Etching method compatible with etched silicon and polycrystalline silicon

By using a physical bombardment etching method combining HBr and SF6 gases, the problem of abnormal morphology during the etching of Si and polysilicon was solved, achieving morphological consistency of silicon and polysilicon vias and stability of the etching process, thereby improving etching efficiency and metal filling effect.

CN118888437APending Publication Date: 2024-11-01ZHEJIANG XINSHENG SEMICON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410816899.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When Si and poly are etched simultaneously, conventional etching methods can lead to abnormal morphology and drilling, which affects the metal filling effect and makes it difficult to ensure the morphological consistency of silicon holes and polysilicon holes.

Method used

HBr was used as the main etching gas and SF6 as the auxiliary etching gas. Etching was carried out by physical bombardment, and the etching rate and depth were controlled. Polymer was generated to protect the sidewalls and prevent drilling. The etching process was optimized by combining appropriate cavity pressure and power parameters.

Benefits of technology

It effectively controls the morphological consistency of silicon vias and polysilicon vias, prevents drilling and erosion, improves the stability and efficiency of the etching process, and ensures the metal filling effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888437A_ABST
    Figure CN118888437A_ABST
Patent Text Reader

Abstract

The invention discloses an etching method compatible with etched silicon and polycrystalline silicon, and the method comprises the steps: employing HBr as a main etching gas, employing SF6 as an auxiliary etching gas, and carrying out the etching in a bombardment mode till a preset etching time length or a preset etching depth is reached. According to the method, when silicon and polycrystalline silicon are etched at the same time, HBr is used as a main etching gas, SF6 is used as an auxiliary etching gas, compared with SF6 used as the main etching gas, the anisotropic reaction is very small, a large amount of polymer (products / polymers) can be generated in the HBr etching process to protect the side wall, the side wall undercutting phenomenon of polycrystalline silicon holes cannot be caused, and the etching efficiency of the polycrystalline silicon holes is improved. However, since the etching rate of HBr is very slow, a small amount of SF6 is added to improve the etching rate. According to the invention, the etching depth can be better controlled, and the morphology of the silicon hole and the polycrystalline silicon hole can be better improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chip etching, and in particular to an etching method capable of etching silicon and polysilicon compatibly. Background Art

[0002] In hole etching, a small part of the opening is located on poly (polycrystalline silicon). During the etching process, Si and poly will be etched at the same time. Polycrystalline silicon will be doped to a certain extent during the film formation process, and there are structural differences between polycrystalline silicon and silicon itself. Conventional silicon hole etching uses SF 6 +O 2 In this system, during the etching process, the two films will also have different etching effects due to differences in structure and the doping concentration of polysilicon itself. In actual etching, polysilicon will be etched differently due to SF 6 The isotropic reaction of the gas causes a lot of drilling on the polysilicon sidewalls, resulting in uncontrollable polysilicon morphology, which is very different from the silicon hole pattern. Conventional polycrystalline etching mostly uses Cl 2 +HBr or SF 6 +O 2 System, these two systems are mostly used for polycrystalline gate etching. Using them in polycrystalline hole etching will also cause drilling to a large extent, and the poly morphology after etching will be abnormal.

[0003] Subsequently, both silicon holes and poly holes will be filled with metal. If the morphology after etching is different or the drilling is abnormal, it will affect the metal filling and ultimately affect the product performance. Therefore, how to ensure the morphology of both when etching Si and poly at the same time is a technical problem that needs to be solved urgently. Summary of the invention

[0004] In view of the problem in the prior art that abnormal morphology is prone to occur when Si and poly are etched simultaneously, the present invention provides an etching method that is compatible with etching silicon and polysilicon. By adjusting the type and flow of gas, etching is mainly performed by bombardment, thereby reducing anisotropic reaction and etching rate, preventing drilling from occurring, and ensuring the morphology consistency of silicon holes and polycrystalline holes.

[0005] The following is the technical solution of the present invention.

[0006] An etching method compatible with etching silicon and polysilicon, using HBr as the main etching gas and SF 6 As auxiliary etching gas, the etching is performed in a bombardment manner until a preset etching time or a preset etching depth is reached.

[0007] In the present invention, when silicon and polysilicon are etched simultaneously, HBr is used as the main etching gas, and SF 6 As an auxiliary etching gas, the reaction principle is: Si+Brˉ->SiBr4 +eˉHBr, this reaction is compared with SF 6 As the main etching gas, the anisotropic reaction is very small, and a large amount of polymer will be generated during HBr etching to protect the side wall, which will not cause the side wall drilling of polysilicon holes. However, since the HBr etching rate is very slow, a small amount of SF 6 Generally speaking, the present invention mainly relies on physical bombardment for etching, the overall etching rate is not fast, the etching depth can be better controlled, and the morphology of silicon holes and polysilicon holes can be better improved.

[0008] Preferably, the flow rate of the main etching gas is three times or more than that of the auxiliary etching gas.

[0009] Preferably, the flow rate of HBr is controlled at 150-300 sccm, wherein sccm refers to standard cubic centimeters per minute. HBr will generate a large amount of polymer during the etching process to protect the sidewalls and will not cause the sidewall drilling of the polysilicon hole.

[0010] Preferably, the SF 6 The flow rate is controlled at 10-40 sccm. It can help control the morphology and selectivity of etching.

[0011] Preferably, the chamber pressure is controlled at 15 to 30 mTorr. The chamber pressure refers to the pressure of the reaction chamber inside the etching device. Here, the chamber pressure is set between 15 and 30 mTorr (mTorr, a unit of pressure) to ensure stability and efficiency during the etching process.

[0012] Preferably, during the bombardment, the RF power is controlled at 300-600 W, and the bias power is controlled at 20-100 W. This RF power range helps to generate appropriate plasma, thereby effectively etching, and the bias power can affect the uniformity and selectivity of etching, so the appropriate power can control the bombardment intensity to control the etching rate.

[0013] Preferably, the auxiliary etching gas also includes O 2 and / or CHF 3 The additional auxiliary etching gas can further dilute the SF 6 The reaction of the gas can be used to adjust the etching rate and selectivity, prevent undercutting, and help reduce post-etching residues.

[0014] Preferably, the auxiliary etching gas uses O 2 and / or CHF 3 When the flow rate of a single gas is controlled at 50sccm or less.

[0015] The substantial effects of the present invention include: when etching silicon and polysilicon simultaneously, HBr is used as the main etching gas, SF 6 As an auxiliary etching gas, the reaction principle is: Si+Brˉ->SiBr 4 +eˉHBr, this reaction is compared with SF 6 As the main etching gas, the anisotropic reaction is very small, and a large amount of polymer will be generated during HBr etching to protect the side wall, which will not cause the side wall drilling of polysilicon holes. However, since the HBr etching rate is very slow, a small amount of SF 6 Generally speaking, the present invention mainly relies on physical bombardment for etching, the overall etching rate is not fast, the etching depth can be better controlled, and the morphology of silicon holes and polysilicon holes can be better improved.

[0016] For shallow process depth, if the etching rate is too fast, it will be difficult to control the etching depth, which may also cause abnormal morphology. However, if SF is not used at all, 6 Gas will cause the etching rate to be extremely slow, affecting the process efficiency. Therefore, a small amount of SF is added to the gas used. 6 Improve the etching rate, but compared with the main use of SF 6 Compared with the existing etching technology, the etching depth and morphology can be better controlled. In the preferred embodiment, other auxiliary etching gases can also be used to dilute the SF 6 The reaction of the gas prevents drilling and further ensures the consistency of the etched hole morphology of different materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Schematic diagram of etching holes according to an embodiment of the present invention. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution will be clearly and completely described below in combination with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] It should be understood that in various embodiments of the present invention, the size of the sequence number of each process does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.

[0020] It should be understood that in the present invention, "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products or apparatuses.

[0021] It should be understood that in the present invention, "plurality" refers to two or more than two. "And / or" is merely a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The character " / " generally indicates that the objects associated before and after are in an "or" relationship. "Contains A, B and C", "Contains A, B, C" means that A, B, and C are all included, "Contains A, B or C" means that one of A, B, and C is included, and "Contains A, B and / or C" means that any one, any two, or any three of A, B, and C are included.

[0022] The technical solution of the present invention is described in detail with specific embodiments below. The embodiments may be combined with each other, and the same or similar concepts or processes may not be described in detail in some embodiments.

[0023] Embodiment 1: A method for etching silicon and polysilicon compatible with each other, in the case of Figure 1 When silicon and polysilicon are etched simultaneously (the uppermost layer is silicon oxide), HBr is used as the main etching gas, and SF 6 As auxiliary etching gas, the etching is performed in a bombardment manner until a preset etching time or a preset etching depth is reached.

[0024] Generally speaking, the flow rate of the main etching gas is three times or more than that of the auxiliary etching gas. In this embodiment, the flow rate of HBr is controlled at 150-300 sccm, and the flow rate of SF 6 The flow rate is controlled at 10-40 sccm. Among them, sccm refers to standard cubic centimeters per minute. It should be noted that the flow rate of the gas can be adjusted in real time within the above range during the entire etching process, or it can be fixed to a certain value within the above range. For example, the flow rate of HBr is 200 sccm, and the flow rate of SF 6 The flow rate is 25sccm.

[0025] In this embodiment, HBr is used as the main etching gas, SF 6 As an auxiliary etching gas, the reaction principle is: Si+Brˉ->SiBr 4 +eˉHBr, this reaction is compared with SF 6As the main etching gas, the anisotropic reaction is very small, and a large amount of polymer will be generated during HBr etching to protect the side wall, which will not cause the side wall drilling of polysilicon holes. However, since the HBr etching rate is very slow, a small amount of SF 6 To increase the etching rate. 6 The etching speed can be appropriately increased to help control the etching morphology and selectivity.

[0026] At the same time, in this embodiment, the chamber pressure is controlled at 15 to 30 mt. The chamber pressure refers to the pressure of the reaction chamber inside the etching equipment. Here, the chamber pressure is set between 15 and 30 mt (mTorr, a unit of pressure), which can ensure the stability and efficiency of the etching process. Similarly, the chamber pressure can be adjusted in real time within the above range, or it can be fixed to a certain value within the above range, for example, the chamber pressure is set at 22 mt.

[0027] In this embodiment, during bombardment, the RF power is controlled at 300-600W, and the bias power is controlled at 20-100W. This RF power range helps to generate appropriate plasma, thereby effectively etching, and the bias power can affect the uniformity and selectivity of etching, so the appropriate power can control the bombardment intensity to control the etching rate. Generally speaking, the power during the bombardment process is fixed to a value within the above range, for example, the RF power is controlled at 450W and the bias power is controlled at 60W, but in some cases, it can also be adjusted in real time within the above range.

[0028] After all the parameters are set, gas is introduced into the etching chamber, and after the pressure is stabilized, the step of applying radio frequency is started for etching.

[0029] In general, the present invention mainly relies on physical bombardment for etching, the overall etching rate is not fast, the etching depth can be better controlled, and the morphology of silicon holes and polysilicon holes can be better improved.

[0030] like Figure 1 As shown, in the hole etching, there is a small part of the opening position on poly (polycrystalline silicon). During the etching process, Si and poly will be etched at the same time. The etching process is controlled by the above scheme, taking into account the morphology of silicon holes and polycrystalline silicon holes.

[0031] Embodiment 2: This embodiment provides another etching method compatible with etching silicon and polysilicon. The overall scheme is consistent with the first embodiment, except that the auxiliary etching gas also includes O 2 .

[0032] In addition, in this embodiment, the flow rate of HBr is controlled at 300 sccm, and the flow rate of SF 6The flow rate is controlled at 40 sccm, O 2 The flow rate is controlled at 50sccm. The chamber pressure is controlled at 30mt. The RF power is controlled at 600W and the bias power is controlled at 100W.

[0033] O 2 Can dilute SF 6 The reaction of the gas can be used to adjust the etching rate and selectivity, prevent undercutting, and help reduce post-etching residues.

[0034] Embodiment three: This embodiment provides another etching method compatible with etching silicon and polysilicon. The overall scheme is consistent with the first embodiment, except that the auxiliary etching gas also includes O 2 and CHF 3 .O 2 and CHF 3 The flow rate is controlled below 50sccm.

[0035] The additional auxiliary etching gas is mainly used to dilute SF 6 The reaction of the gas can be used to adjust the etching rate and selectivity, prevent undercutting, and help reduce post-etching residues.

[0036] In summary, the substantial effects of the above embodiments include: Use HBr as the main etching gas, SF 6 As an auxiliary etching gas, compared with SF 6 As the main etching gas, the anisotropic reaction is very small, and a large amount of polymer will be generated during HBr etching to protect the side wall, which will not cause the side wall drilling of polysilicon holes. Adding a small amount of SF 6 The etching rate can be appropriately increased to help control the etching morphology and selectivity.

[0037] For shallow process depth, if the etching rate is too fast, it will be difficult to control the etching depth, which may also cause abnormal morphology. However, if SF is not used at all, 6 Gas will cause the etching rate to be extremely slow, affecting the process efficiency. Therefore, a small amount of SF is added to the gas used. 6 Improve the etching rate, but compared with the main use of SF 6 Compared with the existing etching technology, it can better control the etching depth and morphology. If necessary, other auxiliary etching gases can also be used to dilute SF 6 The reaction of the gas prevents drilling and further ensures the consistency of the etched hole morphology of different materials.

[0038] In the embodiments provided in the present application, it should be understood that the disclosed structures and methods can be implemented in other ways. For example, some features can be ignored or not performed. Some or all of the features can be selected according to actual needs to achieve the purpose of the present embodiment.

[0039] The above contents are only specific implementation methods of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. An etching method compatible with etching silicon and polysilicon, characterized in that: HBr is used as the main etching gas, SF6 is used as the auxiliary etching gas, and the etching is performed in a bombardment manner until a preset etching time or a preset etching depth is reached.

2. The etching method for etching silicon and polysilicon compatible according to claim 1, characterized in that: The flow rate of the main etching gas is three times or more than that of the auxiliary etching gas.

3. The etching method for etching silicon and polysilicon compatible according to claim 1, characterized in that: The flow rate of HBr is controlled at 150-300 sccm.

4. The etching method for etching silicon and polysilicon compatible according to claim 1, characterized in that: The flow rate of SF6 is controlled at 10-40 sccm.

5. The etching method for etching silicon and polysilicon compatible according to claim 1, characterized in that: The chamber pressure is controlled at 15-30 mt.

6. The etching method for etching silicon and polysilicon compatible according to claim 1, characterized in that: During the bombardment, the radio frequency power is controlled within the range of 300-600W, and the bias power is controlled within the range of 20-100W.

7. The etching method for etching silicon and polysilicon compatible according to claim 1, characterized in that: The auxiliary etching gas also includes O2 and / or CHF3.

8. The etching method for etching silicon and polysilicon compatible according to claim 6, characterized in that: When O2 and / or CHF3 are used as the auxiliary etching gas, the flow rate of each gas is controlled at 50 sccm or less.