Varnish color difference detection method
By using a combination technology of isolation film and test substrate in the automotive coating process, the problem of inaccurate chromatic aberration evaluation of varnish is solved, more accurate chromatic aberration detection is achieved, reducing the rework rate and improving the coating efficiency and quality.
Patent Information
- Application Number
- CN202410907491.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
AI Technical Summary
In automotive coating process, inaccurate evaluation of varnish color difference leads to batch color difference rework after body spraying, affecting the coating quality and efficiency.
A substrate equipped with an isolation film is used to spray the modulated varnish and dry it, and the isolation film is peeled off to obtain a single-layer film of varnish, which is coated on the test substrate to detect the color difference value, eliminate external interference factors, and accurately evaluate the color difference of varnish.
By making the varnish into a single-layer film to detect its chromatic aberration, the accuracy of chromatic aberration evaluation is improved, the rework rate is reduced, and the coating efficiency and quality are improved.
Smart Images

Figure BDA0004932563790000061 
Figure BDA0004932563790000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of color difference detection, and in particular to a method for detecting color difference of varnish. Background Art
[0002] Color difference control is an important item in the quality of automobile appearance. In the automobile painting process, color difference is affected by the color of the clearcoat layer in addition to the base material, midcoat and color paint. Except for colored clearcoats, most clearcoats are transparent and almost colorless, so they are often ignored. When changing batches of clearcoats at the painting site, individual colors often have color difference deviations.
[0003] At most painting sites, when changing batches of clearcoat paint, the clearcoat paint is directly added to the clearcoat paint delivery system for spraying. By adding new batches of paint after natural consumption, the amount of new batches of paint in the main tank increases from small to large, ensuring that the color difference will not deviate drastically. However, this also causes a delay in color difference deviation, leading to inaccurate evaluation of color difference performance on site, which in turn leads to batch color difference repair after the car body is sprayed, affecting the quality and efficiency of painting. Summary of the invention
[0004] The main purpose of the present invention is to provide a method for detecting varnish color difference, aiming to solve the problem of inaccurate varnish color difference assessment in the prior art.
[0005] To achieve the above object, the present invention provides a method for detecting color difference of varnish, which is characterized by comprising the following steps:
[0006] S10. A substrate having an isolation film is provided, wherein the isolation film is formed of a soluble substance such as KBr or PVA;
[0007] S20. The varnish is sprayed on the isolation film of the substrate to obtain a varnish experimental film plate;
[0008] S30. After the varnish test film is dried, the varnish-coated isolation film is peeled off to obtain a varnish film;
[0009] S40. Immersing the varnish film in a working medium, removing the isolation film, and obtaining a varnish monolayer film;
[0010] S50. The varnish monolayer film is coated on the test substrate to obtain a varnish test plate;
[0011] S60. Detect the color difference values of the test substrate and the varnish test plate respectively, that is, the color difference of the varnish.
[0012] In one embodiment, step S10 includes the following steps:
[0013] A tinplate plate is taken as a substrate, and an isolation film is laid and fixed on the tinplate plate to obtain a substrate provided with an isolation film.
[0014] In one embodiment, in step S10, the thickness of the varnish single-layer film in the varnish experimental film plate is 55-60 μm.
[0015] In one embodiment, in step S20, the prepared varnish includes a varnish base, a curing agent and an auxiliary agent.
[0016] In one embodiment, the auxiliary agent includes at least one of butyl acetate and ethyl propionate.
[0017] In one embodiment, the varnish comprises a one-component varnish or a two-component varnish.
[0018] In one embodiment, in step S30, the drying temperature is 140-150° C.; and / or,
[0019] In step S30, the drying time is 20 to 30 minutes.
[0020] In one embodiment, in step S40, the working medium can dissolve the isolation film but cannot dissolve the varnish single-layer film, and the working medium includes water.
[0021] In one embodiment, in step S50, the test substrate includes a standard plain white board or a standard plain black board.
[0022] In one embodiment, in step S60, the varnish color difference value includes an L value, an a value, and a b value.
[0023] The technical solution of the present invention is to prepare a varnish test board by making the varnish into a single-layer film and then covering it on a test substrate to detect the color difference between the test substrate and the varnish test board. Such a setting can eliminate external interference factors and confirm the color difference caused by the varnish single-layer film based on the color difference between the test substrate before lamination and the varnish test board after lamination to confirm the color difference of the varnish. DETAILED DESCRIPTION
[0024] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them.
[0025] It should be noted that, in the embodiments, those without specifying specific conditions are carried out according to normal conditions or conditions recommended by the manufacturer. Those without specifying the manufacturer of reagents or instruments used are conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, and "A and / or B" is taken as an example, including schemes A, B, or A and B that meet the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of the technical schemes is contradictory or cannot be achieved, it should be considered that the combination of such technical schemes does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work, all belong to the scope of protection of the present invention.
[0026] At present, in most painting sites, when changing batches of clearcoat paint, the clearcoat paint is directly added to the clearcoat paint delivery system for spraying. By adding new batches of paint after natural consumption, the amount of new batches of paint in the main tank increases from small to large, ensuring that the color difference will not deviate drastically. However, it also causes a delay in color difference deviation, leading to inaccurate evaluation of color difference performance on site, which in turn leads to batch color difference repair after the car body is sprayed, affecting the painting quality and efficiency.
[0027] In view of this, the present invention proposes a method for detecting color difference of varnish, which is characterized in that it includes the following steps: S10. Providing a substrate provided with an isolation film; S20. Spraying the modulated varnish on the isolation film of the substrate to obtain a varnish experimental film plate; S30. After drying the varnish experimental film plate, peeling off the isolation film coated with the varnish to obtain a varnish film; S40. Soaking the varnish film in a working medium, removing the isolation film, and obtaining a varnish single-layer film; S50. Covering the varnish single-layer film on a test substrate to obtain a varnish test board; S60. Respectively detecting the color difference values of the test substrate and the varnish test board, that is, the color difference of the varnish.
[0028] The technical solution of the present invention is to prepare a varnish test board by making the varnish into a single-layer film and then covering it on a test substrate to detect the color difference between the test substrate and the varnish test board. Such a setting can eliminate external interference factors and confirm the color difference caused by the varnish single-layer film based on the color difference between the test substrate before lamination and the varnish test board after lamination to confirm the color difference of the varnish.
[0029] It should be noted that the isolation membrane can be a KBr membrane or a PVA membrane, which is not limited here, as long as the varnish monolayer film can be separated from the substrate; correspondingly, the working medium can dissolve the isolation membrane but not the varnish, and the specific components are not limited here; the auxiliary agent can be a diluent, a leveling agent, or a co-solvent, and the specific components are not limited, as long as it can; the spraying method can be manual spraying with a spray gun, or it can be robot spraying, which is not limited here.
[0030] In one embodiment, step S10 includes the following steps: taking a tinplate plate as a substrate, laying and fixing an isolation film on the tinplate plate, and obtaining a substrate provided with an isolation film.
[0031] The technical solution of the present invention adopts a tinplate as a substrate, and its surface is plated with a layer of tin, so that it has a smooth surface. Using a tinplate as a substrate can improve the flatness of the varnish film sprayed on the substrate isolation film, so that the thickness of the varnish film is consistent everywhere, reducing the error caused by uneven thickness when detecting color difference; by laying and fixing the isolation film on the tinplate plate, the spraying stability and uniformity are guaranteed, and the flatness of the varnish film is further improved. The fixing method can be bonding or magnetic attraction, and the specific fixing method is not limited here. In some embodiments of the present invention, the size of the isolation film is smaller than the size of the substrate.
[0032] In one embodiment, in step S10, the thickness of the varnish single-layer film in the varnish experimental film plate is 55-60 μm.
[0033] The technical solution of the present invention adjusts the thickness of the varnish single-layer film to 55-60μm, and the color difference value is most significant within this thickness range; if the thickness is less than 55μm, the color difference value is too small, the color difference phenomenon is not significant, and the color difference of the varnish cannot be accurately measured; if the thickness is greater than 60μm, the color difference value is too large, and the qualified color difference range of the varnish is difficult to define.
[0034] In one embodiment, in step S20, the prepared varnish includes a varnish base, a curing agent and an auxiliary agent.
[0035] The technical solution of the present invention accelerates the curing of the modulated varnish by adding a curing agent, reduces the time required for high-temperature curing, reduces costs and improves detection efficiency; and adjusts the viscosity of the modulated varnish by adding an auxiliary agent, thereby improving the fluidity and film-forming property of the modulated varnish.
[0036] In one embodiment, the auxiliary agent includes at least one of butyl acetate and ethyl propionate.
[0037] The technical solution of the present invention uses at least one of butyl acetate and ethyl propionate as an auxiliary agent to change the viscosity of the prepared varnish and improve the fluidity and film-forming property of the prepared varnish. In some embodiments of the present invention, the viscosity of the prepared varnish is adjusted to 28-32s by adding an auxiliary agent.
[0038] In one embodiment, the varnish comprises a one-component varnish or a two-component varnish; and / or, the varnish comprises a solvent-based varnish or a water-based varnish.
[0039] The technical solution of the present invention adopts a one-component varnish or a two-component varnish. The one-component varnish simplifies the construction process and reduces the complexity of operation due to its ready-to-use convenience, and is particularly suitable for occasions with high requirements for construction efficiency. The two-component varnish can provide better physical properties after curing, such as higher hardness, stronger chemical resistance and wear resistance, by mixing the curing agent on site, and is suitable for surface treatment requiring long-term durability and high protection. The flexible selection of different varnishes achieves wide adaptability to different application scenarios.
[0040] In one embodiment, in step S30, the drying temperature is 140-150° C.; and / or, in step S30, the drying time is 20-30 min.
[0041] The technical solution of the present invention adjusts the drying temperature to 140-150°C, thereby ensuring that the coating is fully cured and the water is effectively evaporated, while avoiding excessive energy consumption and possible damage to the coating; by adjusting the drying time to 20-30 minutes, this time period ensures that the coating has enough time to complete the transition from a wet film to a dry film, thereby avoiding residual solvents in the coating due to too short a time, and preventing aging or performance degradation of the coating due to long-term drying.
[0042] In one embodiment, in step S40, the working medium can dissolve the isolation film but cannot dissolve the varnish single-layer film, and the working medium includes water.
[0043] The technical solution of the present invention uses water as the working medium to separate the isolation film from the varnish film while retaining the varnish film. It has low cost, simple process, is not easy to introduce impurities, and does not affect the accuracy of varnish color difference detection.
[0044] In one embodiment, in step S50, the test substrate includes a standard plain white board or a standard plain black board.
[0045] The technical solution of the present invention can detect the color difference effect of varnish on different color bases by adopting a standard plain white board or a standard plain black board as a test substrate, thereby expanding the application scope of the detection method; specifically, in one embodiment of the present invention, a standard plain white board and a standard plain black board are respectively used as test substrates to perform two color difference detections to detect the color difference effect of varnish from two base colors of black and white.
[0046] In one embodiment, in step S60, the varnish color difference value includes an L value, an a value, and a b value.
[0047] It should be noted that the L value represents the brightness value, the a value represents the red and green value, a positive value represents red, and a negative value represents green, and the b value represents the yellow and blue value, a positive value represents yellow, and a negative value represents blue.
[0048] The technical solution of the present invention can detect the color difference value from three directions of brightness and two hues by detecting the L value, the a value and the b value, thereby improving the accuracy of detecting the color difference value.
[0049] Specifically, in one embodiment of the present invention, by detecting the difference between the L value, a value and b value of the test substrate and the varnish test plate, the color difference values are obtained, which are dL, da and db respectively.
[0050] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0051] Example 1
[0052] This embodiment provides a method for detecting color difference of varnish, comprising the following steps:
[0053] 1. After the new batch of varnish arrives, take 1L of varnish coating and adjust the viscosity to 30s with additives, take 340mL of the prepared varnish, add 100mL of curing agent, stir evenly and add to the spray gun;
[0054] 2. Place a 300mm*40mm tinplate on the test bench, lay a 100mm*200mm water-soluble temperature-resistant isolation film on the tinplate, and use tape or magnetic strips to fix the isolation film on the tinplate. Spray the varnish twice to form a varnish experimental film plate. [The spraying flow rate and speed are set through verification to ensure that the single-layer film thickness of the varnish is between 55-60μm (the film thickness will affect the hue)];
[0055] 3.Put the varnish test film into the oven for drying at 145℃*25min;
[0056] 4. After drying, remove the isolation film together with the varnish on it to obtain a varnish film. Soak the varnish film in the working medium, remove the isolation film, and form a varnish single-layer film;
[0057] 5. Cover the varnish monolayer film on the test standard plain white test plate (measure the color difference of the plain white plate when using it, and if the deviation from the reference value is controlled within dL±0.2, da±0.1, db±0.1, the standard white plate can be used, otherwise it needs to be replaced), use BYK colorimeter and plain white color standard to measure the composite color difference dL1, da1, db1 of the monolayer film covered with varnish;
[0058] 6. Composite color difference of white board: dL1 range (-0.5, 0.2), da1 range (-0.2, 0.2) and db1 range (0, 0.4) are qualified; those exceeding are unqualified;
[0059] 7. Cover the varnish monolayer film on the test standard plain black test board (measure the color difference of the plain blackboard when using it. If the deviation from the reference value is controlled within dL±0.2, da±0.1, db±0.1, the standard blackboard can be used, otherwise it needs to be replaced). Use BYK colorimeter and plain white color standard to measure the composite color difference of the varnish monolayer film;
[0060] 8. The composite color difference of blackboard dL2 range is (-0.5, 0.5), da2 range is (-0.2, 0.2) and db2 range is (-0.4, 0.4) within which it is qualified; if it exceeds, it is unqualified;
[0061] 9. If the two sets of color difference deviations are within the range, the varnish color difference is judged to be qualified and the batch of varnish can be used; otherwise, the varnish color difference is judged to be unqualified, and then the coating is judged to be unqualified, and the batch of varnish is not allowed to be used.
[0062] According to the detection method in Example 1, a varnish standard product was used to prepare a modulated varnish, and the color difference of the modulated varnish was detected. The detection results are shown in Table 1.
[0063] Table 1 Color difference detection results of the prepared varnish in Example 1
[0064]
[0065]
[0066] As shown in Table 1, the detection pass rate is 100%.
[0067] Example 2
[0068] This embodiment provides a method for detecting color difference of varnish, and its steps are similar to those of embodiment 1, except that step 1 includes the following steps:
[0069] 1. After the new batch of varnish arrives, take 1L of varnish paint and adjust the viscosity to 32s with additives, take 340mL of the prepared varnish, add 10mL of isobutyl alcohol and 90mL of curing agent, stir evenly and add to the spray gun.
[0070] According to the detection method in Example 2, a varnish standard was added with white acrylic pigment to prepare a modulated varnish, and the color difference of the modulated varnish was detected. The detection results are shown in Table 2.
[0071] Table 2 Color difference detection results of the prepared varnish in Example 2
[0072] Serial number dL1 da1 db1 dL2 da2 db2 determination 1 0.2 0.1 0.1 0.6 -0.1 -0.1 Failure 2 0.3 0 -0.1 0.4 0 0.1 qualified 3 0 -0.1 0 0.7 0 -0.1 Failure 4 0.1 0.1 0.1 0.8 -0.1 0 Failure 5 0.2 0 -0.1 0.3 -0.1 -0.1 qualified 6 0.1 0.1 -0.1 0.6 0.1 0 Failure 7 0 0 0 0.7 0.1 0.1 Failure 8 0.1 0.1 0.1 0.7 0.1 0.1 Failure 9 0 -0.1 -0.1 0.8 0 0 Failure 10 0.1 -0.1 0 0.4 -0.1 -0.1 qualified
[0073] As shown in Table 2, the qualified rate is 30%, and those that fail the color difference test are all the modulated varnishes with high black base color difference brightness values.
[0074] Example 3
[0075] This embodiment provides a method for detecting color difference of varnish, and its steps are similar to those of embodiment 1, except that step 1 includes the following steps:
[0076] 1. After the new batch of varnish arrives, take 1L of paint and add additives to adjust the viscosity to 30s, take 340m of the prepared varnish, add 2mL of naphtha and 98mL of curing agent, stir evenly and add to the spray gun.
[0077] According to the detection method in Example 3, a varnish standard was added with black acrylic pigment to prepare a modulated varnish, and the color difference of the modulated varnish was detected. The detection results are shown in Table 3.
[0078] Table 3 Color difference detection results of the prepared varnish in Example 3
[0079] Serial number dL1 da1 db1 dL2 da2 db2 determination 1 -0.5 0.1 0 -0.1 -0.1 0.1 Failure 2 -0.8 0 -0.1 -0.1 0 0.1 Failure 3 -0.7 0 0.1 -0.1 0.1 0 Failure 4 -0.6 0.1 0 0 -0.1 0.1 Failure 5 -1.0 0 0 0 -0.1 -0.1 Failure 6 -0.4 0.1 0.1 -0.1 0.1 0 qualified 7 -0.8 -0.1 0.1 0 0.1 0 Failure 8 -0.3 0 0 0.1 0.1 0.1 qualified 9 -0.9 0.1 -0.1 0 0 -0.1 Failure 10 -0.7 0.1 0 0.1 0 0.1 Failure
[0080] As shown in Table 3, the qualified rate is 20%, and those that fail the color difference test are all the modulated varnishes with low black base color difference brightness values.
[0081] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for detecting color difference of varnish, characterized in that: The following steps are involved: S10. Providing a substrate provided with an isolation film; S20. The varnish is sprayed on the isolation film of the substrate to obtain a varnish experimental film plate; S30. After the varnish test film is dried, the varnish-coated isolation film is peeled off to obtain a varnish film; S40. Immersing the varnish film in a working medium, removing the isolation film, and obtaining a varnish monolayer film; S50. The varnish monolayer film is coated on the test substrate to obtain a varnish test plate; S60. Detect the color difference values of the test substrate and the varnish test plate respectively, that is, the color difference of the varnish.
2. The method for detecting color difference of varnish according to claim 1, characterized in that: Step S10 includes the following steps: A tinplate plate is taken as a substrate, and an isolation film is laid and fixed on the tinplate plate to obtain a substrate provided with an isolation film.
3. The method for detecting color difference of varnish according to claim 1, characterized in that: In step S10, the thickness of the varnish single-layer film in the varnish experimental film plate is 55-60 μm.
4. The method for detecting color difference of varnish according to claim 1, characterized in that: In step S20, the varnish is prepared to include varnish base, curing agent and auxiliary agent.
5. The method for detecting color difference of varnish according to claim 4, characterized in that: The auxiliary agent includes at least one of butyl acetate and ethyl propionate.
6. The method for detecting color difference of varnish according to claim 4, characterized in that: The varnish base paint includes a one-component varnish or a two-component varnish.
7. The method for detecting color difference of varnish according to claim 1, characterized in that: In step S30, the drying temperature is 140-150° C.; and / or, In step S30, the drying time is 20 to 30 minutes.
8. The method for detecting color difference of varnish according to claim 1, characterized in that: In step S40, the working medium can dissolve the isolation film but cannot dissolve the varnish single-layer film, and the working medium includes water.
9. The method for detecting color difference of varnish according to claim 1, characterized in that: In step S50, the test substrate includes a standard plain white board or a standard plain black board.
10. The method for detecting color difference of varnish according to claim 1, characterized in that: In step S60, the varnish color difference value includes L value, a value and b value.