Method for detecting core-shell structure of sintered NdFeB permanent magnet alloy subjected to Tb diffusion treatment
By pretreatment, thermal inlay and corrosion detection of sintered NdFeB permanent magnet alloy for Tb diffusion treatment, the problem of lack of effective detection of core-shell structures in the prior art is solved, and clear observation of metallographic grain boundaries and shell structures is achieved, which promotes the promotion of Optimization of diffusion process parameters.
Patent Information
- Application Number
- CN202410858362.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The prior art lacks effective detection methods to observe and determine the core-shell structure of the sintered NdFeB permanent magnet alloy in Tb diffusion treatment, which affects the optimization of diffusion process parameters.
After pretreatment, thermal inlay, grinding and polishing, the samples were used to conduct corrosion detection using specific corrosion agents, including nitric acid, hydrochloric acid and phosphoric acid solutions. The metallographic structure was observed through scanning electron microscopy to clearly display (Nd, Tb)2Fe14B shell structure. .
Through this method, the metallographic grain boundary and shell structure can be clearly observed, helping to determine the optimal diffusion parameters, and improving detection efficiency and accuracy.
Smart Images

Figure CN118883192A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of alloy detection, and in particular to a method for detecting the core-shell structure of a Tb-diffused sintered NdFeB permanent magnet alloy. Background Art
[0002] NdFeB permanent magnet is a tetragonal crystal formed by neodymium, iron and boron. 2 FE 14 B, as the sintered main body, is the only hard magnetic item and the main source of magnetism. Due to its structural characteristics, it can have high magnetic properties at room temperature and is widely used in the automotive field. In automotive motors and generators, due to its high magnetic energy product and good magnetic permeability, this magnet can increase the speed and power density while reducing the total weight and fuel consumption of the engine. In addition, in the motors and drive systems of electric and hybrid vehicles, NdFeB magnets also play a vital role, providing effective energy and high power output. They are also used in components such as sensors and brakes in automotive braking systems. Its good magnetic force and magnetic permeability also help to improve braking effect and sensitivity, thereby enhancing the safety of the vehicle. Studies have found that for this material, Nd 2 Fe 14 B as the sintering body, using Tb 2 Fe 14 After replacing part B, the magnetic crystal performance field is three times larger, which can effectively improve the coercivity, Tb 2 Fe 14 B forms a shell structure through the diffusion process, effectively suppressing the nucleation of phase domains and improving the coercive force. The finer the grain size, the more and more uniform the shell structure can be formed on the grain boundary, and the higher the coercive force is, so the magnetic properties of the magnet are optimized. Therefore, the observation of the core-shell structure has important reference value for determining the optimal grain boundary diffusion process parameters. However, there is no good detection method for its core-shell structure. Summary of the invention
[0003] The present application provides a method for detecting the core-shell structure of a Tb diffusion treated sintered NdFeB permanent magnet alloy, which can better detect the core-shell structure of the alloy and further help determine the optimal diffusion parameters.
[0004] The present application provides a method for detecting the core-shell structure of a Tb diffusion treated sintered NdFeB permanent magnet alloy, the method comprising:
[0005] Pre-treating the alloy to be tested to remove the magnetism of the alloy to be tested and clean the alloy to be tested, thereby obtaining a pre-treated sample;
[0006] Hot mounting the pretreated alloy to obtain a mounted sample;
[0007] Grinding and polishing the inlaid sample to obtain a bright surface sample;
[0008] preparing a corrosive agent, wherein the corrosive agent comprises a nitric acid solution, a hydrochloric acid solution and a phosphoric acid solution;
[0009] The bright surface sample is corroded by the corrosive agent and then tested.
[0010] As an optional implementation, the components of the corrosive agent include, by volume percentage: 4% to 5% nitric acid solution, 1% to 2% hydrochloric acid solution and 1.5% to 2.5% phosphoric acid solution, with the remainder being water.
[0011] As an optional embodiment, the mass percentage concentration of the nitric acid solution is 65% to 69%; and / or
[0012] The mass percentage concentration of the hydrochloric acid solution is 36% to 38%; and / or
[0013] The mass percentage concentration of the phosphoric acid solution is 83% to 90%.
[0014] As an optional implementation manner, the corrosion temperature is 22°C to 28°C.
[0015] As an optional implementation manner, the corrosion time is 15 to 20 seconds.
[0016] As an optional embodiment, the composition of the alloy to be tested includes, in terms of mole fraction: 29% to 32.5% neodymium; and / or
[0017] In terms of molar fraction, the composition of the alloy to be tested includes: 63.95% to 68.65% iron; and / or
[0018] In terms of molar fraction, the composition of the alloy to be tested includes: 1.1% to 1.2% boron; and / or
[0019] In terms of molar fraction, the composition of the alloy to be tested includes: 0.6% to 8% dysprosium; and / or
[0020] In terms of molar fraction, the composition of the alloy to be tested includes: 0.3% to 0.5% niobium; and / or
[0021] In terms of mole fraction, the composition of the alloy to be tested includes: 0.3% to 0.5% aluminum;
[0022] In terms of molar fraction, the composition of the alloy to be tested includes: 0.05% to 0.15% copper; and / or
[0023] Calculated by mole fraction, the components of the alloy to be tested include: Tb content is 1% to 2%.
[0024] As an optional implementation, the pretreatment includes demagnetization and cleaning.
[0025] As an optional implementation, the hot mounting is performed using HM1 phenolic resin.
[0026] As an optional embodiment, the grinding includes coarse grinding and fine grinding.
[0027] As an optional embodiment, the polishing sandpaper is at least 800 mesh.
[0028] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0029] The method provided in the embodiment of the present application adopts a specific corrosive agent to treat the treated Tb diffusion treated sintered NdFeB permanent magnet alloy. The metallographic grain boundary is clearly displayed, and the (Nd, Tb) formed by the diffusion process can be clearly observed. 2 Fe 14 B shell structure, which can help determine the optimal diffusion parameters. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0032] Figure 1 A schematic diagram of a process for a method provided in an embodiment of the present application;
[0033] Figure 2 This is a test result diagram provided in Example 1 of the present application;
[0034] Figure 3 The test result diagram provided for comparative example 1 of the present application;
[0035] Figure 4 The test result diagram provided for comparative example 2 of this application;
[0036] Figure 5 This is a test result diagram provided for comparative example 3 of the present application. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0039] like Figure 1 As shown, the embodiment of the present application provides a method for detecting the core-shell structure of a sintered NdFeB permanent magnet alloy subjected to Tb diffusion treatment, and the specific process is as follows:
[0040] The alloy to be tested is pretreated, including demagnetization and cleaning. Demagnetization is to facilitate subsequent grinding and polishing of the sample, and cleaning is to remove dirt and oil on the sample surface.
[0041] In some embodiments, the composition of the alloy to be tested includes, by mole fraction, 29% to 32.5% rare earth metal neodymium, 63.95% to 68.65% metal element iron, 1.1% to 1.2% non-metallic element boron, 0.6% to 8% added dysprosium, 0.3% to 0.5% niobium, 0.3% to 0.5% aluminum, 0.05% to 0.15% copper and other elements, and the content of the diffusion element Tb is 1% to 2%.
[0042] Secondly, the samples were hot mounted using HM1 phenolic resin, with resin powder added to more than 1 / 3 of the volume of the medium-sized cavity mold of the mounting machine. The temperature of the mounting machine was set to 170°C, the heating time was 800s, the insulation time was 200s, and the pressure in the cavity was 8000N.
[0043] Then, the sample is ground and polished, and the sample is polished after being polished with at least 800-grit sandpaper; preferably, the sample is polished after being polished with at least 1200-grit sandpaper.
[0044] Specifically, the grinding mainly includes coarse grinding and fine grinding.
[0045] Rough grinding is generally carried out on a 320 mesh belt grinder with a rotation speed of 800r / min. The abrasive particles fixed on the belt pass over the sample surface with high stress, removing the material in the form of grinding chips, leaving wear marks on the sample surface and forming a deformation damage layer with a certain depth, grinding off the edges and flash of the sample. The coarseness of the abrasive particle size has a certain influence on the surface roughness and grinding efficiency of the sample. During rough grinding, the water valve should be continuously opened for cooling to prevent structural changes.
[0046] Through fine grinding, i.e. the polishing step, we are ready for the next step of polishing. This is because although the surface of the sample is flat after rough grinding, there are still deep wear marks and surface processing deformation layers, which need to be gradually reduced by grinding with different metallographic sandpapers from coarse to fine. Metallographic sandpaper is an important material for polishing metallographic specimens, and the abrasive generally used is silicon carbide. Polish with 120 mesh, 320 mesh, 800 mesh, and 1200 mesh metallographic sandpaper in turn. Each time a layer of sandpaper is changed, the sample should be rotated 90 degrees, and the wear marks of the previous layer should be completely removed. Before polishing, apply a layer of glycerin on the sandpaper in advance to prevent sand grains from embedding into the grinding surface of the sample.
[0047] The sample is polished. The purpose of polishing is to remove the fine wear marks and surface deformation layer left by fine grinding on the metallographic grinding surface, so that the grinding surface becomes a smooth mirror without scratches. The polishing of metallographic samples is divided into rough polishing and fine polishing. The rough polishing fabric plays an important role in the polishing of metallographic samples. The friction between the fabric and the grinding surface makes the grinding surface bright. During the polishing process, the fiber gaps of the fabric can store and support the polishing powder, thereby producing a grinding effect. Generally, canvas is used for rough polishing fabrics, and 9μm diamond suspension polishing agent is used. Velvet or silk is used for fine polishing fabrics, and 3μm and 1μm diamond suspension polishing agents are used successively. During the polishing operation, the pressure applied to the sample should be balanced, and should be heavy first and then light. The polishing disc is set to 300r / min. In the early stage of polishing, the direction of the wear marks on the sample should be perpendicular to the direction of rotation of the polishing disc to facilitate faster removal of the wear marks. In the later stage of polishing, the sample needs to be rotated slowly, which is conducive to obtaining a bright and smooth grinding surface, and at the same time can prevent inclusions and hard phases from producing tailing phenomena.
[0048] Then, prepare the corrosive agent, which needs to be freshly prepared. Add a certain amount of nitric acid, hydrochloric acid and phosphoric acid into deionized water to prepare a corrosive solution, wherein the volume fractions of nitric acid, hydrochloric acid and phosphoric acid are 4% to 5%, 1% to 2% and 1.5% to 2.5% respectively, and the balance is deionized water. When preparing, first add nitric acid, then add hydrochloric acid, and finally add phosphoric acid and deionized water, and stir evenly with a glass rod. The mass percentage concentration of the nitric acid is 65 to 69%, the mass percentage concentration of the hydrochloric acid is 36 to 38%, and the mass percentage concentration of the phosphoric acid is 83 to 90%.
[0049] Specifically, the corrosive agent needs to be freshly prepared. If the corrosive agent is left for a long time after preparation, the components in the corrosive agent will volatilize and the concentration of the corrosive agent will decrease, resulting in poor subsequent corrosion effect, which will cause problems for the subsequent grain boundary appearance of the neodymium magnet alloy metallographic structure.
[0050] Next, the sample is corroded, and the petri dish with the corrosive solution is placed in a constant temperature water bath at 22-28°C. The metallographic sample processed in the above steps is placed in the petri dish, immersed in the corrosive solution for 15-20 seconds. After the corrosion process is completed, the sample is taken out, rinsed with anhydrous ethanol, and then dried with cold air.
[0051] Finally, the metallographic structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy was observed under a scanning electron microscope and photographed and recorded.
[0052] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0053] Example 1
[0054] A method for detecting the core-shell structure of a Tb-diffused sintered NdFeB permanent magnet alloy, the process is as follows:
[0055] a. The Tb diffusion treated sintered NdFeB permanent magnet alloy sample was sequentially demagnetized, pre-cleaned, hot mounted, mechanically ground and mechanically polished, then rinsed with clean water and dried with cold air to obtain a metallographic sample.
[0056] The specific process of hot embedding is as follows: use HM1 phenolic resin for hot embedding, add resin powder to reach more than 1 / 3 of the volume of the medium-sized cavity mold of the embedding machine, set the embedding machine temperature to 170°C, heating time 800s, insulation time 200s, and cavity pressure 8000N.
[0057] Mechanical grinding includes coarse grinding and fine grinding. Coarse grinding is carried out on a 320-mesh belt grinder with a rotation speed of 800r / min. The abrasive particles fixed on the belt pass over the sample surface with high stress to remove the material in the form of grinding chips, leaving wear marks on the sample surface and forming a deformation damage layer with a certain depth, grinding off the edges and flash of the sample. The abrasive used for fine grinding is silicon carbide. Polish with 120-mesh, 320-mesh, 800-mesh, and 1200-mesh metallographic sandpaper in turn. Each time a layer of sandpaper is changed, the sample should be rotated 90 degrees and the wear marks of the previous layer should be completely removed. Before grinding, apply a layer of glycerin on the sandpaper in advance to prevent sand particles from embedding into the grinding surface of the sample.
[0058] Mechanical polishing includes rough polishing and fine polishing. For rough polishing, canvas is used with 9μm diamond suspension polishing agent. For fine polishing, velvet is used with 3μm and 1μm diamond suspension polishing agents. During the polishing operation, the pressure applied to the sample should be balanced, and should be heavy first and then light. The polishing disc is set to 300r / min. In the early stage of polishing, the direction of the wear marks on the sample should be perpendicular to the direction of rotation of the polishing disc to facilitate faster removal of the wear marks. In the later stage of polishing, the sample needs to be rotated slowly.
[0059] b. In a container, 4.5 mL of nitric acid, 1.5 mL of hydrochloric acid, 2 mL of phosphoric acid, and 92 mL of deionized water were added sequentially to obtain a metallographic etchant. The mass percentage concentration of nitric acid used was 65 to 69%, the mass percentage concentration of hydrochloric acid was 36 to 38%, and the mass percentage concentration of phosphoric acid was 83 to 90%.
[0060] c. Pour the metallographic etchant into a culture dish, place the culture dish in a constant temperature water bath at 25°C, immerse the metallographic sample obtained in step a into the metallographic etchant, and after etching for 18 seconds, rinse the sample with anhydrous ethanol and blow dry with cold air. Observe the metallographic structure of the sintered NdFeB permanent magnet alloy treated with Tb diffusion under a scanning electron microscope. The morphology after corrosion is as shown in Figure 2 shown.
[0061] Comparative Example 1
[0062] A method for detecting the core-shell structure of a Tb-diffused sintered NdFeB permanent magnet alloy, the process is as follows:
[0063] a. The Tb diffusion treated sintered NdFeB permanent magnet alloy sample was sequentially demagnetized, pre-cleaned, hot mounted, mechanically ground and mechanically polished, then rinsed with clean water and dried with cold air to obtain a metallographic sample.
[0064] The specific process of hot embedding is as follows: use HM1 phenolic resin for hot embedding, add resin powder to reach more than 1 / 3 of the volume of the medium-sized cavity mold of the embedding machine, set the embedding machine temperature to 170°C, heating time 800s, insulation time 200s, and cavity pressure 8000N.
[0065] Mechanical grinding includes coarse grinding and fine grinding. Coarse grinding is carried out on a 320-mesh belt grinder with a rotation speed of 800r / min. The abrasive particles fixed on the belt pass over the sample surface with high stress to remove the material in the form of grinding chips, leaving wear marks on the sample surface and forming a deformation damage layer with a certain depth, grinding off the edges and flash of the sample. The abrasive used for fine grinding is silicon carbide. Polish with 120-mesh, 320-mesh, 800-mesh, and 1200-mesh metallographic sandpaper in turn. Each time a layer of sandpaper is changed, the sample should be rotated 90 degrees and the wear marks of the previous layer should be completely removed. Before grinding, apply a layer of glycerin on the sandpaper in advance to prevent sand particles from embedding into the grinding surface of the sample.
[0066] Mechanical polishing includes rough polishing and fine polishing. For rough polishing, canvas is used with 9μm diamond suspension polishing agent. For fine polishing, velvet is used with 3μm and 1μm diamond suspension polishing agents. During the polishing operation, the pressure applied to the sample should be balanced, and should be heavy first and then light. The polishing disc is set to 300r / min. In the early stage of polishing, the direction of the wear marks on the sample should be perpendicular to the direction of rotation of the polishing disc to facilitate faster removal of the wear marks. In the later stage of polishing, the sample needs to be rotated slowly.
[0067] b was added nitric acid 5.5mL, hydrochloric acid 2.5mL, deionized water 92mL were mixed in a container to obtain a metallographic etchant, the mass percentage concentration of nitric acid and hydrochloric acid used was the same as in Example 1;
[0068] c. Pour the metallographic etchant into a culture dish, place the culture dish in a constant temperature water bath at 25°C, immerse the metallographic sample obtained in step a into the metallographic etchant, and after etching for 18 seconds, rinse the sample with anhydrous ethanol and blow dry it with cold air. Observe the metallographic structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy under a scanning electron microscope. The morphology after corrosion is as shown in Figure 3 shown.
[0069] Comparative Example 2
[0070] A method for detecting the core-shell structure of a Tb-diffused sintered NdFeB permanent magnet alloy, the process is as follows:
[0071] a. The Tb diffusion treated sintered NdFeB permanent magnet alloy sample was sequentially demagnetized, pre-cleaned, hot mounted, mechanically ground and mechanically polished, then rinsed with clean water and dried with cold air to obtain a metallographic sample.
[0072] The specific process of hot embedding is as follows: use HM1 phenolic resin for hot embedding, add resin powder to reach more than 1 / 3 of the volume of the medium-sized cavity mold of the embedding machine, set the embedding machine temperature to 170°C, heating time 800s, insulation time 200s, and cavity pressure 8000N.
[0073] Mechanical grinding includes coarse grinding and fine grinding. Coarse grinding is carried out on a 320-mesh belt grinder with a rotation speed of 800r / min. The abrasive particles fixed on the belt pass over the sample surface with high stress to remove the material in the form of grinding chips, leaving wear marks on the sample surface and forming a deformation damage layer with a certain depth, grinding off the edges and flash of the sample. The abrasive used for fine grinding is silicon carbide. Polish with 120-mesh, 320-mesh, 800-mesh, and 1200-mesh metallographic sandpaper in turn. Each time a layer of sandpaper is changed, the sample should be rotated 90 degrees and the wear marks of the previous layer should be completely removed. Before grinding, apply a layer of glycerin on the sandpaper in advance to prevent sand particles from embedding into the grinding surface of the sample.
[0074] Mechanical polishing includes rough polishing and fine polishing. For rough polishing, canvas is used with 9μm diamond suspension polishing agent. For fine polishing, velvet is used with 3μm and 1μm diamond suspension polishing agents. During the polishing operation, the pressure applied to the sample should be balanced, and should be heavy first and then light. The polishing disc is set to 300r / min. In the early stage of polishing, the direction of the wear marks on the sample should be perpendicular to the direction of rotation of the polishing disc to facilitate faster removal of the wear marks. In the later stage of polishing, the sample needs to be rotated slowly.
[0075] b. 5.5mL of nitric acid, 2.5mL of phosphoric acid and 92mL of deionized water were added sequentially to the container to obtain a metallographic etchant, the mass percentage concentration of nitric acid and hydrochloric acid used was the same as in Example 1;
[0076] c. Pour the metallographic etchant into a culture dish, place the culture dish in a constant temperature water bath at 25°C, immerse the metallographic sample obtained in step a into the metallographic etchant, and after etching for 18 seconds, rinse the sample with anhydrous ethanol and blow dry it with cold air. Observe the metallographic structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy under a scanning electron microscope. The morphology after corrosion is as shown in Figure 4 shown.
[0077] Comparative Example 3
[0078] a. The Tb diffusion treated sintered NdFeB permanent magnet alloy sample was sequentially demagnetized, pre-cleaned, hot mounted, mechanically ground and mechanically polished, then rinsed with clean water and dried with cold air to obtain a metallographic sample.
[0079] The specific process of hot embedding is as follows: use HM1 phenolic resin for hot embedding, add resin powder to reach more than 1 / 3 of the volume of the medium-sized cavity mold of the embedding machine, set the embedding machine temperature to 170°C, heating time 800s, insulation time 200s, and cavity pressure 8000N.
[0080] Mechanical grinding includes coarse grinding and fine grinding. Coarse grinding is carried out on a 320-mesh belt grinder with a rotation speed of 800r / min. The abrasive particles fixed on the belt pass over the sample surface with high stress to remove the material in the form of grinding chips, leaving wear marks on the sample surface and forming a deformation damage layer with a certain depth, grinding off the edges and flash of the sample. The abrasive used for fine grinding is silicon carbide. Polish with 120-mesh, 320-mesh, 800-mesh, and 1200-mesh metallographic sandpaper in turn. Each time a layer of sandpaper is changed, the sample should be rotated 90 degrees and the wear marks of the previous layer should be completely removed. Before grinding, apply a layer of glycerin on the sandpaper in advance to prevent sand particles from embedding into the grinding surface of the sample.
[0081] Mechanical polishing includes rough polishing and fine polishing. For rough polishing, canvas is used with 9μm diamond suspension polishing agent. For fine polishing, velvet is used with 3μm and 1μm diamond suspension polishing agents. During the polishing operation, the pressure applied to the sample should be balanced, and should be heavy first and then light. The polishing disc is set to 300r / min. In the early stage of polishing, the direction of the wear marks on the sample should be perpendicular to the direction of rotation of the polishing disc to facilitate faster removal of the wear marks. In the later stage of polishing, the sample needs to be rotated slowly.
[0082] b. 3.5mL of hydrochloric acid, 4.5mL of phosphoric acid and 92mL of deionized water were sequentially added to the container to obtain a metallographic etchant, the mass percentage concentration of nitric acid and hydrochloric acid used was the same as in Example 1;
[0083] c. Pour the metallographic etchant into a culture dish, place the culture dish in a constant temperature water bath at 25°C, immerse the metallographic sample obtained in step a into the metallographic etchant, and after etching for 18 seconds, rinse the sample with anhydrous ethanol and blow dry it with cold air. Observe the metallographic structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy under a scanning electron microscope. The morphology after corrosion is as shown in Figure 5 shown.
[0084] The composition of each 100 mL of the etchant, the corrosion time and the corrosion temperature in each embodiment and comparative example are shown in the following table.
[0085] <![CDATA[HNO 3 ]]> HCl <![CDATA[H 3 AFTER 4 ]]> <![CDATA[H 2 The]]> time temperature Example 1 4.5mL 1.5mL 2mL 92mL 18s 25℃ Comparative Example 1 5.5mL 2.5mL / 92mL 18s 25℃ Comparative Example 2 5.5mL / 2.5mL 92mL 18s 25℃ Comparative Example 3 / 3.5mL 4.5mL 92mL 18s 25℃
[0086] from Figure 2 It can be seen that the metallographic grain boundaries of the Tb diffusion treated sintered NdFeB permanent magnet alloy treated by the metallographic corrosion method of the present application are clearly displayed, and the (Nd, Tb)2Fe14B shell structure formed by the diffusion process can be clearly observed; Figure 3 It can be seen that only obvious grain boundaries can be observed in the Tb diffusion treated sintered NdFeB permanent magnet alloy treated by the metallographic corrosion method of Comparative Example 1, but no shell structure can be observed; Figure 4 , 5 It can be seen that only some fuzzy grain boundaries can be observed in the Tb diffusion treated sintered NdFeB permanent magnet alloys treated by the metallographic etching methods of Comparative Examples 2 and 3, and no shell structure can be observed;
[0087] Therefore, the grain boundaries and grains of the Tb diffusion treated sintered NdFeB permanent magnet alloy treated by the metallographic corrosion method of the present application are clearly displayed, and an obvious shell structure can be observed. In addition, the corrosion time is short, and the observation is efficient and quick.
[0088] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0089] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0090] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for detecting the core-shell structure of Tb-diffused sintered NdFeB permanent magnet alloy. It is characterized in that The method comprises: Pre-treating the alloy to be tested to remove the magnetism of the alloy to be tested and clean the alloy to be tested, thereby obtaining a pre-treated sample; Hot mounting the pretreated alloy to obtain a mounted sample; Grinding and polishing the inlaid sample to obtain a bright surface sample; preparing a corrosive agent, wherein the corrosive agent comprises a nitric acid solution, a hydrochloric acid solution and a phosphoric acid solution; The bright surface sample is corroded by the corrosive agent and then tested.
2. The method for detecting the core-shell structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy according to claim 1, It is characterized in that Measured by volume percentage, the components of the corrosive agent include: 4% to 5% nitric acid solution, 1% to 2% hydrochloric acid solution and 1.5% to 2.5% phosphoric acid solution, and the balance is water.
3. The method for detecting the core-shell structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy according to claim 1 or 2, It is characterized in that The mass percentage concentration of the nitric acid solution is 65% to 69%; and / or The mass percentage concentration of the hydrochloric acid solution is 36% to 38%; and / or The mass percentage concentration of the phosphoric acid solution is 83% to 90%.
4. The method for detecting the core-shell structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy according to claim 1 or 2, It is characterized in that The corrosion temperature is 22°C to 28°C.
5. The method for detecting the core-shell structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy according to claim 1 or 2, It is characterized in that The corrosion time is 15 to 20 seconds.
6. The method for detecting the core-shell structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy according to claim 1, It is characterized in that In terms of molar fraction, the composition of the alloy to be tested includes: 29% to 32.5% neodymium; and / or In terms of molar fraction, the composition of the alloy to be tested includes: 63.95% to 68.65% iron; and / or In terms of molar fraction, the composition of the alloy to be tested includes: 1.1% to 1.2% boron; and / or In terms of molar fraction, the composition of the alloy to be tested includes: 0.6% to 8% dysprosium; and / or In terms of molar fraction, the composition of the alloy to be tested includes: 0.3% to 0.5% niobium; and / or In terms of mole fraction, the composition of the alloy to be tested includes: 0.3% to 0.5% aluminum; In terms of molar fraction, the composition of the alloy to be tested includes: 0.05% to 0.15% copper; and / or Calculated by mole fraction, the components of the alloy to be tested include: Tb content is 1% to 2%.
7. The method for detecting the core-shell structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy according to claim 1, It is characterized in that The pretreatment includes demagnetization and cleaning.
8. The method for detecting the core-shell structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy according to claim 1, It is characterized in that The hot mounting is performed using HM1 phenolic resin.
9. The method for detecting the core-shell structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy according to claim 1, It is characterized in that The grinding includes coarse grinding and fine grinding.
10. The method for detecting the core-shell structure of the Tb diffusion treated sintered NdFeB permanent magnet alloy according to claim 1, It is characterized in that The polishing sandpaper is at least 800 grit.
Citation Information
Patent Citations
Neodymium iron boron metallographic analysis sample preparation method
CN102928275A
Pure nickel chemical polishing etching solution and application method
CN103822817A
Treating method for improving performance of sintered NdFeB (neodymium iron boron) materials
CN104681225A
U-yZr alloy grain size detection method
CN106706640A
Preparation method of neodymium iron boron metallographic phase