Multifunctional anti-perspective fiber for spinning and preparation method thereof

By combining nanotitanium dioxide with polyamic acid solution, nanotitanium dioxide composite aerogel is prepared, and cross-linking modifier is added during spinning, the problem of insufficient fiber anti-film and anti-UV performance is solved, and high efficiency is achieved The anti-perspective, anti-UV performance and mechanical performance are improved, suitable for summer clothing.

CN118880487APending Publication Date: 2024-11-01QINGDAO BANGTE ECOLOGICAL TEXTILE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411043940.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When existing synthetic fibers improve anti-film and UV resistance, the increase in weight leads to a decrease in breathability, and the dispersion performance of titanium dioxide in the fibers is poor, affecting the fiber strength, and cannot meet the national standards of anti-film and UV resistance.

Method used

The nanotitanium dioxide composite aerogel is prepared by combining amino-amino acid solution by ultrasonic dispersion, liquid nitrogen freeze-drying and thermal annealing. Combined with cross-linking modifiers, a three-dimensional network structure is formed during the spinning process to improve the fibers. Anti-follow-proof, UV-resistant and mechanical properties.

Benefits of technology

Prepare light and comfortable multifunctional anti-perspective fibers, with high moisture rebate, excellent anti-perspective effect, excellent ultraviolet protection performance, and improved mechanical performance. They are suitable for summer clothing and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004973016360000101
    Figure BDA0004973016360000101
Patent Text Reader

Abstract

The invention belongs to the technical field of synthetic fibers, and particularly relates to a multifunctional anti-perspective fiber for spinning and a preparation method of the multifunctional anti-perspective fiber for spinning, and the preparation method comprises preparation of aminated nano titanium dioxide, preparation of a precursor, preparation of nano titanium dioxide composite aerogel, preparation of anti-perspective master batch and spinning. The amino-modified nano titanium dioxide and polyimide are compounded to prepare the nano titanium dioxide composite aerogel, and the nano titanium dioxide is good in dispersity and good in compatibility with polymer slices, so that the influence of the addition of inorganic powder on the mechanical property of the fiber is avoided. Fabric made of the multifunctional anti-perspective fiber is light, thin, comfortable and breathable and has excellent anti-perspective, anti-UV, cool and quick-drying effects and the like, and the anti-perspective effect is higher than 96%; the ultraviolet protection coefficient UPF is larger than 50, the ultraviolet protection coefficient UPFAV is larger than 1900, the ultraviolet transmittance T (UVA) AV is smaller than or equal to 0.1%, and the ultraviolet transmittance T (UVB) AV is smaller than or equal to 0.1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of synthetic fibers, and in particular relates to a multifunctional anti-see-through fiber for textile use and a preparation method thereof. Background Art

[0002] The continuous high temperature in summer makes consumers have higher requirements for clothing fabrics. Light, comfortable and UV-proof clothing fabrics are more popular among consumers. However, most summer fabrics are light and thin, but have poor anti-see-through performance and wear resistance. Synthetic fibers are widely used in summer sun protection clothing, sportswear, etc. Therefore, synthetic fibers with anti-see-through, anti-UV, and breathable functions have good market application value.

[0003] At present, researchers in the market usually improve the anti-see-through and anti-UV properties of fabrics by adding titanium dioxide and increasing the weight of the fabrics. However, the increase in weight will reduce the air permeability of the fabrics, resulting in reduced comfort of the finished garments. Titanium dioxide is used to improve the anti-see-through and anti-UV properties of polyester, but titanium dioxide has poor dispersion in fiber raw materials and poor compatibility with fiber raw materials, which can easily affect the strength of synthetic fibers. In order to ensure the strength of the fibers, the amount of titanium dioxide added must be reduced as much as possible, which will cause the anti-see-through and anti-UV properties of the fabrics woven with it to fail to meet the national standards. In addition, most anti-see-through fabrics on the market can prevent the naked eye from seeing through them, but in infrared transmission environments, there is still a risk of being secretly photographed.

[0004] Patent number "CN201510296932.X" entitled "A method for preparing regenerated cellulose fibers with high optical shielding properties" uses a dispersant and a plate-and-frame filter to filter a uniform high-refractive powder dispersion emulsion and a mixed solution of viscose into a wet spinning process for spinning, but the resulting fiber strength is not high. In addition, the preparation temperature of the synthetic fiber is relatively high, which easily causes the dispersant on the powder surface to fall off and the fiber to break. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a multifunctional anti-see-through fiber for textile use and a preparation method thereof, so as to achieve the invention purpose of preparing a synthetic fiber with anti-see-through, anti-UV, breathable and other functions and avoiding the decrease in the strength of the synthetic fiber.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A multifunctional anti-see-through fiber for textile use and a preparation method thereof, the preparation method comprising the following steps:

[0008] S1. Preparation of amino-modified nano-titanium dioxide

[0009] Add nano titanium dioxide into deionized water and ultrasonically disperse for 3 to 5 minutes, then add ammonia water and 3-aminopropyltrimethoxysilane, heat to 50 to 60°C and stir to react for 4 to 6 hours. After the reaction is completed, cool to room temperature, centrifuge, and ultrasonically vibrate, wash, dry, and ball-mill the precipitate to obtain amino nano titanium dioxide.

[0010] Preferably, the particle size of the nano titanium dioxide is 20-40 nm; the mass ratio of the nano titanium dioxide to deionized water is 1:8-10.

[0011] Preferably, the mass fraction of the ammonia water is 20-30%.

[0012] Preferably, the amount of ammonia water added is 35-50% of the mass of the nano-titanium dioxide, and the amount of 3-aminopropyltrimethoxysilane added is 18-25% of the mass of the nano-titanium dioxide.

[0013] Preferably, the ball milling speed is 300-400 r / min, and the ball milling time is 9-10 h.

[0014] S2. Preparation of Precursors

[0015] 4,4 ’ -diaminodiphenyl ether is added to N-methylpyrrolidone, stirred under nitrogen protection until dissolved, and then pyromellitic anhydride is added and stirred for 2 to 3 hours, followed by adding a carboxyl protecting agent N, N-diethylethylamine solution and continuing to stir for 60 to 90 minutes to obtain a precursor solution.

[0016] Preferably, the 4,4 ’ The mass ratio of diaminodiphenyl ether to N-methylpyrrolidone is 1:4-5.

[0017] Preferably, the 4,4 ’ The molar ratio of diaminodiphenyl ether to pyromellitic dianhydride is 1:1.05-1.15.

[0018] Preferably, the concentration of the N,N-diethylethylamine solution is 4-6%, and the amount added is 4,4 ’ -Diaminodiphenyl ether and 4,4 ’ -9 to 13% of the total mass of diaminodiphenyl ether.

[0019] S3. Preparation of nano-titanium dioxide composite aerogel

[0020] The aminated nano-titanium dioxide is added to anhydrous ethanol and ultrasonically dispersed for 3 to 5 minutes to obtain a nano-titanium dioxide dispersion; the aminated nano-titanium dioxide dispersion is added to the precursor solution while stirring, the pH is adjusted to 4.5 to 5.5 and stirring is continued for 2 to 4 hours, and then the nano-titanium dioxide composite aerogel is obtained after liquid nitrogen freezing, freeze drying, thermal annealing and crushing.

[0021] Preferably, the mass ratio of nano-titanium dioxide to anhydrous ethanol in the amino-treated nano-titanium dioxide dispersion is 1:8-10.

[0022] Preferably, the mass ratio of nano-titanium dioxide in the amino-treated nano-titanium dioxide dispersion to the precursor solution is 1:6-8.

[0023] Preferably, the temperature of the liquid nitrogen freezing is -50°C to -40°C, and the time is 30 to 40 minutes.

[0024] Preferably, the freeze-drying temperature is -10°C to -5°C, and the time is 48 to 72 hours.

[0025] Preferably, the thermal annealing temperature is 240-320° C. and the time is 50-60 min.

[0026] Preferably, the particle size of the crushed nano-titanium dioxide composite aerogel is 2 to 10 μm.

[0027] The precursor solution is a polyamic acid salt solution. Under acidic conditions, the amino groups modified on the aminated nano-titanium dioxide condense with the carboxylate molecules in the polyamic acid salt solution to form amides, thereby obtaining an aerogel with a three-dimensional network structure. The aerogel is then imidized by thermal annealing to obtain a nano-titanium dioxide composite aerogel of nano-titanium dioxide and polyimide.

[0028] S4. Preparation of anti-see-through masterbatch

[0029] The polymer slices and the nano-titanium dioxide composite aerogel are uniformly mixed and granulated by a twin-screw extruder. After granulation, the mixture is dried to a moisture content of less than 100 ppm to obtain an anti-see-through masterbatch.

[0030] Preferably, the ratio of the nano-titanium dioxide composite aerogel to the polymer slice is 40-50:50-60; the polymer slice is preferably one of PET or PA.

[0031] S5. Spinning

[0032] The anti-see-through masterbatch, polymer slices and cross-linking modifier are mixed evenly and then spun, and then oiled after cooling to obtain a multifunctional anti-see-through fiber.

[0033] Preferably, the mass ratio of the anti-see-through masterbatch, the polymer slice and the cross-linking modifier is 3-5:92-97:1.02-1.17.

[0034] Preferably, the cross-linking modifier is triglycidyl isocyanurate.

[0035] Preferably, the spinning rate is 1000-1200 m / min, the box temperature is 220-290° C.; and the cross-sectional shape of the spinning spinneret is a “cross”.

[0036] Due to the adoption of the above technical solution, the technical effects achieved by the present invention are:

[0037] 1. The multifunctional anti-see-through fiber prepared by the present invention is made into a fabric that is light, comfortable and breathable, and has excellent anti-see-through and anti-UV effects. The fiber regain is greater than 2%, and the anti-see-through effect is higher than 96% (determined according to JIS L 1923B method); the ultraviolet protection factor UPF>50, the ultraviolet protection factor UPF AV >1900, UV transmittance T(UVA) AV ≤0.1%, UV transmittance T(UVB) AV ≤0.1% (measured according to JIS L 1925).

[0038] 2. The precursor solution prepared by the present invention is a polyamic acid salt solution. Under acidic conditions, the amino groups modified on the aminated nano-titanium dioxide condense with the carboxylate molecules in the polyamic acid salt solution to form amides, thereby obtaining an aerogel having a three-dimensional network structure, and then undergoing thermal annealing and imidization to obtain a nano-titanium dioxide composite aerogel composited with nano-titanium dioxide and polyimide; under the action of polyimide, the nano-titanium dioxide has good dispersibility and good compatibility with polymer slices, thereby avoiding the addition of inorganic powders to affect the mechanical properties of the fiber. In addition, a cross-linking modifier is added during the spinning mixing process, and under the high temperature conditions of spinning, the epoxy groups in triglycidyl isocyanurate are ring-opened, and the hydroxyl groups in the polyester, the imide groups in the polyimide and the ring-opened epoxy groups are cross-linked to form a network structure, thereby further improving the mechanical properties of the multifunctional anti-perspective fiber.

[0039] 3. The fabric made of the multifunctional anti-see-through fiber prepared by the present invention has the effect of cooling and quick drying, and the contact cooling coefficient (Q max ) is greater than 0.27 (determined according to JIS L 1927), the water absorption is 1s (determined according to the JIS L 1907 dropping method), and the diffusible residual moisture rate is less than 13%. It can be used in summer light-colored sportswear, sailor suits, military uniforms and other fields. DETAILED DESCRIPTION

[0040] The present invention is further described below in conjunction with specific embodiments.

[0041] Example 1

[0042] S1. Preparation of amino-modified nano-titanium dioxide

[0043] Nano-titanium dioxide was added into deionized water and ultrasonically dispersed for 5 minutes, then ammonia water and 3-aminopropyltrimethoxysilane were added, the temperature was raised to 55°C and stirred for reaction for 5 hours, after which the reaction was cooled to room temperature, centrifuged and the precipitate was ultrasonically vibrated, washed, dried and ball-milled to obtain amino-nano-titanium dioxide.

[0044] The particle size of the nano titanium dioxide is 30 nm; the mass ratio of the nano titanium dioxide to deionized water is 1:9.

[0045] The mass fraction of the ammonia water is 27%.

[0046] The amount of ammonia water added is 42% of the mass of nano-titanium dioxide, and the amount of 3-aminopropyltrimethoxysilane added is 23% of the mass of nano-titanium dioxide.

[0047] The ball milling speed is 350 r / min, and the ball milling time is 10 h.

[0048] S2. Preparation of Precursors

[0049] 4,4 ’ -Diaminodiphenyl ether was added to N-methylpyrrolidone, stirred under nitrogen protection until dissolved, and then pyromellitic anhydride was added and stirred for 2.5 hours, followed by adding a carboxyl protecting agent N, N-diethylethylamine solution and continuing to stir for 80 minutes to obtain a precursor solution.

[0050] 4,4 ’ The mass ratio of diaminodiphenyl ether to N-methylpyrrolidone is 1:4.5.

[0051] 4,4 ’ The molar ratio of diaminodiphenyl ether to pyromellitic dianhydride is 1:1.1.

[0052] The concentration of the N,N-diethylethylamine solution is 5%, and the amount added is 4,4 ’ -Diaminodiphenyl ether and 4,4 ’ -11% of the total mass of diaminodiphenyl ether.

[0053] S3. Preparation of nano-titanium dioxide composite aerogel

[0054] The aminated nano-titanium dioxide was added to anhydrous ethanol and ultrasonically dispersed for 5 minutes to obtain a nano-titanium dioxide dispersion; the aminated nano-titanium dioxide dispersion was added to the precursor solution while stirring, the pH was adjusted to 5 and stirring was continued for 3 hours, and then the nano-titanium dioxide composite aerogel was obtained after liquid nitrogen freezing, freeze drying, thermal annealing and crushing.

[0055] The mass ratio of nano-titanium dioxide to anhydrous ethanol in the amination nano-titanium dioxide dispersion is 1:7. The mass ratio of nano-titanium dioxide to precursor solution in the amination nano-titanium dioxide dispersion is 1:7.

[0056] The temperature of the liquid nitrogen freezing is -50°C and the time is 35 minutes.

[0057] The freeze-drying temperature is -10°C and the time is 56 hours.

[0058] The thermal annealing temperature is 280° C. and the time is 55 min.

[0059] The particle size of the crushed nano titanium dioxide composite aerogel is 2 μm.

[0060] S4. Preparation of anti-see-through masterbatch

[0061] The PET slices and the nano-titanium dioxide composite aerogel were uniformly mixed and granulated by a twin-screw extruder. After granulation, the mixture was dried to a moisture content of less than 100 ppm to obtain an anti-see-through masterbatch.

[0062] The ratio of the nano-titanium dioxide composite aerogel to the PET slice is 45:55.

[0063] S5. Spinning

[0064] The anti-see-through masterbatch, PET chips and cross-linking modifier are mixed evenly and then spun, and then oiled after cooling to obtain multifunctional anti-see-through fibers.

[0065] The mass ratio of the anti-see-through masterbatch, the PET slice and the cross-linking modifier is 4:94:1.13.

[0066] The cross-linking modifier is triglycidyl isocyanurate.

[0067] The spinning rate is 1100 m / min, the box temperature is 280° C., and the cross-sectional shape of the spinning spinneret is a “cross”.

[0068] Example 2

[0069] S1. Preparation of amino-modified nano-titanium dioxide

[0070] Nano-titanium dioxide was added into deionized water and ultrasonically dispersed for 3 minutes, then ammonia water and 3-aminopropyltrimethoxysilane were added, the temperature was raised to 50°C and stirred for reaction for 4 hours, after the reaction was completed, it was cooled to room temperature, centrifuged and the precipitate was ultrasonically vibrated, washed, dried and ball-milled to obtain amino-nano-titanium dioxide.

[0071] The particle size of the nano titanium dioxide is 40 nm; the mass ratio of the nano titanium dioxide to deionized water is 1:8.

[0072] The mass fraction of the ammonia water is 20%.

[0073] The amount of ammonia water added is 50% of the mass of nano-titanium dioxide, and the amount of 3-aminopropyltrimethoxysilane added is 18% of the mass of nano-titanium dioxide.

[0074] The ball milling speed is 300 r / min, and the ball milling time is 9 h.

[0075] S2. Preparation of Precursors

[0076] 4,4 ’ -Diaminodiphenyl ether was added to N-methylpyrrolidone, stirred under nitrogen protection until dissolved, and then pyromellitic anhydride was added and stirred for 2 hours, followed by adding a carboxyl protecting agent N, N-diethylethylamine solution and continued stirring for 60 minutes to obtain a precursor solution.

[0077] 4,4 ’ The mass ratio of diaminodiphenyl ether to N-methylpyrrolidone is 1:4.

[0078] 4,4 ’ The molar ratio of diaminodiphenyl ether to pyromellitic dianhydride is 1:1.05.

[0079] The concentration of the N,N-diethylethylamine solution is 4%, and the amount added is 4,4 ’ -Diaminodiphenyl ether and 4,4 ’ -9% of the total mass of diaminodiphenyl ether.

[0080] S3. Preparation of nano-titanium dioxide composite aerogel

[0081] The aminated nano-titanium dioxide was added to anhydrous ethanol and ultrasonically dispersed for 3 minutes to obtain a nano-titanium dioxide dispersion; the aminated nano-titanium dioxide dispersion was added to the precursor solution while stirring, the pH was adjusted to 4.5 and stirring was continued for 2 hours, and then the nano-titanium dioxide composite aerogel was obtained after liquid nitrogen freezing, freeze drying, thermal annealing and crushing.

[0082] The mass ratio of nano-titanium dioxide to anhydrous ethanol in the amination nano-titanium dioxide dispersion is 1:6. The mass ratio of nano-titanium dioxide to precursor solution in the amination nano-titanium dioxide dispersion is 1:6.

[0083] The temperature of the liquid nitrogen freezing is -40°C and the time is 30 minutes.

[0084] The freeze-drying temperature is -5°C and the time is 48 hours.

[0085] The thermal annealing temperature is 240° C. and the time is 50 min.

[0086] The particle size of the crushed nano titanium dioxide composite aerogel is 10 μm.

[0087] S4. Preparation of anti-see-through masterbatch

[0088] The PET slices and the nano-titanium dioxide composite aerogel were uniformly mixed and granulated by a twin-screw extruder. After granulation, the mixture was dried to a moisture content of less than 100 ppm to obtain an anti-see-through masterbatch.

[0089] The ratio of the nano-titanium dioxide composite aerogel to the PET slice is 40:60.

[0090] S5. Spinning

[0091] The anti-see-through masterbatch, PET chips and cross-linking modifier are mixed evenly and then spun, and then oiled after cooling to obtain multifunctional anti-see-through fibers.

[0092] The mass ratio of the anti-see-through masterbatch, the PET slice and the cross-linking modifier is 3:97:1.02.

[0093] The cross-linking modifier is triglycidyl isocyanurate.

[0094] The spinning rate is 1000 m / min, the box temperature is 270° C., and the cross-sectional shape of the spinning spinneret is a “cross”.

[0095] Example 3

[0096] S1. Preparation of amino-modified nano-titanium dioxide

[0097] Nano-titanium dioxide was added into deionized water and ultrasonically dispersed for 4 minutes, then ammonia water and 3-aminopropyltrimethoxysilane were added, the temperature was raised to 60°C and stirred for reaction for 6 hours, after which the reaction was cooled to room temperature, centrifuged and the precipitate was ultrasonically vibrated, washed, dried and ball-milled to obtain amino-nano-titanium dioxide.

[0098] The particle size of the nano titanium dioxide is 20 nm; the mass ratio of the nano titanium dioxide to deionized water is 1:10.

[0099] The mass fraction of the ammonia water is 30%.

[0100] The amount of ammonia water added is 35% of the mass of nano-titanium dioxide, and the amount of 3-aminopropyltrimethoxysilane added is 25% of the mass of nano-titanium dioxide.

[0101] The ball milling speed is 400 r / min, and the ball milling time is 9.5 h.

[0102] S2. Preparation of Precursors

[0103] 4,4 ’ -Diaminodiphenyl ether was added to N-methylpyrrolidone, stirred under nitrogen protection until dissolved, and then pyromellitic anhydride was added and stirred for 3 hours, followed by adding a carboxyl protecting agent N, N-diethylethylamine solution and continued stirring for 90 minutes to obtain a precursor solution.

[0104] 4,4 ’ The mass ratio of diaminodiphenyl ether to N-methylpyrrolidone is 1:5.

[0105] 4,4 ’ The molar ratio of diaminodiphenyl ether to pyromellitic dianhydride is 1:1.15.

[0106] The concentration of the N,N-diethylethylamine solution is 6%, and the amount added is 4,4 ’ -Diaminodiphenyl ether and 4,4 ’ -13% of the total mass of diaminodiphenyl ether.

[0107] S3. Preparation of nano-titanium dioxide composite aerogel

[0108] The aminated nano-titanium dioxide was added to anhydrous ethanol and ultrasonically dispersed for 4 minutes to obtain a nano-titanium dioxide dispersion; the aminated nano-titanium dioxide dispersion was added to the precursor solution while stirring, the pH was adjusted to 5.5 and stirring was continued for 4 hours, and then the nano-titanium dioxide composite aerogel was obtained after liquid nitrogen freezing, freeze drying, thermal annealing and crushing.

[0109] The mass ratio of nano-titanium dioxide to anhydrous ethanol in the amination nano-titanium dioxide dispersion is 1:8. The mass ratio of nano-titanium dioxide to precursor solution in the amination nano-titanium dioxide dispersion is 1:8.

[0110] The temperature of the liquid nitrogen freezing is -45°C and the time is 40 minutes.

[0111] The freeze-drying temperature is -7°C and the time is 72h.

[0112] The thermal annealing temperature is 320° C. and the time is 60 min.

[0113] The particle size of the crushed nano titanium dioxide composite aerogel is 5 μm.

[0114] S4. Preparation of anti-see-through masterbatch

[0115] The PET slices and the nano-titanium dioxide composite aerogel were uniformly mixed and granulated by a twin-screw extruder. After granulation, the mixture was dried to a moisture content of less than 100 ppm to obtain an anti-see-through masterbatch.

[0116] The ratio of the nano titanium dioxide composite aerogel to the PET slice is 50:50.

[0117] S5. Spinning

[0118] The anti-see-through masterbatch, PET chips and cross-linking modifier are mixed evenly and then spun, and then oiled after cooling to obtain multifunctional anti-see-through fibers.

[0119] The mass ratio of the anti-see-through masterbatch, the PET slice and the cross-linking modifier is 4:92:1.17.

[0120] The cross-linking modifier is triglycidyl isocyanurate.

[0121] The spinning rate is 1200 m / min, the box temperature is 290° C., and the cross-sectional shape of the spinning spinneret is a “cross”.

[0122] Comparative Example 1

[0123] Representative Example 1 was selected, the nano-titanium dioxide composite aerogel was removed, and the nano-titanium dioxide composite aerogel was replaced with an equal amount of nano-titanium dioxide, and a conventional dispersant of 1% by weight of the PET slice was added during the mixing process in step S4, and the rest was consistent with Example 1, as Comparative Example 1.

[0124] Comparative Example 2

[0125] Representative Example 1 was selected, S2 and S3 were removed, and the nano-titanium dioxide composite aerogel was replaced with an equal amount of amino-treated nano-titanium dioxide. The rest was consistent with Example 1, as Comparative Example 2.

[0126] Comparative Example 3

[0127] Representative Example 1 was selected as Comparative Example 3, with the crosslinking modifier in S5 removed and the rest being the same as Example 1.

[0128] The multifunctional anti-see-through fibers prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests, and the specific test results are shown in Table 1.

[0129] Table 1

[0130]

[0131] As can be seen from Table 1, in Comparative Example 1, nano-titanium dioxide treated with conventional dispersants replaces nano-titanium dioxide composite aerogels, and all properties are reduced, especially the mechanical properties are greatly reduced. This is because the dispersant on the surface of nano-titanium dioxide falls off during the melting process, affecting its dispersibility and compatibility; in Comparative Example 2, an equal amount of amino-treated nano-titanium dioxide is used to replace the nano-titanium dioxide composite aerogels, and the performance is slightly improved compared with Comparative Example 1, indicating that 3-aminopropyltrimethoxysilane has a certain interface modification effect. Comparative Examples 1 and 2 show that the nano-titanium dioxide composite aerogel has better dispersibility and compatibility in PET slices, and the polyimide in the nano-titanium dioxide composite aerogel has a flexible structure and hygroscopicity, which improves the regain and elongation of the fiber, and the elongation at break is significantly improved. In Comparative Example 3, the cross-linking modifier is removed, and the mechanical properties are significantly reduced. The reduction in fiber elongation leads to a decrease in elongation at break.

[0132] In addition, the fibers prepared in Examples 1-3 also have excellent UV resistance, cool feeling, and quick-drying functions, wherein the ultraviolet protection factor UPF>50, and the ultraviolet protection factor UPF AV >1900, UV transmittance T(UVA) AV ≤0.1%, UV transmittance T(UVB) AV ≤0.1% (measured in accordance with JIS L 1925); contact coolness coefficient (Qmax) is greater than 0.27 (measured in accordance with JIS L1927), water absorption is 1s (measured in accordance with JIS L 1907 drip method), and the diffusible residual moisture rate is less than 13%.

[0133] Unless otherwise specified, the ratios and percentages described in the present invention are all weight ratios and weight percentages; and the raw materials are all commercially available.

[0134] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a multifunctional anti-see-through fiber for textile use, characterized in that: The preparation method comprises the preparation of amino-treated nano titanium dioxide, the preparation of a precursor, the preparation of nano titanium dioxide composite aerogel, the preparation of anti-see-through masterbatch and spinning.

2. The method for preparing a multifunctional anti-see-through fiber for textile use according to claim 1, characterized in that: The preparation of the amino-modified nano titanium dioxide is as follows: adding nano titanium dioxide into deionized water and ultrasonically dispersing for 3 to 5 minutes, then adding ammonia water and 3-aminopropyltrimethoxysilane, heating to 50 to 60° C. and stirring for reaction for 4 to 6 hours, cooling to room temperature after the reaction is completed, centrifuging, ultrasonically oscillating, washing, drying, and ball-milling the precipitate to obtain the amino-modified nano titanium dioxide.

3. The method for preparing a multifunctional anti-see-through fiber for textile use according to claim 2, characterized in that: The mass fraction of the ammonia water is 20-30%; The amount of ammonia water added is 35-50% of the mass of nano-titanium dioxide, and the amount of 3-aminopropyltrimethoxysilane added is 18-25% of the mass of nano-titanium dioxide; The ball mill has a rotation speed of 300 to 400 r / min and a ball milling time of 9 to 10 hours.

4. The method for preparing a multifunctional anti-see-through fiber for textile use according to claim 1, characterized in that: The precursor is prepared by: ’ -diaminodiphenyl ether is added to N-methylpyrrolidone, stirred under nitrogen protection until dissolved, and then pyromellitic anhydride is added and stirred for 2 to 3 hours, followed by adding a carboxyl protecting agent N, N-diethylethylamine solution and continuing to stir for 60 to 90 minutes to obtain a precursor solution.

5. The method for preparing a multifunctional anti-see-through fiber for textile use according to claim 4, characterized in that: 4,4 ’ -The mass ratio of diaminodiphenyl ether to N-methylpyrrolidone is 1:4-5; 4,4 ’ - the molar ratio of diaminodiphenyl ether to pyromellitic dianhydride is 1:1.05-1.15; The concentration of the N,N-diethylethylamine solution is 4-6%, and the amount added is 4,4 ’ -Diaminodiphenyl ether and 4,4 ’ -9 to 13% of the total mass of diaminodiphenyl ether.

6. The method for preparing a multifunctional anti-see-through fiber for textile use according to claim 1, characterized in that: The preparation of the nano titanium dioxide composite aerogel comprises the following steps: adding aminated nano titanium dioxide into anhydrous ethanol and ultrasonically dispersing the mixture for 3 to 5 minutes to obtain a nano titanium dioxide dispersion; adding the aminated nano titanium dioxide dispersion into a precursor solution while stirring, adjusting the pH to 4.5 to 5.5 and continuing stirring for 2 to 4 hours, and then freezing the mixture with liquid nitrogen, freeze drying, thermal annealing, and crushing the mixture to obtain the nano titanium dioxide composite aerogel.

7. The method for preparing a multifunctional anti-see-through fiber for textile use according to claim 6, characterized in that: The mass ratio of nano-titanium dioxide to anhydrous ethanol in the amino-treated nano-titanium dioxide dispersion is 1:8-10; The mass ratio of the nano-titanium dioxide in the amino-treated nano-titanium dioxide dispersion to the precursor solution is 1:6-8.

8. The method for preparing a multifunctional anti-see-through fiber for textile use according to claim 6, characterized in that: The temperature of the liquid nitrogen freezing is -50°C to -40°C, and the time is 30 to 40 minutes; The freeze drying temperature is -10°C to -5°C and the time is 48 to 72 hours; The thermal annealing temperature is 240-320°C and the time is 50-60min; The particle size of the nano titanium dioxide composite aerogel after crushing is 2 to 10 μm.

9. The method for preparing a multifunctional anti-see-through fiber for textile use according to claim 1, characterized in that: The preparation of the anti-see-through masterbatch is as follows: the polymer slices and the nano-titanium dioxide composite aerogel are uniformly mixed and then granulated by a twin-screw extruder, and after the granulation is completed, the anti-see-through masterbatch is dried to a moisture content of less than 100 ppm to obtain the anti-see-through masterbatch; The ratio of the nano titanium dioxide composite aerogel to the polymer slice is 40-50:50-60; the polymer slice is one of PET or PA.

10. The method for preparing a multifunctional anti-see-through fiber for textile use according to claim 1, characterized in that: The spinning method comprises the following steps: uniformly mixing the anti-see-through masterbatch, the polymer slices and the cross-linking modifier, spinning the mixture, cooling the mixture and applying oil to obtain a multifunctional anti-see-through fiber. The mass ratio of the anti-see-through masterbatch, polymer slice and cross-linking modifier is 3-5:92-97:1.02-1.17; The cross-linking modifier is triglycidyl isocyanurate.