Processing method of semiconductor device and semiconductor device
By laser etching on the silicon carbide substrate of semiconductor devices to form grooves and fill the metal layer, the problems of high on-resistance and difficulty in etching in traditional processes are solved, and lower resistivity and better heat dissipation effect are achieved .
Patent Information
- Application Number
- CN202410936417.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-01
AI Technical Summary
In traditional semiconductor device processes, the back thinning + metal deposition method is difficult to meet the requirements of semiconductor devices for low on-resistance, and silicon carbide is difficult to etch in typical acid or alkali solutions, the gas etching rate is slow and the surface is damaged, and the The groove inclination angle is difficult to control.
The silicon carbide substrate is etched with a laser and a metal layer is filled in the groove. By adjusting the spot diameter and the number of holes, the grooves with a preset inclination angle are formed, and the grooves are thinned to 170-190um, and the grooves are lined. Ni, Ti, and Ag metal layers are formed on the bottom side.
A lower resistivity and better heat dissipation structure are achieved, reducing surface damage and metal filling difficulty while reducing costs.
Smart Images

Figure CN118888436A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor technology, and in particular, relates to a processing method for a semiconductor device and a semiconductor device. Background Art
[0002] like Figure 5 As shown, the common back-side process flow technology of semiconductor devices is: front-side film protection → back-side thinning → film tearing → back-side metal.
[0003] As power devices pursue better heat dissipation and lower resistivity, they are required to achieve better conduction effects. That is, the traditional process of backside thinning + metal deposition has been difficult to meet the requirements of semiconductor devices for low on-resistance.
[0004] It is desirable to provide an improved method of processing semiconductor devices. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for processing a semiconductor device, the purpose of which is to reduce the on-resistance of the semiconductor device.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is: a method for processing a semiconductor device, comprising:
[0007] A semiconductor device is provided, the semiconductor device comprising a silicon carbide substrate and an epitaxial layer located on one side of the silicon carbide substrate;
[0008] Performing a thinning process on a side of the silicon carbide substrate away from the epitaxial layer;
[0009] forming a groove on a side of the silicon carbide substrate away from the epitaxial layer, wherein the depth of the groove is less than or equal to the thickness of the silicon carbide substrate;
[0010] A metal layer is formed on a side of the silicon carbide substrate away from the epitaxial layer, and the metal layer fills the groove.
[0011] The thinning process of the side of the silicon carbide substrate away from the epitaxial layer includes: thinning the side of the silicon carbide substrate away from the epitaxial layer to 170-190 um.
[0012] Forming the groove on a side of the silicon carbide substrate away from the epitaxial layer includes: using a laser to perform laser processing on the side of the silicon carbide substrate away from the epitaxial layer.
[0013] Using the laser to perform laser processing on the side of the silicon carbide substrate away from the epitaxial layer includes: using the laser to perform laser processing on the side of the silicon carbide substrate away from the epitaxial layer multiple times to form the groove whose sidewall has a preset inclination angle.
[0014] Using the laser to perform multiple laser treatments on a side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has the preset inclination angle includes: sequentially using a first spot and a second spot of the laser to perform laser treatments, the diameter of the first spot is larger than the diameter of the second spot, and the laser treatment depth of the first spot is smaller than the laser treatment depth of the second spot.
[0015] Using the laser to perform multiple laser treatments on a side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has the preset inclination angle includes: sequentially using a first spot and a second spot of the laser to perform treatments, the diameter of the first spot is smaller than the diameter of the second spot, and the laser treatment depth of the first spot is greater than the laser treatment depth of the second spot.
[0016] Using the laser to perform multiple laser treatments on a side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has the preset inclination angle includes: using the laser to perform multiple laser treatments on a side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has the preset inclination angle of 60° to 90°.
[0017] Using the laser to perform multiple laser treatments on the side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has a preset inclination angle includes using the laser to perform multiple laser treatments on the side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has a preset inclination angle and a diameter of 0.5um to 10um.
[0018] Forming the metal layer on a side of the silicon carbide substrate away from the epitaxial layer comprises:
[0019] Evaporating Ni on a side of the silicon carbide substrate away from the epitaxial layer;
[0020] Performing laser annealing on a side of the silicon carbide substrate away from the epitaxial layer;
[0021] Ti, Ni and Ag are evaporated in sequence on a side of the silicon carbide substrate away from the epitaxial layer to form the metal layer.
[0022] The present invention also provides a semiconductor device, which is prepared by using the processing method of the semiconductor device.
[0023] The processing method of the semiconductor device of the present invention performs back side groove etching on the silicon carbide substrate and fills the groove with metal, so that the semiconductor device can obtain a better heat dissipation structure and a lower resistivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] This specification includes the following drawings, which show the following contents:
[0025] Figure 1 is a flow chart of a method for processing a semiconductor device of the present invention;
[0026] Figure 2 It is a schematic diagram of the structure after the first hole is punched on the semiconductor device;
[0027] Figure 3 It is a schematic diagram of the structure after the second drilling on the semiconductor device;
[0028] Figure 4 It is a schematic diagram of the structure of a semiconductor device;
[0029] Figure 5 It is a schematic diagram of the structure of a semiconductor device in the prior art;
[0030] The markings in the figure are:
[0031] 1. Back metal layer; 2. Silicon carbide substrate; 3. Epitaxial layer; 4. Protective film; 5. Groove. DETAILED DESCRIPTION
[0032] The specific implementation methods of the present invention are further explained in detail below by describing the embodiments with reference to the accompanying drawings, with the aim of helping those skilled in the art to have a more complete, accurate and in-depth understanding of the concept and technical solution of the present invention and facilitating its implementation.
[0033] Since silicon carbide has strong resistance to chemical corrosion and radiation, it is difficult to etch in typical acid or alkaline solutions. However, the gas etching technology commonly used in the prior art has problems such as slow etching rate, low etching selectivity and surface damage.
[0034] Therefore, in the prior art, the processing method of semiconductor devices has the following defects:
[0035] 1. The traditional process uses backside thinning + metal deposition, which results in a high on-resistance of semiconductor devices;
[0036] 2. In wet etching, typical acid or alkaline solutions cannot etch silicon carbide;
[0037] 3. In gas etching, there are process problems such as slow etching rate, surface damage, and difficulty in controlling the groove angle.
[0038] like Figure 1 As shown, the present invention provides a method for processing a semiconductor device, comprising the following steps:
[0039] S1. Provide a semiconductor device, wherein the semiconductor device comprises a silicon carbide substrate 2 and an epitaxial layer 3 located on one side of the silicon carbide substrate 2;
[0040] S2, performing a thinning process on a side of the silicon carbide substrate 2 away from the epitaxial layer 3;
[0041] S3, forming a groove 5 on a side of the silicon carbide substrate 2 away from the epitaxial layer 3, wherein the depth of the groove 5 is less than or equal to the thickness of the silicon carbide substrate 2;
[0042] S4 , forming a metal layer on a side of the silicon carbide substrate 2 away from the epitaxial layer 3 , and the metal layer fills the groove 5 .
[0043] Specifically, in the above step S2, before the back side of the silicon carbide substrate 2 is thinned, a front side process is performed on the front side of the silicon carbide substrate 2 to form an epitaxial layer 3 on the silicon carbide substrate 2, and a protective film 4 is formed on the epitaxial layer 3, such as Figure 4 shown.
[0044] In the above step S2, the thinning process of the side of the silicon carbide substrate 2 away from the epitaxial layer 3 includes: thinning the side of the silicon carbide substrate 2 away from the epitaxial layer 3 to 180 um.
[0045] In the above step S3, forming a groove on the side of the silicon carbide substrate 2 away from the epitaxial layer 3 includes: using a laser to perform laser processing on the side of the silicon carbide substrate 2 away from the epitaxial layer 3. In addition, in the process of forming the groove 5, the angle of the groove 5 is adjusted by adjusting different light spots and the number of punching times.
[0046] In the above step S3, using a laser to perform laser processing on the side of the silicon carbide substrate 2 away from the epitaxial layer 3 includes: using a laser to perform laser processing on the side of the silicon carbide substrate 2 away from the epitaxial layer 3 multiple times to form a groove with a side wall having a preset inclination angle. By adjusting the various parameters of the laser, using different spots and controlling the number of punching times to complete the processing of the groove 5 on the entire wafer, the angle of the groove 5 is 60° to 90°, and the diameter of the groove 5 is 0.5um to 10um. The groove 5 is used to fill the metal. If the diameter of the groove 5 is very small, it is difficult to fill the metal and it is easy to cause voids. Therefore, it is necessary to reasonably control the diameter and angle of the groove 5 to ensure that the metal filling meets the requirements.
[0047] In the above step S3, using a laser to perform laser processing on the side of the silicon carbide substrate 2 away from the epitaxial layer 3 for multiple times to form a groove 5 with a side wall having a preset tilt angle includes: sequentially using a first spot and a second spot of the laser for laser processing, the diameter of the first spot is greater than the diameter of the second spot, and the laser processing depth of the first spot is less than the laser processing depth of the second spot. The advantage of using laser to drill holes is that the size of the groove 5 can be adjusted by the size of the spot, and spots of different diameters act on different depths at the same position, so grooves 5 with different tilt angles will be formed.
[0048] As a variant implementation scheme, in the above step S3, a laser is used to perform multiple laser treatments on the side of the silicon carbide substrate 2 away from the epitaxial layer 3 to form a groove 5 whose side wall has a preset inclination angle, including: sequentially using a first spot and a second spot of the laser for treatment, the diameter of the first spot is smaller than the diameter of the second spot, and the laser processing depth of the first spot is greater than the laser processing depth of the second spot.
[0049] like Figure 2 As shown, a first spot of the laser is used to perform laser processing on the side of the silicon carbide substrate 2 away from the epitaxial layer 3 to form a plurality of first holes, the depth of the first holes being less than the thickness of the silicon carbide substrate 2. Then, at the position of each first hole, a second spot of the laser is used to continue to perform laser processing on the side of the silicon carbide substrate 2 away from the epitaxial layer 3, and finally a groove 5 penetrating the silicon carbide substrate 2 is formed, as shown in FIG. Figure 3 shown.
[0050] like Figure 3 As shown, the groove 5 is a conical hole, and the groove 5 has a large diameter end and a small diameter end. The diameter of the large diameter end is larger than the diameter of the small diameter end. The large diameter end of the groove 5 is the end away from the epitaxial wafer, and the small diameter end of the groove 5 is close to the epitaxial wafer.
[0051] In the above step S3, when using a laser to perform multiple laser treatments on the side of the silicon carbide substrate 2 away from the epitaxial layer 3, different light spots are used for the same groove 5 in order to adjust the top and bottom sizes of the groove 5, so as to obtain a groove 5 with a certain inclination angle, which is convenient for the subsequent filling of the back metal.
[0052] The above step S4 comprises:
[0053] Evaporating Ni on the side of the silicon carbide substrate 2 away from the epitaxial layer 3;
[0054] Performing laser annealing on a side of the silicon carbide substrate 2 away from the epitaxial layer 3;
[0055] Ti, Ni and Ag are sequentially evaporated on a side of the silicon carbide substrate 2 away from the epitaxial layer 3 to form a metal layer.
[0056] In the above step S4, by forming a metal layer, the performance and reliability of the semiconductor device can be improved.
[0057] In the present invention, the device is turned on by back-hole drilling + metal filling, which can effectively reduce the resistivity of the semiconductor device compared to the back-side thinning + metal deposition process in the prior art, and enable the semiconductor device to achieve better heat dissipation. By adjusting different light spots and the number of holes, the angle of the groove 5 can be adjusted, reducing surface damage and the difficulty of metal filling while reducing costs.
[0058] The present invention also provides a semiconductor device, which is prepared by using the above-mentioned processing method of the semiconductor device.
[0059] The present invention is described above by way of example in conjunction with the accompanying drawings. Obviously, the specific implementation of the present invention is not limited to the above-mentioned methods. As long as various non-substantial improvements are made using the method concept and technical solution of the present invention; or the above concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A method for processing a semiconductor device, characterized in that: include: A semiconductor device is provided, the semiconductor device comprising a silicon carbide substrate and an epitaxial layer located on one side of the silicon carbide substrate; Performing a thinning process on a side of the silicon carbide substrate away from the epitaxial layer; forming a groove on a side of the silicon carbide substrate away from the epitaxial layer, wherein the depth of the groove is less than or equal to the thickness of the silicon carbide substrate; A metal layer is formed on a side of the silicon carbide substrate away from the epitaxial layer, and the metal layer fills the groove.
2. The method for processing a semiconductor device according to claim 1, wherein: The thinning process of the side of the silicon carbide substrate away from the epitaxial layer includes: thinning the side of the silicon carbide substrate away from the epitaxial layer to 170-190 um.
3. The method for processing a semiconductor device according to any one of claims 1 to 2, characterized in that: Forming the groove on a side of the silicon carbide substrate away from the epitaxial layer includes: using a laser to perform laser processing on the side of the silicon carbide substrate away from the epitaxial layer.
4. The method for processing a semiconductor device according to claim 3, wherein: Using the laser to perform laser processing on the side of the silicon carbide substrate away from the epitaxial layer includes: using the laser to perform laser processing on the side of the silicon carbide substrate away from the epitaxial layer multiple times to form the groove whose sidewall has a preset inclination angle.
5. The method for processing a semiconductor device according to claim 4, characterized in that: Using the laser to perform multiple laser treatments on a side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has the preset inclination angle includes: sequentially using a first spot and a second spot of the laser to perform laser treatments, the diameter of the first spot is larger than the diameter of the second spot, and the laser treatment depth of the first spot is smaller than the laser treatment depth of the second spot.
6. The method for processing a semiconductor device according to claim 4, wherein: Using the laser to perform multiple laser treatments on a side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has the preset inclination angle includes: sequentially using a first spot and a second spot of the laser to perform treatments, the diameter of the first spot is smaller than the diameter of the second spot, and the laser treatment depth of the first spot is greater than the laser treatment depth of the second spot.
7. The method for processing a semiconductor device according to claim 4, wherein: Using the laser to perform multiple laser treatments on a side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has the preset inclination angle includes: using the laser to perform multiple laser treatments on a side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has the preset inclination angle of 60° to 90°.
8. The method for processing a semiconductor device according to claim 4, characterized in that: Using the laser to perform multiple laser treatments on the side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has a preset inclination angle includes using the laser to perform multiple laser treatments on the side of the silicon carbide substrate away from the epitaxial layer to form a groove whose side wall has a preset inclination angle and a diameter of 0.5um to 10um.
9. The method for processing a semiconductor device according to any one of claims 1 to 2, characterized in that: Forming the metal layer on a side of the silicon carbide substrate away from the epitaxial layer comprises: Evaporating Ni on a side of the silicon carbide substrate away from the epitaxial layer; Performing laser annealing on a side of the silicon carbide substrate away from the epitaxial layer; Ti, Ni and Ag are evaporated in sequence on a side of the silicon carbide substrate away from the epitaxial layer to form the metal layer.
10. A semiconductor device, characterized in that The semiconductor device is manufactured by using the processing method of any one of claims 1 to 9.