Ultrathin heat pipe capable of improving heat transfer performance and manufacturing process

By oxidizing salt solution and sonicating the copper mesh of ultra-thin thermal conductors, combining hydrogen sintering and coating of modified carbon nanotubes, forming a burr-like structure, it solves the difficulty of taking into account both heat transfer efficiency and mechanical properties in the prior art. The problem of heat transfer efficiency and service life have been significantly improved.

CN118882384AActive Publication Date: 2024-11-01WUXI LANFENG HEAT TRANSFER TECH CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410938414.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-13
Publication Date
2024-11-01
Estimated Expiration
2044-07-13

AI Technical Summary

Technical Problem

While improving heat transfer efficiency, existing ultra-thin thermal conduits are difficult to take into account both mechanical properties and temperature resistance, resulting in a shortened service life.

Method used

The high thermal conductivity copper mesh is soaked and oxidized by salt solution, combined with acid solution ultrasonic treatment and oxygen heating, forming a burr-like oxide layer, and then sintered in a hydrogen atmosphere to form a stable micropore and burr protrusion structure, increasing the specific surface area and Capillary force and improve the number and stability of capillary structure by covering and filling modified carbon nanotubes Ni@SWCNT@Fe.

Benefits of technology

It significantly improves the heat transfer efficiency and mechanical properties of ultra-thin thermal conduits, extends the service life, and ensures high thermal conductivity and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118882384A_ABST
    Figure CN118882384A_ABST
Patent Text Reader

Abstract

The invention discloses an ultrathin heat pipe capable of improving heat transfer performance and a manufacturing process thereof, and the manufacturing process comprises the following steps: 1) soaking a high-heat-conductivity copper mesh in a salt solution, taking out the copper mesh, and heating the copper mesh in an air atmosphere for oxidation treatment; 2) washing with deionized water, immersing into an acid solution, and carrying out ultrasonic treatment; 3) after washing with deionized water, heating and oxidizing in a mixed gas environment of air and oxygen; and (4) the copper net is inserted into the copper pipe, then the copper pipe is placed in a sintering furnace and sintered in a hydrogen-containing gas environment, after treatment is completed, the copper pipe is cooled to the room temperature along with the furnace, the tail of the copper pipe is sealed, then actuating fluid is injected into the copper pipe, vacuumizing is conducted, the end of the copper pipe is sealed and then flattened, and the ultrathin heat pipe is obtained. The heat transfer efficiency of the finally prepared ultrathin heat pipe can be remarkably improved, meanwhile, the copper net has excellent mechanical performance and heat stability, the long-acting high heat conduction capacity can be guaranteed, the using effect of the ultrathin heat pipe can be guaranteed, and the service life of the ultrathin heat pipe can be prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ultra-thin heat pipes, and in particular to an ultra-thin heat pipe with improved heat transfer performance and a manufacturing process thereof. Background Art

[0002] If the heat generated by electronic devices such as chips cannot be dissipated in time during operation, it will affect their working stability, reduce the mean time between failures, and in serious cases, burn the chips. Therefore, effectively conducting and processing this part of heat consumption is crucial to ensure the working stability and life of the device.

[0003] Heat pipes are currently widely used for heat dissipation of components. They are composed of a metal tube and a capillary structure layer on the inner wall of the tube, and contain a heat dissipation fluid. When one end of the heat pipe is heated, the fluid absorbs heat and vaporizes to form a high-temperature gas. The other end of the heat pipe condenses the high-temperature gas into a liquid fluid due to the lower temperature. The liquid fluid returns to the heated end under the capillary force of the capillary structure layer, and this process is repeated to form a continuous phase change heat transfer system. For example, patent CN101634532A discloses a heat pipe and its manufacturing method, patent CN102331205A discloses a composite heat pipe structure, patent CN102410765A discloses an ultra-thin heat pipe with a composite structure and its manufacturing method, etc.

[0004] Due to the limitation of the external dimensions of the capillary structure used in the existing ultra-thin heat pipe, the internal space is very narrow, so the size of the capillary structure that can be used is limited, and the capillary structure related to the powder sintering type cannot be used. Therefore, the capillary structure currently used is a braided wire structure to be erected in the narrow ultra-thin heat pipe space, but its porosity and specific surface area are still not high enough, and the heat transfer efficiency still needs to be further improved. And while the heat transfer efficiency is improved, its mechanical properties and temperature resistance must also be taken into account to ensure its service life. Patent CN113701535A discloses a manufacturing process for sandblasting to increase the capillary structure in the ultra-thin heat pipe tube. By sandblasting the inner surface of the copper tube to form an uneven shape, the specific surface area of ​​the inner surface of the copper tube is increased, and the heat transfer efficiency of the ultra-thin heat pipe is improved. However, the increase in its capillary structure is limited, and it will inevitably damage the mechanical strength and other properties of the copper tube, which is easy to shorten its service life.

[0005] Therefore, it is necessary to improve the existing technology to provide a more reliable solution. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide an ultra-thin heat pipe and a manufacturing process for improving the heat transfer performance in view of the deficiencies in the above-mentioned prior art.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: In a first aspect of the present invention, a process for manufacturing an ultra-thin heat pipe with improved heat transfer performance is provided, comprising the following steps:

[0008] 1) Soak the high thermal conductivity copper mesh in a salt solution, take it out and heat it in an air atmosphere for oxidation treatment, and cool it to room temperature after the treatment is completed;

[0009] 2) washing the copper mesh obtained in step 1) with deionized water, immersing it in an acid solution, and performing ultrasonic treatment;

[0010] 3) washing the copper mesh obtained in step 2) with deionized water, and then heating and oxidizing it in a mixed gas environment of air and oxygen;

[0011] 4) inserting the copper mesh obtained in step 3) into the copper tube, and then placing the copper tube in a sintering furnace, sintering the copper tube in a hydrogen-containing gas environment, cooling the copper tube to room temperature with the furnace after the treatment, sealing the tail of the copper tube, and then injecting an actuating fluid into the copper tube, evacuating the tube, sealing the end of the copper tube and flattening it to obtain an ultra-thin heat pipe.

[0012] Preferably, the manufacturing process of the ultra-thin heat pipe with improved heat transfer performance comprises the following steps:

[0013] 1) Soak the high thermal conductivity copper mesh in a sodium chloride solution with a mass concentration of 15-40% for 2-10 minutes, take it out and heat it in an air atmosphere at 110-130° C. for 15-60 minutes, and cool it to room temperature;

[0014] 2) washing the copper mesh obtained in step 1) with deionized water, immersing it in citric acid with a mass concentration of 15-45%, and ultrasonically treating it for 15-60 minutes;

[0015] 3) washing the copper mesh obtained in step 2) with deionized water, and then heating and oxidizing it at 110-130° C. and a mixed gas environment with a volume ratio of air to oxygen of 1:2-2:1 for 0.5-2 h;

[0016] 4) inserting the copper mesh obtained in step 3) into a copper tube with a wall thickness of 0.1-0.5 mm, then placing the copper tube in a sintering furnace, sintering at 850-900° C. for 1-4 h in a low-hydrogen mixed gas environment, cooling to room temperature with the furnace, sealing the tail of the copper tube, and then injecting an actuating fluid into the copper tube, evacuating, sealing the end of the copper tube and flattening it to a thickness of 1-5 mm to obtain an ultra-thin heat pipe;

[0017] Among them, the width D of the copper mesh and the inner diameter r of the copper tube satisfy the following relationship:

[0018]

[0019] The actuating fluid is ultrapure water or ethanol.

[0020] Preferably, the manufacturing process of the ultra-thin heat pipe with improved heat transfer performance comprises the following steps:

[0021] 1) Soak the high thermal conductivity copper mesh in a 30% sodium chloride solution for 5 minutes, take it out and heat it at 120°C in air for 30 minutes, and cool it to room temperature;

[0022] 2) washing the copper mesh obtained in step 1) with deionized water, immersing it in 30% citric acid, and ultrasonically treating it for 30 minutes;

[0023] 3) washing the copper mesh obtained in step 2) with deionized water, and then heating and oxidizing it at 120° C. in a mixed gas environment with a volume ratio of air to oxygen of 1:1 for 1 h;

[0024] 4) inserting the copper mesh obtained in step 3) into a copper tube with a wall thickness of 0.2 mm, then placing the copper tube in a sintering furnace, sintering at 880° C. for 2 h in a low-hydrogen mixed gas environment, cooling to room temperature with the furnace, sealing the tail of the copper tube, and then injecting an actuating fluid into the copper tube, evacuating the tube, sealing the end of the copper tube and flattening it to a thickness of 3 mm to obtain an ultra-thin heat pipe;

[0025] The low-hydrogen mixed gas consists of 95% N 2 and 5% H 2 composition;

[0026] Among them, the length of the copper mesh is not less than the length of the copper tube, and the width D of the copper mesh and the inner diameter r of the copper tube satisfy the following relationship:

[0027]

[0028] Among them, the operating fluid is ultrapure water.

[0029] Preferably, the high thermal conductivity copper mesh is prepared by a high thermal conductivity copper alloy, and the raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage:

[0030] Mn: 0.22-0.67%; Co: 0.19-0.74%; Ag: 0.05-0.17%; Cr: 0.85-1.33%; Zr: 0.20-0.45%; Ni@SWCNT@Fe: 2.50-4.00%; surface modified TiC: 2.20-3.50% and the balance of copper;

[0031] The Ni@SWCNT@Fe is a coated, filled and modified carbon nanotube containing a sacrificial element component, wherein the sacrificial element component is Fe.

[0032] Preferably, the raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage:

[0033] Mn: 0.35%; Co: 0.41%; Ag: 0.09%; Cr: 1.10%; Zr: 0.29%; Ni@SWCNT@Fe: 3.75%; surface modified TiC: 2.80% and the balance of copper.

[0034] Preferably, the high thermal conductivity copper mesh is prepared by the following method:

[0035] 1-1) Add all raw materials into a ball mill according to the mass ratio, and ball mill for 1-4 hours under argon protection, with a ball-to-material ratio of 9:1-6:1 and a rotation speed of 200-500rpm;

[0036] 1-2) Add the ball-milled raw materials into a vacuum melting furnace, evacuate to 0.1-0.3 Pa, then heat to 1250-1500° C. under argon protection, melt for 10-30 min, and vacuum cast to obtain an ingot;

[0037] 1-3) Keep the temperature at 850-950℃ for 1-4h to perform homogenization treatment; then perform rotary forging at 600-800℃ to produce a rod with a diameter of 5-20mm, and then perform room temperature drawing after cooling to room temperature to produce a thick copper wire with a diameter of 2-5mm;

[0038] 1-4) heat treating the thick copper wire under argon protection at 550-750° C. for 1-5 min, and then drawing the thick copper wire through a wire drawing die to obtain a thin copper wire with a diameter of 0.02-0.2 mm;

[0039] 1-5) The thin copper wire is kept warm at 550-700° C. for 0.5-1 h under argon protection, and cooled to room temperature to obtain a braided copper wire, and the braided copper wire is weaved into a copper mesh by a wire mesh weaving machine, and the copper mesh is washed with ethanol and deionized water in turn, and vacuum dried at 70-100° C. to constant weight to obtain a high thermal conductive copper mesh with a mesh size of 100-300 meshes.

[0040] Preferably, the coated, filled and modified carbon nanotube Ni@SWCNT@Fe is prepared by the following method:

[0041] S1, single-arm carbon nanotube pretreatment;

[0042] The single-arm carbon nanotubes are added to a mixed acid of 95wt% concentrated sulfuric acid and 65wt% concentrated nitric acid, and ultrasonically dispersed for 15-60min, and then heated to 80-100°C, stirred and refluxed for 2-10h, cooled, filtered, washed with deionized water until neutral, and vacuum dried at 70-100°C to constant weight to obtain pretreated single-arm carbon nanotubes;

[0043] The volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed acid is 1:2-2:1;

[0044] S2. Preparation of internally filled carbon nanotubes:

[0045] 0.5-2g of pretreated single-arm carbon nanotubes and 0.12-0.35g of polyethylene glycol are added to 50-200mL of deionized water, and then 0.241-0.966g of ferric nitrate is added. After ultrasonic dispersion for 30-90min, 10-30mL of ammonia water with a mass concentration of 15-25% is added dropwise. After the addition is completed, the mixture is stirred for 5-30min. The obtained dispersed mixture 1 is transferred to a polytetrafluoroethylene-lined reactor, reacted at 190-200°C for 1-4h, filtered, and the solid product is washed with deionized water, and vacuum dried at 80-100°C for 4-12h to obtain internally filled carbon nanotubes;

[0046] S3. Preparation of Ni@SWCNT@Fe:

[0047] 0.5-2 g of the inner-filled carbon nanotubes were added to 100-400 mL of deionized water, and ultrasonically dispersed at 50-65° C. for 0.5-2 h. Then, 0.27-1.1 g of nickel nitrate was added and ultrasonically dispersed for 1-4 h. The resulting dispersed mixture 2 was transferred to a polytetrafluoroethylene-lined reactor, reacted at 190-220° C. for 1.5-6 h, filtered, and the solid product was washed with deionized water, vacuum dried at 90-110° C. for 2-8 h, and finally calcined at 1000-1150° C. in a reducing gas atmosphere for 1.5-6 h to obtain Ni@SWCNT@Fe.

[0048] The reducing gas is H 2 or CO.

[0049] Preferably, the coated, filled and modified carbon nanotube Ni@SWCNT@Fe is prepared by the following method:

[0050] S1-1, single-arm carbon nanotube pretreatment;

[0051] 2 g of single-arm carbon nanotubes were added to 200 mL of a mixture of 95 wt% concentrated sulfuric acid and 65 wt% concentrated nitric acid in a volume ratio of 1:1, and ultrasonically dispersed for 30 min, then heated to 90° C., stirred and refluxed for 4 h, cooled, filtered, washed with deionized water until neutral, and vacuum dried at 80° C. to constant weight to obtain pretreated single-arm carbon nanotubes;

[0052] S1-2, preparation of internally filled carbon nanotubes:

[0053] 1 g of pretreated single-arm carbon nanotubes and 0.2 g of polyethylene glycol were added to 100 mL of deionized water, and then 0.483 g of ferric nitrate was added. After ultrasonic dispersion for 45 min, 15 mL of 20% ammonia water was added dropwise. After the addition was completed, the mixture was stirred for 10 min. The obtained dispersed mixture 1 was transferred to a polytetrafluoroethylene-lined reactor, reacted at 195 ° C for 2 h, filtered, and the solid product was washed with deionized water and vacuum dried at 90 ° C for 6 h to obtain internally filled carbon nanotubes.

[0054] S1-3. Preparation of Ni@SWCNT@Fe:

[0055] 1 g of the inner-filled carbon nanotubes was added to 200 mL of deionized water and ultrasonically dispersed at 60 °C for 1 h. Then 0.55 g of nickel nitrate was added and ultrasonically dispersed for 2 h. The resulting dispersed mixture 2 was transferred to a polytetrafluoroethylene-lined reactor and reacted at 200 °C for 3 h. The solid product was filtered and washed with deionized water, vacuum dried at 100 °C for 4 h, and finally heated to room temperature in H 2 Atmosphere and calcined at 1050 °C for 3 h to obtain Ni@SWCNT@Fe.

[0056] Preferably, the surface modified TiC is prepared by the following method:

[0057] S2-1, pretreatment:

[0058] After cleaning TiC particles with a particle size of 1-10 μm, they are subjected to coarsening, sensitization and activation treatments in sequence to obtain pretreated TiC;

[0059] S2-2, adding copper nitrate and cerium nitrate into deionized water, stirring until completely dissolved, then adding citric acid and boric acid, stirring until completely dissolved, adjusting the pH to 10.5-11.5 with sodium hydroxide, adding the pretreated TiC, and then adding sodium hypophosphite, and performing chemical plating on the pretreated TiC with the obtained plating solution;

[0060] The concentrations of the components in the obtained plating solution are: copper nitrate 14.5-21 g / L, cerium nitrate 3.5-4.5 g / L, citric acid 11-18 g / L, sodium hypophosphite 15-25 g / L, and boric acid 10-24 g / L;

[0061] The plating process conditions are: pH 10.5-11.5, mechanical stirring 300-650r / min, temperature: 80-90°C, time: 1-3h;

[0062] After the chemical plating is completed, the solid particles are filtered and washed with deionized water, and vacuum dried at 90-100° C. for 4-12 hours to obtain surface-modified TiC.

[0063] A second aspect of the present invention provides an ultra-thin heat pipe, characterized in that it is manufactured by the process described above.

[0064] The beneficial effects of the present invention are:

[0065] The present invention provides a manufacturing process for an ultra-thin heat pipe with improved heat transfer performance. The present invention can significantly improve the heat transfer efficiency of the ultra-thin heat pipe finally prepared by improving the manufacturing process of the heat pipe, improving the alloy material of the copper mesh used for manufacturing the heat pipe, and coordinating the copper mesh with the manufacturing process of the heat pipe. At the same time, the copper mesh also has excellent mechanical properties and thermal stability, which can help ensure long-term high thermal conductivity, ensure the use effect of the ultra-thin heat pipe, and extend its service life.

[0066] The present invention first soaks the copper mesh in salt water, then heats and oxidizes it in air to form a certain corrosion layer and initially form micropores; then, the micropores are further enlarged by acid soaking and corrosion; then, the copper mesh is heated in an oxygen atmosphere to achieve deep oxidation, and this process causes the originally smooth copper wire surface in the copper mesh to form a burr-like oxide layer protrusion structure similar to a hill; finally, the copper mesh is inserted into a copper tube, and the copper mesh is placed in a sintering furnace containing a hydrogen atmosphere for sintering, during which the reducing hydrogen removes the oxide layer on the surface of the copper mesh, and the microporous structure and burr-like protrusions on the copper mesh are basically retained. Under the action of high temperature, metal molecules diffuse and shape to form a stable micropore and burr protrusion structure, thereby increasing the number of capillary structures, enhancing the capillary force in the tube, significantly increasing the specific surface area of ​​the copper mesh on the inner wall of the heat pipe, increasing the effective porosity ratio, and increasing the contact heat exchange area between the heat pipe and the internal working medium, and finally greatly improving the heat transfer efficiency of the obtained heat pipe and the heat removal power.

[0067] The present invention improves the alloy formula of the copper mesh substrate, which can further improve the thermal conductivity of the copper alloy and effectively improve its mechanical properties, wear resistance and thermal stability. On the other hand, by designing the coated and filled modified carbon nanotubes containing sacrificial element components: Ni@SWCNT@Fe as the doping component, and cooperating with the acid leaching process of the copper mesh in the manufacturing process of the ultra-thin heat pipe, a large number of nano-scale micro-pore structures (i.e., capillary structures) can be formed through the preferential solvent decomposition of the sacrificial element components, thereby further increasing the capillary force inside the heat pipe, increasing the effective porosity ratio of the copper mesh, and increasing the heat exchange area between the copper mesh and the working medium, thereby further improving its heat transfer performance, and finally improving the heat transfer efficiency of the ultra-thin heat pipe and the heat removal power of the heat pipe. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] Figure 1 A flow chart of a manufacturing process of an ultra-thin heat pipe for improving heat transfer performance according to the present invention;

[0069] Figure 2 Electron microscopic images of copper wires in the copper mesh before and after citric acid treatment in step 2) of Example 1;

[0070] Figure 3 is the XRD pattern of Ni@SWCNT@Fe prepared in Example 1;

[0071] Figure 4 is the XRD pattern of the surface modified TiC prepared in Example 1;

[0072] Figure 5 This is the physical object of the high thermal conductivity copper mesh prepared in Example 1;

[0073] Figure 6 A physical picture of an ultra-thin heat pipe in a specific application example;

[0074] Figure 7 This is a real picture of the ultra-thin heat pipe after both ends are disassembled;

[0075] Figure 8 The test results of the tensile properties test;

[0076] Fig. 9 This is the test result of thermal resistance. DETAILED DESCRIPTION

[0077] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0078] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0079] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0080] Reference Figure 1 The present invention provides a process for manufacturing an ultra-thin heat pipe with improved heat transfer performance, comprising the following steps:

[0081] (1) soaking the high thermal conductivity copper mesh in a sodium chloride solution with a mass concentration of 15-40% for 2-10 minutes, taking it out and heating it in an air atmosphere at 110-130° C. for 15-60 minutes, and cooling it to room temperature;

[0082] (2) washing the copper mesh obtained in step 1) with deionized water, immersing it in citric acid with a mass concentration of 15-45%, and ultrasonically treating it for 15-60 minutes;

[0083] (3) washing the copper mesh obtained in step 2) with deionized water, and then heating and oxidizing it at 110-130° C. and a mixed gas environment with a volume ratio of air to oxygen of 1:2-2:1 for 0.5-2 h;

[0084] (4) inserting the copper mesh obtained in step 3) into a copper tube with a wall thickness of 0.1-0.5 mm, then placing the copper tube in a sintering furnace, sintering at 850-900° C. for 1-4 h in a low-hydrogen mixed gas environment, cooling to room temperature with the furnace, sealing the tail of the copper tube, and then injecting an actuating fluid into the copper tube, evacuating the tube, sealing the end of the copper tube and flattening it to a thickness of 1-5 mm to obtain an ultra-thin heat pipe;

[0085] Among them, the width D of the copper mesh and the inner diameter r of the copper tube satisfy the following relationship:

[0086]

[0087] The actuating fluid is ultrapure water or ethanol. The actuating fluid is also called working fluid or heat transfer medium.

[0088] In the present invention, the high thermal conductivity copper mesh is prepared by a high thermal conductivity copper alloy, and the raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage:

[0089] Mn: 0.22-0.67%; Co: 0.19-0.74%; Ag: 0.05-0.17%; Cr: 0.85-1.33%; Zr: 0.20-0.45%; Ni@SWCNT@Fe: 2.50-4.00%; surface modified TiC: 2.20-3.50% and the balance of copper;

[0090] Ni@SWCNT@Fe is a coated, filled and modified carbon nanotube containing a sacrificial element component, wherein the sacrificial element component is Fe. When the copper mesh is immersed in an acid solution for treatment, the sacrificial element component can be dissolved preferentially over Cu.

[0091] In the present invention, the high thermal conductivity copper mesh is prepared by the following method:

[0092] 1-1) Add all raw materials into a ball mill according to the mass ratio, and ball mill for 1-4 hours under argon protection, with a ball-to-material ratio of 9:1-6:1 and a rotation speed of 200-500rpm;

[0093] 1-2) Add the ball-milled raw materials into a vacuum melting furnace, evacuate to 0.1-0.3 Pa, then heat to 1250-1500° C. under argon protection, melt for 10-30 min, and vacuum cast to obtain an ingot;

[0094] 1-3) Keep the temperature at 850-950℃ for 1-4h to perform homogenization treatment; then perform rotary forging at 600-800℃ to produce a rod with a diameter of 5-20mm, and then perform room temperature drawing after cooling to room temperature to produce a thick copper wire with a diameter of 2-5mm;

[0095] 1-4) heat treating the thick copper wire under argon protection at 550-750° C. for 1-5 min, and then drawing the thick copper wire through a wire drawing die to obtain a thin copper wire with a diameter of 0.02-0.2 mm;

[0096] 1-5) The thin copper wire is kept warm at 550-700° C. for 0.5-1 h under argon protection, and cooled to room temperature to obtain a braided copper wire, and the braided copper wire is weaved into a copper mesh by a wire mesh weaving machine, and the copper mesh is washed with ethanol and deionized water in turn, and vacuum dried at 70-100° C. to constant weight to obtain a high thermal conductive copper mesh with a mesh size of 100-300 meshes.

[0097] In the present invention, the coated, filled and modified carbon nanotube Ni@SWCNT@Fe is prepared by the following method:

[0098] S1, single-arm carbon nanotube pretreatment;

[0099] The single-arm carbon nanotubes are added to a mixed acid of 95wt% concentrated sulfuric acid and 65wt% concentrated nitric acid, and ultrasonically dispersed for 15-60min, and then heated to 80-100°C, stirred and refluxed for 2-10h, cooled, filtered, washed with deionized water until neutral, and vacuum dried at 70-100°C to constant weight to obtain pretreated single-arm carbon nanotubes;

[0100] The volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed acid is 1:2-2:1;

[0101] S2. Preparation of internally filled carbon nanotubes:

[0102] 0.5-2g of pretreated single-arm carbon nanotubes and 0.12-0.35g of polyethylene glycol are added to 50-200mL of deionized water, and then 0.241-0.966g of ferric nitrate is added. After ultrasonic dispersion for 30-90min, 10-30mL of ammonia water with a mass concentration of 15-25% is added dropwise. After the addition is completed, the mixture is stirred for 5-30min. The obtained dispersed mixture 1 is transferred to a polytetrafluoroethylene-lined reactor, reacted at 190-200°C for 1-4h, filtered, and the solid product is washed with deionized water, and vacuum dried at 80-100°C for 4-12h to obtain internally filled carbon nanotubes;

[0103] S3. Preparation of Ni@SWCNT@Fe:

[0104] 0.5-2 g of the inner-filled carbon nanotubes were added to 100-400 mL of deionized water, and ultrasonically dispersed at 50-65° C. for 0.5-2 h. Then, 0.27-1.1 g of nickel nitrate was added and ultrasonically dispersed for 1-4 h. The resulting dispersed mixture 2 was transferred to a polytetrafluoroethylene-lined reactor, reacted at 190-220° C. for 1.5-6 h, filtered, and the solid product was washed with deionized water, vacuum dried at 90-110° C. for 2-8 h, and finally calcined at 1000-1150° C. in a reducing gas atmosphere for 1.5-6 h to obtain Ni@SWCNT@Fe.

[0105] The reducing gas is H 2 or CO.

[0106] In the present invention, the surface modified TiC is prepared by the following method:

[0107] S2-1, pretreatment:

[0108] After cleaning TiC particles with a particle size of 1-10 μm, they are subjected to coarsening, sensitization and activation treatments in sequence to obtain pretreated TiC;

[0109] S2-2, adding copper nitrate and cerium nitrate into deionized water, stirring until completely dissolved, then adding citric acid and boric acid, stirring until completely dissolved, adjusting the pH to 10.5-11.5 with sodium hydroxide, adding the pretreated TiC, and then adding sodium hypophosphite, and performing chemical plating on the pretreated TiC with the obtained plating solution;

[0110] The concentrations of the components in the obtained plating solution are: copper nitrate 14.5-21 g / L, cerium nitrate 3.5-4.5 g / L, citric acid 11-18 g / L, sodium hypophosphite 15-25 g / L, and boric acid 10-24 g / L;

[0111] The plating process conditions are: pH 10.5-11.5, mechanical stirring 300-650r / min, temperature: 80-90°C, time: 1-3h;

[0112] After the chemical plating is completed, the solid particles are filtered and washed with deionized water, and vacuum dried at 90-100° C. for 4-12 hours to obtain surface-modified TiC.

[0113] The present invention also provides an ultra-thin heat pipe, which is manufactured by the above process.

[0114] The present invention can significantly improve the heat transfer efficiency of the ultra-thin heat pipe finally prepared by improving the heat pipe manufacturing process, improving the alloy material of the copper mesh used for heat pipe manufacturing, and coordinating the copper mesh with the heat pipe manufacturing process. At the same time, the copper mesh also has excellent mechanical properties, thermal stability and wear resistance, which can help ensure long-term high thermal conductivity, ensure the use effect of the ultra-thin heat pipe, and extend its service life. The main principles of the present invention are described in detail below in combination with the specific manufacturing process to facilitate the understanding of the present invention.

[0115] The capillary force of the heat pipe is one of the key factors in realizing its heat transfer function. The capillary force is generated by the capillary structure inside the heat pipe, which can maintain the liquid film state of the working fluid in the heat pipe, so that it can achieve efficient heat transfer (Liu Yanqi. Characterization of capillary force and analysis of heat transfer performance of axial microgroove heat pipe [D]. Lanzhou Jiaotong University [2024-07-09]. DOI: CNKI: CDMD: 2.1017.234219.). Therefore, increasing the capillary structure inside the heat pipe and improving the capillary force are effective means to improve the heat transfer performance. Based on this, the present invention has made a variety of improvements.

[0116] First aspect: Improvement of heat pipe manufacturing process

[0117] The present invention first soaks the copper mesh in salt water (sodium chloride solution), then heats and oxidizes it in air to form a certain corrosion layer and initially form micropores; then, it is soaked and corroded by acid (citric acid) to further expand the micropores (and the process in this step cooperates with the Ni@SWCNT@Fe in the copper mesh substrate to form a large number of nano-scale micro-pore structures inside the copper mesh substrate, which will be described in detail later);

[0118] Then, deep oxidation is achieved by heating in an oxygen atmosphere of a certain purity. This process causes the originally smooth copper wire surface in the copper mesh to form a burr-like oxide layer protrusion structure similar to a hill.

[0119] Insert the copper mesh into the copper tube, and the copper mesh will automatically adhere to the inner wall of the copper tube under the action of stress. Finally, put the copper tube into a sintering furnace containing a hydrogen atmosphere for sintering. During this process, the reducing hydrogen will remove the oxide layer on the surface of the copper mesh, and the microporous structure and burr-like protrusions on the copper mesh will basically be retained. Under the action of high temperature, the metal molecules diffuse and take shape to form a stable microporous and burr-like protrusion structure, thereby increasing the number of capillary structures, enhancing the capillary force in the tube, significantly increasing the specific surface area of ​​the copper mesh on the inner wall of the heat pipe, and increasing the effective porosity ratio. This can increase the contact heat exchange area between the heat pipe and the internal working medium, and ultimately greatly improve the heat transfer efficiency of the obtained heat pipe.

[0120] Second aspect: A. Improvement of copper mesh substrate—Ni@SWCNT@Fe

[0121] Copper has excellent heat transfer ability. When it intersects with copper wire, it is made into copper mesh, which can improve its overall mechanical properties and heat transfer area. The better the thermal conductivity of the copper mesh substrate, the stronger the thermal conductivity of the copper mesh will be. In the present invention, the copper mesh is woven from 0.02-0.2mm fine copper wires, so there are certain requirements for the mechanical properties of the fine copper wires, especially their toughness, to ensure a higher copper mesh yield; at the same time, the working environment of the copper mesh in the inner wall of the heat pipe is in contact with and impacted by the working medium, and the temperature in many application scenarios will be relatively high, which requires the copper mesh to have good friction resistance and thermal stability at the same time to ensure its heat transfer effect and longer service life. The present invention improves the alloy formula of the copper mesh substrate, which can further improve the thermal conductivity of the copper alloy, effectively improve its mechanical properties, wear resistance and thermal stability, and ensure the stability of the capillary structure. On the other hand, by designing the coated filling modified carbon nanotubes containing sacrificial element components: Ni@SWCNT@Fe as the doping component, in conjunction with the acid leaching process of the copper mesh in the manufacturing process of the ultra-thin heat pipe, a large number of nano-scale micro-pore structures (i.e., capillary structures) can be formed through preferential solvent decomposition of the sacrificial element components, thereby further increasing the capillary force inside the heat pipe, increasing the effective porosity of the copper mesh, and increasing the heat exchange area between the copper mesh and the working medium, thereby further improving the heat transfer performance and improving the heat dissipation power of the heat pipe.

[0122] In the high thermal conductivity copper alloy components of the present invention, Mn, Co, and Cr can improve the thermal conductivity of the copper alloy to a certain extent, and Mn can also improve the strength of the alloy and improve the corrosion resistance to a certain extent, Zr can improve the thermal stability and wear resistance of the alloy, and the addition of Ag can improve the mechanical properties of the alloy. The improvement of corrosion resistance can help to enhance the long-term tolerance of the copper tube to the working medium, so that the capillary structure remains stable for a long time; the improvement of wear resistance can help the capillary structure remain stable under the long-term impact of the working medium.

[0123] The main synthesis mechanism of Ni@SWCNT@Fe in the high thermal conductivity copper alloy component of the present invention is as follows:

[0124] (1) First, the single-arm carbon nanotubes are acidified by mixed acid to increase the surface carboxyl content, improve their dispersion performance, and facilitate subsequent filling and coating modifications;

[0125] (2) Then, iron ions are added to the dispersion of the pretreated single-arm carbon nanotubes. The concentration difference and the capillary action formed by the microporous inner cavity of the single-arm carbon nanotubes enable the iron ions to automatically enter the inner cavity of the single-arm carbon nanotubes, and are attached to the iron ions through the coordination of the carboxyl groups on the inner wall. Then, the iron ions are deposited under the action of ammonia water, and finally, iron oxides are formed under high-temperature hydrothermal reaction, so that the inner cavity of the single-arm carbon nanotubes can be filled with iron oxides to obtain inner-filled carbon nanotubes. Of course, in this process, a certain amount of iron oxides will also be grafted and attached to the surface of the single-arm carbon nanotubes.

[0126] (3) Then, nickel ions are added to the dispersion of the carbon nanotubes, and the nickel ions are attached to the surface of the single-arm carbon nanotubes by combining with the functional groups such as carboxyl groups remaining on the surface of the single-arm carbon nanotubes. Since the inner cavity of the single-arm carbon nanotubes has been filled with iron oxide, only a small amount of nickel ions will enter the inner cavity of the single-arm carbon nanotubes; and then, a high-temperature hydrothermal reaction is performed to make the nickel ions form oxides and firmly attach to the single-arm carbon nanotubes.

[0127] Finally, the reducing gas (H 2 ) high temperature reduction, so that the iron oxide is reduced to elemental iron, and the oxides of nickel and cerium are also reduced to the corresponding elements, and finally the coated filled modified carbon nanotubes containing sacrificial element components are obtained, with the inner cavity mainly filled with iron and the outer wall coated with iron and nickel composites: Ni@SWCNT@Fe.

[0128] The effects of Ni@SWCNT@Fe constructed by the present invention include at least the following aspects:

[0129] 1. After Ni@SWCNT@Fe is doped into the high thermal conductivity copper alloy, in the process of making ultra-thin heat pipes, when the copper mesh is immersed in citric acid for corrosion treatment, since the activity of Fe is stronger than that of Cu, during the acid leaching process, Fe can preferentially react with citric acid to generate soluble iron citrate, so that the Fe filled in the inner cavity of the single-arm carbon nanotube is gradually dissolved, thereby re-forming a cavity structure. The formation of the cavity structure produces a capillary effect, which can promote citric acid to enter the cavity and further react with the Fe in the cavity, so that the single-arm carbon nanotube gradually restores the cavity structure. Since the single-arm carbon nanotube can be evenly dispersed in the copper alloy matrix, this will enable the cavity structure of the single-arm carbon nanotube to form a network-like capillary pore structure in the copper alloy matrix. After the ultra-thin heat pipe is made, the capillary force generated by these capillary pore structures can improve the heat transfer capacity, increase the porosity, increase the heat exchange area with the copper tube and the working medium, and ultimately improve the heat transfer efficiency. Of course, during the acid corrosion process, the copper matrix will also undergo certain surface corrosion, forming a certain microporous structure.

[0130] 2. Single-arm carbon nanotubes have excellent mechanical properties, which can significantly improve the mechanical strength of copper alloys, especially toughness, and can be beneficial to the preparation of copper wires, and can also enhance the mechanical strength of the prepared copper mesh; at the same time, single-arm carbon nanotubes also have excellent thermal conductivity, which can improve the thermal conductivity of copper alloy substrates. Then, the defects of poor wettability, difficult dispersion, and easy curling of the nanostructured single-arm carbon nanotubes and the metal copper substrate greatly limit the effect of improving performance. The present invention can also solve this problem by constructing the Ni@SWCNT@Fe structural system. In the present invention, the coating of iron and nickel composites can improve the wettability between single-arm carbon nanotubes and copper substrates (for example, copper and nickel can be infinitely soluble in each other), and promote the uniform dispersion of single-arm carbon nanotubes in the copper substrate; the iron and nickel coated on the single-arm carbon nanotubes are combined with the copper substrate by infiltration and dissolution, which can significantly improve the interfacial bonding force and promote the reinforcement effect of single-arm carbon nanotubes on the mechanical strength of the substrate. And the addition of nickel elements can also improve the mechanical strength and corrosion resistance of the copper substrate. The improvement of the mechanical strength of the matrix by single-arm carbon nanotubes can also make up for the loss of mechanical strength caused by the formation of cavity structure by acid immersion corrosion.

[0131] 3. In the present invention, by pre-occupying the inner cavity of the single-arm carbon nanotube with Fe, other unexpected components can be prevented from occupying the inner cavity; after the inner cavity of the single-arm carbon nanotube is filled with Fe, its overall density will increase, and the density difference between the single-arm carbon nanotube and the copper alloy matrix will decrease, which is beneficial to the dispersion of the single-arm carbon nanotube in the copper alloy melt; and the filling of Fe can also reduce the curling of the single-arm carbon nanotube, which is beneficial to the improvement of the matrix performance. The uniform dispersion of the single-arm carbon nanotube in the copper alloy can form a network structure, which is very beneficial to the improvement of thermal conductivity and mechanical properties.

[0132] Second aspect: B. Improvement of copper mesh substrate - TiC

[0133] The addition of TiC ceramic particles can improve the wear resistance, corrosion resistance and thermal stability of the metal substrate (Bai Fang. Research on the organization and properties of in-situ nano-TiC_x particles reinforced copper-based composites [D]. Jilin University [2024-07-09]. DOI: CNKI: CDMD: 2.1017.156584.). The improvement of wear resistance, corrosion resistance and thermal stability can help the copper mesh cope with the convective impact and corrosion caused by the heat exchange medium during work, as well as the matrix fatigue caused by the temperature environment, and ensure the stability of the micropore structure thereon.

[0134] However, it is difficult for TiC to be evenly dispersed in the copper matrix, which will seriously affect the effect of improving its performance. In the present invention, by performing chemical copper plating on the TiC particles and compounding rare earth cerium in the copper layer composition, the compatibility of TiC particles with the copper matrix can be effectively improved, and its uniform dispersion can be promoted. During the chemical plating process, due to its high activity, some of the rare earth Ce can lose electrons and act as a reducing agent, which can accelerate the deposition of copper. After Ce enters the copper alloy matrix, it can form intermetallic compounds, improve the strength, toughness and high-temperature stability of the matrix. Ce can also play a role in refining grains, purifying interfaces, and improving interface bonding strength, and can improve high-temperature elongation (Jiang Jiaxin, Wen Yongqing. The role and application of rare earths in copper and copper alloys [J]. Rare Earth Information, 2021 (5): 7.), which is extremely beneficial for the preparation of copper wire. Therefore, rare earth Ce can play a positive role in promoting the formation of the coating and the performance improvement of the copper alloy matrix.

[0135] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.

[0136] The sources of some of the raw materials involved in the following examples and comparative examples are as follows:

[0137] Single-arm carbon nanotubes, inner diameter 1-2nm, length 20μm, Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.;

[0138] TiC, particle size 4 μm, Suzhou Beike Nanotechnology Co., Ltd.

[0139] Example 1

[0140] A process for manufacturing an ultra-thin heat pipe with improved heat transfer performance comprises the following steps:

[0141] 1) Soak the high thermal conductivity copper mesh in a 30% sodium chloride solution for 5 minutes, take it out and heat it at 120°C in air for 30 minutes, and cool it to room temperature;

[0142] 2) washing the copper mesh obtained in step 1) with deionized water, immersing it in 30% citric acid, and ultrasonically treating it for 30 minutes;

[0143] 3) washing the copper mesh obtained in step 2) with deionized water, and then heating and oxidizing it at 120° C. in a mixed gas environment with a volume ratio of air to oxygen of 1:1 for 1 h;

[0144] 4) inserting the copper mesh obtained in step 3) into a copper tube with a wall thickness of 0.2 mm, then placing the copper tube in a sintering furnace, sintering at 880° C. for 2 h in a low-hydrogen mixed gas environment, cooling to room temperature with the furnace, welding and sealing the tail of the copper tube, and then injecting an actuating fluid (deionized water) into the copper tube, evacuating the tube, welding and sealing the end of the copper tube, and then flattening it to a thickness of 3 mm to obtain an ultra-thin heat pipe;

[0145] The low-hydrogen mixed gas consists of 95% N 2 and 5% H 2 composition;

[0146] Among them, the length of the copper mesh is not less than the length of the copper tube, and the width D of the copper mesh and the inner diameter r of the copper tube satisfy the following relationship: The inner diameter of the copper tube is designed according to specific use requirements and is not specifically limited. For example, as an illustration, in this embodiment, the inner diameter r of the copper tube is 10 mm.

[0147] In this embodiment, the high thermal conductivity copper mesh is prepared by a high thermal conductivity copper alloy, and the raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage:

[0148] Mn: 0.35%; Co: 0.41%; Ag: 0.09%; Cr: 1.10%; Zr: 0.29%; Ni@SWCNT@Fe: 3.75%; surface modified TiC: 2.80% and the balance of copper.

[0149] Ni@SWCNT@Fe is a coated, filled and modified carbon nanotube containing a sacrificial element component, wherein the sacrificial element component is Fe.

[0150] In this embodiment, the high thermal conductivity copper mesh is prepared by the following method:

[0151] 1-1) All raw materials (Mn powder, Co powder, Ag powder, Cr powder, Zr powder, Ni@SWCNT@Fe, surface-modified TiC particles and copper powder) were added into a ball mill according to the mass ratio and ball milled for 2 h under argon protection, with a ball-to-material ratio of 7:1 and a rotation speed of 300 rpm;

[0152] 1-2) Add the ball-milled raw materials into a vacuum melting furnace, evacuate to 0.1 Pa, then heat to 1350°C under argon protection, melt for 22 minutes, and vacuum cast to obtain an ingot;

[0153] 1-3) Keep at 900℃ for 2h for homogenization; then forge at 750℃ to make a rod with a diameter of 10mm, cool to room temperature and draw at room temperature to make a thick copper wire with a diameter of 2mm;

[0154] 1-4) The thick copper wire is heat treated at 700°C for 30 seconds under argon protection, and then drawn through a multi-pass wire drawing die to obtain a thin copper wire with a diameter of 0.05 mm (the copper wire is soaked with wire drawing oil during each wire drawing to prevent the copper wire from being fuzzed or scratched, improve the surface finish of the copper wire, and extend the service life of the wire drawing die);

[0155] 1-5) The thin copper wire is kept at 600°C for 0.5h under argon protection, cooled to room temperature to obtain a braided copper wire, and the braided copper wire is weaved into a copper mesh by a wire mesh weaving machine. The copper mesh is washed with ethanol and deionized water in turn, and vacuum dried at 80°C to constant weight to obtain a high thermal conductivity copper mesh with a mesh size of 200 mesh.

[0156] In this embodiment, the coated, filled and modified carbon nanotubes Ni@SWCNT@Fe are prepared by the following method:

[0157] S1-1, single-arm carbon nanotube pretreatment;

[0158] 2 g of single-arm carbon nanotubes were added to 200 mL of a mixture of 95 wt% concentrated sulfuric acid and 65 wt% concentrated nitric acid in a volume ratio of 1:1, and ultrasonically dispersed for 30 min, then heated to 90° C., stirred and refluxed for 4 h, cooled, filtered, washed with deionized water until neutral, and vacuum dried at 80° C. to constant weight to obtain pretreated single-arm carbon nanotubes;

[0159] S1-2, preparation of internally filled carbon nanotubes:

[0160] 1 g of pretreated single-arm carbon nanotubes and 0.2 g of polyethylene glycol were added to 100 mL of deionized water, and then 0.483 g of ferric nitrate was added. After ultrasonic dispersion for 45 min, 15 mL of 20% ammonia water was added dropwise. After the addition was completed, the mixture was stirred for 10 min. The obtained dispersed mixture 1 was transferred to a polytetrafluoroethylene-lined reactor, reacted at 195 ° C for 2 h, filtered, and the solid product was washed with deionized water and vacuum dried at 90 ° C for 6 h to obtain internally filled carbon nanotubes.

[0161] S1-3. Preparation of Ni@SWCNT@Fe:

[0162] 1 g of the inner-filled carbon nanotubes was added to 200 mL of deionized water and ultrasonically dispersed at 60 °C for 1 h. Then 0.55 g of nickel nitrate was added and ultrasonically dispersed for 2 h. The resulting dispersed mixture 2 was transferred to a polytetrafluoroethylene-lined reactor and reacted at 200 °C for 3 h. The solid product was filtered and washed with deionized water, vacuum dried at 100 °C for 4 h, and finally heated to room temperature in H 2 atmosphere and calcined at 1050 °C for 3 h to obtain Ni@SWCNT@Fe.

[0163] In this embodiment, surface modified TiC is prepared by the following method:

[0164] S2-1, pretreatment:

[0165] After cleaning, TiC particles with a particle size of 4 μm are subjected to coarsening, sensitization and activation treatment in sequence to obtain pretreated TiC. The specific steps are as follows:

[0166] S2-1-1. Cleaning: 1 g of TiC particles with a particle size of 4 μm was soaked in 200 mL of acetone, ultrasonically vibrated for 30 min, filtered, and washed with ethanol;

[0167] S2-1-2, roughening: then add into 150mL of 10wt% hydrofluoric acid and stir for 20min to roughen, wash with deionized water, and dry at 90°C for 4h;

[0168] S2-1-3, Sensitization: Add to 200 mL of sensitization solution, sensitize for 30 min under stirring, filter, and wash with deionized water;

[0169] Preparation of sensitizing solution: add 2.5g of stannous chloride and 6.5mL of 36% hydrochloric acid to 100mL of deionized water, stir evenly, and obtain sensitizing solution;

[0170] S2-1-4, activation: add the product of step S2-1-3 into 120 mL of activation solution, and soak for 45 min under stirring. The activation solution comprises: 0.8 g / L palladium dichloride, 23 g / L boric acid, and 0.45 g / L hydrochloric acid;

[0171] After activation, the product was filtered, washed with deionized water, and dried under vacuum at 70°C for 4 h to obtain pretreated TiC.

[0172] S2-2, chemical plating:

[0173] Copper nitrate and cerium nitrate are added to deionized water, stirred until completely dissolved, then citric acid and boric acid are added, stirred until completely dissolved, then the pH is adjusted to 11 with sodium hydroxide, the pretreated TiC is added, and then sodium hypophosphite is added, and the pretreated TiC is subjected to chemical plating treatment with the obtained plating solution;

[0174] The concentrations of the components in the obtained plating solution are: copper nitrate 17 g / L, cerium nitrate 4.2 g / L, citric acid 15 g / L, sodium hypophosphite 20 g / L, boric acid 18 g / L;

[0175] The plating process conditions are: pH 11, mechanical stirring 400r / min, temperature: 85°C, time: 2h;

[0176] After the chemical plating, the solid particles were filtered and washed with deionized water and dried under vacuum at 100°C for 6 h to obtain surface-modified TiC.

[0177] Reference Figure 5 , is a physical picture of the high thermal conductivity copper mesh prepared in this embodiment. Figure 6 A physical picture of an ultra-thin heat pipe prepared according to the requirements of process shape, size, etc. in a specific application example, which is generally L-shaped and includes a heat source end and a heat dissipation end; Figure 7 This is a physical picture of the heat source end and heat dissipation end of the ultra-thin heat pipe after disassembly.

[0178] Example 2

[0179] A process for manufacturing an ultra-thin heat pipe with improved heat transfer performance comprises the following steps:

[0180] 1) Soak the high thermal conductivity copper mesh in a 30% sodium chloride solution for 5 minutes, take it out and heat it at 120°C in air for 30 minutes, and cool it to room temperature;

[0181] 2) washing the copper mesh obtained in step 1) with deionized water, immersing it in 30% citric acid, and ultrasonically treating it for 28 minutes;

[0182] 3) washing the copper mesh obtained in step 2) with deionized water, and then heating and oxidizing it at 120° C. in a mixed gas environment with a volume ratio of air to oxygen of 1:1 for 1 h;

[0183] 4) inserting the copper mesh obtained in step 3) into a copper tube with a wall thickness of 0.2 mm, then placing the copper tube in a sintering furnace, sintering at 880° C. for 2 h in a low-hydrogen mixed gas environment, cooling to room temperature with the furnace, welding and sealing the tail of the copper tube, and then injecting an actuating fluid (deionized water) into the copper tube, evacuating the tube, welding and sealing the end of the copper tube, and then flattening it to a thickness of 3 mm to obtain an ultra-thin heat pipe;

[0184] The low hydrogen mixed gas consists of 95% N 2 and 5% H 2 composition;

[0185] Among them, the length of the copper mesh is not less than the length of the copper tube, and the width D of the copper mesh and the inner diameter r of the copper tube satisfy the following relationship: The inner diameter of the copper tube is designed according to specific use requirements and is not specifically limited. For example, as an illustration, in this embodiment, the inner diameter r of the copper tube is 10 mm.

[0186] In this embodiment, the high thermal conductivity copper mesh is prepared by a high thermal conductivity copper alloy, and the raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage:

[0187] Mn: 0.35%; Co: 0.43%; Ag: 0.09%; Cr: 1.10%; Zr: 0.29%; Ni@SWCNT@Fe: 3.50%; surface modified TiC: 2.80% and the balance of copper.

[0188] Ni@SWCNT@Fe is a coated, filled and modified carbon nanotube containing a sacrificial element component, wherein the sacrificial element component is Fe.

[0189] In this embodiment, the high thermal conductivity copper mesh is prepared by the following method:

[0190] 1-1) Add all raw materials into a ball mill according to the mass ratio, and ball mill for 2 hours under argon protection, with a ball-to-material ratio of 7:1 and a rotation speed of 300 rpm;

[0191] 1-2) Add the ball-milled raw materials into a vacuum melting furnace, evacuate to 0.1 Pa, then heat to 1350°C under argon protection, melt for 22 minutes, and vacuum cast to obtain an ingot;

[0192] 1-3) Keep at 900℃ for 2h for homogenization; then forge at 750℃ to make a rod with a diameter of 10mm, cool to room temperature and draw at room temperature to make a thick copper wire with a diameter of 2mm;

[0193] 1-4) The thick copper wire is heat treated at 700°C for 30 seconds under argon protection, and then drawn through a multi-pass wire drawing die to obtain a thin copper wire with a diameter of 0.05 mm (the copper wire is soaked with wire drawing oil during each wire drawing to prevent the copper wire from being fuzzed or scratched, improve the surface finish of the copper wire, and extend the service life of the wire drawing die);

[0194] 1-5) The thin copper wire is kept at 600°C for 0.5h under argon protection, cooled to room temperature to obtain a braided copper wire, and the braided copper wire is weaved into a copper mesh by a wire mesh weaving machine. The copper mesh is washed with ethanol and deionized water in turn, and vacuum dried at 80°C to constant weight to obtain a high thermal conductivity copper mesh with a mesh size of 200 mesh.

[0195] In this embodiment, the coated, filled and modified carbon nanotubes Ni@SWCNT@Fe are prepared by the following method:

[0196] S1-1, single-arm carbon nanotube pretreatment;

[0197] 2 g of single-arm carbon nanotubes were added to 200 mL of a mixture of 95 wt% concentrated sulfuric acid and 65 wt% concentrated nitric acid in a volume ratio of 1:1, and ultrasonically dispersed for 30 min, then heated to 90° C., stirred and refluxed for 4 h, cooled, filtered, washed with deionized water until neutral, and vacuum dried at 80° C. to constant weight to obtain pretreated single-arm carbon nanotubes;

[0198] S1-2, preparation of internally filled carbon nanotubes:

[0199] 1 g of pretreated single-arm carbon nanotubes and 0.2 g of polyethylene glycol were added to 100 mL of deionized water, and then 0.483 g of ferric nitrate was added. After ultrasonic dispersion for 45 min, 15 mL of 20% ammonia water was added dropwise. After the addition was completed, the mixture was stirred for 10 min. The obtained dispersed mixture 1 was transferred to a polytetrafluoroethylene-lined reactor, reacted at 195 ° C for 2 h, filtered, and the solid product was washed with deionized water and vacuum dried at 90 ° C for 6 h to obtain internally filled carbon nanotubes.

[0200] S1-3. Preparation of Ni@SWCNT@Fe:

[0201] Take 1 g of the filled carbon nanotubes and add them to 200 mL of deionized water, ultrasonically disperse them at 60 ° C for 1 h, then add 0.55 g of nickel nitrate and ultrasonically disperse them for 2 h. The resulting dispersed mixture 2 was transferred to a polytetrafluoroethylene-lined reactor and reacted at 200 ° C for 3 h. After filtering, the solid product was washed with deionized water, vacuum dried at 100 ° C for 4 h, and finally calcined at 1050 ° C for 3 h in an H2 atmosphere to obtain Ni@SWCNT@Fe.

[0202] In this embodiment, surface modified TiC is prepared by the following method:

[0203] S2-1, pretreatment:

[0204] After cleaning, TiC particles with a particle size of 4 μm are subjected to coarsening, sensitization and activation treatment in sequence to obtain pretreated TiC. The specific steps are as follows:

[0205] S2-1-1. Cleaning: 1 g of TiC particles with a particle size of 4 μm was soaked in 200 mL of acetone, ultrasonically vibrated for 30 min, filtered, and washed with ethanol;

[0206] S2-1-2, roughening: then add into 150mL of 10wt% hydrofluoric acid and stir for 20min to roughen, wash with deionized water, and dry at 90°C for 4h;

[0207] S2-1-3, Sensitization: Add to 200 mL of sensitization solution, sensitize for 30 min under stirring, filter, and wash with deionized water;

[0208] Preparation of sensitizing solution: add 2.5g of stannous chloride and 6.5mL of 36% hydrochloric acid to 100mL of deionized water, stir evenly, and obtain sensitizing solution;

[0209] S2-1-4, activation: add the product of step S2-1-3 into 120 mL of activation solution, and soak for 45 min under stirring. The activation solution comprises: 0.8 g / L palladium dichloride, 23 g / L boric acid, and 0.45 g / L hydrochloric acid;

[0210] After activation, the product was filtered, washed with deionized water, and dried under vacuum at 70°C for 4 h to obtain pretreated TiC.

[0211] S2-2, chemical plating:

[0212] Copper nitrate and cerium nitrate are added to deionized water, stirred until completely dissolved, then citric acid and boric acid are added, stirred until completely dissolved, then the pH is adjusted to 11 with sodium hydroxide, the pretreated TiC is added, and then sodium hypophosphite is added, and the pretreated TiC is subjected to chemical plating treatment with the obtained plating solution;

[0213] The concentrations of the components in the obtained plating solution are: copper nitrate 17 g / L, cerium nitrate 4.5 g / L, citric acid 15 g / L, sodium hypophosphite 20 g / L, boric acid 18 g / L;

[0214] The plating process conditions are: pH 11, mechanical stirring 400r / min, temperature: 85°C, time: 2h;

[0215] After the chemical plating, the solid particles were filtered and washed with deionized water and dried under vacuum at 100°C for 6 h to obtain surface-modified TiC.

[0216] Example 3

[0217] A process for manufacturing an ultra-thin heat pipe with improved heat transfer performance comprises the following steps:

[0218] 1) Soak the high thermal conductivity copper mesh in a 30% sodium chloride solution for 5 minutes, take it out and heat it at 120°C in air for 30 minutes, and cool it to room temperature;

[0219] 2) washing the copper mesh obtained in step 1) with deionized water, immersing it in 30% citric acid, and ultrasonically treating it for 30 minutes;

[0220] 3) washing the copper mesh obtained in step 2) with deionized water, and then heating and oxidizing it at 120° C. in a mixed gas environment with a volume ratio of air to oxygen of 1:1 for 1 h;

[0221] 4) inserting the copper mesh obtained in step 3) into a copper tube with a wall thickness of 0.2 mm, then placing the copper tube in a sintering furnace, sintering at 880° C. for 2 h in a low-hydrogen mixed gas environment, cooling to room temperature with the furnace, welding and sealing the tail of the copper tube, and then injecting an actuating fluid (deionized water) into the copper tube, evacuating the tube, welding and sealing the end of the copper tube, and then flattening it to a thickness of 3 mm to obtain an ultra-thin heat pipe;

[0222] The low hydrogen mixed gas consists of 95% N 2 and 5% H 2 composition;

[0223] Among them, the length of the copper mesh is not less than the length of the copper tube, and the width D of the copper mesh and the inner diameter r of the copper tube satisfy the following relationship: The inner diameter of the copper tube is designed according to specific use requirements and is not specifically limited. For example, as an illustration, in this embodiment, the inner diameter r of the copper tube is 10 mm.

[0224] In this embodiment, the high thermal conductivity copper mesh is prepared by a high thermal conductivity copper alloy, and the raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage:

[0225] Mn: 0.37%; Co: 0.42%; Ag: 0.11%; Cr: 1.10%; Zr: 0.32%; Ni@SWCNT@Fe: 3.75%; surface modified TiC: 2.85% and the balance of copper.

[0226] Ni@SWCNT@Fe is a coated, filled and modified carbon nanotube containing a sacrificial element component, wherein the sacrificial element component is Fe.

[0227] In this embodiment, the high thermal conductivity copper mesh is prepared by the following method:

[0228] 1-1) Add all raw materials into a ball mill according to the mass ratio, and ball mill for 2 hours under argon protection, with a ball-to-material ratio of 7:1 and a rotation speed of 300 rpm;

[0229] 1-2) Add the ball-milled raw materials into a vacuum melting furnace, evacuate to 0.1 Pa, then heat to 1350°C under argon protection, melt for 22 minutes, and vacuum cast to obtain an ingot;

[0230] 1-3) Keep at 900℃ for 2h for homogenization; then forge at 750℃ to make a rod with a diameter of 10mm, cool to room temperature and draw at room temperature to make a thick copper wire with a diameter of 2mm;

[0231] 1-4) The thick copper wire is heat treated at 700°C for 30 seconds under argon protection, and then drawn through a multi-pass wire drawing die to obtain a thin copper wire with a diameter of 0.05 mm (the copper wire is soaked with wire drawing oil during each wire drawing to prevent the copper wire from being fuzzy and scratched, improve the surface finish of the copper wire, and extend the service life of the wire drawing die;);

[0232] 1-5) The thin copper wire is kept at 600°C for 0.5h under argon protection, cooled to room temperature to obtain a braided copper wire, and the braided copper wire is weaved into a copper mesh by a wire mesh weaving machine. The copper mesh is washed with ethanol and deionized water in turn, and vacuum dried at 80°C to constant weight to obtain a high thermal conductivity copper mesh with a mesh size of 200 mesh.

[0233] In this embodiment, the coated, filled and modified carbon nanotubes Ni@SWCNT@Fe are prepared by the following method:

[0234] S1-1, single-arm carbon nanotube pretreatment;

[0235] 2 g of single-arm carbon nanotubes were added to 200 mL of a mixture of 95 wt% concentrated sulfuric acid and 65 wt% concentrated nitric acid in a volume ratio of 1:1, and ultrasonically dispersed for 30 min, then heated to 90° C., stirred and refluxed for 4 h, cooled, filtered, washed with deionized water until neutral, and vacuum dried at 80° C. to constant weight to obtain pretreated single-arm carbon nanotubes;

[0236] S1-2, preparation of internally filled carbon nanotubes:

[0237] 1 g of pretreated single-arm carbon nanotubes and 0.2 g of polyethylene glycol were added to 100 mL of deionized water, and then 0.483 g of ferric nitrate was added. After ultrasonic dispersion for 45 min, 15 mL of 20% ammonia water was added dropwise. After the addition was completed, the mixture was stirred for 10 min. The obtained dispersed mixture 1 was transferred to a polytetrafluoroethylene-lined reactor, reacted at 195 ° C for 2 h, filtered, and the solid product was washed with deionized water and vacuum dried at 90 ° C for 6 h to obtain internally filled carbon nanotubes.

[0238] S1-3. Preparation of Ni@SWCNT@Fe:

[0239] Take 1 g of the filled carbon nanotubes and add them into 200 mL of deionized water, ultrasonically disperse them at 60 ° C for 1 h, then add 0.60 g of nickel nitrate and ultrasonically disperse them for 2 h. The obtained dispersed mixture 2 is transferred to a polytetrafluoroethylene-lined reactor and reacted at 200 ° C for 3 h. After filtering, the solid product is washed with deionized water, vacuum dried at 100 ° C for 4 h, and finally calcined at 1050 ° C for 3 h in a H2 atmosphere to obtain Ni@SWCNT@Fe.

[0240] In this embodiment, surface modified TiC is prepared by the following method:

[0241] S2-1, pretreatment:

[0242] After cleaning, TiC particles with a particle size of 4 μm are subjected to coarsening, sensitization and activation treatment in sequence to obtain pretreated TiC. The specific steps are as follows:

[0243] S2-1-1. Cleaning: 1 g of TiC particles with a particle size of 4 μm was soaked in 200 mL of acetone, ultrasonically vibrated for 30 min, filtered, and washed with ethanol;

[0244] S2-1-2, roughening: then add into 150mL of 10wt% hydrofluoric acid and stir for 20min to roughen, wash with deionized water, and dry at 90°C for 4h;

[0245] S2-1-3, Sensitization: Add to 200 mL of sensitization solution, sensitize for 30 min under stirring, filter, and wash with deionized water;

[0246] Preparation of sensitizing solution: add 2.5g of stannous chloride and 6.5mL of 36% hydrochloric acid to 100mL of deionized water, stir evenly, and obtain sensitizing solution;

[0247] S2-1-4, activation: add the product of step S2-1-3 into 120 mL of activation solution, and soak for 45 min under stirring. The activation solution comprises: 0.8 g / L palladium dichloride, 23 g / L boric acid, and 0.45 g / L hydrochloric acid;

[0248] After activation, the product was filtered, washed with deionized water, and dried under vacuum at 70°C for 4 h to obtain pretreated TiC.

[0249] S2-2, chemical plating:

[0250] Copper nitrate and cerium nitrate are added to deionized water, stirred until completely dissolved, then citric acid and boric acid are added, stirred until completely dissolved, then the pH is adjusted to 11 with sodium hydroxide, the pretreated TiC is added, and then sodium hypophosphite is added, and the pretreated TiC is subjected to chemical plating treatment with the obtained plating solution;

[0251] The concentrations of the components in the obtained plating solution are: copper nitrate 17 g / L, cerium nitrate 4.5 g / L, citric acid 15 g / L, sodium hypophosphite 20 g / L, boric acid 18 g / L;

[0252] The plating process conditions are: pH 11, mechanical stirring 400r / min, temperature: 85°C, time: 2h;

[0253] After the chemical plating, the solid particles were filtered and washed with deionized water and dried under vacuum at 100°C for 6 h to obtain surface-modified TiC.

[0254] Comparative Example 1

[0255] This example is basically the same as Example 1, except that: in this example, the raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage:

[0256] Mn: 0.35%; Co: 0.41%; Ag: 0.09%; Cr: 1.10%; Zr: 0.29%; surface modified TiC: 2.80% and the balance copper.

[0257] Comparative Example 2

[0258] This example is basically the same as Example 1, except that in this example, Ni@SWCNT@Fe is prepared by the following method:

[0259] S1-1, pretreatment of single-arm carbon nanotubes, the same as in Example 1;

[0260] S1-2, preparing internally filled carbon nanotubes, the same as in Example 1;

[0261] S1-3. Preparation of Ni@SWCNT@Fe:

[0262] 1 g of the filled carbon nanotubes was added to 200 mL of deionized water and ultrasonically dispersed at 60 °C for 3 h. The resulting dispersed mixture 2 was transferred to a polytetrafluoroethylene-lined reactor and reacted at 200 °C for 3 h. The solid product was washed with deionized water and vacuum dried at 100 °C for 4 h. 2 atmosphere and calcined at 1050 °C for 3 h to obtain SWCNT@Fe.

[0263] Comparative Example 3

[0264] This example is basically the same as Example 1, except that: in this example, the raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage:

[0265] Mn: 0.35%; Co: 0.41%; Ag: 0.09%; Cr: 1.10%; Zr: 0.29%; Ni@SWCNT@Fe: 3.75%; and the balance is copper.

[0266] Comparative Example 4

[0267] This example is basically the same as Example 1, except that: in this example, the raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage:

[0268] The raw materials for preparing high thermal conductivity copper alloy include, by mass percentage:

[0269] Mn: 0.35%; Co: 0.41%; Ag: 0.09%; Cr: 1.10%; Zr: 0.29%; Ni@SWCNT@Fe: 3.75%; TiC: 2.80% and the balance is copper.

[0270] Comparative Example 5

[0271] This example is basically the same as Example 1, except that in this example, the surface-modified TiC is prepared by the following method:

[0272] S2-1, pretreatment, the same as in Example 1;

[0273] S2-2, chemical plating:

[0274] Copper nitrate is added into deionized water, and citric acid and boric acid are added after stirring until completely dissolved, and the pH is adjusted to 11 with sodium hydroxide after stirring until completely dissolved, and the pretreated TiC is added, and then sodium hypophosphite is added, and the pretreated TiC is subjected to chemical plating treatment with the obtained plating solution;

[0275] The concentrations of the components in the obtained plating solution are: copper nitrate 17 g / L, citric acid 15 g / L, sodium hypophosphite 20 g / L, boric acid 18 g / L;

[0276] The plating process conditions are: pH 11, mechanical stirring 400r / min, temperature: 85°C, time: 2h;

[0277] After the chemical plating, the solid particles were filtered and washed with deionized water and dried under vacuum at 100°C for 6 h to obtain surface-modified TiC.

[0278] Performance Characterization

[0279] 1. Reference Figure 2 , electron microscopic images of the copper wire in the copper mesh before and after citric acid treatment (washed with deionized water after treatment) in step 2) of Example 1 (the image of the single-arm carbon nanotube SWCNT is shown in the figure), the left side of the figure is the image before treatment, it can be seen that there are a large amount of fillers (mainly Fe) inside, and the right side is the image after treatment, it can be seen that the internal filler is significantly reduced; the scale in the figure is 1nm; it can be seen that after citric acid treatment, the Fe filled in the single-arm carbon nanotube has been dissolved and removed in large quantities.

[0280] 2. Reference Figure 3 , XRD pattern of Ni@SWCNT@Fe prepared in Example 1;

[0281] 3. Reference Figure 4 , XRD pattern of surface modified TiC prepared in Example 1.

[0282] Performance Testing

[0283] 1. Tensile performance test

[0284] The thin copper wire prepared in step 1-5) of Example 1-3 and Comparative Example 1-5 was subjected to a tensile property test, specifically comprising:

[0285] 1. Room temperature tensile performance test, refer to the standard "GB / T 34505-2017 Room temperature tensile test method for copper and copper alloy materials" for testing;

[0286] 2. High temperature tensile performance test: refer to the above standards and test the tensile strength at 120°C.

[0287] The test results are shown in Table 1 and Figure 8 As shown:

[0288] Table 1

[0289]

[0290] According to Table 1 and Figure 8 It can be seen from the test results that the thin copper wires of Examples 1-3 have high tensile strength and appropriate elongation at break, and excellent thermal stability. The tensile properties and thermal stability of Comparative Example 1 both decreased, which was attributed to the fact that Ni@SWCNT@Fe was not added to the raw materials for the preparation of its copper alloy; the tensile properties of Comparative Example 2 decreased slightly, which explained the performance enhancement effect of nickel coating in the coated and filled modified carbon nanotubes; the thermal stability of Comparative Example 3 decreased significantly, which was attributed to the fact that surface-modified TiC was not added to the raw materials for the preparation of its copper alloy; Unmodified TiC was used in the raw materials for the preparation of the copper alloy of Comparative Example 4, and TiC was difficult to disperse evenly, resulting in a decrease in thermal stability; Ce ions were not added to the chemical plating solution in Comparative Example 5, resulting in a certain decrease in tensile properties and thermal stability.

[0291] 2. Measuring thermal resistance

[0292] The ultra-thin heat pipes of the embodiment and the comparative example were prepared into test samples with a total length of 200 mm, and then the thermal resistance of the heat pipes was tested by a conventional thermal simulation test method in the industry (refer to the flat heat pipe of patent CN102326046A). The specific method is as follows:

[0293] The first end (i.e., the heat source end) of the heat pipe is given a heating area of ​​30 mm × 30 mm (in contact with the surface of the electric heater), and the second end (i.e., the heat dissipation end) is given a heat dissipation area of ​​60 mm × 60 mm (in contact with the surface of the aluminum heat dissipation plate). At room temperature, the first end of the heat pipe is heated by the electric heater, and the heat input Q of the electric heater and the temperature T of the contact point between the electric heater and the first end of the heat pipe are calculated. 1 , the temperature T at the contact point between the second end of the heat pipe and the aluminum heat sink 2 , calculate the thermal resistance R according to the following formula:

[0294] Unit: °C / W.

[0295] The test results are shown in Table 2 and Fig. 9 As shown:

[0296] Table 2

[0297]

[0298] According to Table 2 and Fig. 9 It can be seen from the test results that the ultra-thin heat pipes prepared in Examples 1-3 have excellent heat transfer capabilities. In Comparative Example 1, Ni@SWCNT@Fe is not added to the copper alloy raw material for preparing the copper wire, which greatly reduces its heat transfer capability. The heat transfer capability of Comparative Example 2 also decreases to a certain extent, which is attributed to the fact that nickel coating is not performed in the coated, filled and modified carbon nanotubes. The heat transfer capabilities of Comparative Examples 3-5 remain basically unchanged.

[0299] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. A process for manufacturing an ultra-thin heat pipe with improved heat transfer performance. It is characterized in that The following steps are involved: 1) Soak the high thermal conductivity copper mesh in a salt solution, take it out and heat it in an air atmosphere for oxidation treatment, and cool it to room temperature after the treatment is completed; 2) washing the copper mesh obtained in step 1) with deionized water, immersing it in an acid solution, and performing ultrasonic treatment; 3) washing the copper mesh obtained in step 2) with deionized water, and then heating and oxidizing it in a mixed gas environment of air and oxygen; 4) inserting the copper mesh obtained in step 3) into the copper tube, and then placing the copper tube in a sintering furnace, sintering the copper tube in a hydrogen-containing gas environment, cooling the copper tube to room temperature with the furnace after the treatment, sealing the tail of the copper tube, and then injecting an actuating fluid into the copper tube, evacuating the tube, sealing the end of the copper tube and flattening it to obtain an ultra-thin heat pipe.

2. The manufacturing process of the ultra-thin heat pipe with improved heat transfer performance according to claim 1, It is characterized in that The following steps are involved: 1) Soak the high thermal conductivity copper mesh in a sodium chloride solution with a mass concentration of 15-40% for 2-10 minutes, take it out and heat it in an air atmosphere at 110-130° C. for 15-60 minutes, and cool it to room temperature; 2) washing the copper mesh obtained in step 1) with deionized water, immersing it in citric acid with a mass concentration of 15-45%, and ultrasonically treating it for 15-60 minutes; 3) washing the copper mesh obtained in step 2) with deionized water, and then heating and oxidizing it at 110-130° C. and a mixed gas environment with a volume ratio of air to oxygen of 1:2-2:1 for 0.5-2 h; 4) inserting the copper mesh obtained in step 3) into a copper tube with a wall thickness of 0.1-0.5 mm, then placing the copper tube in a sintering furnace, sintering at 850-900° C. for 1-4 h in a low-hydrogen mixed gas environment, cooling to room temperature with the furnace, sealing the tail of the copper tube, and then injecting an actuating fluid into the copper tube, evacuating, sealing the end of the copper tube and flattening it to a thickness of 1-5 mm to obtain an ultra-thin heat pipe; Among them, the width D of the copper mesh and the inner diameter r of the copper tube satisfy the following relationship: The actuating fluid is ultrapure water or ethanol.

3. The process for manufacturing an ultra-thin heat pipe with improved heat transfer performance according to claim 2, It is characterized in that The following steps are involved: 1) Soak the high thermal conductivity copper mesh in a 30% sodium chloride solution for 5 minutes, take it out and heat it at 120°C in air for 30 minutes, and cool it to room temperature; 2) washing the copper mesh obtained in step 1) with deionized water, immersing it in 30% citric acid, and ultrasonically treating it for 30 minutes; 3) washing the copper mesh obtained in step 2) with deionized water, and then heating and oxidizing it at 120° C. in a mixed gas environment with a volume ratio of air to oxygen of 1:1 for 1 h; 4) inserting the copper mesh obtained in step 3) into a copper tube with a wall thickness of 0.2 mm, then placing the copper tube in a sintering furnace, sintering at 880° C. for 2 h in a low-hydrogen mixed gas environment, cooling to room temperature with the furnace, sealing the tail of the copper tube, and then injecting an actuating fluid into the copper tube, evacuating the tube, sealing the end of the copper tube and flattening it to a thickness of 3 mm to obtain an ultra-thin heat pipe; The low-hydrogen mixed gas consists of 95% N 2 and 5% H 2 composition; Among them, the length of the copper mesh is not less than the length of the copper tube, and the width D of the copper mesh and the inner diameter r of the copper tube satisfy the following relationship: Among them, the operating fluid is ultrapure water.

4. The process for manufacturing an ultra-thin heat pipe with improved heat transfer performance according to claim 1, It is characterized in that The high thermal conductivity copper mesh is prepared by a high thermal conductivity copper alloy, and the raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage: Mn: 0.22-0.67%; Co: 0.19-0.74%; Ag: 0.05-0.17%; Cr: 0.85-1.33%; Zr: 0.20-0.45%; Ni@SWCNT@Fe: 2.50-4.00%; surface modified TiC: 2.20-3.50% and the balance of copper; The Ni@SWCNT@Fe is a coated, filled and modified carbon nanotube containing a sacrificial element component, wherein the sacrificial element component is Fe.

5. The process for manufacturing an ultra-thin heat pipe with improved heat transfer performance according to claim 4, It is characterized in that The raw materials for preparing the high thermal conductivity copper alloy include, by mass percentage: Mn: 0.35%; Co: 0.41%; Ag: 0.09%; Cr: 1.10%; Zr: 0.29%; Ni@SWCNT@Fe: 3.75%; surface modified TiC: 2.80% and the balance of copper.

6. The process for manufacturing an ultra-thin heat pipe with improved heat transfer performance according to claim 4, It is characterized in that The high thermal conductivity copper mesh is prepared by the following method: 1-1) Add all raw materials into a ball mill according to the mass ratio, and ball mill for 1-4 hours under argon protection, with a ball-to-material ratio of 9:1-6:1 and a rotation speed of 200-500rpm; 1-2) Add the ball-milled raw materials into a vacuum melting furnace, evacuate to 0.1-0.3 Pa, then heat to 1250-1500° C. under argon protection, melt for 10-30 min, and vacuum cast to obtain an ingot; 1-3) Keep the temperature at 850-950℃ for 1-4h to perform homogenization treatment; then perform rotary forging at 600-800℃ to produce a rod with a diameter of 5-20mm, and then perform room temperature drawing after cooling to room temperature to produce a thick copper wire with a diameter of 2-5mm; 1-4) heat treating the thick copper wire under argon protection at 550-750° C. for 1-5 min, and then drawing the thick copper wire through a wire drawing die to obtain a thin copper wire with a diameter of 0.02-0.2 mm; 1-5) The thin copper wire is kept warm at 550-700° C. for 0.5-1 h under argon protection, and cooled to room temperature to obtain a braided copper wire, and the braided copper wire is weaved into a copper mesh by a wire mesh weaving machine, and the copper mesh is washed with ethanol and deionized water in turn, and vacuum dried at 70-100° C. to constant weight to obtain a high thermal conductive copper mesh with a mesh size of 100-300 meshes.

7. The process for manufacturing an ultra-thin heat pipe with improved heat transfer performance according to claim 4, It is characterized in that The coated, filled and modified carbon nanotube Ni@SWCNT@Fe is prepared by the following method: S1, single-arm carbon nanotube pretreatment; The single-arm carbon nanotubes are added to a mixed acid of 95wt% concentrated sulfuric acid and 65wt% concentrated nitric acid, and ultrasonically dispersed for 15-60min, and then heated to 80-100°C, stirred and refluxed for 2-10h, cooled, filtered, washed with deionized water until neutral, and vacuum dried at 70-100°C to constant weight to obtain pretreated single-arm carbon nanotubes; The volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed acid is 1:2-2:1; S2. Preparation of internally filled carbon nanotubes: 0.5-2g of pretreated single-arm carbon nanotubes and 0.12-0.35g of polyethylene glycol are added to 50-200mL of deionized water, and then 0.241-0.966g of ferric nitrate is added. After ultrasonic dispersion for 30-90min, 10-30mL of ammonia water with a mass concentration of 15-25% is added dropwise. After the addition is completed, the mixture is stirred for 5-30min. The obtained dispersed mixture 1 is transferred to a polytetrafluoroethylene-lined reactor, reacted at 190-200°C for 1-4h, filtered, and the solid product is washed with deionized water, and vacuum dried at 80-100°C for 4-12h to obtain internally filled carbon nanotubes; S3. Preparation of Ni@SWCNT@Fe: 0.5-2 g of the inner-filled carbon nanotubes were added to 100-400 mL of deionized water, and ultrasonically dispersed at 50-65° C. for 0.5-2 h, and then 0.27-1.1 g of nickel nitrate was added and ultrasonically dispersed for 1-4 h. The obtained dispersed mixture 2 was transferred to a polytetrafluoroethylene-lined reactor, reacted at 190-220° C. for 1.5-6 h, filtered, and the solid product was washed with deionized water, vacuum dried at 90-110° C. for 2-8 h, and finally calcined at 1000-1150° C. in a reducing gas atmosphere for 1.5-6 h to obtain Ni@SWCNT@Fe; The reducing gas is H 2 or CO.

8. The process for manufacturing an ultra-thin heat pipe with improved heat transfer performance according to claim 7, It is characterized in that The coated, filled and modified carbon nanotube Ni@SWCNT@Fe is prepared by the following method: S1-1, single-arm carbon nanotube pretreatment; 2 g of single-arm carbon nanotubes were added to 200 mL of a mixture of 95 wt% concentrated sulfuric acid and 65 wt% concentrated nitric acid in a volume ratio of 1:1, and ultrasonically dispersed for 30 min, then heated to 90° C., stirred and refluxed for 4 h, cooled, filtered, washed with deionized water until neutral, and vacuum dried at 80° C. to constant weight to obtain pretreated single-arm carbon nanotubes; S1-2, preparation of internally filled carbon nanotubes: 1 g of pretreated single-arm carbon nanotubes and 0.2 g of polyethylene glycol were added to 100 mL of deionized water, and then 0.483 g of ferric nitrate was added. After ultrasonic dispersion for 45 min, 15 mL of 20% ammonia water was added dropwise. After the addition was completed, the mixture was stirred for 10 min. The obtained dispersed mixture 1 was transferred to a polytetrafluoroethylene-lined reactor, reacted at 195 ° C for 2 h, filtered, and the solid product was washed with deionized water and vacuum dried at 90 ° C for 6 h to obtain internally filled carbon nanotubes. S1-3. Preparation of Ni@SWCNT@Fe: 1 g of the inner-filled carbon nanotubes was added to 200 mL of deionized water and ultrasonically dispersed at 60 °C for 1 h. Then 0.55 g of nickel nitrate was added and ultrasonically dispersed for 2 h. The resulting dispersed mixture 2 was transferred to a polytetrafluoroethylene-lined reactor and reacted at 200 °C for 3 h. The solid product was filtered and washed with deionized water, vacuum dried at 100 °C for 4 h, and finally heated to room temperature in H 2 Atmosphere and calcined at 1050 °C for 3 h to obtain Ni@SWCNT@Fe.

9. The process for manufacturing an ultra-thin heat pipe with improved heat transfer performance according to claim 4, It is characterized in that The surface modified TiC is prepared by the following method: S2-1, pretreatment: After cleaning TiC particles with a particle size of 1-10 μm, they are subjected to coarsening, sensitization and activation treatments in sequence to obtain pretreated TiC; S2-2, adding copper nitrate and cerium nitrate into deionized water, stirring until completely dissolved, then adding citric acid and boric acid, stirring until completely dissolved, adjusting the pH to 10.5-11.5 with sodium hydroxide, adding the pretreated TiC, and then adding sodium hypophosphite, and performing chemical plating on the pretreated TiC with the obtained plating solution; The concentrations of the components in the obtained plating solution are: copper nitrate 14.5-21 g / L, cerium nitrate 3.5-4.5 g / L, citric acid 11-18 g / L, sodium hypophosphite 15-25 g / L, and boric acid 10-24 g / L; The plating process conditions are: pH 10.5-11.5, mechanical stirring 300-650r / min, temperature: 80-90°C, time: 1-3h; After the chemical plating is completed, the solid particles are filtered and washed with deionized water, and vacuum dried at 90-100° C. for 4-12 hours to obtain surface-modified TiC.

10. An ultra-thin heat pipe, It is characterized in that The method is prepared by the process described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Heat pipe and manufacturing method thereof

    CN101634532A

  • Flat heat pipe

    CN102326046A

  • Composite heat pipe structure

    CN102331205A

  • Ultra-thin heat pipe of composite structure and manufacturing method thereof

    CN102410765A

  • Manufacturing process for adding capillary structure in ultra-thin heat pipe through sand blasting

    CN113701535A