Preparation method of Ce ion doped delta-MnO2 supercapacitor electrode material

The preparation of Ce ion-doped δ-MnO2 supercapacitor electrode material by hydrothermal method solved the problem of low MnO2 conductivity, achieved high specific capacitance and good rate performance, and improved the cyclic stability and electrochemical performance of the material.

CN118888342APending Publication Date: 2024-11-01SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410870471.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The intrinsic conductivity of MnO2 is low, which limits its reversible capacity and high-rate performance, and the improvement effect of existing metal cation doping is not significant.

Method used

The Ce ion-doped δ-MnO2 supercapacitor electrode material was prepared by hydrothermal method. By adjusting the reaction conditions and doping ratio, a nanoflower spherical structure was formed to improve the specific surface area and electrochemical properties of the material.

Benefits of technology

The specific capacitance and rate performance of MnO2 are significantly improved, the utilization rate of active substances is increased, the volume changes during buffering and charging and discharging are improved, and the cycle performance and structural stability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888342A_ABST
    Figure CN118888342A_ABST
Patent Text Reader

Abstract

A preparation method of a Ce ion doped delta-MnO2 supercapacitor electrode material comprises the following steps: respectively weighing manganese sulfate monohydrate (MnSO4.H2O) and potassium permanganate (KMnO4), and dissolving the manganese sulfate monohydrate and the potassium permanganate in deionized water to obtain a solution; 2, weighing cerium nitrate hexahydrate [Ce (NO3) 3.6 H2O], pouring the cerium nitrate hexahydrate [Ce (NO3) 3.6 H2O] into the solution obtained in the step 1, and stirring the mixed solution on a magnetic stirrer to obtain a mixed solution; 3, transferring the mixed solution obtained in the step 2 into a high-pressure reaction kettle with a polytetrafluoroethylene lining, and carrying out heat preservation to obtain a product; and step 4, after the reaction is finished, putting a product into a centrifugal tube, putting the product into a centrifugal machine, centrifuging the product with deionized water for multiple times, then centrifuging the product with absolute ethyl alcohol for multiple times, and finally putting the product into a vacuum drying oven for drying to obtain the Ce ion doped delta-MnO2. The Ce-MnO2 nanoparticles are prepared by a hydrothermal method, and the adopted preparation process is simple and environment-friendly; the obtained product is uniform in chemical component, small in particle size and uniform in distribution; and the material has relatively high charge-discharge specific capacitance and good rate capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of supercapacitor electrode materials, and in particular relates to a method for preparing a Ce ion-doped delta-MnO2 supercapacitor electrode material. Background Art

[0002] Although supercapacitors have a low energy density, they have attracted widespread attention due to their advantages that cannot be replaced by other energy storage devices, such as rapid charging and discharging, long cycle life, simple structure, and safe application. In supercapacitors, electrode materials often occupy an important position, and the quality of electrode materials can directly affect the performance of supercapacitors. MnO2 has a high theoretical specific capacitance (~1370F·g -1 ), and has the characteristics of simple preparation process, abundant reserves and environmental protection, and is considered to be an electrode material with development prospects.

[0003] The structural unit of MnO2 crystal is [MnO6] octahedron. According to the different bonding modes of [MnO6] octahedron, MnO2 can be divided into one-dimensional tunnel structure (α-MnO2, β-MnO2, γ-MnO2, etc.), two-dimensional layered structure (δ-MnO2) and three-dimensional mesh structure (λ-MnO2). Among them, the interlayer spacing in the δ-MnO2 lattice is about 0.7nm, and there are some cations and water molecules between the layers that play a role in stabilizing the structure. These structural characteristics give MnO2 excellent ion exchange and redox capabilities. However, the intrinsic conductivity of MnO2 is low, which limits its reversible capacity and high rate performance.

[0004] At present, the main methods for modifying the existing problems include morphology and structure design, ion doping, and composite conductive polymers. Among them, ion doping is an effective means to improve the conductivity of materials by introducing impurity energy levels in the band gap and forming more stable chemical bonds to improve the electrochemical properties of materials. In recent years, research has mainly focused on metal cation doping of MnO2. For example, Hu et al. prepared Al 3+ Doped MnO2, doped samples at 0.1A·g -1 The specific capacitance at the current density is 213F·g -1 , in 0.1-5A·g -1 The rate performance in the current density range reaches 51.6%, which shows that its rate performance is poor. 3+ The improvement of its electrochemical performance is not obvious. Summary of the invention

[0005] In order to overcome the above problems existing in the prior art, the purpose of the present invention is to provide a method for preparing Ce ion doped δ-MnO2 supercapacitor electrode material, in which Ce-MnO2 nanoparticles are prepared by a hydrothermal method. The preparation process adopted is simple and environmentally friendly; the obtained product has uniform chemical composition, small particle size and uniform distribution; it has high charge and discharge specific capacitance and good rate performance.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a Ce ion-doped delta-MnO2 supercapacitor electrode material comprises the following steps:

[0008] Step 1: Weigh manganese sulfate monohydrate (MnSO4·H2O) and potassium permanganate (KMnO4) respectively, and dissolve them in deionized water to obtain a solution;

[0009] Step 2: Weigh cerium nitrate hexahydrate [Ce(NO3)3·6H2O], pour it into the solution of step 1, and stir the mixed solution on a magnetic stirrer to obtain a mixed solution;

[0010] Step 3: transferring the mixed solution in step 2 into a polytetrafluoroethylene-lined autoclave, and obtaining the product after heat preservation;

[0011] Step 4: After the reaction is completed, the product is placed in a centrifuge tube and placed in a centrifuge. It is centrifuged several times with deionized water and then several times with anhydrous ethanol. Finally, it is placed in a vacuum drying oven and dried to obtain Ce ion-doped δ-MnO2.

[0012] In step 1, MnSO4·H2O and KMnO4 are weighed and dissolved in 30-40 mL of deionized water, wherein the molar ratio of MnSO4·H2O to KMnO4 is 1:4-1:10. Such a ratio is set so that there are enough potassium ions in the solution, thereby having a better stabilizing effect on the layered structure of δ-MnO2.

[0013] In step 2, weigh Ce(NO3)3·6H2O and pour it into the solution of step 1, so that the molar ratio of Ce(NO3)3·6H2O to MnSO4·H2O is 1:50 to 1:10, and stir the mixed solution on a magnetic stirrer for 10 to 30 minutes. By setting the ratio in this way, the most suitable ratio of Ce ion doping δ-MnO2 can be found to ensure its successful incorporation into the MnO2 lattice.

[0014] In step 3, the volume of the solution is controlled at 60-80% of the volume of the reactor, and the solution is heated at 120-180° C. for 12-20 hours. Setting the reaction conditions in this way can allow δ-MnO2 to have sufficient nucleation and growth time at a suitable temperature, and finally form a nano flower ball structure.

[0015] In step 4, the product is centrifuged 3 to 5 times with deionized water and then 3 to 5 times with anhydrous ethanol to wash away excess impurity ions that have not reacted completely. Finally, the product is dried at 60° C. to 80° C. for 8 to 16 hours. Setting the temperature in this way ensures that the product is fully dried without affecting its structure and morphology due to excessively high temperature.

[0016] The Ce ion-doped δ-MnO2 is used for supercapacitor electrodes.

[0017] The Ce ion-doped δ-MnO2 product is uniform in size and flower-ball-shaped, the nano-flower-balls grow well, and the average diameter of the MnO2 nano-flower-balls decreases from 2 μm of pure phase MnO2 to 300 nm of Ce ion-doped δ-MnO2, and no nanosheet collapse occurs.

[0018] Beneficial effects of the present invention:

[0019] The invention utilizes a hydrothermal method to prepare Ce ion-doped delta-MnO2. The experimental operation is simple, convenient and pollution-free. The experimental raw materials are cheap and easily available. The obtained product has high purity, good dispersibility, high rate performance and cycle stability.

[0020] In the present invention, Ce ion doping can effectively increase the specific surface area of ​​MnO2, which is beneficial for MnO2 to fully contact with the electrolyte during the reaction process, thereby increasing the utilization rate of the active material. Ce-doped MnO2 has a nanostructure, which can buffer the volume change of MnO2 during the charge and discharge process, which is beneficial to improving the structural stability of the electrode material, thereby improving its cycle performance and rate performance.

[0021] The present invention selects Ce ions as doping ions, and synthesizes flower ball-shaped particles of δ-MnO2 doped with rare earth element Ce ions by a hydrothermal method. After doping, the diameter of the nano flower balls of the sample is significantly reduced, which is conducive to the increase of the specific surface area of ​​the electrode material, and provides more reaction sites for the adsorption / desorption and embedding / ejection of MnO2 during the charge and discharge process, which is conducive to the improvement of electrochemical performance. After electrochemical performance testing, the material prepared by the method has good cycle stability as a supercapacitor electrode material, has good electrochemical properties such as high charge and discharge specific capacitance at high current density. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is the XRD spectrum of the product prepared by the present invention.

[0023] Figure 2 It is a SEM picture of the product of the present invention.

[0024] Figure 3 It is a TEM picture of the product of the present invention.

[0025] Figure 4 It is the EDS spectrum diagram of the product of the present invention.

[0026] Figure 5 It is the XPS spectrum of the product of the present invention.

[0027] Figure 6 It is a GCD curve diagram of the product of the present invention at different current densities.

[0028] Figure 7 These are the rate performance test results of the product of the present invention at different current densities.

[0029] Figure 8 The product of the present invention is 10A·g -1 Cyclic curves at different current densities. DETAILED DESCRIPTION

[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0031] Embodiment 1

[0032] The preparation method of Ce ion doped delta-MnO2 comprises the following steps:

[0033] Step 1: Weigh 0.3 g KMnO4 and 0.03 g MnSO4·H2O, and add 35 mL deionized water to prepare a mixed solution.

[0034] Step 2: Add 0.0015 g Ce(NO3)3·6H2O to the mixed solution and stir on a magnetic stirrer for 10 min to mix evenly.

[0035] Step 3: Transfer the solution in step 2 into a 50 mL polytetrafluoroethylene-lined autoclave with a solution volume of 35 ml and keep it at 100°C for 12 h.

[0036] Step 4: After the reaction is completed, the product is poured into a centrifuge tube and placed in a centrifuge, centrifuged 4 times with deionized water and then 4 times with anhydrous ethanol, and finally dried at 60°C for 16 hours to obtain Ce ion-doped δ-MnO2 nanoparticles.

[0037] Embodiment 2

[0038] The preparation method of Ce ion doped delta-MnO2 comprises the following steps:

[0039] Step 1: Weigh 0.25 g KMnO4 and 0.035 g MnSO4·H2O, and add 40 mL deionized water to prepare a mixed solution.

[0040] Step 2: Add 0.0044 g Ce(NO3)3·6H2O to the mixed solution and stir on a magnetic stirrer for 15 min to mix it evenly.

[0041] Step 3: Transfer the solution in step 2 into a 50 mL polytetrafluoroethylene-lined autoclave with a solution volume of 40 ml and keep it at 100°C for 12 h.

[0042] Step 4: After the reaction is completed, the product is poured into a centrifuge tube and placed in a centrifuge, centrifuged 4 times with deionized water and then 4 times with anhydrous ethanol, and finally dried at 65°C for 12 hours to obtain Ce ion-doped δ-MnO2 nanoparticles.

[0043] Embodiment 3

[0044] The preparation method of Ce ion doped delta-MnO2 comprises the following steps:

[0045] Step 1: Weigh 0.15 g KMnO4 and 0.05 g MnSO4·H2O, and add 35 mL deionized water to prepare a mixed solution.

[0046] Step 2: Add 0.0058 g Ce(NO3)3·6H2O to the mixed solution and stir on a magnetic stirrer for 20 min to mix it evenly.

[0047] Step 3: Transfer the solution in step 2 into a 50 mL polytetrafluoroethylene-lined autoclave with a solution volume of 35 ml and keep it at 140°C for 16 h.

[0048] Step 4: After the reaction is completed, the product is poured into a centrifuge tube and placed in a centrifuge, centrifuged 4 times with deionized water and then 4 times with anhydrous ethanol, and finally dried at 60°C for 12 hours to obtain Ce ion-doped δ-MnO2 nanoparticles.

[0049] Embodiment 4

[0050] The preparation method of Ce ion doped delta-MnO2 comprises the following steps:

[0051] Step 1: Weigh 0.19 g KMnO4 and 0.034 g MnSO4·H2O, and add 40 mL deionized water to prepare a mixed solution.

[0052] Step 2: Add 0.0087 g Ce(NO3)3·6H2O to the mixed solution and stir on a magnetic stirrer for 30 min to mix evenly.

[0053] Step 3: Transfer the solution in step 2 into a 50 mL polytetrafluoroethylene-lined autoclave with a solution volume of 40 ml and keep it at 160°C for 16 h.

[0054] Step 4: After the reaction is completed, the product is poured into a centrifuge tube and placed in a centrifuge, centrifuged three times with deionized water and then three times with anhydrous ethanol, and finally dried at 70°C for 12 hours to obtain Ce ion-doped δ-MnO2 nanoparticles.

[0055] like Figure 1 As shown, compared with the standard card JCPDS#NO.86-0666, the position of the diffraction peak of the prepared Ce ion-doped δ-MnO2 is completely consistent with the position of the diffraction peak of the standard card and there are no other impurity peaks, and no other diffraction peaks containing impurities containing Ce compounds are found, indicating that Ce is successfully incorporated into the δ-MnO2 lattice.

[0056] like Figure 2 As shown in the figure, it can be seen that both pure phase δ-MnO2 and Ce ion doped δ-MnO2 present nano flower ball granular structure, among which the diameter of the nano flower ball particles of pure phase δ-MnO2 is larger, and after being doped with Ce ions, the diameter of the nano flower ball particles becomes significantly smaller, and the particles are uniform, the nano flower balls grow well, and there is no nanosheet collapse phenomenon.

[0057] like Figure 3 As shown in the figure, it can be seen that the prepared Ce ion doped δ-MnO2 sample is still in the shape of a flower ball, and the average diameter of the flower ball is 300nm, which is consistent with Figure 2 The sizes of the nanoflower balls in the SEM images of the samples shown are consistent.

[0058] like Figure 4 As shown, it can be clearly seen from the EDS energy spectrum that Mn, O, K and Ce elements exist in the Ce ion-doped δ-MnO2 sample, further indicating that Ce ions are successfully incorporated into the δ-MnO2 lattice.

[0059] like Figure 5 As shown in the Ce3dXPS spectrum, it can be seen that the valence state of the element Ce in the Ce ion-doped δ-MnO2 sample is mainly Ce 3+ and Ce 4+ exist.

[0060] like Figure 6 As shown in the figure, it can be seen that at 1A·g -1 The specific capacitance is 192F·g -1 , as the current density increases, the specific capacitance shows a downward trend.

[0061] like Figure 7As shown in the figure, it can be seen that Ce ion doped δ-MnO2 at 1, 2, 3, 5, 8, 10 A·g -1 The discharge specific capacitances under these conditions are 192.09, 181.74, 179.15, 174.19, 168.67, and 165.95 F·g, respectively. -1 , where 10A·g -1 The discharge specific capacitance is 1A·g -1 The results show that the material has good rate performance and high discharge specific capacitance at high current density.

[0062] like Figure 8 As shown in the figure, after 10,000 cycles, the specific capacitance retention rate of the sample is 83.3%, which has good cycle stability.

Claims

1. A method for preparing Ce ion doped δ-MnO2 supercapacitor electrode material, characterized in that: The steps include: Step 1: Weigh manganese sulfate monohydrate (MnSO4·H2O) and potassium permanganate (KMnO4) respectively, and dissolve them in deionized water to obtain a solution; Step 2: Weigh cerium nitrate hexahydrate [Ce(NO3)3·6H2O], pour it into the solution of step 1, and stir the mixed solution on a magnetic stirrer to obtain a mixed solution; Step 3: transferring the mixed solution in step 2 into a polytetrafluoroethylene-lined autoclave and heat-insulating to obtain a product; Step 4: After the reaction is completed, the product is placed in a centrifuge tube and placed in a centrifuge. It is centrifuged several times with deionized water and then several times with anhydrous ethanol. Finally, it is placed in a vacuum drying oven and dried to obtain Ce ion-doped δ-MnO2.

2. The method for preparing a Ce ion-doped δ-MnO2 supercapacitor electrode material according to claim 1, characterized in that: In the step 1, MnSO4·H2O and KMnO4 are weighed respectively and dissolved in 30-40 mL of deionized water, wherein the molar ratio of MnSO4·H2O to KMnO4 is 1:4-1:

10.

3. The method for preparing a Ce ion-doped δ-MnO2 supercapacitor electrode material according to claim 1, characterized in that: In the step 2, weigh Ce(NO3)3·6H2O and pour it into the solution of step 1 so that the molar ratio of Ce(NO3)3·6H2O to MnSO4·H2O is 1:50 to 1:10, and stir the mixed solution on a magnetic stirrer for 10 to 30 minutes.

4. The method for preparing a Ce ion-doped δ-MnO2 supercapacitor electrode material according to claim 1, characterized in that: In the step 3, the volume of the solution is controlled at 60-80% of the volume of the reactor, and the solution is heated at 120-180° C. for 12-20 hours.

5. The method for preparing a Ce ion-doped δ-MnO2 supercapacitor electrode material according to claim 1, characterized in that: In step 4, the mixture is centrifuged 3 to 5 times with deionized water and then 3 to 5 times with anhydrous ethanol to wash away excess unreacted impurity ions.

6. Ce ion-doped δ-MnO2 prepared by the method according to any one of claims 1 to 5, characterized in that: The Ce ion-doped δ-MnO2 product is uniform in size and flower-ball-shaped, the nano-flower-balls grow well, and the average diameter of the MnO2 nano-flower-balls decreases from 2 μm of pure phase MnO2 to 300 nm of Ce ion-doped δ-MnO2, and no nanosheet collapse occurs.