Epoxy resin and polyimide mixed matrix semi-cured magnetic film and preparation and application thereof
By coating the surface of magnetic powder with a SiO2 insulating layer and dispersing it in a mixed matrix of epoxy resin and polyimide, a peelable semi-cured magnetic film is prepared, which solves the problems of high eddy current loss and complex integration process at high frequencies, and realizes efficient and low-cost integration of inductors and improved electromagnetic performance.
Patent Information
- Application Number
- CN202411188321.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-01
Smart Images

Figure CN118888321A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of integrated magnetic devices of printed circuit boards, in particular to a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide, and a preparation method and application thereof. Background Art
[0002] With the advent of the post-Moore's Law era, the available volume of integrated inductors used in power management, high-frequency circuits, and power amplifiers needs to be further reduced. How to reduce the volume of integrated inductors while enhancing their electromagnetic performance has become one of the key technologies for the miniaturization of electronic products. Adding magnetic core materials to inductors can greatly improve the performance of inductors. Ideal magnetic core materials must meet physical properties such as high magnetic permeability, high resistivity, low coercivity, and high saturation flux density to improve the inductance of air-core inductors and reduce eddy current losses and hysteresis losses caused by adding magnetic cores. At the same time, their integration process should be compatible with the preparation process of inductors and have low manufacturing costs. Metal-based soft magnetic materials are a type of material with excellent soft magnetic properties. They have high saturation magnetization, low coercivity, low hysteresis losses, and lower preparation costs than other soft magnetic materials. However, due to the direct electrical contact between adjacent metal powder particles, their resistivity is low, so the eddy current loss is high in high-frequency applications, and it is very complicated to press powder particles into magnetic cores for integrated high-frequency magnetic devices. Therefore, there is an urgent need to develop a magnetic core material with low eddy current loss at high frequency, an integration process that is compatible with the printed circuit board manufacturing process, and a low manufacturing cost. Summary of the invention
[0003] In view of the status and shortcomings of the prior art, the present invention provides a method for preparing a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide. The method forms a SiO2 insulating coating layer on the surface of magnetic powder by using a silane coupling agent to improve its resistivity and reduce eddy current loss under high frequency. The coated magnetic powder is then dispersed in a mixed matrix of epoxy resin and polyimide, an epoxy resin curing agent and a curing accelerator are added, and the film is coated on a PET film to prepare a semi-cured composite magnetic film that can be peeled off and hot-pressed and integrated, providing a simple and efficient solution for the integrated packaging of high-frequency power inductors.
[0004] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0005] A method for preparing a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide comprises the following steps:
[0006] Step 1: SiO2 insulation coating of raw magnetic powder
[0007] (1.1) Ultrasonic cleaning of 30-50 g of magnetic powder with anhydrous ethanol mixed with deionized water, filtration, and drying in a 60°C forced air oven for 4-5 h;
[0008] (1.2) Dispersing 30-50 g of the dried magnetic powder into 260-425 ml of anhydrous ethanol and 50-75 ml of deionized water, adding 1.5-2.5 ml of a silane coupling agent dropwise, and mechanically stirring for 1-2 hours to obtain a magnetic powder mixture;
[0009] (1.3) Add 2.7-4.5 ml of tetraethoxysilane to the magnetic powder mixture in step (1.2), adjust the pH of the mixture to 10-11 with aqueous ammonia, and then mechanically stir for 1-2 hours in a 40° C. water bath to obtain a suspension;
[0010] (1.4) After the suspension in step (1.3) is filtered, the coated magnetic powder is washed with anhydrous ethanol until the pH of the filtrate is 7, and then dried in a forced air oven at 60°C for 4 to 6 hours;
[0011] Step 2: Preparation of semi-cured magnetic film with epoxy resin and polyimide mixed matrix
[0012] (2.1) Add 30-50 g of the SiO2-insulated magnetic powder obtained in step 1 to a mixture of 10 g of epoxy resin and polyimide stock solution, and heat and dry out the solvent while mechanically stirring in a fume hood, stirring for 2 h at a stirring rate of 450-600 rpm to obtain a mixture;
[0013] (2.2) Add 0.17-0.25 g of epoxy resin curing agent and 0.003-0.01 g of epoxy resin curing accelerator to the mixture of step (2.1), continue heating and mechanical stirring for 2-3 hours, and obtain a uniformly mixed magnetic slurry;
[0014] (2.3) The magnetic slurry mixed evenly in step (2.2) is coated on a PET film, placed in a 120-140° C. forced air oven, and semi-cured for 10-15 minutes to obtain a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide.
[0015] As a preferred embodiment, the magnetic powder in step (1.1) is one or more of Fe-Si polycrystalline magnetic powder, Fe-Cr-Si amorphous magnetic powder, and Fe-Ni powder, and the average particle size of the magnetic powder is 2 to 10 μm.
[0016] As a preferred embodiment, the silane coupling agent in step (1.2) is selected from methyltriethoxysilane, γ-aminopropyltrimethoxysilane and γ-aminopropyltriethoxysilane.
[0017] As a preferred embodiment, the epoxy resin in step (2.1) is bisphenol A epoxy resin, and the polyimide stock solution is a thermoplastic polyimide liquid with N,N-dimethylacetamide as solvent and a polyimide mass ratio of 20%.
[0018] As a preferred embodiment, the mass ratio of epoxy resin to polyimide in step (2.1) is 1:1 to 10:1.
[0019] As a preferred embodiment, the epoxy resin curing agent in step (2.2) is a latent epoxy resin curing agent, preferably one of dicyandiamide, diaminodiphenyl sulfone, aluminum acetylacetonate, and boron trinitride.
[0020] As a preferred embodiment, the epoxy resin curing accelerator in step (2.2) is an imidazole accelerator.
[0021] The second object of the present invention is to provide a semi-cured magnetic film with a mixed matrix of epoxy resin and polyimide, which is obtained according to any one of the above-mentioned preparation methods.
[0022] The third object of the present invention is to provide an application of a semi-cured magnetic film with a mixed matrix of epoxy resin and polyimide: the prepared semi-cured magnetic film with a mixed matrix of epoxy resin and polyimide is peeled off from the PET film, placed on the inductor or substrate to be integrated, and then placed in a hot press, the pressure is set to 1MPa, the temperature is increased to 90°C at a heating rate of 5°C / min, hot pressed for 30 minutes, then the temperature is increased to 170°C at a heating rate of 5°C / min and hot pressed for 20 minutes, and cooled to room temperature at room temperature and pressure to complete the curing and integration of the semi-cured composite magnetic film.
[0023] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in:
[0024] (1) A layer of SiO2 insulating layer is coated on the surface of the magnetic powder by the sol-gel method, which increases the resistivity of the magnetic powder, reduces the saturation magnetization intensity and magnetic permeability of the magnetic powder, and significantly improves the magnetic loss at high frequencies.
[0025] (2) The coated magnetic powder was dispersed in a mixed matrix of epoxy resin and polyimide to prepare a semi-cured composite magnetic film. Compared with the pure epoxy resin matrix, the mixed matrix with the addition of polyimide solved the problem of difficulty in removing the solvent and forming a film during the preparation of the semi-cured magnetic film, which greatly improved the success rate of magnetic film preparation.
[0026] (3) The semi-cured composite magnetic film is easy to integrate. When used, it only needs to be placed on the required device and hot-pressed in a hot press to complete the curing and integration. The thermal performance test of the cured magnetic film shows that its thermal stability can meet the corresponding requirements of consumer electronic products. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The microscopic morphology of the original Fe-Cr-Si amorphous magnetic powder in Example 2;
[0028] Figure 2The microscopic morphology of the Fe-Cr-Si amorphous magnetic powder after insulation coating in Example 2;
[0029] Figure 3 The microscopic morphology of the semi-cured magnetic film of the epoxy resin and polyimide mixed matrix in Example 2;
[0030] Figure 4 is the complex magnetic permeability of the magnetic film after curing in Example 2;
[0031] Figure 5 This is the TGA test diagram of the magnetic film after curing in Example 2. DETAILED DESCRIPTION
[0032] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0033] Example 1
[0034] This embodiment provides a method for preparing a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide, comprising the following steps:
[0035] Step 1: SiO2 insulation coating of raw magnetic powder
[0036] (1.1) Ultrasonic cleaning of 30 g of Fe-Si polycrystalline magnetic powder with anhydrous ethanol mixed with deionized water, filtration, and drying in a 60°C forced air oven for 4 h;
[0037] (1.2) Disperse 30 g of dried Fe-Si polycrystalline magnetic powder into 260 ml of anhydrous ethanol and 50 ml of deionized water, add 1.6 ml of methyltriethoxysilane dropwise, and stir mechanically for 1 h;
[0038] (1.3) Add 2.7 ml of tetraethoxysilane to the magnetic powder mixture in step (1.2), adjust the pH of the mixture to about 11 with aqueous ammonia, and then mechanically stir for 1 h in a 40° C. water bath to obtain a suspension;
[0039] (1.4) After the suspension in step (1.3) is filtered, the coated magnetic powder is washed with anhydrous ethanol until the pH of the filtrate is 7, and then dried in a forced air oven at 60°C for 4 hours.
[0040] Step 2: Preparation of semi-cured magnetic film with epoxy resin and polyimide mixed matrix
[0041] (2.1) Add 30 g of the SiO2 insulation-coated magnetic powder prepared in step 1 to 10 g of a mixture of epoxy resin and polyimide stock solutions, wherein the mass ratio of epoxy resin to polyimide is 1:1, and heat to remove the solvent while mechanically stirring the mixture in a fume hood for 2 h at a stirring rate of 450 rpm; the epoxy resin in step (2.1) is bisphenol A epoxy resin, and the polyimide stock solution is a thermoplastic polyimide liquid with N,N-dimethylacetamide as solvent and a polyimide mass ratio of 20%.
[0042] (2.2) Add 0.17 g of diaminodiphenyl sulfone and 0.003 g of 2-methylimidazole to the mixture of step (2.1), continue heating and mechanical stirring for 2 h, and obtain a uniformly mixed magnetic slurry;
[0043] (2.3) The magnetic slurry mixed evenly in step (2.2) is coated on a PET film, placed in a 120° C. forced air oven, and semi-cured for 10 minutes to obtain a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide.
[0044] The application of the epoxy resin and polyimide mixed matrix semi-cured magnetic film in this embodiment is as follows:
[0045] The prepared epoxy resin and polyimide mixed matrix semi-cured magnetic film is peeled off from the PET film, placed on the inductor or substrate to be integrated, and then placed in a hot press with the pressure set to 1MPa. The temperature is increased to 90°C at a heating rate of 5°C / min and hot pressed for 30 minutes. The temperature is then increased to 170°C at a heating rate of 5°C / min and hot pressed for 20 minutes. The semi-cured composite magnetic film is cooled to room temperature at room temperature and pressure to complete the curing and integration.
[0046] Example 2
[0047] This embodiment provides a preparation method and application of a semi-cured magnetic film with a mixed matrix of epoxy resin and polyimide, comprising the following steps:
[0048] Step 1: SiO2 insulation coating of raw magnetic powder
[0049] (1.1) 40 g of Fe-Cr-Si amorphous magnetic powder was ultrasonically cleaned with anhydrous ethanol mixed with deionized water, filtered, and dried in a 60°C forced air oven for 4 h;
[0050] (1.2) Disperse 40 g of the dried Fe-Cr-Si amorphous magnetic powder into 340 ml of anhydrous ethanol and 60 ml of deionized water, dropwise add 1.9 ml of γ-aminopropyltriethoxysilane, and mechanically stir for 1.5 h to obtain a magnetic powder mixture;
[0051] (1.3) Add 3.6 ml of tetraethoxysilane to the magnetic powder mixture in the above step (1.2), adjust the pH value of the mixture to about 11 with aqueous ammonia, and then mechanically stir for 1.5 hours in a 40°C water bath to obtain a suspension;
[0052] (1.4) After the suspension in step (1.3) is filtered, the coated magnetic powder is washed with anhydrous ethanol until the pH of the filtrate is 7, and then dried in a forced air oven at 60°C for 4 hours.
[0053] Step 2: Preparation of semi-cured magnetic film with epoxy resin and polyimide mixed matrix
[0054] (2.1) 40g of the SiO2-insulated magnetic powder in step 1 is added to 10g of a mixture of epoxy resin and polyimide stock solution, the mass ratio of epoxy resin to polyimide being 4:1, and the mixture is heated to remove the solvent while being mechanically stirred in a fume hood for 2h at a stirring rate of 500rpm. The epoxy resin in step (2.1) is bisphenol A epoxy resin, and the polyimide stock solution is a thermoplastic polyimide liquid with N,N-dimethylacetamide as solvent and a polyimide mass ratio of 20%.
[0055] (2.2) Add 0.19 g of dicyandiamide and 0.004 g of 2-methylimidazole to the mixture in step (2.1) above, continue heating and mechanically stirring for 2 h, and obtain a uniformly mixed magnetic slurry.
[0056] (2.3) The magnetic slurry mixed evenly in step (2.2) is coated on a PET film, placed in a 130° C. forced air oven, and semi-cured for 15 minutes to obtain a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide.
[0057] The application of the epoxy resin and polyimide mixed matrix semi-cured magnetic film in this embodiment is as follows:
[0058] The prepared epoxy resin and polyimide mixed matrix semi-cured magnetic film is peeled off from the PET film, placed on the inductor or substrate to be integrated, and then placed in a hot press with the pressure set to 1MPa. The temperature is increased to 90°C at a heating rate of 5°C / min and hot pressed for 30 minutes. The temperature is then increased to 170°C at a heating rate of 5°C / min and hot pressed for 20 minutes. The semi-cured composite magnetic film is cooled to room temperature at room temperature and pressure to complete the curing and integration.
[0059] The microscopic morphology of the original Fe-Cr-Si amorphous magnetic powder used in this embodiment is shown in FIG. Figure 1 As shown. The powder is spherical or nearly spherical with a relatively smooth surface.
[0060] The microscopic morphology of the Fe-Cr-Si amorphous magnetic powder after SiO2 insulation coating in this embodiment is shown in FIG. Figure 2As shown in the figure, it can be seen that there is an obvious coating layer on the surface of the magnetic powder, and the coating layer is rough, which is obviously different from the original magnetic powder without coating.
[0061] The microscopic morphology of the semi-cured magnetic film of the epoxy resin and polyimide mixed matrix in this embodiment is shown in FIG. Figure 3 As shown, it can be seen that the magnetic powder is evenly mixed with the epoxy resin and polyimide mixed matrix.
[0062] The complex magnetic permeability of the magnetic film after curing in this embodiment is as follows: Figure 4 It can be seen that when the frequency is 100MHz, the magnetic permeability of the magnetic film is 4.06, the magnetic loss tanδ is only 0.018, and the magnetic properties are good.
[0063] In this embodiment, the TGA test of the magnetic film after curing is as follows: Figure 5 It can be seen that the magnetic film loses 2% of its weight at 320°C, and has good thermal stability.
[0064] Example 3
[0065] This embodiment provides a preparation method and application of a semi-cured magnetic film with a mixed matrix of epoxy resin and polyimide, comprising the following steps:
[0066] Step 1: SiO2 insulation coating of raw magnetic powder
[0067] (1.1) 50 g of Fe-Ni powder was ultrasonically cleaned with anhydrous ethanol mixed with deionized water, filtered, and dried in a forced air oven at 60 °C for 5 h;
[0068] (1.2) Disperse 50 g of the dried Fe-Ni powder into 425 ml of anhydrous ethanol and 75 ml of deionized water, add 2.5 ml of γ-aminopropyltrimethoxysilane dropwise, and mechanically stir for 1.5 h to obtain a magnetic powder mixture;
[0069] (1.3) Add 4.5 ml of tetraethoxysilane to the magnetic powder mixture in the above step (1.2), adjust the pH value of the mixture to about 11 with aqueous ammonia, and then mechanically stir for 2 h in a 40°C water bath to obtain a suspension;
[0070] (1.4) After the suspension in step (1.3) is filtered, the coated magnetic powder is washed with anhydrous ethanol until the pH of the filtrate is 7, and then dried in a forced air oven at 60°C for 4 hours.
[0071] Step 2: Preparation of semi-cured magnetic film with epoxy resin and polyimide mixed matrix
[0072] (2.1) Add 50g of the SiO2 insulated magnetic powder in step 1 to 10g of epoxy resin and polyimide stock solution mixture, the epoxy resin and polyimide mass ratio is 10:1, and heat to remove the solvent while mechanically stirring in a fume hood, stirring for 2h, and the stirring rate is 600rpm. The epoxy resin in step (2.1) is bisphenol A epoxy resin, and the polyimide stock solution is a thermoplastic polyimide liquid with N,N-dimethylacetamide as solvent and a polyimide mass ratio of 20%.
[0073] (2.2) Add 0.25 g of aluminum acetylacetonate and 0.01 g of 2-methylimidazole to the mixture of step (2.1) above, continue heating and mechanical stirring for 2 h, and obtain a uniformly mixed magnetic slurry.
[0074] (2.3) The magnetic slurry mixed evenly in step (2.2) is coated on a PET film, placed in a 140° C. forced air oven, and semi-cured for 15 minutes to obtain a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide.
[0075] The application of the epoxy resin and polyimide mixed matrix semi-cured magnetic film in this embodiment is as follows:
[0076] The prepared epoxy resin and polyimide mixed matrix semi-cured magnetic film is peeled off from the PET film, placed on the inductor or substrate to be integrated, and then placed in a hot press with the pressure set to 1MPa. The temperature is increased to 90°C at a heating rate of 5°C / min and hot pressed for 30 minutes. The temperature is then increased to 170°C at a heating rate of 5°C / min and hot pressed for 20 minutes. The semi-cured composite magnetic film is cooled to room temperature at room temperature and pressure to complete the curing and integration.
[0077] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide, characterized in that The steps include: Step 1: SiO2 insulation coating of raw magnetic powder (1.1) Ultrasonic cleaning of 30-50 g of magnetic powder with anhydrous ethanol mixed with deionized water, filtration, and drying in a 60°C forced air oven for 4-5 h; (1.2) Dispersing 30-50 g of the dried magnetic powder into 260-425 ml of anhydrous ethanol and 50-75 ml of deionized water, adding 1.5-2.5 ml of a silane coupling agent dropwise, and mechanically stirring for 1-2 hours to obtain a magnetic powder mixture; (1.3) Add 2.7-4.5 ml of tetraethoxysilane to the magnetic powder mixture in step (1.2), adjust the pH of the mixture to 10-11 with aqueous ammonia, and then mechanically stir for 1-2 hours in a 40° C. water bath to obtain a suspension; (1.4) After the suspension in step (1.3) is filtered, the coated magnetic powder is washed with anhydrous ethanol until the pH of the filtrate is 7, and then dried in a forced air oven at 60°C for 4 to 6 hours; Step 2: Preparation of semi-cured magnetic film with epoxy resin and polyimide mixed matrix (2.1) Add 30-50 g of the SiO2-insulated magnetic powder obtained in step 1 to a mixture of 10 g of epoxy resin and polyimide stock solution, and heat and dry out the solvent while mechanically stirring in a fume hood, stirring for 2 h at a stirring rate of 450-600 rpm to obtain a mixture; (2.2) Add 0.17-0.25 g of epoxy resin curing agent and 0.003-0.01 g of epoxy resin curing accelerator to the mixture of step (2.1), continue heating and mechanical stirring for 2-3 hours, and obtain a uniformly mixed magnetic slurry; (2.3) The magnetic slurry mixed evenly in step (2.2) is coated on a PET film, placed in a 120-140° C. forced air oven, and semi-cured for 10-15 minutes to obtain a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide.
2. The method for preparing a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide according to claim 1, characterized in that: The magnetic powder in the step (1.1) is one or more of Fe-Si polycrystalline magnetic powder, Fe-Cr-Si amorphous magnetic powder, and Fe-Ni powder, and the average particle size of the magnetic powder is 2 to 10 μm.
3. The method for preparing a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide according to claim 1, characterized in that: The silane coupling agent in the step (1.2) is selected from one of methyltriethoxysilane, γ-aminopropyltrimethoxysilane and γ-aminopropyltriethoxysilane.
4. The method for preparing a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide according to claim 1, characterized in that: In the step (2.1), the epoxy resin is bisphenol A epoxy resin, and the polyimide stock solution is a thermoplastic polyimide liquid with N,N-dimethylacetamide as solvent and a polyimide mass ratio of 20%.
5. The method for preparing a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide according to claim 1, characterized in that: In the step (2.1), the mass ratio of epoxy resin to polyimide is 1:1 to 10:
1.
6. The method for preparing a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide according to claim 1, characterized in that: The epoxy resin curing agent in the step (2.2) is a latent epoxy resin curing agent, preferably one of dicyandiamide, diaminodiphenyl sulfone, aluminum acetylacetonate, and boron trinitride.
7. The method for preparing a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide according to claim 1, characterized in that: The epoxy resin curing accelerator in the step (2.2) is an imidazole accelerator.
8. A semi-cured magnetic film with a mixed matrix of epoxy resin and polyimide, characterized in that: Obtained according to the preparation method according to any one of claims 1 to 7.
9. The use of a semi-cured magnetic film of a mixed matrix of epoxy resin and polyimide as claimed in claim 8, characterized in that: The prepared epoxy resin and polyimide mixed matrix semi-cured magnetic film is peeled off from the PET film, placed on the inductor or substrate to be integrated, and then placed in a hot press with the pressure set to 1MPa. The temperature is increased to 90°C at a heating rate of 5°C / min and hot pressed for 30 minutes. The temperature is then increased to 170°C at a heating rate of 5°C / min and hot pressed for 20 minutes. The semi-cured composite magnetic film is cooled to room temperature at room temperature and pressure to complete the curing and integration.