Q460-grade improved high-toughness corrosion-resistant steel plate as well as production method and application thereof
Through the design of Ni-Cu-Sb corrosion-resistant alloy and TMCP+ tempering process, the chemical composition and process flow of Q460 grade steel plates are optimized, and the problem of difficult to take into account both toughness and corrosion resistance in marine engineering in the existing technology is solved, and the problem of steel plates in marine engineering is realized. It has improved high toughness and corrosion resistance, and is suitable for engineering applications in complex marine environments.
Patent Information
- Application Number
- CN202410964835.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, Q460 steel plates face complex environments of high humidity, heat, salt and radiation in marine engineering such as island and reef infrastructure, cross-sea bridges and coastal buildings, and are difficult to take into account both toughness and corrosion resistance, especially thick-specification steel plates. The impact toughness is unstable and the toughness of the welding heat-affected zone is insufficient.
Designed with Ni-Cu-Sb corrosion-resistant alloy, the structural structure and performance of steel plates are optimized by controlling the content of chemical components such as C, Mn, Ni, Cu, Sb and the use of trace elements Nb and Ti, combined with TMCP+ tempering technology. , adopts a fully protected casting and controlled rolling cooling process to control the segregation resolution and quench tempering treatment of the steel plate to improve the corrosion and impact resistance of the steel plate.
The high toughness and corrosion resistance of Q460 grade steel plates have been achieved. The yield strength, tensile strength and low-temperature impact toughness of the steel plate have been significantly improved. It is suitable for marine engineering such as island and reef infrastructure, cross-sea bridges and coastal buildings, and has excellent physical and chemical properties and Weather resistance.
Smart Images

Figure CN118880199A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, in particular to a Q460 grade improved toughness high corrosion resistant steel plate and a production method and application thereof. Background Art
[0002] With the development of island and reef infrastructure construction, cross-sea bridge construction, seaside buildings, and marine engineering, the demand for offshore structural steel for marine atmospheric and seawater corrosion environments has greatly increased. According to the unique, complex, and changeable marine corrosion environment of high humidity, high salt, high radiation, and strong tropical storms in the offshore area, studying the mechanical properties and corrosion resistance of steel used in infrastructure and key projects, and developing steel with high corrosion resistance alloying and organizational structure that matches them is one of the key research directions of the metallurgical industry.
[0003] The patent with publication number CN102586686B discloses a clean, corrosion-resistant marine engineering steel and a production method thereof, but the steel provided in the technical solution has a high P content, which is not conducive to the toughness of the parent material and the welding heat-affected zone. The patent with publication number CN104419871B discloses a welded structural steel with excellent corrosion resistance in marine environments and a manufacturing method thereof, but the steel provided in the technical solution has a large amount of Cu and Mo added. Cu will increase the cracks of the ingot during the continuous casting process, and too much Mo will increase the production cost of raw materials, while increasing the hardness after welding and the sensitivity of post-weld cracks. The technical solution of the invention adopts a low-carbon component design TMCP+tempering process for production, and the core of the thick-gauge steel plate is affected by the cooling rate, and the impact toughness is difficult to stabilize.
[0004] Patent publication number CN112746216B discloses a steel plate resistant to alternating wet and dry corrosion in marine seawater. It is produced by a TMCP process designed with low carbon components. The impact toughness of thick-gauge steel plates is difficult to stabilize, and the P content is high, which is not conducive to the toughness of the base material and the welding heat-affected zone.
[0005] Based on the above situation, how to provide an improved toughness and corrosion-resistant steel plate is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0006] In view of this, the present invention provides a Q460 grade improved toughness high corrosion resistant steel plate and its production method and application, which improves the quality of the core of the steel plate through in-situ analysis, and the statistical segregation of C, Mn, Ni, Cu, and Sb is ≤0.05. The steel used in the production of island and reef infrastructure construction, cross-sea bridge construction, coastal building construction, and ship and marine engineering has better physical and chemical properties.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] Firstly, the present invention provides a Q460 grade improved toughness high corrosion resistant steel plate, the chemical composition weight percentage of the Q460 grade improved toughness high corrosion resistant steel plate is: C: 0.06% ~ 0.08%, Si: 0.15% ~ 0.40%, Mn: 1.28% ~ 1.45%, P≤0.020%, S≤0.003%, Nb: 0.01% ~ 0.02%, Ti: 0.01% ~ 0.02%, Als: 0.02% ~ 0.05%, Cu: 0.30% ~ 0.70%, Ni: 0.7% ~ 1.5%, Sb: 0.08% ~ 0.30%, and the rest is Fe and unavoidable impurity elements.
[0009] The present invention adopts Ni-Cu-Sb corrosion-resistant alloy design, wherein:
[0010] Ni is a relatively stable element. Adding Ni can change the self-corrosion potential of steel in a positive direction, thus increasing the stability of the steel. Atmospheric exposure tests show that when the Ni content is around 4%, the atmospheric corrosion resistance of offshore atmospheric corrosion-resistant steel can be significantly improved. The enrichment of Ni in the stable rust layer can effectively inhibit the intrusion of Cl- ions, promote the formation of a protective rust layer, and reduce the corrosion rate of steel. However, a higher Ni content will inevitably lead to an increase in the cost of steel, which is not conducive to the use of large-scale industrial production. Therefore, under the consideration of meeting a certain balance between marine weather resistance and economy, the present invention selects a Ni mass percentage of 0.7% to 1.5%.
[0011] Cu is increasingly added to steel as a strengthening element, especially ultra-low carbon steel. After the solid solution treatment of copper-containing high-purity steel, the copper solute atoms are not evenly distributed in the ferrite matrix, but exist in an uneven short-range ordered form. The existence of ordered domains can create favorable conditions for subsequent aging precipitation, thereby having a certain effect on the aging strengthening behavior of copper-containing steel. Cu is a very important alloying element for improving the atmospheric corrosion resistance of steel. Adding an appropriate amount of Cu to steel can significantly improve the corrosion resistance of steel, and at the same time improve the strength of steel through solid solution strengthening. The mass percentage of Cu selected in the present invention is 0.30% to 0.70%.
[0012] Si is an element with a greater strengthening effect in steel. It replaces Fe atoms in the lattice to produce a solid solution strengthening effect. A notable feature of solid solution strengthening is that as the solute atoms increase, the strength and hardness increase, while the plasticity and toughness decrease. The greater the strengthening effect, the more the plasticity and toughness decrease. At the same time, studies have shown that in an atmospheric corrosion environment, a large amount of Si can increase the content of paramagnetic α-FeOOH in the protective rust layer, refine α-FeOOH, and thus reduce the corrosion rate of the material. The corrosion rate of carbon steel is related to the properties of α-Fe2O3 and α-FeOOH. Large particles of α-FeOOH and magnetic α-Fe2O3 will hinder the complete formation of the protective rust layer, resulting in an increase in the corrosion rate. The superparamagnetic α-FeOOH can refine the FeOOH particles, thereby reducing the corrosion rate of carbon steel. The mass percentage of Si selected in the present invention is 0.15% to 0.40%.
[0013] As a common element in low carbon steel, the increase of Mn content within a certain range is beneficial to the performance of low carbon steel. Mn is one of the cheapest elements to improve the strength of steel. It can significantly expand the austenite phase area in steel, reduce the phase transition temperature, refine the phase transition organization, and change the organizational structure. When the C content is low, Mn not only plays a role in improving strength, but also can effectively ensure plasticity and toughness, and has no obvious effect on the corrosion resistance of low alloy steel. Studies on deformation strengthening phase transformation in low carbon manganese steel show that the increase of Mn content delays the phase transformation process from austenite to ferrite, and the strain required to complete the phase transformation increases, but the final ferrite grains are finer. It is generally believed that during the hot deformation process, the main recovery mechanism of ferrite is dynamic recovery, and dynamic recrystallization is difficult to occur. Mn expands the austenite phase area of steel and reduces the phase transition point. During the hot deformation process, Mn atoms delay the recrystallization of austenite and increase the deformation resistance of austenite, which will have a certain impact on the phase transformation of low carbon steel and the deformation behavior and recrystallization behavior of austenite during hot working. The mass percentage of Mn selected in the present invention is 1.28% to 1.45%.
[0014] The presence of Cr will significantly accelerate the development of electrochemical corrosion products to a thermodynamically stable state. The analysis and research on the rust layer found that the alloying element Cr can significantly accelerate (Fe x HYO z )-→γ-FeOOH→α-FeOOH→α-Fe2O3, promoting the formation of spinel compounds; at the same time, Cr can partially replace Fe to form chromium-iron light-based oxide CrXFe1-xOOH, making the α-FeOOH rust layer cationic selective, preventing Cl-, SO4 2 - Kamimura uses Cr-containing 3+The effect of Cr on atmospheric corrosion of low carbon steel was studied by dry-wet alternating cyclic corrosion test in sulfate electrolyte. 3+ The corrosion rate is greatly affected. Even when the surface polarization potential reaches -200mV (VS SCE), the corrosion rate is still very low. 3+ There is no obvious effect on the composition of the rust layer, but there is a Cr-rich area near the interface between the rust layer and the substrate, which is consistent with Cr-containing steel. The presence of Cr in the rust layer hinders the reduction of the rust layer and the intermediate Fe 2+ However, considering the performance of Cr element under marine atmospheric conditions, less or no Cr should be added. Therefore, the present invention does not add chromium.
[0015] The main functions of the microalloying element Nb in steel are as follows: the undissolved Nb (C, N) at high temperature prevents the growth of austenite grains; the undissolved or strain-induced precipitated Nb (C, N) at the rolling temperature prevents the growth of recrystallized grains; when the Nb content is less than 0.1wt%, the microalloying carbonitrides of the solid-solution Nb and the strain-induced precipitated Nb at the rolling temperature inhibit the recrystallization behavior of the matrix as the Nb content increases; the solid-solution Nb delays the matrix γ→α phase transformation, and the precipitation of Nb (C, N) promotes the γ→α phase transformation; the microalloying carbonitrides of very small size precipitated at a relatively low temperature produce a strong precipitation strengthening effect, which is further strengthened during the rolling process by adopting the micro-Nb rolling technology. The invention selects to add 0.01% to 0.02% by mass of Nb to effectively reduce the production cost.
[0016] Adding Ti, a strong carbonitride-forming element, to steel can combine C and N atoms with it to form Ti(C,N) particles, which can hinder the recrystallization of austenite, thus creating conditions for refining ferrite grains. On the one hand, Ti(C,N) particles, as second-phase precipitation particles, play a precipitation strengthening role on the ferrite matrix. This is the physical metallurgical basis of Ti-containing microalloyed steel. On the other hand, the addition of Ti can fix C and N atoms in the steel to achieve pearlite-free steel, purify ferrite grain boundaries and enhance its corrosion resistance. Since Ti and Nb have similar properties and the cost of Ti is much lower than that of Nb, Ti is considered to replace Nb.
[0017] Ti(effective)=Ti(total)-3.4N-3S-TiC(strain-induced precipitation)
[0018] Only when Ti% in steel is ≥ (3.4N+3S), the precipitation strengthening effect of TiC particles is shown. According to the actual stable content of N and S in the ingot, the present invention adopts 0.01% to 0.02% Ti by mass to meet the requirements.
[0019] Sb forms an oxide protective film on the surface of the material, effectively inhibiting Cl - The intrusion of ions reduces the corrosion rate of steel and increases the corrosion resistance in marine climate environment. Too high Sb will affect the surface quality of the ingot, so the present invention uses 0.08% to 0.30% Sb by mass to meet the demand.
[0020] The Q460 grade improved toughness high corrosion resistant steel plate described in the present invention has a yield strength of ≥460MPa, such as 498MPa, 500MPa, 502MPa, 504MPa, 512MPa, and 517MPa.
[0021] The tensile strength of the Q460 grade improved toughness high corrosion resistant steel plate described in the present invention is ≥570MPa, such as 665MPa, 666MPa, 673MPa, 674MPa, and 681MPa.
[0022] The Q460 grade improved toughness high corrosion resistant steel plate described in the present invention has an elongation after fracture A≥30%, such as 33.5%, 34%, 34.5%, 36%, 38.5%.
[0023] The Q460 grade improved toughness high corrosion resistant steel plate described in the present invention has a low temperature -60°C impact toughness KV2≥120J, a low temperature -60°C impact toughness KV2≥120J at 1 / 2 thickness of the steel plate, and a lamellar tearing resistance Z≥35%.
[0024] In certain embodiments of the present invention, the content of C is 0.06% to 0.08%, such as 0.06%, 0.07% or 0.08%;
[0025] The content of Si is 0.25-0.40%, for example, 0.25%, 0.28%, 0.30%, 0.39%;
[0026] The content of Mn is 1.28-1.45%, such as 1.28%, 1.29%, 1.32%, 1.38%, 1.39%, 1.44%; the content of P is ≤ 0.0140%, such as 0.014%, 0.012%, 0.010%, 0.009%;
[0027] The content of S is ≤ 0.002%, for example 0.002%, 0.001%;
[0028] The content of Nb is 0.01% to 0.02%, for example, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.020%;
[0029] The content of Ti is 0.01-0.02%, such as 0.010%, 0.011%, 0.017%, 0.018%, 0.020%; the content of Als is 0.02-0.05%, such as 0.022%, 0.025%, 0.035%, 0.039%, 0.045%, 0.047%;
[0030] The Cu content is 0.30-0.70%, for example, 0.30%, 0.35%, 0.36%, 0.45%, 0.57%, and 0.63%; the Ni content is 0.7%-1.5%, for example, 0.74%, 0.99%, 1.05%, 1.29%, 1.39%, and 1.47%; the Sb content is 0.08%-0.30%, for example, 0.09%, 0.15%, 0.17%, 0.20%, 0.21%, and 0.29%.
[0031] The present invention also provides a production method of Q460 grade improved toughness high corrosion resistant steel plate as described in the above technical solution, the production process includes molten iron pretreatment → converter steelmaking → furnace refining LF → vacuum treatment RH → continuous casting → heating → rolling → controlled rolling cooling → quenching → tempering → finishing, and the key process steps include:
[0032] Continuous casting: The superheat of molten steel is less than 15℃; the continuous casting adopts full protection pouring to avoid the contact between molten steel and air, so as to control the absorption of nitrogen in the air by molten steel during the pouring process; the continuous casting adopts the heavy pressure reduction technology at the end of solidification to improve the internal segregation and internal looseness of the slab.
[0033] Heating: The heating furnace adopts reducing atmosphere, the temperature of the heating section is 1100℃~1240℃, the temperature of the soaking section is 1100℃~1200℃, and the holding time of the soaking section is ≥30min;
[0034] Rolling: Rough rolling adopts a large reduction system to ensure that the reduction rate of three consecutive passes after widening is ≥14%; the final rolling temperature of finishing rolling is 750℃~820℃, and the reduction rate of the first three passes of finishing rolling is ≥10%;
[0035] Controlled rolling cooling: directly into water, red-return temperature 600℃~660℃, cooling rate 3~10℃ / s;
[0036] Quenching: 900℃~920℃ quenching, the time in the furnace is plate thickness mm×(1.4~2.5)min / mm, water cooling; quenching ensures that the high-pressure section pressure of the quenching machine is ≥8bar, the low-pressure section pressure is ≥3.5bar, and the surface temperature of the steel plate after quenching is ≤40℃.
[0037] Tempering: Tempering at 650-670℃, the time in the furnace is plate thickness mm×(2.0-3.5)min / mm, air cooling + stack cooling. Stack cooling is performed after tempering, the stack cooling temperature is 200-300℃, and the stack cooling time is ≥24 hours before destacking.
[0038] In the present invention, the reducing atmosphere is a mixed coal gas, which can control the oxygen content, reduce the oxidation of the Sb element, and improve the surface quality of the steel plate.
[0039] In certain embodiments of the present invention, the quenching temperature is 900°C to 920°C, for example, 900°C, 907°C, 909°C, 915°C, 919°C, and 920°C; the time in the furnace is plate thickness mm×(1.4-2.5) min / mm, for example, 183min, 200min, 202min, 204min, 235min, and 245min.
[0040] In certain embodiments of the present invention, the pressure in the high-pressure section of the quenching machine is ≥8 bar, for example, 8.1 bar, 8.2 bar, 8.3 bar, 8.4 bar; the pressure in the low-pressure section of the quenching machine is ≥3.5 bar, for example, 3.9 bar, 4.0 bar, 4.1 bar, 4.2 bar, 4.3 bar.
[0041] In certain embodiments of the present invention, the tempering temperature is 650-670°C, for example, 652°C, 654°C, 655°C, 668°C, 670°C; the time in the furnace is plate thickness mm×(2.0-3.5) min / mm, for example, 239min, 254min, 256min, 284min, 305min, 345min.
[0042] In the present invention, the thickness of the Q460 grade improved toughness high corrosion resistant steel plate is ≤100mm.
[0043] The present invention also provides an application of the Q460 grade improved toughness high corrosion resistant steel plate in the production of steel for island and reef infrastructure construction, cross-sea bridge construction, seaside building construction and ship and ocean engineering.
[0044] It can be seen from the above technical solutions that, compared with the prior art, the present invention discloses a Q460 grade improved toughness high corrosion resistant steel plate and a production method and application thereof, which have the following beneficial effects:
[0045] (1) The present invention has overcome the key technologies of coordinated regulation of high corrosion-resistant alloy composition design, metallurgical quality, microstructure, and material properties, and developed improved toughness high corrosion-resistant steel plates; solved the problem that the impact toughness of thick-gauge low-carbon bainitic steel is unstable, and the preferential corrosion after the formation of pearlite is affected by the cooling rate after rolling; the serialized organizational design is tempered bainite steel; through in-situ analysis technology, the quality of the core of the steel plate is improved, and the statistical segregation degree of C, Mn, Ni, Cu, and Sb is ≤0.05; a trace amount of Nb is added: 0.01% to 0.02%, and the rolling process is further strengthened by the micro-Nb rolling technology.
[0046] (2) The present invention adopts reasonable component design and microalloy strengthening technology combined with rolling and tempering processes, and is used for the development of high corrosion-resistant steel in marine climate environment in island and reef infrastructure construction, cross-sea bridge construction, coastal building construction, and ship and marine engineering. The steel plate strength grade is Q460, the steel plate thickness specification is ≤100mm, the yield strength is ≥460MPa, the tensile strength is ≥570MPa, the elongation after fracture A is ≥30%, the low-temperature -60℃ impact toughness KV2 is ≥120J, the low-temperature -60℃ impact toughness KV2 at 1 / 2 thickness of the steel plate is ≥120J, and the lamellar tearing resistance Z is ≥35%. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0048] Figure 1 This is a metallographic structure photograph of a 1 / 2 thickness 100 mm steel plate of Example 2;
[0049] Figure 2 This is a two-dimensional distribution diagram of the Sb element content in situ analysis of Example 2;
[0050] Figure 3 The center temperature distribution of the ingot with different sections in Example 2;
[0051] Figure 4 This is the Raman spectrum of the rust layer in Example 2. DETAILED DESCRIPTION
[0052] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] The preparation processes of the following Examples 1-6 and Comparative Example 1 include:
[0054] Hot metal pretreatment → converter steelmaking → refining outside the furnace LF → vacuum treatment RH → continuous casting → heating → rolling → controlled rolling cooling → quenching → tempering → finishing → performance inspection → ultrasonic flaw detection.
[0055] Among them, hot metal pretreatment refers to a hot metal treatment process that removes impurity elements before adding hot metal to the converter, including hot metal desiliconization, desulfurization, dephosphorization, etc., to improve the purity of hot metal;
[0056] Converter steelmaking uses molten iron, scrap steel and ferroalloy as the main raw materials. It does not rely on external energy sources. It relies on the physical heat of the molten iron itself and the heat generated by the chemical reaction between the components of the molten iron to complete the steelmaking process. In this process, the initial adjustment of the chemical composition is completed;
[0057] LF is a furnace refining technology that uses electric arc heating under vacuum conditions.
[0058] Vacuum treatment RH is a method of vacuum cycle degassing of molten steel, which is suitable for removing gas from steel and reducing the occurrence rate of hairline cracks, hydrogen-induced cracks and lamellar fracture defects in steel;
[0059] Continuous casting is continuous steel casting. In this process, in-situ analysis technology is used to improve the process cyclically, obtain the best segregation quality of each chemical element, and optimize the core performance. Continuous casting adopts full protection pouring to avoid contact between molten steel and air, so as to control the absorption of nitrogen in the air by molten steel during the pouring process. Continuous casting adopts heavy pressure reduction technology at the end of solidification to improve the internal segregation and internal looseness of the slab.
[0060] Heating refers to heating the steel billet to a temperature suitable for the rolling process, which provides the necessary conditions for rolling forming. A suitable heating process can greatly refine the austenite grains, greatly improve the toughness of the product and optimize the core performance;
[0061] Rolling refers to the deformation process of billet metal. The appropriate rolling process can obtain accurate product dimensions and required performance;
[0062] Controlled rolling and cooling refers to controlled rolling and controlled cooling, which is an extension of the rolling process and can obtain more precise product performance.
[0063] Quenching and tempering are combined heat treatment processes. After heat treatment, tempered troostite structure is obtained, which has excellent strength and toughness, as well as stronger corrosion resistance. The pressure control of the quenching machine ensures that the steel plate is hardened thoroughly and improves the performance of the steel plate at 1 / 2. After tempering, stack cooling reduces the internal stress of the steel plate, and the steel plate has better processing performance.
[0064] Finishing is a series of operations to meet the user's final requirements for the product in terms of surface quality, size, shape and certain performance;
[0065] Performance testing is a series of tests conducted to verify whether the technical requirements are met and is used to measure the final use of the product;
[0066] Ultrasonic flaw detection is a non-destructive test. It is a means of inspecting the surface and internal quality of the inspected parts. It is used to measure the surface and internal quality of the product.
[0067] In each experimental example, the thickness of the cast slab was 300 mm, and the thickness of the rolled steel plate was 100 mm.
[0068] Example 1
[0069] The chemical composition of the steel plate is as follows by weight: C 0.08%, Si 0.25%, Mn 1.38%, P 0.014%, S0.001%, Nb 0.013%, Ti 0.011%, Als 0.045%, Cu 0.35%, Ni 1.29%, Sb 0.17%, and the rest are Fe and unavoidable impurity elements.
[0070] Continuous casting: molten steel superheat degree is 12℃; full protection pouring is adopted in continuous casting to avoid molten steel from contacting with air, so as to control the absorption of nitrogen in the air by molten steel during pouring; heavy pressure reduction technology is adopted at the end of solidification to improve the internal segregation and internal looseness of slab;
[0071] Heating: The heating furnace adopts a mixed gas reducing atmosphere, the heating section temperature is 1180℃~1240℃, the soaking section temperature is 1190℃, and the soaking section is kept warm for 35min;
[0072] Rolling: Rough rolling adopts a large reduction system, and the reduction rates of the three consecutive passes after widening are 16%, 16%, and 17% respectively; the final rolling temperature of finishing rolling is 788℃, and the reduction rates of the first three passes of finishing rolling are 12%, 12%, and 12% respectively;
[0073] Controlled rolling cooling: directly into water, red-return temperature 626℃, cooling rate 3~10℃ / s;
[0074] Quenching: 900℃ quenching, furnace time is 245min, water cooling; quenching machine high pressure section pressure is 8.2bar, low pressure section pressure is 4.1bar, and the surface temperature of the steel plate after quenching is 40℃.
[0075] Tempering: Tempering at 654℃, 256min in furnace, air cooling + stack cooling. Stack cooling after tempering, stack cooling temperature 268℃, stack cooling time 35 hours, then destacking.
[0076] Example 2
[0077] The chemical composition of the steel plate is as follows by weight: C 0.07%, Si 0.30%, Mn 1.28%, P 0.010%, S 0.001%, Nb 0.012%, Ti 0.017%, Als 0.025%, Cu 0.57%, Ni 1.05%, Sb 0.09%, and the rest are Fe and unavoidable impurity elements.
[0078] Continuous casting: molten steel superheat degree is 10℃; full protection pouring is adopted in continuous casting to avoid molten steel from contacting with air, so as to control the absorption of nitrogen in the air by molten steel during the pouring process; heavy pressure reduction technology is adopted at the end of solidification to improve the internal segregation and internal looseness of slab;
[0079] Heating: The heating furnace adopts a mixed gas reducing atmosphere, the heating section temperature is 1140℃~1190℃, the soaking section temperature is 1155℃, and the soaking section is kept warm for 39 minutes;
[0080] Rolling: Rough rolling adopts a large reduction system, and the reduction rates of the three consecutive passes after widening are 15%, 16%, and 15% respectively; the final rolling temperature of finishing rolling is 758℃, and the reduction rates of the first three passes of finishing rolling are 11%, 11%, and 12% respectively;
[0081] Controlled rolling cooling: directly into water, red-return temperature 648℃, cooling rate 3~10℃ / s;
[0082] Quenching: 915℃ quenching, 200min in furnace, water cooling; quenching machine high pressure section pressure 8.3bar, low pressure section pressure 4.0bar, steel plate surface temperature after quenching 38℃.
[0083] Tempering: Tempering at 655℃, 239min in furnace, air cooling + stack cooling. Stack cooling after tempering, stack cooling temperature 288℃, stack cooling time 32 hours, then destacking.
[0084] Example 3
[0085] The chemical composition of the steel plate is as follows by weight: C 0.08%, Si 0.25%, Mn 1.39%, P 0.012%, S 0.002%, Nb 0.011%, Ti 0.018%, Als 0.022%, Cu 0.45%, Ni 0.99%, Sb 0.21%, and the rest are Fe and unavoidable impurity elements.
[0086] Continuous casting: molten steel superheat degree is 7℃; full protection pouring is adopted in continuous casting to avoid molten steel from contacting with air, so as to control the absorption of nitrogen in the air by molten steel during pouring; heavy pressure reduction technology is adopted at the end of solidification to improve the internal segregation and internal looseness of slab;
[0087] Heating: The heating furnace adopts a mixed gas reducing atmosphere, the heating section temperature is 1200℃~1240℃, the soaking section temperature is 1210℃, and the soaking section is kept warm for 30min;
[0088] Rolling: Rough rolling adopts a large reduction system, and the reduction rates of the three consecutive passes after widening are 16%, 18%, and 18% respectively; the final rolling temperature of finishing rolling is 806℃, and the reduction rates of the first three passes of finishing rolling are 12%, 12%, and 13% respectively;
[0089] Controlled rolling cooling: directly into water, red-return temperature 633℃, cooling rate 3~10℃ / s;
[0090] Quenching: 919℃ quenching, furnace time 202min, water cooling; quenching machine high pressure section pressure 8.1bar, low pressure section pressure 3.9bar, steel plate surface temperature after quenching 36℃.
[0091] Tempering: Tempering at 670℃, 305min in furnace, air cooling + stack cooling. Stack cooling after tempering, stack cooling temperature 255℃, stack cooling time 25 hours, then destacking.
[0092] Example 4
[0093] The chemical composition of the steel plate is as follows by weight: C 0.06%, Si 0.39%, Mn 1.44%, P 0.010%, S 0.001%, Nb 0.015%, Ti 0.010%, Als 0.039%, Cu 0.36%, Ni 1.47%, Sb 0.29%, and the rest are Fe and unavoidable impurity elements.
[0094] Continuous casting: molten steel superheat degree is 8℃; continuous casting adopts full protection pouring to avoid molten steel from contacting with air, so as to control the absorption of nitrogen in the air by molten steel during pouring; continuous casting adopts heavy pressure reduction technology at the end of solidification to improve the internal segregation and internal looseness of slab;
[0095] Heating: The heating furnace adopts a mixed gas reducing atmosphere, the heating section temperature is 1160℃~1220℃, the soaking section temperature is 1178℃, and the soaking section is kept warm for 31min;
[0096] Rolling: Rough rolling adopts a large reduction system, and the reduction rates of the three consecutive passes after widening are 16%, 16%, and 17% respectively; the final rolling temperature of finishing rolling is 753℃, and the reduction rates of the first three passes of finishing rolling are 11%, 11%, and 12% respectively;
[0097] Controlled rolling cooling: directly into water, red-return temperature 604℃, cooling rate 3~10℃ / s;
[0098] Quenching: 907℃ quenching, 183min in furnace, water cooling; quenching machine high pressure section pressure 8.2bar, low pressure section pressure 4.0bar, steel plate surface temperature after quenching 35℃.
[0099] Tempering: Tempering at 652℃, 254min in furnace, air cooling + stack cooling. Stack cooling after tempering, stack cooling temperature 245℃, stack cooling time 25 hours, then destacking.
[0100] Example 5
[0101] The chemical composition of the steel plate is as follows by weight: C 0.07%, Si 0.28%, Mn 1.29%, P 0.009%, S 0.002%, Nb 0.014%, Ti 0.011%, Als 0.035%, Cu 0.63%, Ni 0.74%, Sb 0.15%, and the rest are Fe and unavoidable impurity elements.
[0102] Continuous casting: molten steel superheat degree is 14℃; full protection pouring is adopted in continuous casting to avoid molten steel from contacting with air, so as to control the absorption of nitrogen in the air by molten steel during pouring; heavy pressure reduction technology is adopted at the end of solidification to improve the internal segregation and internal looseness of slab;
[0103] Heating: The heating furnace adopts a mixed gas reducing atmosphere, the heating section temperature is 1165℃~1190℃, the soaking section temperature is 1168℃, and the soaking section is kept warm for 39 minutes;
[0104] Rolling: Rough rolling adopts a large reduction system, and the reduction rates of the three consecutive passes after widening are 16%, 14%, and 17% respectively; the final rolling temperature of finishing rolling is 809℃, and the reduction rates of the first three passes of finishing rolling are 14%, 16%, and 13% respectively;
[0105] Controlled rolling cooling: directly into water, red-return temperature 642℃, cooling rate 3~10℃ / s;
[0106] Quenching: 920℃ quenching, furnace time is 235min, water cooling; quenching machine high pressure section pressure is 8.1bar, low pressure section pressure is 4.3bar, and the surface temperature of the steel plate after quenching is 32℃.
[0107] Tempering: Tempering at 668℃, 345min in furnace, air cooling + stack cooling. Stack cooling after tempering, stack cooling temperature 298℃, stack cooling time 31 hours, then destacking.
[0108] Example 6
[0109] The chemical composition of the steel plate is as follows by weight: C 0.08%, Si 0.25%, Mn 1.32%, P 0.009%, S0.001%, Nb 0.020%, Ti 0.020%, Als 0.047%, Cu 0.30%, Ni 1.39%, Sb 0.20%, and the rest are Fe and unavoidable impurity elements.
[0110] Continuous casting: molten steel superheat degree is 8℃; continuous casting adopts full protection pouring to avoid molten steel from contacting with air, so as to control the absorption of nitrogen in the air by molten steel during pouring; continuous casting adopts heavy pressure reduction technology at the end of solidification to improve the internal segregation and internal looseness of slab;
[0111] Heating: The heating furnace adopts a mixed gas reducing atmosphere, the heating section temperature is 1170℃~1230℃, the soaking section temperature is 1190℃, and the soaking section is kept warm for 41min;
[0112] Rolling: Rough rolling adopts a large reduction system, and the reduction rates of the three consecutive passes after widening are 15%, 15%, and 15% respectively; the final rolling temperature of finishing rolling is 799℃, and the reduction rates of the first three passes of finishing rolling are 14%, 14%, and 14% respectively;
[0113] Controlled rolling cooling: directly into water, red-return temperature 615℃, cooling rate 3~10℃ / s;
[0114] Quenching: 909℃ quenching, furnace time is 204min, water cooling; quenching machine high pressure section pressure is 8.4bar, low pressure section pressure is 4.2bar, and the surface temperature of the steel plate after quenching is 30℃.
[0115] Tempering: Tempering at 669℃, 284min in furnace, air cooling + stack cooling. Stack cooling after tempering, stack cooling temperature 268℃, stack cooling time 30 hours, then destacking.
[0116] Comparative Example 1
[0117] Bridge steel Q460qENH, the chemical composition of the steel plate is as follows by weight: C 0.07%, Si 0.29%, Mn1.39%, P 0.009%, S 0.001%, Nb 0.035%, Ti 0.019%, Als 0.037%, Cu 0.28%, Ni0.35%, Mo 0.12%, Cr 0.48%, B 0.0011, and the rest are Fe and unavoidable impurity elements.
[0118] Continuous casting: molten steel superheat 9°C;
[0119] Heating: The heating furnace adopts a mixed gas reducing atmosphere, the heating section temperature is 1180℃~1200℃, the soaking section temperature is 1195℃, and the soaking section is kept warm for 38min;
[0120] Rolling: Rough rolling adopts a large reduction system, and the reduction rates of the three consecutive passes after widening are 18%, 18%, and 19% respectively; the final rolling temperature of finishing rolling is 777℃, and the reduction rates of the first three passes of finishing rolling are 14%, 14%, and 14% respectively;
[0121] Controlled rolling cooling: directly into water, red-return temperature 609℃, cooling rate 3~10℃ / s;
[0122] Quenching: 915℃ quenching, furnace time 208min, water cooling;
[0123] Tempering: Tempering at 668℃, 279min in furnace, air cooling.
[0124] Experimental example
[0125] The performance tests were carried out on the steel plates prepared in Examples 1-6 of the present invention and Comparative Example 1. The specific results are shown in Figure 1-3 and Table 1-2.
[0126] Table 1 Properties of the steels of the present invention and the comparative examples
[0127]
[0128] The statistical segregation of C, Mn, Ni, Cu and Sb of the steel plates prepared in Examples 1 to 6 and Comparative Example 1 was measured according to the general rules of the metal in-situ statistical distribution method GB / T 24213-2009. The results are shown in Table 2.
[0129] Table 2 Statistical segregation of C, Mn, Ni, Cu and Sb in the steels of the present invention and the comparative example
[0130] Statistical segregation C Mn Ni Cu Sb Example 1 0.030 0.020 0.006 0.025 0.044 Example 2 0.034 0.014 0.008 0.031 0.042 Example 3 0.032 0.019 0.009 0.039 0.042 Example 4 0.035 0.019 0.007 0.032 0.043 Example 5 0.028 0.017 0.012 0.036 0.043 Example 6 0.027 0.022 0.012 0.028 0.040 Comparative Example 0.153 0.036 0.027 0.068 0.193
[0131] Corrosion test:
[0132] The dry-wet cyclic immersion experiment utilizes a periodic immersion corrosion test chamber to simulate marine atmospheric corrosion. The experiment was carried out for a total of 336 hours, and samples were taken once at 48 hours, 96 hours, 144 hours, 240 hours and 336 hours, respectively. Eight parallel samples were taken for each steel of Examples 1-6 and Comparative Example 1, of which three samples were used for corrosion weight loss measurement. The physical phase of the corrosion rust layer of the three samples was analyzed by X-ray diffractometer (XRD), the morphology of the surface of the rust layer of one of the samples was observed by scanning electron microscopy (SEM), and the cross-sectional morphology and alloy element distribution of the other sample were observed by SEM.
[0133] The corrosive medium is 0.5% NaCl (mass fraction) solution, and the temperature is constant at (42±1)°C; the temperature in the drying box is (45±1)°C, and the humidity is (30±2)%. Each dry-wet cycle is 80 minutes, of which the soaking time is 18 minutes and the drying time is 62 minutes.
[0134] Immerse the weightless sample in the prepared rust removal solution (500ml hydrochloric acid + 500ml distilled water + 20g hexamethylenetetramine) for ultrasonic cleaning. The rust-removed sample is cleaned with anhydrous ethanol, quickly blown dry and weighed to record W1. By (W0-W1) / (Sρ) (where S is the corrosion area of the sample, unit: cm 2 ; ρ is the density of the experimental steel, unit is g / cm 3 ) to calculate the corrosion reduction. By K(W0-W1) / (T Sρ) (where K is a constant, here 8.76×10 4 ; T is the acceleration time, in h) to calculate the average corrosion rate.
[0135] Results Figure 4 and Table 3.
[0136] Table 3 Relative corrosion rates of the steels of the present invention and the comparative steels (336 h)
[0137]
[0138] In summary, a trace amount of Sb element is added to the Ni-Cu system in the corrosion-resistant system of the present invention, and the core quality is improved by in-situ analysis technology. Compared with the control example, the core toughness is more excellent, and the corrosion resistance is far better than the control example, which has application prospects in resistance to marine atmospheric corrosion.
[0139] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0140] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A Q460 grade improved toughness high corrosion resistant steel plate, characterized in that: The chemical composition weight percentage of the Q460 grade improved toughness and high corrosion-resistant steel plate is: C: 0.06%~0.08%, Si: 0.15%~0.40%, Mn: 1.28%~1.45%, P≤0.020%, S≤0.003%, Nb: 0.01%~0.02%, Ti: 0.01%~0.02%, Als: 0.02%~0.05%, Cu: 0.30%~0.70%, Ni: 0.7%~1.5%, Sb: 0.08%~0.30%, and the rest is Fe and unavoidable impurity elements.
2. The Q460 grade improved toughness high corrosion resistant steel plate according to claim 1, characterized in that: The steel plate has a yield strength ReL ≥ 460 MPa, such as 498 MPa, 500 MPa, 502 MPa, 504 MPa, 512 MPa, 517 MPa; and / or, the steel plate has a tensile strength Rm ≥ 570 MPa, such as 665 MPa, 666 MPa, 673 MPa, 674 MPa, 681 MPa; and / or, the elongation after fracture A of the steel plate is ≥30%, such as 33.5%, 34%, 34.5%, 36%, 38.5%; and / or, the low temperature -60°C impact toughness KV2 of the steel plate is ≥120J; And / or, the low temperature -60°C impact toughness KV2 of the steel plate at 1 / 2 thickness is ≥120J; And / or, the steel plate has a lamellar tearing resistance Z ≥ 35%.
3. The Q460 grade improved toughness high corrosion resistant steel plate according to claim 1, characterized in that: The content of C is 0.06-0.08%, for example 0.06%, 0.07% or 0.08%; and / or Si content is 0.25-0.40%, for example 0.25%, 0.28%, 0.30%, 0.39%; and / or the content of Mn is 1.28-1.45%, for example 1.28%, 1.29%, 1.32%, 1.38%, 1.39%, 1.44%; and / or P content ≤ 0.0140%, such as 0.014%, 0.012%, 0.010%, 0.009%; and / or S content ≤ 0.002%, for example 0.002%, 0.001%; and / or Nb content is 0.01-0.02%, for example, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.020%; and / or the content of Ti is 0.01-0.02%, for example, 0.010%, 0.011%, 0.017%, 0.018%, 0.020%; and / or the content of Als is 0.02-0.05%, for example, 0.022%, 0.025%, 0.035%, 0.039%, 0.045%, 0.047%; and / or Cu content is 0.30-0.70%, for example 0.30%, 0.35%, 0.36%, 0.45%, 0.57%, 0.63%; and / or Ni content is 0.7% to 1.5%, for example 0.74%, 0.99%, 1.05%, 1.29%, 1.39%, 1.47%, And / or the Sb content is 0.08% to 0.30%, for example, 0.09%, 0.15%, 0.17%, 0.20%, 0.21%, 0.29%.
4. A method for producing Q460 grade improved toughness high corrosion resistant steel plate according to any one of claims 1 to 3, wherein the production process comprises molten iron pretreatment → converter steelmaking → refining outside the furnace LF → vacuum treatment RH → continuous casting → heating → rolling → controlled rolling cooling → quenching → tempering → finishing, characterized in that: The key process steps include: Continuous casting: The superheat of molten steel is less than 15℃; full protection casting is adopted to avoid the contact between molten steel and air, so as to control the absorption of nitrogen in the air by molten steel during the casting process; the heavy pressure reduction technology at the end of solidification is adopted to improve the internal segregation and internal looseness of the slab; Heating: The heating furnace adopts reducing atmosphere, the heating section temperature is 1100℃~1240℃, the soaking section temperature is 1100℃~1200℃, and the soaking section insulation time is ≥30min; Rolling: Rough rolling adopts a large reduction system to ensure that the reduction rate of three consecutive passes after widening is ≥14%; the final rolling temperature of finishing rolling is 750℃~820℃, and the reduction rate of the first three passes of finishing rolling is ≥10%; Controlled rolling cooling: directly into water, red-return temperature 600℃~660℃, cooling rate 3~10℃ / s; Quenching: 900℃~920℃ quenching, the furnace time is plate thickness mm×(1.4~2.5)min / mm, water cooling, quenching ensures that the high pressure section pressure of the quenching machine is ≥8bar, the low pressure section pressure is ≥3.5bar, and the surface temperature of the steel plate after quenching is ≤40℃; Tempering: Tempering at 650-670℃, the time in the furnace is plate thickness mm×(2.0-3.5)min / mm, air cooling + stack cooling, stack cooling after tempering, stack cooling temperature 200-300℃, stack cooling time ≥24 hours before destacking.
5. The method for producing a Q460 grade improved toughness high corrosion resistant steel plate according to claim 4, characterized in that: The reducing atmosphere is mixed coal gas.
6. The method for producing a Q460 grade improved toughness high corrosion resistant steel plate according to claim 4, characterized in that: The quenching temperature is 900°C to 920°C, for example, 900°C, 907°C, 909°C, 915°C, 919°C, 920°C; And / or the time in the furnace is plate thickness mm×(1.4-2.5) min / mm, for example 183 min, 200 min, 202 min, 204 min, 235 min, 245 min.
7. The method for producing a Q460 grade improved toughness high corrosion resistant steel plate according to claim 4, characterized in that: The pressure of the high-pressure section of the quenching machine is ≥8 bar, such as 8.1 bar, 8.2 bar, 8.3 bar, 8.4 bar; and / or the pressure of the low-pressure section of the quenching machine is ≥3.5 bar, such as 3.9 bar, 4.0 bar, 4.1 bar, 4.2 bar, 4.3 bar.
8. The method for producing a Q460 grade improved toughness high corrosion resistant steel plate according to claim 4, characterized in that: The tempering temperature is 650-670°C, for example, 652°C, 654°C, 655°C, 668°C, 670°C; And / or the time in the furnace is plate thickness mm×(2.0~3.5)min / mm, for example 239min, 254min, 256min, 284min, 305min, 345min.
9. A method for producing a Q460 grade improved toughness high corrosion resistant steel plate according to any one of claims 5 to 8, characterized in that: The thickness of the Q460 grade improved toughness high corrosion resistant steel plate is ≤100mm.
10. An application of the Q460 grade improved toughness high corrosion resistant steel plate as claimed in any one of claims 1 to 3 in the production of steel for island and reef infrastructure construction, cross-sea bridge construction, coastal building construction and ship and marine engineering.
Citation Information
Patent Citations
Production method of quenched and tempered steel plate for Q460-grade high-corrosion-resistance high-strength offshore structure
CN115216609A
Production method of S690QL1-grade extra-thick high-strength structural steel
CN115216698A
Quenched and tempered steel plate for 960MPa-grade extra-thick high-strength structure and production method of quenched and tempered steel plate
CN117286414A
Production method of 960MPa-grade steel for crane jib
CN117778899A
Q500-grade improved high-toughness corrosion-resistant steel plate as well as production method and application thereof
CN117821853A