty of cold rolling. The thickness of the hot rolled coil is between 2.5 and 4.0mm.
[0026] Pickling: Remove the iron oxide scale generated on the hot-rolled surface to ensure the surface quality of the cold-rolled steel plate.
[0027] Cold rolling: The cold rolling reduction rate is 40% to 60%, ensuring a cold rolling reduction of more than 40% to promote tissue fiberization in the cold rolling configuration; at the same time, prevent the cold rolling reduction rate from being too high, resulting in excessive deformation resistance and difficulty in rolling to the target thickness.
[0028] Continuous annealing aluminum silicon:
[0029] ① The heating isothermal temperature is 760-840℃, the isothermal time is 80-150s, the slow cooling temperature is 650-700℃, and the slow cooling rate is controlled at 0.5-5℃ / s; this heating temperature and isothermal time ensure that the cold-rolled structure can recover and recrystallize to form a two-phase structure of ferrite and austenite, and ensure the homogenization of the austenite composition; the slow cooling process will generate ferrite and pearlite; this process promotes the enrichment of C atoms in the supercooled austenite.
[0030] ② Aluminum-silicon plating: After slow cooling, the strip enters the aluminum-silicon plating solution to obtain a surface coating. The temperature of the aluminum-silicon plating solution is 650-700°C, and the aluminum-silicon plating time is 3-10s. The composition of the aluminum-silicon plating solution is: Al content 88-93%, Si content 7-12%.
[0031] ③ After aluminum silicon plating, cool to the over-aging temperature of 320-420°C at a cooling rate greater than 10°C / s, the over-aging isothermal time is 200-650s, and then cool to room temperature at a cooling rate greater than 2°C / s; then, the steel plate enters the skin pass mill for plate shape adjustment, which is controlled at 0.1%-0.8%.
[0032] The mechanism is as follows: first, annealing in the austenite region or the two-phase region obtains a suitable proportion of ferrite and original austenite; slowly cools to 650-700°C for hot-dip aluminum silicon, and then cools to 320-420°C to isothermally obtain martensite and bainite structures. Since the hot-dip aluminum silicon is in the slow cooling stage, the time of the over-aging stage of the present invention can be flexibly adjusted according to the needs of phase transformation, breaking the limitation that the hot-dip galvanized steel sheet must be over-aged at high temperature for a short time, and can make the bainite transformation fully, which is beneficial to the hole expansion performance and mechanical properties of the complex phase steel.
[0033] The final structure of the steel plate of the present invention is ferrite + bainite + martensite + pearlite, and the surface of the steel plate is an aluminum silicon coating. It can be seen that the present invention adopts a novel hot coating process matched with a heat treatment process, and the obtained new complex phase steel has a tensile strength of more than 600MPa, a yield strength of 400-550MPa, an elongation of more than 20%, and a hole expansion value of more than 90%, achieving good strength, plasticity and formability of the steel plate.
[0034] The beneficial effects of the present invention are:
[0035] 1. The chemical composition of the steel material of the present invention mainly contains C and Mn as the main elements, without obvious precious alloys, and the C content is less than 0.12%, which is conducive to laser welding and resistance spot welding in the production and application process;
[0036] 2. The present invention adopts a novel hot-dip aluminum-silicon method to obtain the surface coating of the complex phase steel, and ingeniously performs hot-dip aluminum-silicon in the slow cooling stage, which perfectly matches the heat treatment system, breaks the limitation that hot-dip galvanized steel sheets must be aged at high temperature for a short time, and can fully transform bainite, which is beneficial to the hole expansion performance and mechanical properties of the complex phase steel;
[0037] 3. The present invention achieves good strength, plasticity and formability of the steel plate through low-cost alloy design and ingenious process design. The final structure of the steel plate of the present invention is ferrite + bainite + martensite + pearlite, with a ferrite content of 35% to 61%, a bainite content of 20% to 35%, a pearlite content of 6% to 12%, and a martensite content of 12% to 25%. The surface of the steel plate is an aluminum-silicon coating.
[0038] 4. The present invention adopts a novel hot-dip coating process matched with a heat treatment process, and the obtained new type of complex phase steel has a tensile strength of ≥600MPa, a yield strength of 400-550MPa, an elongation of ≧20%, and a hole expansion value of ≥90%, achieving good strength, plasticity and formability of the steel plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Picture 1 This is a typical SEM microstructure metallographic image of Example 1 of the present invention. DETAILED DESCRIPTION
[0040] The present invention will be further described below by way of examples.
[0041] The embodiment of the present invention carries out alloying smelting, hot rolling, pickling, cold rolling, continuous stripping of aluminum silicon, and skin finishing according to the component ratio of the technical solution.
[0042] Hot rolling: heating temperature is between 1200 and 1250℃, holding time is ≧100min; starting rolling temperature is between 1100 and 1150℃, final rolling temperature is above 900℃, coiling temperature is between 560 and 700℃, hot rolled coil thickness is 2.5 to 4.0mm;
[0043] Cold rolling: The cold rolling reduction rate is 40% to 60%;
[0044] Continuous stripping of aluminum silicon:
[0045] ① The heating isothermal temperature is 760-840℃, the isothermal time is 80-150s, the slow cooling temperature is 650-700℃, and the slow cooling rate is controlled at 0.5-5℃ / s;
[0046] ② Aluminum-silicon plating: After slow cooling, immerse the steel plate in an aluminum-silicon plating solution to obtain a coating on the surface of the steel plate. The temperature of the aluminum-silicon plating solution is 650-700°C, and the aluminum-silicon plating time is 3-10s;
[0047] ③ After aluminum silicon plating, cool to the over-aging temperature of 320-420°C at a cooling rate greater than 10°C / s, the over-aging isothermal time is 200-650s, and then cool to room temperature at a cooling rate greater than 2°C / s;
[0048] Furthermore, after continuous annealing, the steel sheet enters a skin pass mill for sheet shape adjustment, and the skin pass elongation is 0.1% to 0.8%.
[0049] Furthermore, the composition of the aluminum-silicon liquid plated on the steel plate is: Al content 88-93%, Si content 7-12%.
[0050] The composition of the steel of the present invention is shown in Table 1. The main process parameters of hot rolling and cold rolling of the steel of the present invention are shown in Table 2. The main process parameters of annealing and aluminum-silicon plating of the steel of the present invention are shown in Table 3. The performance and microstructure of the steel of the present invention are shown in Table 4.
[0051] Table 1 Chemical composition of example steel, wt%
[0052] No. C Mn Cr Mo S Ti Nb P S Mn+Cr Mo / Cr 1 0.09 0.5 0.2 0.1 1.6 0.02 0.015 0.010 0.005 0.7 0.5 2 0.08 0.3 0.3 0.1 1.2 0.02 0.01 0.009 0.005 0.6 0.3 3 0.11 0.4 0.3 0.2 1.1 0.025 0.015 0.010 0.003 0.7 0.7 4 0.09 0.4 0.2 0.1 1.9 0.03 0.02 0.005 0.005 0.6 0.5 5 0.08 0.2 0.4 0.2 1.7 0.02 0.01 0.009 0.003 0.6 0.5 6 0.11 0.4 0.3 0.1 1.2 0.035 0.015 0.008 0.005 0.7 0.3 7 0.10 0.4 0.3 0.2 1.8 0.02 0.01 0.01 0.005 0.7 0.7 8 0.080 0.2 0.4 0.2 1.4 0.015 0.025 0.02 0.004 0.6 0.5
[0053] Table 2 Hot rolling and cold rolling process of example steel
[0054]
[0055] Table 3 Example steel annealing aluminum silicon coating process
[0056]
[0057] Table 4 Mechanical properties and microstructure of example steel
[0058]
[0059]
[0060] It can be seen from the above embodiments that through low-cost alloy design and ingenious process design, a hot-dip aluminum-silicon steel plate with a tensile strength of more than 600MPa, a yield strength of 400-550MPa, an elongation of more than 20%, and a hole expansion value of more than 90% is prepared; the microstructure of the steel plate is ferrite + bainite + martensite + pearlite, and in terms of area percentage, the ferrite content is 35%-61%, the bainite content is 20%-35%, the pearlite content is 6%-12%, and the martensite content is between 12% and 25%, thereby achieving good strength, plasticity and formability of the steel plate.
[0061] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.
Claims
1. A 600MPa grade hot-dip aluminum-silicon high hole expansion complex phase steel, comprising a substrate and a coating, characterized in that: The chemical composition of the substrate includes the following components by weight percentage: C: 0.08% to 0.12%, Si: 1.0% to 2.0%, Mn: 0.2% to 0.5%, Cr: 0.1% to 0.4%, Mo: 0.05% to 0.2%, P≤0.02%, S≤0.005%, Ti: 0.01% to 0.03%, Nb: 0.01% to 0.03%, and the balance is Fe and unavoidable impurities.
2. The 600MPa grade hot-dip aluminum-silicon high hole expansion complex phase steel according to claim 1, characterized in that: In the substrate, Mn+Cr=0.5% to 0.8%.
3. The 600MPa grade hot-dip aluminum-silicon high hole expansion complex phase steel according to claim 1, characterized in that: In the substrate, Mo / Cr=1 / 3 to 2 / 3.
4. The 600MPa grade hot-dip aluminum-silicon high hole expansion complex phase steel according to claim 1, characterized in that: The chemical composition of the coating includes the following components by weight percentage: Al content is 88-93%, Si content is 7-12%.
5. The 600MPa grade hot-dip aluminum-silicon high hole expansion complex phase steel according to claim 1, characterized in that: The steel plate has a tensile strength of ≥600 MPa, a yield strength of 400-550 MPa, an elongation of >20%, and a hole expansion value of ≥90%.
6. The 600MPa grade hot-dip aluminum-silicon high hole expansion complex phase steel according to claim 1, characterized in that: The steel plate microstructure is ferrite+bainite+martensite+pearlite. In terms of area percentage, the ferrite content is 35% to 61%, the bainite content is 20% to 35%, the pearlite content is 6% to 12%, and the martensite content is between 12% and 25%.
7. A method for manufacturing a 600MPa grade hot-dip aluminum-silicon high hole expansion complex phase steel according to any one of claims 1 to 6, comprising smelting, hot rolling, pickling, cold rolling, continuous aluminum-silicon stripping, and skin-passing, characterized in that: Hot Rolling The heating temperature is between 1200 and 1250°C, and the holding time is ≧100 min; the starting rolling temperature is between 1100 and 1150°C, and the final rolling temperature is above 900°C; the coiling temperature is between 560 and 700°C, and the thickness of the hot rolled coil is between 2.5 and 4.0 mm; Cold Rolling The cold rolling reduction rate is 40% to 60%; Continuous annealing aluminum silicon ① The heating isothermal temperature is 760-840℃, the isothermal time is 80-150s, the slow cooling temperature is 650-700℃, and the slow cooling rate is controlled at 0.5-5℃ / s; ② Aluminum-silicon plating: After slow cooling, the strip enters the aluminum-silicon plating solution to obtain a surface coating on the steel plate. The aluminum-silicon plating solution temperature is 650-700°C, and the aluminum-silicon plating time is 3-10s; ③ After aluminum silicon plating, cool to 320-420°C at a cooling rate greater than 10°C / s, the isothermal time is 200-650s, and then cool to room temperature at a cooling rate greater than 2°C / s.
8. The method for manufacturing a 600MPa grade hot-dip aluminum-silicon high hole expansion complex phase steel according to claim 7, characterized in that: After continuous annealing, the steel plate enters the skin pass mill for plate shape adjustment, and the skin pass elongation is 0.1% to 0.8%.
9. The method for manufacturing a 600MPa grade hot-dip aluminum-silicon high hole expansion complex phase steel according to claim 7, characterized in that: The aluminum-silicon liquid used to plate the steel plate has the following components: Al content of 88-93% and Si content of 7-12%.
Citation Information
Patent Citations
High-strength cold-rolled steel sheet with highly even stretchabilty and excellent hole expansibility, and process for producing same
CN103492599A
Ultrahigh-strength hot-rolled complex phase steel plate and steel strip with good bending and broaching performance and manufacturing method thereof
CN104513930A
High-strength high-toughness hot-dip aluminized steel plate and manufacturing method thereof
CN105506470A
1900MPa-grade high-strength and high-toughness aluminum-silicon coated steel plate for hot stamping and preparation method thereof
CN111893377A
High-reaming high-plasticity 980MPa-grade dual-phase galvanized steel plate and preparation method thereof
CN113416888A