Polishing solution for planarization of chip copper interconnection as well as preparation method and application of polishing solution

By using a polishing liquid composed of amino polycarboxylic acid chelating agent and pyridine heterocyclic carboxylic complexing agent in semiconductor chip manufacturing, the copper-cobalt polishing rate is controlled, and the problem of difficult to control the polishing speed of the cobalt barrier layer is solved, and the electricity is reduced The risk of corrosion increases the performance and production reliability of the chip.

CN118880338APending Publication Date: 2024-11-01SHANGHAI INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410935573.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In semiconductor chip manufacturing, during the polishing process of the copper interconnect layer, the polishing speed of the cobalt barrier layer is difficult to control, which easily leads to butterfly pits and galvanic corrosion, affecting the performance and reliability of the chip.

Method used

Using a polishing liquid including amino polycarboxylic acid chelating agent, pyridine heterocyclic carboxylic complexing agent and inhibitor, the copper-cobalt polishing rate ratio is controlled by adjusting the pH value and adding an oxidizing agent, combining colloid SiO2 as an abrasive, and controlling the copper-cobalt polishing rate ratio to achieve copper. High-speed removal and low-speed removal of cobalt reduce the risk of galvanic corrosion.

Benefits of technology

It achieves extremely low galvanic corrosion difference between copper and cobalt, ensures controllability and quality of the polishing process, avoids damage to the cobalt film, and improves the chip's performance and production reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880338A_ABST
    Figure CN118880338A_ABST
Patent Text Reader

Abstract

The invention relates to a polishing solution for chip copper interconnection planarization and a preparation method and application thereof, and belongs to the field of semiconductor chip manufacturing copper interconnection chemical mechanical polishing, the polishing solution comprises the following raw material components by mass: 0.02-2% of an aminopolycarboxylic acid chelating agent, 0.1-3% of a pyridine heterocyclic carboxyl complexing agent, 0.01-0.5% of an inhibitor, 0.5-4.5% of an oxidant, and the balance of water. And the balance of deionized water. The pyridine heterocyclic carboxyl complexing agent is quinoline carboxylic acid or pyridine dicarboxylic acid. Compared with the prior art, galvanic corrosion of copper and cobalt in the polishing solution provided by the invention is eliminated, and the risk of quality defects caused by overlarge metal potential difference in the copper polishing process is reduced; in addition, the polishing solution with the large copper-cobalt rate selection ratio can automatically stop polishing on a cobalt barrier layer under the condition that excessive copper is rapidly removed, and damage to a cobalt film caused by excessive polishing is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical mechanical polishing of copper interconnects in semiconductor chip manufacturing, and in particular to a polishing liquid for planarizing copper interconnects of chips, and a preparation method and application thereof. Background Art

[0002] When the technology node of integrated circuits developed to 0.25μm~0.35μm, chemical mechanical polishing (CMP) technology became the key process of IC manufacturing and officially became the only technology that can achieve global flattening. Copper appeared in chip manufacturing as the interconnection line of the device, which realized the rapid increase of chip integration and continuously improved the performance of the chip. However, due to the high impedance of its barrier layer Ta / TaN, copper below the 20nm node has quality problems such as signal delay due to small size and electron scattering. Therefore, in order to improve the defects of copper interconnection in low-node process, the metal cobalt film with better conductivity is used as the barrier layer of copper wire. The emergence of this system brings new challenges to the application of chemical mechanical polishing technology. For example: the thickness of the barrier layer cobalt is only 2nm, and cobalt is a relatively active metal, which is susceptible to chemical corrosion and easy to form galvanic corrosion with copper, causing corrosion defects. In addition, in order to prevent the occurrence of butterfly pits, the polishing rate ratio between copper and cobalt should be controlled, and the polishing rate of cobalt should not be as large as possible during the process of polishing excessive copper. In other words, in order to achieve safe polishing of a large amount of copper, it is hoped that the polishing can automatically stop at the cobalt barrier layer.

[0003] At present, more research is focused on how to solve the problem of not causing butterfly quality defects when polishing the cobalt barrier layer, so as to achieve a copper-cobalt polishing removal rate ratio close to 1:1 as much as possible, and at the same time hope to solve the copper-cobalt galvanic corrosion. For example: corrosion inhibitors (benzotriazole, 1,2,4-triazole) are used to solve galvanic corrosion, and at the same time, suitable complexing agents and oxidants are selected to adjust the metal dissolution to control the copper-cobalt polishing rate ratio close to 1:1.

[0004] However, before polishing the barrier layer, the excess copper filled in the Damascus copper plating process must be polished. The polishing speed of this link is often much faster than the polishing speed of the barrier layer. If it cannot automatically stop at the cobalt barrier layer, over-polishing is likely to occur, resulting in a higher defective rate in production.

[0005] The Chinese patent application number CN202211345251.4 discloses an alkaline polishing liquid for inhibiting copper-cobalt galvanic corrosion and a preparation method thereof, comprising the following raw material components by mass fraction: 0.3-2% aminopolycarboxylic acid chelating agent, 0.03-0.15% BTA inhibitor, 0.05-0.2% hydrogen peroxide oxidizing agent, and the rest is deionized water; the aminopolycarboxylic acid chelating agent is tetrasodium iminodisuccinate. However, the above patent only solves the copper-cobalt galvanic corrosion, and does not solve the polishing inhibition of cobalt. Summary of the invention

[0006] The purpose of the present invention is to provide a polishing liquid for chip copper interconnection planarization and its preparation method and application in order to overcome at least one of the defects of the above-mentioned prior art. The polishing liquid is used for polishing the copper interconnection layer when metal cobalt is used as a barrier layer. During the copper chemical mechanical polishing process, high-speed copper removal is achieved while the cobalt material has an extremely low or even zero removal rate, thereby obtaining a larger copper-cobalt removal rate selectivity and achieving an extremely low galvanic corrosion difference between copper and cobalt.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] One of the purposes of the present invention is a polishing liquid for planarizing copper interconnects of chips, comprising the following raw material components by mass fraction: 0.02-2% of aminopolycarboxylic acid type chelating agent, 0.1-3% of pyridine heterocyclic carboxyl complexing agent, 0.01-0.5% of inhibitor, 0.5-4.5% of oxidant, and the rest is deionized water;

[0009] Wherein, the pyridine heterocyclic carboxyl complexing agent is quinolinecarboxylic acid (QA) or pyridinedicarboxylic acid.

[0010] Furthermore, the aminopolycarboxylic acid chelating agent is ethylenediaminetetraacetic acid (EDTA) or tetrasodium iminodisuccinate (IDS).

[0011] Furthermore, the oxidant is hydrogen peroxide.

[0012] Furthermore, the inhibitor is benzotriazole (BTA) or 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole (TAZ).

[0013] Furthermore, the mass fraction of the aminopolycarboxylic acid type chelating agent is 0.02%, 1% or 2%.

[0014] Furthermore, the mass fraction of the pyridine heterocyclic carboxyl complexing agent is 0.1%, 1% or 3%.

[0015] Furthermore, the mass fraction of the inhibitor is 0.01%, 0.08%, 0.5% or 0.1%.

[0016] Furthermore, the mass fraction of the oxidant is 0.5%, 2% or 4.5%.

[0017] The second object of the present invention is to provide a method for preparing the polishing liquid for planarizing the copper interconnection of a chip as described above, comprising the following preparation method:

[0018] An oxidant, a pyridine heterocyclic carboxyl complexing agent, an amino polycarboxylic acid chelating agent and an inhibitor are sequentially added into deionized water and mixed to obtain a mixed solution;

[0019] The pH of the mixed solution is adjusted to be alkaline, thereby obtaining a polishing solution for planarizing copper interconnects of a chip. Preferably, the pH of the mixed solution is adjusted to 10, and the pH adjusting agent used is a KOH aqueous solution.

[0020] The third object of the present invention is to use the polishing liquid for planarizing the copper interconnection of a chip as described above in chemical mechanical polishing, which is suitable for the copper interconnection layer when metal cobalt is used as a barrier layer. When the polishing liquid is used for polishing, the abrasive used is colloidal SiO2. Preferably, the physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] (1) The galvanic corrosion of copper and cobalt in the polishing liquid provided by the present invention is eliminated, thereby reducing the risk of quality defects caused by excessive metal potential difference during copper polishing.

[0023] (2) The present invention provides a polishing liquid with a large copper-cobalt rate selectivity ratio, which can automatically terminate polishing at the cobalt barrier layer while removing excess copper quickly, thereby preventing damage to the cobalt film caused by excessive polishing.

[0024] (3) The present invention does not require the use of a highly acidic polishing solution to promote the polishing removal rate of copper and cobalt, thus avoiding corrosion of the machine, improving the controllability of the polishing process, and facilitating large-scale industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the galvanic corrosion difference of the copper-cobalt electrode in Example 1. DETAILED DESCRIPTION

[0026] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0027] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. If no specific conditions are specified, the conventional conditions or the conditions recommended by the manufacturer shall be followed. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0028] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0029] A polishing liquid for planarizing copper interconnection of a chip comprises the following raw material components in mass fraction: 0.02-2% of aminopolycarboxylic acid type chelating agent, 0.1-3% of pyridine heterocyclic carboxyl complexing agent, 0.01-0.5% of inhibitor, 0.5-4.5% of oxidant, and the rest is deionized water; the pyridine heterocyclic carboxyl complexing agent is quinolinecarboxylic acid or pyridinedicarboxylic acid.

[0030] In some embodiments of the present invention, the aminopolycarboxylic acid chelating agent is ethylenediaminetetraacetic acid or tetrasodium iminodisuccinate.

[0031] In some embodiments of the present invention, the oxidant is hydrogen peroxide.

[0032] In some embodiments of the present invention, the inhibitor is benzotriazole or 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole.

[0033] In some embodiments of the present invention, the mass fraction of the aminopolycarboxylic acid type chelating agent is 0.02%, 1% or 2%.

[0034] In some embodiments of the present invention, the mass fraction of the pyridine heterocyclic carboxyl complexing agent is 0.1%, 1% or 3%.

[0035] In some embodiments of the present invention, the mass fraction of the inhibitor is 0.01%, 0.08%, 0.5% or 0.1%.

[0036] In some embodiments of the present invention, the mass fraction of the oxidant is 0.5%, 2% or 4.5%.

[0037] In the following examples and comparative examples, the corrosion potential test of copper and cobalt was performed using a Chenhua CHI-660E electrochemical workstation and a standard three-electrode electrolytic cell to compare their galvanic corrosion trends. In the test, a Pt electrode was used as a counter electrode, a saturated calomel electrode (SCE) was used as a reference electrode, and copper (purity of 99.99%) and cobalt (purity of 99.99%) were used as working electrodes.

[0038] In the following embodiments and comparative examples, the test method of the polishing removal rate of copper and cobalt is as follows: The polishing experiment is carried out on the UNIPOL-802 polishing machine of Shenyang Kejing. After polishing, it is rinsed with deionized water and cleaned with acetone solution to remove most of the colloidal silica particles and other impurity particles adsorbed on the copper surface due to electronegativity. After cleaning, it is cleaned with anhydrous ethanol and deionized water respectively, and blown dry with argon gas. The Cu-MRR and Co-MRR are calculated by the weight difference of the sample weighed before and after the polishing experiment. The calculation formula is as follows:

[0039]

[0040] Where: MRR is the polishing rate; Δm is the mass difference before and after polishing; ρ is the density of copper / cobalt; r is the radius of the polishing metal disk; t is the polishing time.

[0041] Comparative Example 1:

[0042] Add hydrogen peroxide to 47.88 g of deionized water while stirring to prepare a polishing solution with a H2O2 content of 2 wt%, and adjust the solution pH to 10.

[0043] The polishing liquid prepared in this comparative example uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0044] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1, and the calculated corrosion potential difference between Cu and Co is 72mV.

[0045] After CMP polishing of copper and cobalt for 5 minutes, the polishing removal rates of Cu and Co were calculated to be The removal rate selection ratio of the two is 1.15:1.

[0046] This indicates that under the condition of only oxidant, there is a risk of galvanic corrosion between copper and cobalt, and the polishing rates are not much different.

[0047] Comparative Example 2:

[0048] Hydrogen peroxide was added to 47.88 g of deionized water while stirring, and quinolinecarboxylic acid was added while continuing to stir. Finally, a pH adjusting agent potassium hydroxide aqueous solution was used to adjust the pH to 10 to obtain a polishing liquid. The content of H2O2 in the polishing liquid was 2 wt%, and the content of quinolinecarboxylic acid was 0.1 wt%.

[0049] The polishing liquid prepared in this comparative example uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0050] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1, and the calculated corrosion potential difference between Cu and Co is 15mV.

[0051] After CMP polishing of the copper and cobalt targets for 5 minutes, the polishing removal rates of Cu and Co were calculated to be The removal rate selection ratio of the two is 1.39:1.

[0052] The results show that the addition of complexing agent reduces the potential difference between copper and cobalt and increases the polishing speed of the metal, but the selectivity of the two is not significantly improved.

[0053] Comparative Example 3:

[0054] Add hydrogen peroxide to 100 ml of deionized water while stirring, then add tetrasodium iminodisuccinate while continuing to stir, and finally use a pH adjuster potassium hydroxide aqueous solution to adjust the pH to 10 to obtain a polishing liquid, in which the content of H2O2 and the content of tetrasodium iminodisuccinate are 2wt%.

[0055] The polishing liquid prepared in this comparative example uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0056] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1, and the calculated corrosion potential difference between Cu and Co is 20mV.

[0057] After CMP polishing of the copper and cobalt targets for 5 minutes, the polishing removal rates of Cu and Co were calculated to be The removal rate selection ratio of the two is 1.41:1.

[0058] The results showed that aminopolycarboxylic acid chelating agent has an activation effect on copper and cobalt, can promote the dissolution of metals, reduce the potential difference between copper and cobalt, and increase the polishing speed of metals, but the selectivity ratio of the two has not been significantly improved.

[0059] Comparative Example 4:

[0060] Add hydrogen peroxide to 100 ml of deionized water while stirring, then continue to add pyridinedicarboxylic acid while stirring, and finally use a pH adjuster potassium hydroxide aqueous solution to adjust the pH to 10 to obtain a polishing liquid, in which the content of H2O2 is 2wt%, and the content of pyridinedicarboxylic acid is 0.1wt%.

[0061] The polishing liquid prepared in this comparative example uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0062] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1, and the calculated corrosion potential difference between Cu and Co is 51mV.

[0063] After CMP polishing of the copper and cobalt targets for 5 minutes, the polishing removal rates of Cu and Co were calculated to be The removal rate selection ratio of the two is 2:1.

[0064] The results showed that the addition of pyridine heterocyclic carboxyl complexing agents reduced the potential difference between copper and cobalt and increased the polishing speed of the metal, but the selectivity of the two was not significantly improved.

[0065] Comparative Example 5:

[0066] Add hydrogen peroxide to 100 ml of deionized water while stirring, then add quinolinecarboxylic acid while continuing to stir, then add tetrasodium iminodisuccinate while continuing to stir, and finally use a pH adjuster potassium hydroxide aqueous solution to adjust the pH to 10 to obtain a polishing liquid, wherein the content of H2O2 in the polishing liquid is 2wt%, the content of quinolinecarboxylic acid is 0.1wt%, and the content of tetrasodium iminodisuccinate is 2wt%.

[0067] The polishing liquid prepared in this comparative example uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0068] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1, and the calculated corrosion potential difference between Cu and Co is 119mV.

[0069] After CMP polishing of the copper and cobalt targets for 5 minutes, the polishing removal rates of Cu and Co were calculated to be The removal rate selection ratio of the two is 10.2:1.

[0070] The results showed that the compounding of tetrasodium iminodisuccinate and quinolinecarboxylic acid increased the potential difference between copper and cobalt, increased the polishing speed of copper, inhibited the polishing speed of cobalt, and the selectivity of the two was significantly improved.

[0071] Comparative Example 6:

[0072] Add hydrogen peroxide to 100 ml of deionized water while stirring, then add quinolinecarboxylic acid while continuing to stir, then add ethylenediaminetetraacetic acid while continuing to stir, and finally use a pH adjuster potassium hydroxide aqueous solution to adjust the pH to 10 to obtain a polishing liquid, in which the content of H2O2, the content of quinolinecarboxylic acid, and the content of ethylenediaminetetraacetic acid are 2wt%.

[0073] The polishing liquid prepared in this comparative example uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0074] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1, and the calculated corrosion potential difference between Cu and Co is 123mV.

[0075] After CMP polishing of the copper and cobalt targets for 5 minutes, the polishing removal rates of Cu and Co were calculated to be The removal rate selection ratio of the two is 9.8:1.

[0076] The results showed that the compounding of EDTA and quinolinecarboxylic acid increased the potential difference between copper and cobalt, increased the polishing speed of copper, inhibited the polishing speed of cobalt, and significantly improved the selectivity of the two.

[0077] Comparative Example 7:

[0078] Add hydrogen peroxide to 100 ml of deionized water while stirring, then add pyridinedicarboxylic acid while continuing to stir, then add tetrasodium iminodisuccinate while continuing to stir, and finally use a pH adjuster potassium hydroxide aqueous solution to adjust the pH to 10 to obtain a polishing liquid, in which the content of H2O2 is 4wt%, the content of pyridinedicarboxylic acid is 0.1wt%, and the content of tetrasodium iminodisuccinate is 2wt%.

[0079] The polishing liquid prepared in this comparative example uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0080] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1, and the calculated corrosion potential difference between Cu and Co is 104mV.

[0081] After CMP polishing of the copper and cobalt targets for 5 minutes, the polishing removal rates of Cu and Co were calculated to be The removal rate selection ratio of the two is 9.3:1.

[0082] The results showed that the increase of hydrogen peroxide concentration had little effect on the removal rate, selectivity and potential difference between copper and cobalt.

[0083] Comparative Example 8:

[0084] Add hydrogen peroxide to 100 ml of deionized water while stirring, then continue to add benzotriazole while stirring, and finally use a pH adjuster potassium hydroxide aqueous solution to adjust the pH to 10 to obtain a polishing liquid, in which the content of H2O2 is 2wt%, and the content of benzotriazole is 0.1wt%.

[0085] The polishing liquid prepared in this comparative example uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0086] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1, and the calculated corrosion potential difference between Cu and Co is 51mV.

[0087] After CMP polishing of the copper and cobalt targets for 5 minutes, the polishing removal rates of Cu and Co were calculated to be The removal rate selection ratio of the two is 1.5:1.

[0088] The results showed that the addition of inhibitors reduced the potential difference between copper and cobalt, inhibited the polishing speed of the metal, and the selectivity of the two was not significantly improved.

[0089] Comparative Example 9:

[0090] Add hydrogen peroxide to 100 ml of deionized water while stirring, then add tetrasodium iminodisuccinate and benzotriazole in sequence while continuing to stir, and finally use a pH adjuster potassium hydroxide aqueous solution to adjust the pH to 10 to obtain a polishing liquid, in which the content of H2O2, the content of tetrasodium iminodisuccinate and the content of benzotriazole are 2wt%.

[0091] The polishing liquid prepared in this comparative example uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0092] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1, and the calculated corrosion potential difference between Cu and Co is 12mV.

[0093] After CMP polishing of the copper and cobalt targets for 5 minutes, the polishing removal rates of Cu and Co were calculated to be The removal rate selection ratio of the two is 1.1:1.

[0094] The results show that the combined use of aminopolycarboxylic acid and inhibitor can inhibit the galvanic corrosion between copper and cobalt. However, since their complexation with copper and cobalt does not achieve high-speed dissolution of copper, the copper polishing speed is insufficient, while the cobalt dissolves quickly. It cannot meet the safe polishing of copper.

[0095] Embodiment 1:

[0096] Add hydrogen peroxide to 100 ml of deionized water while stirring, and then add quinolinecarboxylic acid, tetrasodium iminodisuccinate, and benzotriazole in sequence while continuing to stir. Finally, use a pH adjuster potassium hydroxide aqueous solution to adjust the pH to 10 to obtain a polishing liquid. The content of H2O2 in the polishing liquid is 4.5wt%, the content of quinolinecarboxylic acid is 3wt%, the content of tetrasodium iminodisuccinate is 2wt%, and the content of benzotriazole is 0.01wt%.

[0097] The polishing liquid prepared in this embodiment uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0098] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. Figure 1 The calculated corrosion potential difference between Cu and Co is only 1 mV. Compared with Comparative Examples 1 and 2, the potential difference is significantly reduced, indicating that the polishing liquid effectively controls the galvanic corrosion between Cu and Co. The calculated polishing removal rates of Cu and Co are The removal rate selectivity ratio reaches 21.8:1, indicating that the polishing liquid effectively improves the removal rate selectivity between copper and cobalt.

[0099] Embodiment 2:

[0100] Add hydrogen peroxide to 100 ml of deionized water with stirring, then add quinolinecarboxylic acid, tetrasodium iminodisuccinate, and 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole in sequence with continued stirring, and finally add a pH regulator, potassium hydroxide aqueous solution, to adjust the pH to 10 to obtain a polishing liquid, wherein the content of H2O2 in the polishing liquid is 2wt%, the content of quinolinecarboxylic acid is 3wt%, the content of tetrasodium iminodisuccinate is 2wt%, and the content of 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole is 0.5wt%.

[0101] The polishing liquid prepared in this embodiment uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0102] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1. The calculated corrosion potential difference between Cu and Co is 5 mV. Compared with Comparative Examples 1 and 2, the potential difference is significantly reduced, indicating that the polishing liquid effectively controls the galvanic corrosion between Cu and Co. The calculated polishing removal rates of Cu and Co are The removal rate selection ratio of the two is 19.4:1.

[0103] Embodiment 3:

[0104] Add hydrogen peroxide to 47.88g of deionized water while stirring, then add ethylenediaminetetraacetic acid, dipyridinecarboxylic acid, and benzotriazole in sequence while continuing to stir, and finally use a pH adjuster, sodium hydroxide aqueous solution, to adjust the pH to 10 to obtain a polishing liquid, in which the content of H2O2, the content of ethylenediaminetetraacetic acid, the content of dipyridinecarboxylic acid, and the content of benzotriazole are 2wt%.

[0105] The polishing liquid prepared in this embodiment uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0106] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1. The calculated corrosion potential difference between Cu and Co is 9 mV. Compared with Comparative Example 1, the potential difference is significantly reduced, indicating that the polishing liquid effectively controls the galvanic corrosion between Cu and Co. The calculated polishing removal rates of Cu and Co are The removal rate selection ratio of the two is 8.1:1.

[0107] Embodiment 4:

[0108] Add hydrogen peroxide to 100 ml of deionized water with stirring, and then add quinolinecarboxylic acid, tetrasodium iminodisuccinate, and 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole in sequence with stirring, and finally adjust the pH to 10 with a pH adjuster to obtain a polishing liquid, wherein the content of H2O2 in the polishing liquid is 0.5wt%, the content of quinolinecarboxylic acid is 0.1wt%, the content of tetrasodium iminodisuccinate is 0.02wt%, and the content of 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole is 0.08wt%.

[0109] The polishing liquid prepared in this embodiment uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0110] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1. The calculated corrosion potential difference between Cu and Co is 11 mV. Compared with Comparative Example 1, the potential difference is significantly reduced, indicating that the polishing liquid effectively controls the galvanic corrosion between Cu and Co. The calculated polishing removal rates of Cu and Co are The removal rate selection ratio of the two is 5.5:1.

[0111] Embodiment 5:

[0112] Add hydrogen peroxide to 47.35g of deionized water while stirring, then add ethylenediaminetetraacetic acid, dipyridinecarboxylic acid, and benzotriazole in sequence while continuing to stir, and finally use a pH adjuster to adjust the pH to 10 to obtain a polishing liquid, in which the content of H2O2, the content of ethylenediaminetetraacetic acid, the content of dipyridinecarboxylic acid, and the content of benzotriazole are 2wt%.

[0113] The polishing liquid prepared in this embodiment uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0114] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1. The calculated corrosion potential difference between Cu and Co is 2mV. Compared with Comparative Example 1, the potential difference is significantly reduced, indicating that the polishing liquid effectively controls the galvanic corrosion between Cu and Co. The calculated polishing removal rates of Cu and Co are The removal rate selection ratio of the two is 21.8:1.

[0115] Embodiment 6:

[0116] Add hydrogen peroxide to 47.35g of deionized water while stirring, and then add quinolinecarboxylic acid, ethylenediaminetetraacetic acid, and benzotriazole in sequence while continuing to stir. Finally, use a pH adjuster to adjust the pH to 10 to obtain a polishing liquid. The content of H2O2 in the polishing liquid is 2wt%, the content of quinolinecarboxylic acid is 0.1wt%, the content of ethylenediaminetetraacetic acid is 2wt%, and the content of benzotriazole is 0.1wt%.

[0117] The polishing liquid prepared in this embodiment uses colloidal SiO2 as the abrasive during polishing, and the amount of the abrasive added is 1% of the total mass of the polishing liquid. The physical parameters of the polishing liquid during polishing are: pressure: 1psi; polishing disc speed: 70rpm; polishing head speed: 40rpm; polishing liquid flow rate: 100ml / min; polishing time: 5min.

[0118] Copper and cobalt were used as research electrodes to conduct Tafel curve tests. The specific results are shown in Table 1. The calculated corrosion potential difference between Cu and Co is 2mV. Compared with Comparative Example 1, the potential difference is significantly reduced, indicating that the polishing liquid effectively controls the galvanic corrosion between Cu and Co. The calculated polishing removal rates of Cu and Co are The removal rate selection ratio of the two is 20:1.

[0119] Table 1. Cu, Co corrosion potential difference and removal rate selectivity in comparative examples and examples 1-6

[0120]

[0121] From the analysis of Table 1, it can be seen that Comparative Example 1 shows that under the condition of only oxidant, there is a risk of galvanic corrosion between copper and cobalt, and the polishing rate is not much different.

[0122] In Comparative Example 2, the addition of the complexing agent reduced the potential difference between copper and cobalt and increased the polishing speed of the metal, but the selectivity ratio of the two was not significantly improved.

[0123] In Comparative Example 3, the aminopolycarboxylic acid chelating agent has an activation effect on copper and cobalt, can promote the dissolution of the metal, reduce the potential difference between copper and cobalt, and increase the polishing speed of the metal, but the selectivity ratio between the two is not significantly improved.

[0124] In Comparative Example 4, the addition of the pyridine heterocyclic carboxyl complexing agent reduced the potential difference between copper and cobalt and increased the polishing speed of the metal, but the selectivity ratio of the two was not significantly improved.

[0125] In Comparative Example 5, the compounding of tetrasodium iminodisuccinate and quinolinecarboxylic acid increases the potential difference between copper and cobalt, increases the polishing speed of copper, and inhibits the polishing speed of cobalt, and the selectivity of the two is significantly improved.

[0126] In Comparative Example 6, the compounding of ethylenediaminetetraacetic acid and quinolinecarboxylic acid increases the potential difference between copper and cobalt, increases the polishing speed of copper, and inhibits the polishing speed of cobalt, and the selectivity of the two is significantly improved.

[0127] In Comparative Example 7, the increase in hydrogen peroxide concentration had little effect on the removal rate, selectivity and potential difference between copper and cobalt.

[0128] The addition of the inhibitor in Comparative Example 8 reduced the potential difference between copper and cobalt, inhibited the polishing speed of the metal, and the selectivity of the two was not significantly improved.

[0129] The combined use of aminopolycarboxylic acid and inhibitor in Comparative Example 9 can inhibit the galvanic corrosion between copper and cobalt. However, since the complexation between them and copper and cobalt does not achieve high-speed dissolution of copper, the polishing speed of copper is insufficient, while cobalt dissolves quickly, which cannot meet the safe polishing of copper.

[0130] In Examples 1-6, H2O2, aminopolycarboxylic acid chelating agents, pyridine heterocyclic carboxyl complexing agents, and inhibitors were added. The results showed that the combination of aminopolycarboxylic acid chelating agents and pyridine heterocyclic carboxyl complexing agents and the change of the concentration of benzotriazole can affect the solubility of copper and cobalt, indicating that the synergistic effect of the three will affect the activity of the metal.

[0131] Among them, the oxidation of hydrogen peroxide can promote the generation of metal ions. Aminopolycarboxylic acid and pyridine hybrid carboxylic acid complexing agents have selective complexing ability for copper and cobalt, and the solubility of copper-cobalt complexes can be adjusted by adjusting the type and dosage of chelating agents. Pyridine hybrid carboxylic acid can accelerate the rapid dissolution of copper ions due to the complexing effect, while cobalt ions hinder the dissolution of cobalt due to the formation of insoluble complexes. This directional complexation and solubility adjustment enables copper to be polished at a high speed while the polishing will stop safely at the cobalt barrier layer, thereby improving the yield of copper after polishing. The corrosion inhibition of benzotriazole comes from adsorption on the surface of copper and cobalt. The concentration of copper and cobalt can be adjusted to adjust the corrosion potential of the two, thereby reducing the galvanic corrosion between the two.

[0132] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A polishing liquid for planarizing chip copper interconnects, characterized in that: The method comprises the following raw material components in mass fractions: 0.02-2% of aminopolycarboxylic acid type chelating agent, 0.1-3% of pyridine heterocyclic carboxyl type complexing agent, 0.01-0.5% of inhibitor, 0.5-4.5% of oxidant, and the rest is deionized water; The pyridine heterocyclic carboxyl complexing agent is quinolinecarboxylic acid or dipyridinecarboxylic acid.

2. The polishing liquid for planarizing chip copper interconnects according to claim 1, characterized in that: The aminopolycarboxylic acid chelating agent is ethylenediaminetetraacetic acid or tetrasodium iminodisuccinate.

3. The polishing liquid for planarizing chip copper interconnects according to claim 1, characterized in that: The oxidant is hydrogen peroxide.

4. The polishing liquid for planarizing chip copper interconnects according to claim 1, characterized in that: The inhibitor is benzotriazole or 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole.

5. The polishing liquid for planarizing chip copper interconnects according to claim 1, characterized in that: The mass fraction of the aminopolycarboxylic acid type chelating agent is 0.02%, 1% or 2%.

6. The polishing liquid for planarizing chip copper interconnects according to claim 1, characterized in that: The mass fraction of the pyridine heterocyclic carboxyl complexing agent is 0.1%, 1% or 3%.

7. The polishing liquid for planarizing chip copper interconnects according to claim 1, characterized in that: The mass fraction of the inhibitor is 0.01%, 0.08%, 0.5% or 0.1%.

8. The polishing liquid for planarizing chip copper interconnects according to claim 1, characterized in that: The mass fraction of the oxidant is 0.5%, 2% or 4.5%.

9. A method for preparing a polishing liquid for planarizing chip copper interconnects according to any one of claims 1 to 8, characterized in that: The invention comprises the following preparation method: An oxidant, a pyridine heterocyclic carboxyl complexing agent, an amino polycarboxylic acid chelating agent and an inhibitor are sequentially added into deionized water and mixed to obtain a mixed solution; The pH of the mixed solution is adjusted to be alkaline, thereby obtaining a polishing solution for planarizing copper interconnections of chips.

10. Use of the polishing liquid for planarizing chip copper interconnects according to any one of claims 1 to 8 in chemical mechanical polishing, characterized in that: Suitable for copper interconnect layers with metallic cobalt as a barrier layer.