Corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating on surface of magnesium alloy and preparation method
By preparing a coating consisting of a niobium-containing ceramic inner layer and a nano-silver-copper alloy powder outer layer on the surface of magnesium alloy, the corrosion, conductivity, and mildew prevention problems of magnesium alloy in harsh environments were solved, achieving an integrated coating effect of corrosion resistance, conductivity, thermal control, and mildew prevention.
Patent Information
- Application Number
- CN202410910093.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
Magnesium alloys are prone to corrosion in harsh environments such as high temperature, high humidity, and high salt. Existing coatings cannot simultaneously possess corrosion resistance, electrical conductivity, thermal control, and mildew prevention properties, which affects their service life and the normal operation of equipment.
A corrosion-resistant ceramic layer containing niobium is prepared on the surface of a magnesium alloy, and a modified graphite-epoxy resin organic layer containing nano-silver copper alloy powder is prepared on the outer layer. An integrated coating is formed by micro-arc oxidation and spraying. The thickness of the inner layer is 3-10 μm and the thickness of the outer layer is 10-40 μm.
It achieves dense and uniform surface coating on magnesium alloys, possesses good electrical conductivity, corrosion resistance and mildew resistance, and is suitable for service requirements in harsh marine atmospheric environments.
Smart Images

Figure CN118880412A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnesium alloy surface treatment, and in particular to a magnesium alloy surface corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating and a preparation method thereof. Background Art
[0002] Magnesium and its alloys are known as "the green engineering materials with the most development and application potential in the century". Magnesium alloys have the advantages of high specific strength and high specific stiffness. In recent years, magnesium alloy-related industries have developed rapidly, and magnesium and its alloys have been widely used in marine engineering equipment, aerospace, military industry, automobiles, machinery manufacturing and other fields. The 21st century is a critical period for my country to vigorously develop the blue economy and build a "maritime power". With the implementation of the strategy of building a maritime power, advanced magnesium alloy structural materials have gradually begun to be used in marine equipment. However, because the chemical properties of magnesium alloys are relatively active, the equilibrium potential is low, and the corrosion resistance and wear resistance are poor, they will suffer severe corrosion in harsh environments such as high temperature, high humidity, and high salt. In various service environments, corrosion will affect the service life of magnesium alloys and increase the risk factor. Therefore, it is necessary to improve the comprehensive performance of magnesium alloys through surface treatment technology and better play their excellent characteristics.
[0003] Surface treatment technology for improving corrosion resistance of magnesium alloys. Common protective coatings are mostly electrically insulating. While improving the corrosion resistance of magnesium alloys, they significantly reduce surface conductivity and cannot meet the application of low contact resistance conductivity in equipment. The accumulation of surface charges seriously interferes with the normal operation of radio equipment, so it is necessary to conduct conductive treatment on its surface to release static electricity on its surface. At the same time, when magnesium alloy coatings are used in humid marine atmospheric environments, mold will grow on the surface due to nutrients on the coating surface, and pitting will occur in local locations, affecting the service safety of magnesium alloy structural parts. Therefore, the magnesium alloy coatings currently prepared are required to have corrosion resistance, conductivity, thermal control, and mildew resistance. Summary of the invention
[0004] In order to overcome the above problems existing in the prior art, the present invention proposes an integrated corrosion-resistant, conductive, thermally-controlled and mildew-proof coating on the surface of a magnesium alloy and a preparation method thereof.
[0005] The technical solution adopted by the present invention to solve its technical problems is: a corrosion-resistant, conductive, thermally controlled and mildew-proof integrated coating on the surface of a magnesium alloy comprises an inner layer and an outer layer, wherein the inner layer is a corrosion-resistant ceramic layer containing niobium elements, and the outer layer is a modified graphite-epoxy resin organic layer containing nano silver-copper alloy powder, wherein the thickness of the inner layer is 3-10 μm, and the thickness of the outer layer is 10-40 μm.
[0006] The above-mentioned magnesium alloy surface corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating, wherein the inner layer is prepared by a micro-arc oxidation process, and the outer layer is prepared by spraying.
[0007] The method for preparing the corrosion-resistant, conductive, thermally controlled and mildew-proof integrated coating on the surface of a magnesium alloy is used to prepare the above-mentioned corrosion-resistant, conductive, thermally controlled and mildew-proof integrated coating on the surface of a magnesium alloy, and specifically comprises:
[0008] Step 1, cleaning the surface of the magnesium alloy with deionized water and ethanol, and preparing a micro-arc oxidation electrolyte containing niobium element;
[0009] Step 2, placing the cleaned magnesium alloy into the micro-arc oxidation electrolyte prepared in step 1, mechanically stirring the micro-arc oxidation electrolyte, and maintaining the electrolyte temperature below 20° C. to perform micro-arc oxidation to obtain an inner layer;
[0010] Step 3, preparing a modified graphite-epoxy resin organic slurry containing nano silver-copper alloy powder, and spraying the organic slurry onto the surface of the magnesium alloy that has been subjected to micro-arc oxidation treatment to form an inner layer;
[0011] Step 4, placing the magnesium alloy obtained in step 3 into a drying oven and drying at 40-50° C. for 10-24 hours.
[0012] The above-mentioned method for preparing the corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating on the surface of the magnesium alloy, wherein the micro-arc oxidation electrolyte in step 1 comprises: 10 g / L sodium hexametaphosphate, 8 g / L sodium silicate, 4 g / L sodium hydroxide, and 8-12 g / L niobium element.
[0013] The above-mentioned method for preparing the corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating on the surface of magnesium alloy, the niobium element includes nano niobium powder and nano niobium pentoxide, the content of the nano niobium powder is 2-3g / L, and the content of the nano niobium pentoxide is 6-9g / L.
[0014] The above-mentioned method for preparing the corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating on the surface of the magnesium alloy, the organic slurry components and mass percentages in step 3 are specifically: 5-8% conductive carbon black, 15-20% nano silver copper alloy powder, 10% polyamide, 0.2% silane coupling agent, and the remainder is epoxy resin and acetone, and the mass ratio of epoxy resin to acetone is 3:1.
[0015] The preparation method of the above-mentioned magnesium alloy surface corrosion-resistant, conductive, thermally controlled and mildew-proof integrated coating, the conductive carbon black particle size is 2-3nm, the nano silver-copper alloy powder particle size is 100-800 mesh, and the mass ratio of Ag to Cu is greater than or equal to 1:4.
[0016] The beneficial effect of the present invention is that the present invention can obtain a magnesium alloy long-term protective layer with a dense and uniform surface microstructure, and has good electrical conductivity, corrosion resistance, and thermal control properties. At the same time, based on the principle that Ag and Cu particles inhibit biological activity, the coating also has the performance of preventing bacterial growth, meeting the service requirements of harsh marine atmospheric environments.
[0017] The process flow of the present invention is simple and easy to operate. The coating formed on the surface of the magnesium alloy has excellent corrosion resistance and integrated multifunctionality of electrical conductivity, thermal control and mildew resistance. It has significant application value and can meet the actual needs of aerospace, amphibious equipment and other fields for new corrosion-resistant conductive magnesium alloy materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0019] Figure 1 This is a schematic diagram of polarization curve testing of the surface of VW75 magnesium alloy before and after coating is prepared in Example 1 of the present invention;
[0020] Figure 2 This is a schematic diagram of the antibacterial effect test before and after the coating is prepared on the surface of the VW75 magnesium alloy in Example 1 of the present invention;
[0021] Figure 3 This is a schematic diagram of polarization curve testing of the surface of VW75 magnesium alloy before and after coating is prepared in Example 2 of the present invention;
[0022] Figure 4 Schematic diagram of the antibacterial effect test before and after the coating is prepared on the surface of the ZK61 magnesium alloy in Example 2 of the present invention. DETAILED DESCRIPTION
[0023] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0024] This embodiment discloses a magnesium alloy surface corrosion-resistant, conductive, thermally controlled and mildew-proof integrated coating, including an inner layer and an outer layer, wherein the inner layer is a corrosion-resistant ceramic layer containing niobium elements, and the outer layer is a modified graphite-epoxy resin organic layer containing nano silver-copper alloy powder, wherein the inner layer has a thickness of 3-10 μm and the outer layer has a thickness of 10-40 μm. The inner layer is prepared by a micro-arc oxidation process, and the outer layer is prepared by spraying.
[0025] The specific preparation method of the corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating on the surface of magnesium alloy specifically includes:
[0026] Step 1: Clean the surface of the magnesium alloy with deionized water and ethanol, and prepare a micro-arc oxidation electrolyte containing niobium element.
[0027] The micro-arc oxidation electrolyte includes: 10g / L sodium hexametaphosphate, 8g / L sodium silicate, 4g / L sodium hydroxide, 8-12g / L niobium element, the niobium element includes nano niobium powder and nano niobium pentoxide, the content of the nano niobium powder is 2-3g / L, and the content of the nano niobium pentoxide is 6-9g / L.
[0028] Step 2: Place the cleaned magnesium alloy into the micro-arc oxidation electrolyte prepared in step 1, mechanically stir the micro-arc oxidation electrolyte, and maintain the electrolyte temperature below 20° C. to perform micro-arc oxidation to obtain an inner layer.
[0029] Step 3: Prepare a modified graphite-epoxy resin organic slurry containing nano silver-copper alloy powder, and spray the organic slurry onto the surface of the magnesium alloy that has been treated with micro-arc oxidation to form an inner layer.
[0030] The organic slurry components and mass percentages are as follows: 5-8% conductive carbon black, 15-20% nano silver copper alloy powder, 10% polyamide, 0.2% silane coupling agent, and the remainder is epoxy resin and acetone, wherein the mass ratio of epoxy resin to acetone is 3:1. The particle size of the conductive carbon black is 2-3nm, the particle size of the nano silver copper alloy powder is 100-800 mesh, and the mass ratio of Ag to Cu is greater than or equal to 1:4.
[0031] Step 4, placing the magnesium alloy obtained in step 3 into a drying oven and drying at 40-50° C. for 10-24 hours.
[0032] Example 1
[0033] The micro-arc oxidation corrosion-resistant coating was first prepared on VW75 magnesium alloy. The electrolyte formula was: 10 g / L sodium hexametaphosphate, 8 g / L sodium silicate, 4 g / L sodium hydroxide, niobium powder / niobium pentoxide (Nb: Nb 2 O 5 ≥1:3)8g / L.
[0034] Organic slurry formula: carbon black addition amount is 5%, the mass ratio of epoxy resin to acetone is 3:1, polyamide addition amount is 10%, silane coupling agent addition amount is 0.2%, nano silver copper alloy powder (Ag: Cu = 1:4), the mass percentage of nano silver copper alloy powder is 15%, and the spraying thickness is 20μm. The VW75 magnesium alloy coated with organic conductive graphite is placed in a drying oven, the temperature is set to 40°C, and the drying time is 24h.
[0035] The prepared integrated coating has a uniform, dense and relatively smooth surface, completely covering the surface of the VW75 magnesium alloy.
[0036] from Figure 1 It can be seen that the corrosion resistance of the magnesium alloy surface is greatly improved, the electrochemical corrosion potential moves significantly in the positive direction, and the self-corrosion current density is greatly reduced.
[0037] After multimeter testing, the conductivity of the coating surface is 0.1 / cm 2 , with good electrical conductivity.
[0038] After the laboratory anti-aflatoxin test, the antibacterial rate of the coating surface can reach 99.15%. Figure 2 shown.
[0039] Example 2
[0040] The micro-arc oxidation corrosion-resistant coating was first prepared on ZK61 magnesium alloy. The electrolyte formula was: 10 g / L sodium hexametaphosphate, 8 g / L sodium silicate, 4 g / L sodium hydroxide, niobium powder / niobium pentoxide (Nb: Nb 2 O 5 =2:3)12g / L.
[0041] Organic slurry formula: carbon black addition amount is 8%, the mass ratio of epoxy resin to acetone is 3:1, polyamide addition amount is 10%, silane coupling agent addition amount is 0.2%, nano silver copper alloy powder (Ag: Cu = 1:3), the mass percentage of nano silver copper alloy powder is 20%, and the spraying thickness is 30μm. The ZK61 magnesium alloy coated with organic conductive graphite is placed in a drying oven, the temperature is set to 45°C, and the drying time is 20h.
[0042] The prepared integrated coating has a uniform, dense and relatively smooth surface, completely covering the surface of the ZK61 magnesium alloy.
[0043] from Figure 3 It can be seen that the corrosion resistance of the magnesium alloy surface is greatly improved, the electrochemical corrosion potential moves significantly in the positive direction, and the self-corrosion current density is greatly reduced.
[0044] After testing with a multimeter, the conductivity of the coating surface is 0.08 / cm 2 , with good electrical conductivity.
[0045] Figure 4 After the anti-aflatoxin test in the laboratory, the antibacterial rate of the coating surface reached 99.70%.
[0046] The above embodiments are only exemplary embodiments of the present invention and are not intended to limit the present invention. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present invention, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present invention.
Claims
1. The magnesium alloy surface has corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating, characterized in that: It comprises an inner layer and an outer layer, wherein the inner layer is a corrosion-resistant ceramic layer containing niobium element, and the outer layer is a modified graphite-epoxy resin organic layer containing nano silver-copper alloy powder. The thickness of the inner layer is 3-10 μm, and the thickness of the outer layer is 10-40 μm.
2. The magnesium alloy surface corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating according to claim 1, characterized in that: The inner layer is prepared by a micro-arc oxidation process, and the outer layer is prepared by spraying.
3. A method for preparing a corrosion-resistant, conductive, thermally controlled and mildew-proof integrated coating on the surface of a magnesium alloy, characterized in that: The method is used to prepare the magnesium alloy surface corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating as claimed in any one of claims 1 to 2, specifically comprising: Step 1, cleaning the surface of the magnesium alloy with deionized water and ethanol, and preparing a micro-arc oxidation electrolyte containing niobium element; Step 2, placing the cleaned magnesium alloy into the micro-arc oxidation electrolyte prepared in step 1, mechanically stirring the micro-arc oxidation electrolyte, and maintaining the electrolyte temperature below 20° C. to perform micro-arc oxidation to obtain an inner layer; Step 3, preparing a modified graphite-epoxy resin organic slurry containing nano silver-copper alloy powder, and spraying the organic slurry onto the surface of the magnesium alloy that has been subjected to micro-arc oxidation treatment to form an inner layer; Step 4, placing the magnesium alloy obtained in step 3 into a drying oven and drying at 40-50° C. for 10-24 hours.
4. The method for preparing the corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating on the surface of magnesium alloy according to claim 3, characterized in that: The micro-arc oxidation electrolyte in step 1 includes: 10 g / L sodium hexametaphosphate, 8 g / L sodium silicate, 4 g / L sodium hydroxide, and 8-12 g / L niobium element.
5. The method for preparing the corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating on the surface of magnesium alloy according to claim 4, characterized in that: The niobium element includes nano niobium powder and nano niobium pentoxide. The content of the nano niobium powder is 2-3 g / L, and the content of the nano niobium pentoxide is 6-9 g / L.
6. The method for preparing the corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating on the surface of magnesium alloy according to claim 1, characterized in that: The organic slurry components and mass percentages of step 3 are specifically: 5-8% conductive carbon black, 15-20% nano silver copper alloy powder, 10% polyamide, 0.2% silane coupling agent, and the remainder is epoxy resin and acetone, and the mass ratio of epoxy resin to acetone is 3:
1.
7. The method for preparing the corrosion-resistant, conductive, thermal-control and mildew-proof integrated coating on the surface of magnesium alloy according to claim 6, characterized in that: The particle size of the conductive carbon black is 2-3 nm, the particle size of the nano silver-copper alloy powder is 100-800 mesh, and the mass ratio of Ag to Cu is greater than or equal to 1:4.