Martensitic stainless steel hardening method
Through the combination technology of sand blowing, ultrasonic cleaning and high-temperature permeability media, the problem of difficulty in infiltration of carbon and nitrogen atoms in the hardening of martensite stainless steel is solved, and more efficient hardening treatment is achieved, which significantly improves hardness and wear resistance.
Patent Information
- Application Number
- CN202410944725.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, during the hardening of martensite stainless steel, carbon and nitrogen atoms are difficult to penetrate into the matrix, resulting in poor hardness improvement effect and low heat treatment efficiency, mainly due to the presence of the surface passivation film and the uneven distribution of heat energy inside the furnace.
Use sand blowing treatment, ultrasonic cleaning and copper chloride hydrochloride solution to remove surface impurities, and combine high-temperature permeability medium for carbon and nitrogen co-permeability to ensure that carbon and nitrogen atoms penetrate at critical temperatures, and use muffle tank well furnaces Distribute heat quickly.
The infiltration activity and hardening efficiency of carbon and nitrogen atoms are improved, and a uniform carbon-nitrogen co-permeability layer is formed, which significantly improves the hardness and wear resistance of martensitic stainless steel.
Smart Images

Figure CN118880221A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat treatment technology, and in particular relates to a martensitic stainless steel hardening method. Background Art
[0002] Martensitic stainless steel is a type of hardenable stainless steel. Typical martensitic stainless steel grades include 2Cr13, 3Cr13, 4Cr13, etc. Martensitic stainless steel has a martensitic crystal structure, which is a body-centered tetragonal structure. Since martensitic stainless steel is magnetic, it can be used in various occasions that require magnetism, such as aircraft engines, motors or transformers. Since martensitic stainless steel contains a higher content of carbon and less nickel, the martensitic crystal structure can be hardened by heat treatment, thereby improving the strength and hardness of martensitic stainless steel.
[0003] For example, the patent document with publication number "CN102168254A" discloses a surface hardening method for martensitic stainless steel, and its technical solution is: firstly place the treated martensitic stainless steel workpiece on the workbench of the vacuum chamber of the ion implanter, and evacuate to 2.0×10 -3 ~3.0×10 -3 Pa, the passivation layer on the surface of the workpiece is removed by an ion cleaning source; then nitrogen ions are injected into the martensitic stainless steel workpiece with the surface passivation layer removed to obtain surface hardened martensitic stainless steel. The conditions for injecting nitrogen ions are: vacuum degree of 5.0×10 -4 ~5.0×10 -2 Pa, the ion source acceleration voltage is 10-100 kV, and the injection dose is 5.0×10 15 ~5.0×10 19 ions / cm 2 The working conditions of the cleaning source are: filament current 6-10A, arc voltage 40-70V, extraction voltage 0.6-1.5kV, extraction current 40-70mA. For another example, the patent document with publication number "CN117626166A" discloses a method for surface nitriding superhardening of high nitrogen martensitic stainless steel, including: step 1, spheroidizing treatment and quenching and tempering treatment; step 2, long-term surface nitriding treatment, nitriding time more than 25h; step 3, organization stabilization tempering.
[0004] It can be seen that carbonitriding of martensitic stainless steel is the main way to improve the hardness and wear resistance of martensitic stainless steel. However, when storing martensitic stainless steel, the matrix material on the surface of the martensitic stainless steel will combine with elements such as oxygen atoms in the atmospheric environment to form a passivation film on the surface of the martensitic stainless steel. The passivation film prevents carbon and nitrogen atoms from penetrating into the martensitic stainless steel matrix, resulting in a low thickness of the carbon and nitrogen co-penetration layer and a poor effect on improving the surface hardness of the martensitic stainless steel. In the technology disclosed in the aforementioned patent document, before hardening the surface of the martensitic stainless steel, corresponding technical means have to be taken to remove the passivation film on the surface of the martensitic stainless steel. In addition, the prior art usually uses a special furnace to harden the martensitic stainless steel. When the furnace door is opened and the workpiece is loaded, the heat energy in the furnace is transferred to the workpiece, so that the heat energy inside the furnace is redistributed. At this time, the surface temperature of the workpiece has not yet reached the critical temperature for carbon and nitrogen atoms to penetrate into the martensitic stainless steel matrix, and carbon and nitrogen atoms cannot penetrate, which affects the hardening efficiency of the martensitic stainless steel. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for hardening martensitic stainless steel.
[0006] The present invention is achieved through the following technical solutions.
[0007] The present invention provides a method for hardening martensitic stainless steel, comprising the following steps:
[0008] Step 1: providing a workpiece, wherein the workpiece is made of martensitic stainless steel;
[0009] Step 2: performing sand blasting on the workpiece;
[0010] Step 3: putting the workpiece into an ultrasonic cleaning machine, and putting a cleaning agent into the ultrasonic cleaning machine, and cleaning the workpiece with the ultrasonic cleaning machine to form a water film on the surface of the workpiece;
[0011] Step 4: Soak the workpiece in a copper chloride solution and then take it out, and then wash the workpiece with clean water;
[0012] Step 5: Drain the workpiece;
[0013] Step 6: providing a furnace, and then placing the workpiece into the furnace;
[0014] Step 7: treating the workpiece once: maintaining the temperature in the furnace at the first characteristic temperature within a first characteristic time, and continuously feeding the infiltration layer medium into the furnace;
[0015] Step 8: performing secondary treatment on the workpiece: maintaining the temperature in the furnace at a second characteristic temperature within a second characteristic time, wherein the second characteristic temperature is not greater than the first characteristic temperature, and continuously feeding the infiltration layer medium into the furnace;
[0016] Step nine: Take out the workpiece and allow it to cool naturally to room temperature.
[0017] The process conditions for sandblasting the workpiece in step 2 are: feeding white corundum gravel with a particle size of 180# into a sandblasting machine to accelerate the movement to form a gravel flow, and allowing the gravel flow to continue flowing along the surface of the workpiece for at least 5 minutes.
[0018] The process conditions for cleaning the workpiece with an ultrasonic cleaning machine in step three are: the specification model of the ultrasonic cleaning machine is: LK / CS-72, the cleaning agent is 5948 cleaning agent or acetone solution, the ultrasonic vibration frequency is 28Hz-30Hz, and the cleaning duration is 10min-15min.
[0019] The process conditions for immersing the workpiece in the cupric chloride solution in step 4 are: the volume concentration of the cupric chloride solution is 5%, and the workpiece is immersed in the cupric chloride solution for 10 min-20 min.
[0020] The martensitic stainless steel hardening method further comprises the following steps: before performing step six, steps three to five are repeated at least once.
[0021] The process conditions for treating the workpiece once in step seven are: the first characteristic time is more than 30 minutes, the first characteristic temperature is 570°C, the diffusion layer medium includes ammonia and ethanol, the flow rate of ammonia into the furnace is 0.8 L / min, and the flow rate of ethanol into the furnace is 75 drops / min.
[0022] The process conditions for the secondary treatment of the workpiece in step eight are: the second characteristic time is 420min to 480min, the second characteristic temperature is 560°C, the diffusion layer medium includes ammonia and ethanol, the flow rate of ammonia into the furnace is 0.65L / min, and the flow rate of ethanol into the furnace is 65 drops / min.
[0023] The furnace is a muffle pit furnace.
[0024] A supporting device is provided in the furnace, and the supporting device includes a column, a supporting ring, a seat ring, a plurality of spokes and a plurality of carrier wires. The column is fixedly connected between the supporting ring and the seat ring, the spokes are fixedly connected between the supporting ring and the column, and between the seat ring and the column, and both ends of the carrier wire are bolted between the supporting ring and the seat ring.
[0025] A fan is also provided in the stove, and the fan is arranged above the supporting device.
[0026] The beneficial effects of the present invention are as follows: by adopting the technical scheme of the present invention, firstly, the surface of the workpiece is subjected to sandblasting treatment, so that the surface roughness of the workpiece is improved, so that carbon and nitrogen atoms can more easily penetrate into the workpiece matrix, and then the surface of the workpiece is repeatedly cleaned by an ultrasonic cleaning machine and a hydrochloric acid copper chloride solution, so that various impurities, passivation films and protective films on the surface of the workpiece are thoroughly removed, which is further conducive to promoting the carbon and nitrogen atoms to penetrate into the interior of the workpiece matrix, and when carbon and nitrogen are co-diffused, the workpiece is first subjected to carbonitriding under the condition of being higher than the critical temperature for carbon and nitrogen atoms to penetrate into the martensitic stainless steel matrix, which is conducive to enhancing the activity of carbon and nitrogen atoms so that they can more actively penetrate into the interior of the workpiece matrix at the beginning of heat treatment; on the other hand, when the furnace door is opened and the workpiece is loaded, since the internal temperature of the furnace is higher than the aforementioned critical temperature, the internal heat energy of the furnace can be quickly redistributed, the surface temperature of the workpiece quickly reaches the aforementioned critical temperature, and carbon and nitrogen atoms quickly penetrate into the interior of the workpiece matrix, thereby improving the hardening treatment efficiency of the martensitic stainless steel; and then, the workpiece is subjected to carbonitriding under the condition of the critical temperature, which is conducive to forming a uniform carbonitriding layer on the surface of the workpiece. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a process flow chart of the present invention;
[0028] Figure 2 It is a structural schematic diagram of the stove, the supporting device and the fan of the present invention;
[0029] Figure 3 It is a schematic structural diagram of the support ring, spokes and pillars of the present invention.
[0030] In the figure: 1-workpiece, 2-furnace, 3-support device, 4-column, 5-support ring, 6-seat ring, 7-spoke, 8-wire, 9-fan, 10-inlet pipe, 11-exhaust pipe. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.
[0032] like Figures 1 to 3 As shown, the present invention provides a method for hardening martensitic stainless steel, comprising the following steps:
[0033] Step 1: providing a workpiece 1, wherein the workpiece 1 is made of martensitic stainless steel;
[0034] Step 2: performing sand blasting on the workpiece 1;
[0035] Step 3: Put the workpiece 1 into an ultrasonic cleaning machine, and put a cleaning agent into the ultrasonic cleaning machine, and use the ultrasonic cleaning machine to clean the workpiece 1 so that a water film is formed on the surface of the workpiece 1;
[0036] Step 4: Soak the workpiece 1 in a hydrochloric acid copper chloride solution, take it out, and then wash the workpiece 1 with clean water;
[0037] Step 5: Drain the workpiece 1;
[0038] Step 6: Provide a furnace 2, and then put the workpiece 1 into the furnace 2;
[0039] Step 7: Performing a treatment on the workpiece 1: maintaining the temperature in the furnace 2 at the first characteristic temperature within the first characteristic time, and continuously feeding the infiltration layer medium into the furnace 2;
[0040] Step 8: Perform secondary treatment on the workpiece 1: keep the temperature in the furnace 2 at a second characteristic temperature within a second characteristic time, and the second characteristic temperature is not greater than the first characteristic temperature, and continuously feed the infiltration layer medium into the furnace 2;
[0041] Step nine: Take out the workpiece 1 and allow the workpiece 1 to cool naturally to room temperature.
[0042] Specifically, the grade of the workpiece 1 is 2Cr13, the workpiece 1 is cylindrical, and the outer dimensions of the workpiece 1 are: outer diameter×inner diameter×thickness=φ8mm×φ6mm×1mm. According to the technical solution of the present invention, the surface of the workpiece is firstly subjected to sandblasting treatment to improve the surface roughness of the workpiece, so that carbon and nitrogen atoms can more easily penetrate into the workpiece matrix. Then, the surface of the workpiece is repeatedly cleaned by an ultrasonic cleaning machine and a hydrochloric acid and copper chloride solution to thoroughly remove various impurities, passivation films and protective films on the surface of the workpiece, which is further conducive to promoting the penetration of carbon and nitrogen atoms into the interior of the workpiece matrix. When carbon and nitrogen co-diffusion is performed, the workpiece is first subjected to carbonitriding under conditions higher than the critical temperature for carbon and nitrogen atoms to penetrate into the martensitic stainless steel matrix. On the one hand, it is conducive to enhancing the activity of carbon and nitrogen atoms so that they can more actively penetrate into the interior of the workpiece matrix at the beginning of heat treatment. On the other hand, when the furnace door is opened and the workpiece is loaded, the internal temperature of the furnace is higher than the aforementioned critical temperature, so that the internal heat energy of the furnace can be quickly redistributed, the surface temperature of the workpiece quickly reaches the aforementioned critical temperature, and carbon and nitrogen atoms quickly penetrate into the interior of the workpiece matrix, thereby improving the hardening treatment efficiency of the martensitic stainless steel. Then, the workpiece is subjected to carbonitriding under the conditions of the critical temperature, which is conducive to forming a uniform carbonitriding layer on the surface of the workpiece.
[0043] Specifically, the process conditions for sandblasting the workpiece 1 in step 2 are: feeding white corundum gravel with a particle size of 180# into the sandblasting machine to accelerate the movement to form a gravel flow, and allowing the gravel flow to flow along the surface of the workpiece 1 for at least 5 minutes. By sandblasting the workpiece, the surface roughness of the workpiece reaches more than 1.2um. When the workpiece is subjected to carbonitriding, the matrix structure on the surface of the workpiece will produce a capillary effect, allowing carbon and nitrogen atoms to more easily penetrate into the matrix structure of the workpiece.
[0044] Furthermore, the process conditions for cleaning the workpiece 1 with an ultrasonic cleaning machine in step three are: the specification model of the ultrasonic cleaning machine is: LK / CS-72, the cleaning agent is 5948 cleaning agent or acetone solution, the ultrasonic vibration frequency is 28Hz-30Hz, and the cleaning duration is 10min-15min. The process conditions for soaking the workpiece 1 in a hydrochloric acid copper chloride solution in step four are: the volume concentration of the hydrochloric acid copper chloride solution is 5%, and the soaking duration of the workpiece 1 in the hydrochloric acid copper chloride solution is 10min-20min. The martensitic stainless steel hardening method also includes the following steps: before performing step six, steps three to five are repeated at least once. Using the technical solution of the present invention, an ultrasonic cleaning machine and a hydrochloric acid copper chloride solution are used to repeatedly clean the surface of the workpiece, and various impurities, passivation films and protective films on the surface of the workpiece are thoroughly removed, which is further conducive to promoting carbon and nitrogen atoms to penetrate into the workpiece matrix.
[0045] In addition, the process conditions for the primary treatment of the workpiece 1 in step 7 are: the first characteristic time is more than 30 minutes, the first characteristic temperature is 570°C, the infiltration medium includes ammonia and ethanol, the flow rate of ammonia into the furnace 2 is 0.8L / min, and the flow rate of ethanol into the furnace 2 is 75 drops / min. The process conditions for the secondary treatment of the workpiece 1 in step 8 are: the second characteristic time is 420min to 480min, the second characteristic temperature is 560°C, the infiltration medium includes ammonia and ethanol, the flow rate of ammonia into the furnace 2 is 0.65L / min, and the flow rate of ethanol into the furnace 2 is 65 drops / min. Preferably, the furnace 2 is a muffle pit furnace. By adopting the technical solution of the present invention, when carbonitriding is performed, the workpiece is first carbonitrided under conditions higher than the critical temperature for carbon and nitrogen atoms to penetrate into the martensitic stainless steel matrix. On the one hand, this is beneficial to enhancing the activity of carbon and nitrogen atoms so that they can more actively penetrate into the interior of the workpiece matrix at the beginning of heat treatment; on the other hand, when the furnace door is opened and the workpiece is loaded, since the internal temperature of the furnace is higher than the aforementioned critical temperature, the internal heat energy of the furnace can be quickly redistributed, the surface temperature of the workpiece quickly reaches the aforementioned critical temperature, and carbon and nitrogen atoms quickly penetrate into the interior of the workpiece matrix, thereby improving the hardening treatment efficiency of the martensitic stainless steel; then, the workpiece is carbonitrided under the critical temperature condition, which is beneficial to forming a uniform carbonitriding layer on the surface of the workpiece.
[0046] Specifically, the furnace 2 is provided with a support device 3, which includes a column 4, a support ring 5, a seat ring 6, a plurality of spokes 7 and a plurality of carrier wires 8. The column 4 is fixedly connected between the support ring 5 and the seat ring 6, the spokes 7 are fixedly connected between the support ring 5 and the column 4, between the seat ring 6 and the column 4, and the two ends of the carrier wire 8 are bolted between the support ring 5 and the seat ring 6. The workpiece can be connected in series to each carrier wire 8, and the material of the carrier wire 8 is preferably nickel-iron alloy. The number of spokes 7 is more than 6, so that the martensitic stainless steel workpieces are heat treated in batches. The furnace 2 is also provided with a fan 9, and the fan 9 is arranged above the support device 3. When the workpiece is carbonitrided, the fan 9 is operated to make the carbon and nitrogen atoms sent into the furnace evenly distributed and evenly penetrate into the workpiece surface matrix, so that a more uniform carbonitrided layer is formed on the workpiece surface.
[0047] In addition, the furnace 2 is also provided with an input pipe 10. The furnace 2 is also provided with an exhaust pipe 11. The input pipe 10 is used to continuously feed the infiltration medium such as ammonia and ethanol into the furnace, and the remaining gas in the furnace that has not penetrated into the workpiece matrix is discharged through the exhaust pipe 11. At the end of the exhaust pipe, the excess infiltration medium can be ignited to burn to generate methylamine and water, so as to avoid the infiltration medium being directly discharged into the atmosphere to cause environmental pollution.
[0048] Taking a 2Cr13 martensitic stainless steel workpiece as an example, after being processed by the technical solution of the present invention, the hardness of the carbonitriding layer on the surface of the workpiece can reach HV0.3=970, and the thickness of the carbonitriding layer can reach more than 12 mm. The wear resistance of the carbonitriding layer of the workpiece is tested. The test results show that the wear resistance of the carbonitriding layer on 500# sandpaper can reach 20 turns / 0.01 mm, which significantly improves the hardness and wear resistance of the 2Cr13 martensitic stainless steel workpiece.
Claims
1. A method for hardening martensitic stainless steel, characterized in that: The following steps are involved: Step 1: providing a workpiece (1), wherein the workpiece (1) is made of martensitic stainless steel; Step 2: performing sandblasting treatment on the workpiece (1); Step 3: putting the workpiece (1) into an ultrasonic cleaning machine, and putting a cleaning agent into the ultrasonic cleaning machine, and cleaning the workpiece (1) with the ultrasonic cleaning machine to form a water film on the surface of the workpiece (1); Step 4: soaking the workpiece (1) in a copper chloride solution, taking it out, and then washing the workpiece (1) with clean water; Step 5: draining the workpiece (1); Step 6: providing a furnace (2), and then placing the workpiece (1) into the furnace (2); Step 7: performing a treatment on the workpiece (1): maintaining the temperature in the furnace (2) at the first characteristic temperature within a first characteristic time, while continuously supplying a diffusion layer medium into the furnace (2); Step eight: performing secondary treatment on the workpiece (1): maintaining the temperature in the furnace (2) at a second characteristic temperature within a second characteristic time, wherein the second characteristic temperature is not greater than the first characteristic temperature, and continuously feeding the infiltration layer medium into the furnace (2); Step nine: taking out the workpiece (1) and allowing the workpiece (1) to cool naturally to room temperature.
2. The method for hardening martensitic stainless steel according to claim 1, characterized in that: The process conditions for sandblasting the workpiece (1) in step 2 are: feeding white corundum gravel with a particle size of 180# into a sandblasting machine to accelerate the movement to form a gravel flow, and allowing the gravel flow to continue flowing along the surface of the workpiece (1) for at least 5 minutes.
3. The method for hardening martensitic stainless steel according to claim 1, characterized in that: The process conditions for cleaning the workpiece (1) with an ultrasonic cleaning machine in step 3 are: the specification model of the ultrasonic cleaning machine is: LK / CS-72, the cleaning agent is 5948 cleaning agent or acetone solution, the ultrasonic vibration frequency is 28Hz-30Hz, and the cleaning duration is 10min-15min.
4. The method for hardening martensitic stainless steel according to claim 1, characterized in that: The process conditions for immersing the workpiece (1) in the copper chloride solution for immersion in step 4 are: the volume concentration of the copper chloride solution is 5%, and the workpiece (1) is immersed in the copper chloride solution for 10 minutes to 20 minutes.
5. The method for hardening martensitic stainless steel according to claim 1, characterized in that: The martensitic stainless steel hardening method further comprises the following steps: before performing step six, steps three to five are repeated at least once.
6. The method for hardening martensitic stainless steel according to claim 1, characterized in that: The process conditions for treating the workpiece (1) once in step seven are: the first characteristic time is more than 30 minutes, the first characteristic temperature is 570°C, the diffusion layer medium includes ammonia and ethanol, the flow rate of ammonia into the furnace (2) is 0.8 L / min, and the flow rate of ethanol into the furnace (2) is 75 drops / min.
7. The method for hardening martensitic stainless steel according to claim 1, characterized in that: The process conditions for the secondary treatment of the workpiece (1) in step eight are: the second characteristic time is 420 min to 480 min, the second characteristic temperature is 560° C., the infiltration layer medium includes ammonia and ethanol, the flow rate of ammonia into the furnace (2) is 0.65 L / min, and the flow rate of ethanol into the furnace (2) is 65 drops / min.
8. The method for hardening martensitic stainless steel according to claim 1, 6 or 7, characterized in that: The furnace (2) is a muffle pit furnace.
9. The method for hardening martensitic stainless steel according to claim 1, characterized in that: The furnace (2) is provided with a supporting device (3), and the supporting device (3) comprises a column (4), a supporting ring (5), a seat ring (6), a plurality of spokes (7) and a plurality of carrier wires (8); the column (4) is fixedly connected between the supporting ring (5) and the seat ring (6); the spokes (7) are fixedly connected between the supporting ring (5) and the column (4), and between the seat ring (6) and the column (4); and both ends of the carrier wire (8) are bolted between the supporting ring (5) and the seat ring (6).
10. The method for hardening martensitic stainless steel according to claim 9, characterized in that: A fan (9) is also provided in the furnace (2), and the fan (9) is arranged above the supporting device (3).