Method for eliminating internal stress of CVD (Chemical Vapor Deposition) diamond wafer

The CVD diamond sheet is stressed through the wrapping and assembly structure, which solves the problem of high internal stress in the diamond sheet, realizes stress elimination, improves the quality and yield of diamonds, and is suitable for diamond sheets of different sizes and thicknesses.

CN118880472APending Publication Date: 2024-11-01ZHENGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410939571.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the existing CVD diamond preparation technology, diamond sheets generally have large internal stresses, which lead to lobe problems, limiting the high quality and yield of diamonds, especially the use of large-sized crystals.

Method used

CVD diamond sheets are wrapped and assembled through wrapping parts to form assembly blocks, and then stress-removing treatment is performed on a domestic six-sided top press, using molybdenum foil, gold foil or platinum foil as wrapping parts, combining leaf wax stone containers and conductive metals The assembly structure of the steel cap is subject to high temperature and high pressure treatment.

Benefits of technology

It realizes effective elimination of internal stress of CVD diamond sheets and is suitable for diamond sheets of different sizes and thicknesses. It has direct effect, short time, low cost and simple operation, which improves the quality and yield of diamonds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880472A_ABST
    Figure CN118880472A_ABST
Patent Text Reader

Abstract

The invention discloses a method for eliminating internal stress of a CVD (Chemical Vapor Deposition) diamond wafer, and belongs to the technical field of diamond crystal preparation, and the method for eliminating the internal stress of the CVD diamond wafer comprises the following steps: obtaining at least one CVD diamond wafer, independently wrapping the at least one CVD diamond wafer by using a wrapping piece, and assembling the at least one CVD diamond wafer. And the assembled block is placed on a domestic cubic press for stress elimination treatment, and the method has the advantages that the stress is directly eliminated at a time, the stress elimination effect is good, the time is short, the cost is low, the operation is easy, and the application range is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of diamond crystal preparation, in particular to a method for eliminating internal stress of a CVD diamond sheet. Background Art

[0002] Diamond is a material with broad application prospects in the fields of national defense, medical treatment, health and microelectronics. In recent years, scientists have developed many new uses for diamond, such as microsphere electron microscope arrays, medical scalpels, heat dissipation substrates for chips, and gyroscopes and accelerometers for aerospace.

[0003] At present, the mainstream methods used to grow diamond crystals internationally include high temperature and high pressure method and microwave plasma chemical vapor deposition method; among them, microwave plasma chemical vapor deposition method (MPCVD) has the advantages of electrodeless discharge, no pollution and strong epitaxial controllability. It has more obvious advantages in the preparation and doping research of large-size and high-purity diamonds. It is the preferred method for high-quality and multi-field application diamond preparation. The products can be widely used in acoustics, optics, thermal, mechanics, electricity, quantum technology and other fields.

[0004] However, diamonds grown by the MPCVD method currently generally have the problem of large internal stress leading to diamond fracturing, which has become the main reason restricting their high quality and yield rate; more importantly, the larger the size of the grown diamond, the more obvious the internal stress will be, which in turn seriously restricts the use of large-size crystals.

[0005] Therefore, how to eliminate the internal stress in CVD diamond has important and practical application significance for improving the quality and yield of diamond. The existing technology still has a technical gap in achieving effective removal of internal stress in diamond, which is a technical field that needs to be filled.

[0006] Therefore, it is necessary to provide a method for eliminating the internal stress of a CVD diamond sheet in order to solve the above problems. Summary of the invention

[0007] In view of the shortcomings of the prior art, an embodiment of the present invention aims to provide a method for eliminating internal stress of a CVD diamond sheet to solve the problems in the above-mentioned background technology.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A method for eliminating internal stress of a CVD diamond sheet comprises the following steps:

[0010] Step S1, obtaining at least one CVD diamond sheet;

[0011] Step S2, using a packaging member to individually wrap at least one CVD diamond sheet;

[0012] Step S3, assembling at least one CVD diamond sheet to obtain an assembly block;

[0013] Step S4: placing the assembly block on a domestic six-sided press to perform stress relief treatment.

[0014] As a further solution of the present invention, the package in step S2 is one of molybdenum foil, gold foil and platinum foil.

[0015] As a further solution of the present invention, the step of assembling at least one CVD diamond sheet in step S3 comprises:

[0016] Step S31, using a pyrophyllite block as an external container, and stacking the carbon sheet and the sleeve in sequence and placing them inside the pyrophyllite container;

[0017] Step S32, placing a graphite heating tube in the sleeve, and sequentially filling a placement column and a placement tube in the graphite heating tube;

[0018] Step S33, placing the graphite layer and the CVD diamond sheet wrapped by the wrapping member in the placement tube in sequence;

[0019] Step S34, after placing the column cover on the topmost graphite layer, stack the carbon sheet, molybdenum sheet, copper sheet and the conductive metal steel cap with the pyrophyllite ring in sequence and put them into the pyrophyllite container to complete the assembly.

[0020] As a further solution of the present invention, the sleeve in step S32 is MgO+ZrO 2 Casing, the placement column is MgO+ZrO 2 Column, the placement tube is MgO+ZrO 2 Tube.

[0021] As a further solution of the present invention, the maximum number of diamond layers that can be simultaneously accommodated in the pyrophyllite container is:

[0022] n=(hl 1 ) / l 2 ,

[0023] Where n is the maximum number of diamond layers that can be accommodated at the same time, h is the cavity height inside the pyrophyllite container, l 1 is the height of the graphite layer at one end, l 2 is the graphite layer thickness.

[0024] As a further solution of the present invention, the working pressure range of the domestic six-sided top press in step S4 is 1.0-8.0GPa, and the temperature range is 100-2000°C.

[0025] As a further solution of the present invention, the thickness of the graphite layer is not less than 1.0 mm.

[0026] As a further solution of the present invention, the CVD diamond sheet has a thickness of 0.01-30 mm.

[0027] As a further solution of the present invention, the size of the CVD diamond sheet is 0.1-85 mm.

[0028] As a further solution of the present invention, the CVD diamond slices include diamond single crystal slices and diamond multi-crystal slices.

[0029] In summary, compared with the prior art, the embodiments of the present invention have the following beneficial effects:

[0030] The present invention wraps at least one CVD diamond sheet with a wrapping piece, assembles at least one wrapped CVD diamond sheet to obtain an assembly block, and places the assembly block on a domestic six-sided top press to perform a stress elimination treatment, which can meet the stress of CVD diamond sheets of different sizes and thicknesses, and has the effects of direct stress elimination, good stress elimination effect, short time, low cost, easy operation and wide application range.

[0031] In order to more clearly illustrate the structural features and effects of the present invention, the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The figure is a flow chart of the steps of the method for eliminating the internal stress of a CVD diamond sheet in an embodiment of the invention.

[0033] Figure 2 This is a flow chart of the assembly steps of a CVD diamond sheet in an embodiment of the invention.

[0034] Figure 3 This is a diagram of the assembly structure of small pieces in a small cavity in an embodiment of the invention.

[0035] Figure 4 This is a diagram of the assembly structure of small pieces in a large cavity in an embodiment of the invention.

[0036] Figure 5 This is a diagram of the assembly structure of a large piece in a large cavity in an embodiment of the invention.

[0037] Figure 6 a is a stress polarization diagram of the CVD diamond sheet before stress relief in the embodiment of the invention, Figure 6 b is a stress polarization diagram of the CVD diamond sheet after stress elimination in the embodiment of the invention.

[0038] Figure 7This is a comparison diagram of Raman characterization of the CVD diamond sheet before and after annealing in the embodiment of the invention. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0040] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0041] In one embodiment of the present invention, see Figure 1 and Figure 2 The method for eliminating internal stress of a CVD diamond sheet comprises the following steps:

[0042] Step S1, obtaining at least one CVD diamond sheet;

[0043] Step S2, using a packaging member to individually wrap at least one CVD diamond sheet;

[0044] Step S3, assembling at least one CVD diamond sheet to obtain an assembly block;

[0045] Step S4: placing the assembly block on a domestic six-sided press to perform stress relief treatment.

[0046] In this embodiment, the package in step S2 is one of molybdenum foil, gold foil and platinum foil;

[0047] The step of assembling at least one CVD diamond sheet in step S3 comprises:

[0048] Step S31, using a pyrophyllite block as an external container, and stacking the carbon sheet and the sleeve in sequence and placing them inside the pyrophyllite container;

[0049] Step S32: In MgO+ZrO 2 Put a graphite heating tube into the casing, and fill MgO+ZrO into the graphite heating tube in sequence. 2 Column and MgO+ZrO 2 Tube;

[0050] Step S33: In MgO+ZrO 2 A graphite layer and a CVD diamond sheet wrapped by a wrapping member are sequentially placed on the tube;

[0051] Step S34: MgO+ZrO 2 After the column is covered with the top graphite layer, the carbon sheet, molybdenum sheet, copper sheet and a conductive metal steel cap with a pyrophyllite ring are stacked in sequence and placed in a pyrophyllite container to complete the assembly.

[0052] At the same time, the maximum number of diamond layers that can be accommodated in the pyrophyllite container at the same time is:

[0053] n=(hl 1 ) / l 2 ,

[0054] Where n is the maximum number of diamond layers that can be accommodated at the same time, h is the cavity height inside the pyrophyllite container, l 1 is the height of the graphite layer at one end, l 2 is the thickness of the graphite layer. When the thickness of the diamond wafer is 0.1 mm and the thickness of the graphite layer is l 2 When the thickness of the graphite layer is 1.1 mm, a pit with a depth of 0.1 mm and the size of a diamond wafer is dug out on the 1.1 mm graphite layer, and the 0.1 mm diamond wafer is placed in it. 2 The depth of the pits should be adjusted according to the thickness of the diamond sheet and the thickness of the graphite layer between the diamond sheets should be ensured to be l 2 Not less than 1.0mm, for example: if the chip thickness becomes 1.0mm, then the graphite layer thickness l 2 Adjusted to 2.0 mm, at this 2.0 mm thickness graphite layer l 2 A 1.0 mm deep pit is prepared on the wafer and placed therein;

[0055] The working pressure range of the domestic six-sided top press in step S4 is 1.0-8.0GPa, the temperature range is 100-2000℃, the thickness of the graphite layer is not less than 1.0mm, the thickness of the CVD diamond sheet is 0.01-30mm, the size of the CVD diamond sheet is 0.1-85mm, and the CVD diamond sheet includes diamond single crystal sheets and diamond multi-crystal sheets.

[0056] See also Figure 3 When the annealing cavity inside the pyrophyllite container is a small cavity and the diamond sheet is small in size, the internal stress relief treatment can be performed on at least one CVD diamond sheet at a time by arranging the diamond sheets in layers from top to bottom.

[0057] See also Figure 4 When the annealing cavity inside the pyrophyllite container is a large cavity and the diamond slices are small in size, the internal stress elimination treatment of a large number of CVD diamond slices can be achieved by arranging the diamond slices in layers from top to bottom and distributing them evenly in the same layer;

[0058] See also Figure 5 When the annealing cavity inside the pyrophyllite container is a large cavity and the diamond sheet is large in size, the internal stress of large-sized diamond sheets of different shapes can be eliminated by arranging the diamond sheets in layers from top to bottom.

[0059] See also Figure 6 Polaroid is a specially treated optical element that can selectively absorb light in certain directions, so that only light in certain directions remains after the light passes through. Under natural light, light in all directions will be absorbed, and only light with specific directions will remain after passing through the polaroid; if the stress distribution in the chip is uniform, then when we rotate the polaroid, the changes in brightness and color will be relatively uniform; but if there are some local stress distributions in the lens, then when observing these parts, color deviation or brightness changes will occur; in this way, we can understand the distribution of stress inside the chip by observing the color changes on the surface of the lens. It can be clearly seen from the polarization comparison before and after that the chip that has not been stress-relieved shows an overall obvious brightness change, which indicates that the overall internal stress inside the chip is very large. After we use this method to eliminate stress, it can be clearly seen that the brightness of the chip is not obvious, indicating that the internal stress has been effectively eliminated.

[0060] See also Figure 7 , a comparative analysis of Raman tests on CVD diamond wafers before and after high temperature and high pressure annealing was performed; it can be seen that the diamond Raman peak of the crystal before annealing is located at 1329.90cm -1 , and the intensity of the Raman peak is very weak; after high temperature and high pressure annealing, the diamond Raman peak position of the crystal has changed to 1330.60cm -1 , obviously towards the standard diamond peak of 1332cm -1 The Raman peak intensity was significantly enhanced; at the same time, the half-peak width was also increased from 6.61cm before annealing. -1 Reduced to 6.24cm -1; By comparing the Raman peak position and half-peak width before and after annealing, it can be clearly seen that the overall quality of diamond is significantly improved and the internal stress is effectively eliminated.

[0061] In summary, the present application wraps at least one CVD diamond sheet with a wrapping piece, and assembles at least one wrapped CVD diamond sheet to obtain an assembly block, and places the assembly block on a domestic six-sided top press for a stress relief treatment, which can meet the stress of CVD diamond sheets of different sizes and thicknesses, and has the effects of direct stress relief, good stress relief effect, short time, low cost, easy operation and wide application range.

[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for eliminating internal stress of a CVD diamond sheet, characterized in that: The following steps are involved: Step S1, obtaining at least one CVD diamond sheet; Step S2, using a packaging member to individually wrap at least one CVD diamond sheet; Step S3, assembling at least one CVD diamond sheet to obtain an assembly block; Step S4: placing the assembly block on a domestic six-sided press to perform stress relief treatment.

2. The method for eliminating internal stress of a CVD diamond sheet according to claim 1, characterized in that: The package in step S2 is one of molybdenum foil, gold foil and platinum foil.

3. The method for eliminating internal stress of a CVD diamond sheet according to claim 1, characterized in that: The step of assembling at least one CVD diamond sheet in step S3 comprises: Step S31, using a pyrophyllite block as an external container, and stacking the carbon sheet and the sleeve in sequence and placing them inside the pyrophyllite container; Step S32, placing a graphite heating tube in the sleeve, and sequentially filling a placement column and a placement tube in the graphite heating tube; Step S33, placing the graphite layer and the CVD diamond sheet wrapped by the wrapping member in the placement tube in sequence; Step S34, after placing the column cover on the topmost graphite layer, stack the carbon sheet, molybdenum sheet, copper sheet and the conductive metal steel cap with the pyrophyllite ring in sequence and put them into the pyrophyllite container to complete the assembly.

4. The method for eliminating internal stress of a CVD diamond sheet according to claim 3, characterized in that: The casing in step S32 is a MgO+ZrO2 casing, the placement column is a MgO+ZrO2 column, and the placement tube is a MgO+ZrO2 tube.

5. The method for eliminating internal stress of a CVD diamond sheet according to claim 3, characterized in that: The maximum number of diamond layers that can be accommodated in the pyrophyllite container at the same time is: n=(h-l1) / l2, Among them, n is the maximum number of diamond layers that can be accommodated at the same time, h is the cavity height inside the pyrophyllite container, l1 is the height of the graphite layer at one end, and l2 is the thickness of the graphite layer.

6. The method for eliminating internal stress of a CVD diamond sheet according to claim 1, characterized in that: The working pressure range of the domestic six-sided top press in step S4 is 1.0-8.0 GPa, and the temperature range is 100-2000°C.

7. The method for eliminating internal stress of a CVD diamond sheet according to claim 3, characterized in that: The graphite layer has a thickness of not less than 1.0 mm.

8. The method for eliminating internal stress of a CVD diamond sheet according to claim 1, characterized in that: The thickness of the CVD diamond sheet is 0.01-30 mm.

9. The method for eliminating internal stress of a CVD diamond sheet according to claim 1, characterized in that: The size of the CVD diamond sheet is 0.1-85 mm.

10. The method for eliminating internal stress of a CVD diamond sheet according to claim 1, characterized in that: The CVD diamond slices include diamond single crystal slices and diamond multi-crystal slices.