High-temperature-resistant silicon dioxide aerogel thermal insulation material and preparation method thereof
By depositing nanofilms on the silica aerogel framework, the problems of sintering and structural changes of silica aerogel at high temperatures are solved, and the low thermal conductivity and stable pore structure at high temperatures are achieved, and the preparation process is simplified. , improves the high temperature resistance of the material.
Patent Information
- Application Number
- CN202410908151.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
AI Technical Summary
The existing silica aerogels are prone to sintering and structural changes in high temperature environments, resulting in increased thermal conductivity and pore collapse, limiting their application under high temperature conditions. The existing high-temperature aerogel preparation process is complex and difficult to Marketization.
The nanofilm is deposited on the skeleton of the silica aerogel by atomic layer deposition method, and organic salts containing aluminum or zirconium are used as precursors. By controlling the number of deposition cycles and reaction conditions, high-temperature resistant silica aerosol is prepared. Glue insulation material.
At high temperatures above 800°C, the nanopores are relatively stable and have low thermal conductivity, which significantly improves the high-temperature thermal stability and thermal insulation effect of the material.
Smart Images

Figure CN118880281A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high temperature resistant material preparation, and in particular relates to a high temperature resistant silica aerogel thermal insulation material and a preparation method thereof. Background Art
[0002] Aerogels have emerged as an efficient thermal insulation material. Silica aerogels, in particular, are well known for their wide range of industrial uses and cost-effectiveness. Their nanoporous structure minimizes heat transfer, thereby improving energy efficiency and safety in everyday and high-tech applications. However, despite their many advantages, silica aerogels also have limitations. An important challenge is that they are prone to sintering and undergo structural changes at temperatures exceeding 800°C. This limitation hinders the use of aerogels in high-temperature environments.
[0003] To address these limitations, researchers have been working to develop new aerogels that can withstand extreme temperatures. Research has covered various types of aerogels, including low-crystalline ZrO2 nanofiber aerogels, SiC@SiO2 nanowire aerogels, and nanofiber ZrO2-Al2O3 aerogels. However, compared with silica aerogels, complex manufacturing processes have hindered their commercial viability. In addition, the thickness of nanofiber, nanowire, and nanosheet assemblies is usually several hundred nanometers, making it difficult to form nanopores smaller than the mean free path of air, thereby increasing thermal conductivity. Researchers have developed alumina and zirconia aerogels using a sol-gel method to obtain higher thermal stability than silica aerogels. However, they undergo phase transitions at high temperatures, destroying the pore structure. To mitigate these phase transitions, researchers have incorporated elements such as yttrium, lanthanum, and silicon into the aerogels to enhance thermal stability. Despite the progress, the inevitable partial crystal structure still leads to higher thermal conductivity and collapse of nanopores.
[0004] Therefore, there is an urgent need to provide a silica aerogel thermal insulation material that is simple to prepare and has good high temperature resistance. Summary of the invention
[0005] In order to solve the above technical problems, the present invention proposes a high temperature resistant silica aerogel thermal insulation material and a preparation method thereof.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] One of the technical solutions of the present invention:
[0008] A method for preparing a high temperature resistant silica aerogel thermal insulation material, using an organic salt containing aluminum or zirconium as a precursor, and using atomic layer deposition to deposit a layer of nanofilm on the skeleton of the silica aerogel to prepare a high temperature resistant silica aerogel thermal insulation material;
[0009] Wherein, the number of deposition cycles in the atomic layer deposition process is 5-120 times.
[0010] Preferably, the aluminum-containing organic salt is trimethylaluminum;
[0011] The zirconium-containing organic salt is tetramethyl(dimethylamino)zirconium.
[0012] Preferably, when an aluminum-containing organic salt is used as a precursor, one deposition cycle is one cycle, specifically:
[0013] After 0.06 s of aluminum-containing organic salt injection, a purge was performed for 9.94 s, followed by a plasma pulse for 5 s and a purge for 1 s.
[0014] Preferably, when the zirconium-containing organic salt is used as a precursor, one deposition cycle is one cycle, specifically:
[0015] After 0.6 s of zirconium-containing organic salt injection, a purge of 11.4 s was performed, followed by a 5 s plasma pulse and a 3 s purge.
[0016] Preferably, the reaction conditions during the atomic deposition process are:
[0017] Water was used as the oxygen source, nitrogen was used as the carrier gas, and the temperature was 250°C.
[0018] Preferably, the silica aerogel is prepared by a normal pressure drying method, which specifically comprises the following steps:
[0019] 11) ethyl silicate, anhydrous ethanol and deionized water are mixed in a molar ratio of 1:10:5, and then an acid is added to adjust the pH to 2-3, and stirred; then, an alkali is added to adjust the pH to 9-10 to form a gel;
[0020] 12) placing the gel obtained in step 11) in the mixed solution A for aging, and then soaking in anhydrous ethanol;
[0021] 13) soaking the gel obtained in step 12) in the mixed solution B first, and then soaking it in n-hexane for solvent exchange and washing;
[0022] 14) Finally, the gel obtained in step 13) is dried at a gradient atmospheric pressure to finally obtain pure silica aerogel.
[0023] Furthermore, the volume ratio of ethyl silicate to ethanol in the mixed solution A is 1:1.
[0024] Furthermore, the volume ratio of trimethylchlorosilane, ethanol and n-hexane in the mixed solution B is 2:1:8.
[0025] Further, the gradient normal pressure drying is:
[0026] First dry at 60℃ for 2h; then dry at 80℃ for 2h; finally dry at 120℃ for 12h.
[0027] The second technical solution of the present invention:
[0028] A high temperature resistant silica aerogel thermal insulation material is prepared according to the above preparation method.
[0029] Compared with the prior art, the present invention has the following advantages and technical effects:
[0030] In view of the problems that existing silica aerogels are difficult to use under high temperature conditions, the existing high-temperature resistant aerogel preparation process is complicated and difficult to commercialize, and the phase change leads to increased thermal conductivity and pore collapse, the present invention discloses a method using atomic layer deposition, which can deposit a layer of nanofilm on the silica nanoskeleton through a simple method to enhance its high-temperature thermal stability.
[0031] The high temperature resistant silica aerogel thermal insulation material prepared by the preparation method defined in the present invention has relatively stable nanopores at a high temperature exceeding 800° C. and has low thermal conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0033] Figure 1 Element distribution diagram of different elements deposited on the high temperature resistant silica aerogels prepared in Example 2 and Example 5;
[0034] Figure 2 The SEM images of the silica aerogel prepared in Comparative Example 1 and the high temperature resistant silica aerogel prepared in Example 3 after being treated at different temperatures;
[0035] Figure 3 The pore size distribution diagrams of the common silica aerogel prepared in step (1) of Example 1, the Al2O3-120 prepared in Example 3, and the ZrO2-50 prepared in Example 5 before high temperature heat treatment;
[0036] Figure 4 This is the pore size distribution diagram of the common silica aerogel prepared in step (1) of Example 1, the Al2O3-120 prepared in Example 3, and the ZrO2-50 prepared in Example 5 after heat treatment at 1000°C for 72 hours. DETAILED DESCRIPTION
[0037] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0038] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0039] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0040] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0041] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0042] All raw materials used in the examples of the present invention were purchased from the market. Ethyl silicate (Aladdin, ≥99.99%), anhydrous ethanol (Aladdin, AR), trimethylchlorosilane (Aladdin, ≥99.0%), n-hexane (Aladdin, AR), hydrochloric acid (Aladdin, 37%), ammonia (Aladdin, AR, 25-28%), trimethylaluminum (Nanjing Aimuyuan Scientific Instrument Co., Ltd., 99.99%), tetramethyl (dimethylamino) zirconium (Strem Chemicals, 99.99%).
[0043] The technical solution of the present invention is further illustrated by the following embodiments.
[0044] Example 1
[0045] A method for preparing a high temperature resistant silica aerogel thermal insulation material comprises the following steps:
[0046] (1) Preparation of silica aerogel
[0047] 11) Ethyl silicate, anhydrous ethanol and deionized water were mixed in a beaker at a molar ratio of 1:10:5. The pH of the mixture was adjusted to 2.5 with hydrochloric acid and magnetically stirred at room temperature for 2 hours to achieve complete hydrolysis; then, ammonia was added to raise the pH to 9.5 and gel formation began;
[0048] 12) placing the gel obtained in step 11) in a mixed solution of ethyl silicate and anhydrous ethanol at 55° C. (the volume ratio of ethyl silicate to anhydrous ethanol in the mixed solution is 1:1) for aging for 24 hours, and then soaking in anhydrous ethanol for another 24 hours;
[0049] 13) soaking the gel obtained in step 12) in a mixed solution of trimethylchlorosilane, anhydrous ethanol and n-hexane (wherein the volume ratio of trimethylchlorosilane, anhydrous ethanol and n-hexane is 2:1:8) for 48 hours, and then soaking it in n-hexane for 24 hours for solvent exchange and washing;
[0050] 14) Finally, the gel obtained in step 13) is dried at 60° C., 80° C. and 120° C. under normal pressure, and each temperature is maintained for 2 h, 2 h and 12 h, respectively, to finally obtain pure silica aerogel.
[0051] (2) Preparation of high temperature resistant silica aerogel insulation material:
[0052] The silica aerogel is evenly distributed on an 8-inch silicon wafer; then the silicon wafer is introduced into a vacuum atomic layer deposition reaction chamber, trimethylaluminum is used as an aluminum precursor, water is used as an oxygen source, nitrogen is used as a carrier gas, and the reaction chamber temperature is maintained at 250°C (to facilitate the evaporation of the precursor during the reaction) to perform vacuum atomic deposition, wherein the deposition amount is controlled by the number of deposition cycles, and an Al2O3 deposition cycle is: after 0.06s of trimethylaluminum injection, 9.94s of purge, followed by 5s of plasma pulse and 1s of purge. The deposition cycle is repeated 5 times. The high-temperature resistant silica aerogel thermal insulation material finally prepared is recorded as Al2O3-5 (where 5 is the number of deposition cycles).
[0053] Example 2
[0054] The difference from Example 1 is that the number of deposition cycles is 30. The high temperature resistant silica aerogel thermal insulation material finally prepared is recorded as Al2O3-30. Other conditions are the same as those in Example 1.
[0055] Example 3
[0056] The difference from Example 1 is that the number of deposition cycles is 120. The high temperature resistant silica aerogel thermal insulation material finally prepared is recorded as Al2O3-120. Other conditions are consistent with Example 1.
[0057] Example 4
[0058] The difference from Example 1 is that
[0059] In step (2), the precursor is tetramethyl(dimethylamino)zirconium; the number of deposition cycles is 25; one ZrO2 deposition cycle is: 0.6 s of tetramethyl(dimethylamino)zirconium injection, 11.4 s of purge, 5 s of plasma pulse, and 3 s of purge.
[0060] Other conditions were consistent with those in Example 1. The high temperature resistant silica aerogel thermal insulation material finally prepared was recorded as ZrO2-25.
[0061] Example 5
[0062] The difference from Example 4 is that the number of deposition cycles is 50, and the other conditions are consistent with Example 4. The high temperature resistant silica aerogel thermal insulation material finally prepared is recorded as ZrO2-50.
[0063] Comparative Example 1
[0064] The silica aerogel prepared in step (1) of Example 1 is used as Comparative Example 1.
[0065] Effect verification
[0066] The silica aerogels prepared in Examples 1-5 and Comparative Example 1 were placed in a high temperature furnace (air environment) and heat treated at different temperatures (normal temperature, 900°C, 1000°C, 1100°C, 1200°C) and for different times (2h, 24h, 72h, 168h), and then the thermal conductivity under the conditions was measured. Specific data are shown in Tables 1-4.
[0067] Table 1 Thermal conductivity of various silica aerogels at room temperature
[0068]
[0069] Table 2 Thermal conductivity of various silica aerogels at 900℃
[0070]
[0071] Table 3 Thermal conductivity of various silica aerogels at 1000℃
[0072]
[0073]
[0074] Table 4 Thermal conductivity of silica aerogels under heat treatment for 2 h
[0075]
[0076] Conclusion: It can be seen from the above table that the high temperature resistant silica aerogel thermal insulation material prepared by the present invention has lower thermal conductivity than the silica aerogel prepared in Comparative Example 1 at a temperature above 900°C, and the thermal conductivity is reduced by 30-66%, showing an excellent thermal insulation effect.
[0077] Figure 1 The element distribution diagrams of different elements deposited on the high temperature resistant silica aerogels prepared in Example 2 and Example 5; the left diagram is Example 2; the right diagram is Example 5. It can be seen from the diagram that the deposited elements are evenly distributed on the porous skeleton of the aerogel;
[0078] Figure 2 The SEM images of the silica aerogel prepared in Comparative Example 1 and the high temperature resistant silica aerogel prepared in Example 3 before heat treatment and after heat treatment at different temperatures; wherein, (a)-(c) are Comparative Example 1, which are untreated, 1000°C-168h, and 1200°C-2h, respectively; (d)-(f) are Example 3, which are untreated, 1000°C-168h, and 1200°C-2h, respectively; it can be seen from the figure that after high temperature heat treatment, the ordinary silica aerogel undergoes obvious sintering phenomenon, a large number of pores collapse, and the structure is dense; while the high temperature resistant silica aerogel insulation material prepared in Example 3 still retains a large number of pores, and the degree of structural preservation is high;
[0079] Figure 3 The pore size distribution diagrams of the common silica aerogel prepared in step (1) of Example 1, the Al2O3-120 prepared in Example 3, and the ZrO2-50 prepared in Example 5 before high temperature heat treatment;
[0080] Figure 4 The pore size distribution diagram of the ordinary silica aerogel prepared in step (1) of Example 1, the Al2O3-120 prepared in Example 3 and the ZrO2-50 prepared in Example 5 after being heat treated at 1000°C for 72 hours; it can be seen from the figure that the deposition has little effect on the pore size distribution at room temperature, but after high-temperature heat treatment, the pore integrity of Al2O3-120 is better than that of ZrO2-50 and better than that of the undeposited (ordinary silica aerogel).
[0081] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a high temperature resistant silica aerogel thermal insulation material, characterized in that: Using an organic salt containing aluminum or zirconium as a precursor, a nanofilm is deposited on the porous skeleton of the silica aerogel by atomic layer deposition to prepare a high temperature resistant silica aerogel thermal insulation material; Wherein, the number of deposition cycles in the atomic layer deposition process is 5-120 times.
2. The method for preparing a high temperature resistant silica aerogel thermal insulation material according to claim 1, characterized in that: The aluminum-containing organic salt is trimethylaluminum; The zirconium-containing organic salt is tetramethyl(dimethylamino)zirconium.
3. The method for preparing a high temperature resistant silica aerogel thermal insulation material according to claim 1, characterized in that: When aluminum-containing organic salt is used as a precursor, one deposition cycle is one cycle, specifically: After 0.06 s of aluminum-containing organic salt injection, a purge was performed for 9.94 s, followed by a plasma pulse for 5 s and a purge for 1 s.
4. The method for preparing a high temperature resistant silica aerogel thermal insulation material according to claim 1, characterized in that: When zirconium-containing organic salt is used as a precursor, one deposition cycle is one cycle, specifically: After 0.6 s of zirconium-containing organic salt injection, a purge of 11.4 s was performed, followed by a 5 s plasma pulse and a 3 s purge.
5. The method for preparing a high temperature resistant silica aerogel thermal insulation material according to claim 1, characterized in that: The reaction conditions during the atomic deposition process are: Water was used as the oxygen source, nitrogen was used as the carrier gas, and the temperature was 250°C.
6. The method for preparing a high temperature resistant silica aerogel thermal insulation material according to claim 1, characterized in that: The silica aerogel is prepared by a normal pressure drying method, which specifically comprises the following steps: 11) ethyl silicate, anhydrous ethanol and deionized water are mixed in a molar ratio of 1:10:5, and then an acid is added to adjust the pH to 2-3, and stirred; then, an alkali is added to adjust the pH to 9-10 to form a gel; 12) placing the gel obtained in step 11) in the mixed solution A for aging, and then soaking in anhydrous ethanol; 13) soaking the gel obtained in step 12) in the mixed solution B first, and then soaking it in n-hexane for solvent exchange and washing; 14) Finally, the gel obtained in step 13) is dried at a gradient atmospheric pressure to finally obtain pure silica aerogel.
7. The method for preparing a high temperature resistant silica aerogel thermal insulation material according to claim 6, characterized in that: The volume ratio of ethyl silicate to ethanol in the mixed solution A is 1:
1.
8. The method for preparing a high temperature resistant silica aerogel thermal insulation material according to claim 6, characterized in that: The volume ratio of trimethylsilyl chloride, ethanol and n-hexane in the mixed solution B is 2:1:
8.
9. The method for preparing a high temperature resistant silica aerogel thermal insulation material according to claim 6, characterized in that: The gradient normal pressure drying is: First dry at 60℃ for 2h; then dry at 80℃ for 2h; finally dry at 120℃ for 12h.
10. A high temperature resistant silica aerogel thermal insulation material, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Normal pressure preparation method for transparent silica bulk aerogel
CN106629750A
Preparation method of silica aerogel under atmospheric pressure
CN108423685A
Solar thermal aerogel receiver and materials therefor
US20190100439A1