Method for improving uniformity and reducing surface damage after p-GaN corrosion
By employing ICP etching and atomic layer etching techniques, the surface damage and inhomogeneity issues following GaN wet etching have been resolved, resulting in higher etching uniformity and surface quality, thereby improving device performance and reliability.
Patent Information
- Application Number
- CN202410965331.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-01
AI Technical Summary
In existing GaN processing methods, the problems of high surface damage and uneven corrosion caused by wet etching have not been effectively solved.
By employing ICP etching technology combined with atomic layer etching, and through the recycling of oxygen and boron trichloride gas, GaN oxidation and etching are performed, avoiding the damage and inhomogeneity of wet etching.
It effectively reduces damage to the GaN surface, improves corrosion uniformity, avoids lattice damage and anisotropic corrosion, and enhances device performance and reliability.
Smart Images

Figure CN118888438A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor processing technology, and in particular to a method for improving uniformity and reducing surface damage after p-GaN corrosion. Background Art
[0002] GaN (gallium nitride) materials are considered to be the third generation of new wide bandgap semiconductor materials after the first generation of silicon germanium semiconductor materials and GaAs and InP compound semiconductor materials. The advantages of the third generation semiconductor materials represented by GaN are mainly reflected in: (1) extremely large bandgap width: it can bring great anti-breakdown capability, so that the device can adapt to normal operation under high voltage. At the same time, the large bandgap width also allows the device to work at very high temperatures without failure; (2) extremely high breakdown field strength: the breakdown field strength of GaN itself is one order of magnitude higher than that of Si. Materials with high breakdown field strength can achieve very high power performance. (3) high electron saturation drift rate: high electron saturation drift rate can ensure that the device still has a high electron mobility under high electric field conditions, that is, it has a high current density, so that the device can obtain a large power output density. In addition, high electron saturation drift rate can also increase the switching speed of the device, ensuring that wide bandgap-based devices are applied in high-frequency fields. Direct wide bandgap semiconductor GaN has the advantages of high thermal conductivity, high mobility, high breakdown voltage, etc., so it is widely used in short-wavelength optoelectronic devices and high-frequency and high-power electronic devices.
[0003] At present, in the GaN processing process, in order to obtain a suitable table, there are usually two processes: dry etching and wet etching. Dry etching is prone to damage, such as dangling bonds, surface states, etc. These etching damages will not only form non-radiative recombination centers, seriously affecting the internal quantum efficiency of the laser, but also produce strong light absorption, affecting the internal loss of the laser; when using wet etching, the corrosion of chemicals will cause greater damage to the corrosion table and the table will be rougher. Summary of the invention
[0004] The present application provides a method for improving uniformity and reducing surface damage after p-GaN etching, so as to solve the technical problems of high surface damage and uneven etching after the existing wet etching of GaN.
[0005] On the one hand, the present application provides a method for improving uniformity and reducing surface damage after p-GaN etching, the method comprising the following steps:
[0006] Step S1: placing the wafer on a glue spinning machine, vacuuming and dripping glue on the surface of the wafer, and then starting the process so that the photoresist is evenly coated on the surface of the wafer;
[0007] Step S2: placing the wafer after the spin coating on a heating table for baking to better bond the wafer to the photoresist and remove the solvent in the photoresist;
[0008] Step S3: placing the wafer baked in step S2 on the wafer stage of the photolithography machine and fixing it by vacuum suction, and after the vacuum value reaches the requirement, selecting the exposure time for photolithography;
[0009] Step S4: releasing the vacuum state, removing the wafer, and placing it in a developer for development;
[0010] Step S5: After the wafer is hardened and coated with glue, it is placed in a GaN etching solution for etching, and the wafer is shaken up and down during the etching process to prevent jamming;
[0011] Step S6: After placing the etched wafer with the front side facing upward on the carrier plate, the carrier plate is placed into the chamber of the etcher to evacuate the chamber. When the vacuum value reaches the set value, it is sent into the etching projection chamber and a specific gas is introduced for etching.
[0012] In one implementation of the present application, in the step S1, the wafer is spun, and a positive photoresist is used as the photoresist.
[0013] In one implementation of the present application, the wafer is spun, and the thickness of the photoresist spun is 3.8 μm.
[0014] In one implementation of the present application, in the step S2, the heating temperature of the carrier used in the pre-baking is 100±5°C, and the baking time is 2 minutes.
[0015] In one implementation of the present application, in step S3, the exposure amount during the exposure operation is 80 mj, and the vacuum value is set to a relative vacuum value of less than -70 KPa.
[0016] In one implementation of the present application, in step S4, tetramethylammonium hydroxide is used for development during the wafer development process, the developer temperature is controlled at 20±3°C, the development time is 2 minutes, and the flower basket is shaken up and down once every 1-1.5 seconds during the development process.
[0017] In one implementation of the present application, in step S5, the temperature used for hardening the film is 150° C., the hardening time is 15 minutes, and after hardening the film, a plasma glue machine is used for glue application.
[0018] In one implementation of the present application, in step S5, the GaN etching solution uses a hot solution of phosphoric acid, and an 85wt% phosphoric acid solution is used for etching during the etching process, and the solution temperature is maintained at 100°C.
[0019] In one implementation of the present application, in step S6, when an inductively coupled plasma etcher is used for etching, O2 gas is introduced after the vacuum degree in the chamber reaches 5.5mTorr, with an oxygen flow rate of 20sccm, an ICP power of 400W, an RF power of 300W, and an oxidation etching time of 5min; after etching, BCl3 gas is introduced with a BCl3 flow rate of 5sccm, an ICP power of 500W, an RF power of 60W, and an etching time of 2min to oxidize GaN, and then BCl3 gas is introduced to etch away the generated oxide layer without causing too much damage to the GaN surface, and this cycle is repeated to reduce the surface unevenness and damage caused by wet etching.
[0020] The present application provides a method for improving uniformity and reducing surface damage after p-GaN etching, which uses ICP etching to reduce surface unevenness and corrosion damage caused by wet etching. Wet chemical etching is usually used for surface texturing of group III nitride material systems because it has the characteristics of simple equipment setup, no lattice damage, scalability and good selectivity. However, the use of wet etching has the disadvantages of low corrosion rate and easy anisotropy of corrosion, which can be avoided as much as possible by dry etching. Therefore, the etching technology for reducing GaN surface damage based on wet etching can effectively avoid this problem.
[0021] The etching principle mentioned in this application is based on atomic layer etching technology. Atomic layer etching (ALE) is a relatively unique and advantageous etching method. ALE is a technology that uses continuous self-limiting reactions to remove thin layers of material. The method is characterized by continuously repeating two steps to achieve a sufficient etching depth. The first step is generally to modify the surface of the etched material by oxidation and the second step is to selectively remove the oxide formed in the first step by dry etching.
[0022] In this application, oxygen and boron trichloride gas are used to achieve the purpose of atomic layer etching. It is suitable for the process of reducing surface damage and improving corrosion uniformity after wet etching of GaN-related structural products. The whole process is simple and easy to implement. Etching is used to ensure the uniformity of the corrosion surface and reduce surface damage. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0024] Figure 1 A flow chart of a method for improving uniformity and reducing surface damage after p-GaN etching provided in an embodiment of the present application. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present application clearer, the technical solution of the present application will be clearly and completely described below in combination with the specific embodiments of the present application and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
[0026] The embodiment of the present application provides a method for improving uniformity and reducing surface damage after p-GaN corrosion. The technical solution proposed in the embodiment of the present application is described in detail below with reference to the accompanying drawings.
[0027] Figure 1 A flow chart of a method for improving uniformity and reducing surface damage after p-GaN etching provided in an embodiment of the present application. Figure 1 As shown, the method mainly includes the following steps:
[0028] Step S1: placing the wafer on a glue spinning machine, vacuuming and dripping glue on the surface of the wafer, and then starting the process so that the photoresist is evenly coated on the surface of the wafer;
[0029] Step S2: placing the wafer after the spin coating on a heating table for baking to better bond the wafer to the photoresist and remove the solvent in the photoresist;
[0030] Step S3: placing the wafer baked in step S2 on the wafer stage of the photolithography machine and fixing it by vacuum suction, and after the vacuum value reaches the requirement, selecting the exposure time for photolithography;
[0031] Step S4: releasing the vacuum state, removing the wafer, and placing it in a developer for development;
[0032] Step S5: After the wafer is hardened and coated with glue, it is placed in a GaN etching solution for etching, and the wafer is shaken up and down during the etching process to prevent jamming;
[0033] Step S6: After placing the etched wafer with the front side facing upward on the carrier plate, the carrier plate is placed into the chamber of the etcher to evacuate the chamber. When the vacuum value reaches the set value, it is sent into the etching projection chamber and a specific gas is introduced for etching.
[0034] In the embodiment of the present application, in the step S1, the wafer is spun and a positive photoresist is used as the photoresist.
[0035] In the embodiment of the present application, the wafer is spun, and the thickness of the photoresist spun is 3.8 μm.
[0036] In the embodiment of the present application, in the step S2, the heating temperature of the support platform used in the pre-baking is 100±5°C, and the baking time is 2 minutes.
[0037] In the embodiment of the present application, in the step S3, the exposure amount during the exposure operation is 80mj, and the vacuum value is set to a relative vacuum value of less than -70KPa.
[0038] In the embodiment of the present application, in the step S4, tetramethylammonium hydroxide is used for development during the wafer development process, the developer temperature is controlled at 20±3°C, the development time is 2 minutes, and the flower basket is shaken up and down once every 1-1.5 seconds during the development process.
[0039] In the embodiment of the present application, in the step S5, the temperature used during the hardening of the film is 150° C., the hardening time is 15 minutes, and after the hardening of the film, a plasma glue machine is used for glue application.
[0040] In the embodiment of the present application, in step S5, the GaN etching solution uses a hot solution of phosphoric acid, and an 85wt% phosphoric acid solution is used for etching during the etching process, and the solution temperature is maintained at 100°C.
[0041] In the embodiment of the present application, in the step S6, when an inductively coupled plasma etcher is used for etching, O2 gas is introduced after the vacuum degree in the chamber reaches 5.5mTorr, with an oxygen flow rate of 20sccm, an ICP power of 400W, an RF power of 300W, and an oxidation etching time of 5min; after etching, BCl3 gas is introduced with a BCl3 flow rate of 5sccm, an ICP power of 500W, an RF power of 60W, and an etching time of 2min to oxidize GaN, and then BCl3 gas is introduced to etch away the generated oxide layer without causing too much damage to the GaN surface, and this cycle is repeated to reduce the surface unevenness and damage caused by wet etching.
[0042] The present application provides a method for improving uniformity and reducing surface damage after p-GaN etching, which uses ICP etching to reduce surface unevenness and corrosion damage caused by wet etching. Wet chemical etching is usually used for surface texturing of group III nitride material systems because it has the characteristics of simple equipment setup, no lattice damage, scalability and good selectivity. However, the use of wet etching has the disadvantages of low corrosion rate and easy anisotropy of corrosion, which can be avoided as much as possible by dry etching. Therefore, the etching technology for reducing GaN surface damage based on wet etching can effectively avoid this problem.
[0043] The etching principle mentioned in this application is based on atomic layer etching technology. Atomic layer etching (ALE) is a relatively unique and advantageous etching method. ALE is a technology that uses continuous self-limiting reactions to remove thin layers of material. The method is characterized by continuously repeating two steps to achieve a sufficient etching depth. The first step is generally to modify the surface of the etched material by oxidation and the second step is to selectively remove the oxide formed in the first step by dry etching.
[0044] In this application, oxygen and boron trichloride gas are used to achieve the purpose of atomic layer etching. It is suitable for the process of reducing surface damage and improving corrosion uniformity after wet etching of GaN-related structural products. The whole process is simple and easy to implement. Etching is used to ensure the uniformity of the corrosion surface and reduce surface damage.
[0045] Each embodiment in this application is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the device embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0046] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the process, method, commodity or device including the elements.
[0047] The above is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. A method for improving uniformity and reducing surface damage after p-GaN etching, characterized in that: The method comprises the following steps: Step S1: placing the wafer on a glue spinning machine, vacuuming and dripping glue on the surface of the wafer, and then starting the process so that the photoresist is evenly coated on the surface of the wafer; Step S2: placing the wafer after the spin coating on a heating table for baking to better bond the wafer to the photoresist and remove the solvent in the photoresist; Step S3: placing the wafer baked in step S2 on the wafer stage of the photolithography machine and fixing it by vacuum suction, and after the vacuum value reaches the requirement, selecting the exposure time for photolithography; Step S4: releasing the vacuum state, removing the wafer, and placing it in a developer for development; Step S5: After the wafer is hardened and coated with glue, it is placed in a GaN etching solution for etching, and the wafer is shaken up and down during the etching process to prevent jamming; Step S6: After placing the etched wafer with the front side facing upward on the carrier plate, the carrier plate is placed into the chamber of the etcher to evacuate the chamber. When the vacuum value reaches the set value, it is sent into the etching projection chamber and a specific gas is introduced for etching.
2. The method for improving uniformity and reducing surface damage after p-GaN etching according to claim 1, characterized in that: In the step S1, the wafer is spun, and a positive photoresist is used as the photoresist.
3. The method for improving uniformity and reducing surface damage after p-GaN etching according to claim 2, characterized in that: The wafer is spun, and the thickness of the photoresist spun is 3.8 μm.
4. The method for improving uniformity and reducing surface damage after p-GaN etching according to claim 1, characterized in that: In the step S2, the heating temperature of the support platform used in the pre-baking is 100±5°C, and the baking time is 2 minutes.
5. The method for improving uniformity and reducing surface damage after p-GaN etching according to claim 1, characterized in that: In the step S3, the exposure amount during the exposure operation is 80 mj, and the vacuum value is set to a relative vacuum value of less than -70 KPa.
6. The method for improving uniformity and reducing surface damage after p-GaN etching according to claim 1, characterized in that: In the step S4, tetramethylammonium hydroxide is used for developing during the wafer development process, the developer temperature is controlled at 20±3° C., the developing time is 2 minutes, and the flower basket is shaken up and down once every 1-1.5 seconds during the developing process.
7. The method for improving uniformity and reducing surface damage after p-GaN etching according to claim 1, characterized in that: In the step S5, the temperature used for hardening the film is 150° C., the hardening time is 15 minutes, and after hardening the film, a plasma glue machine is used for glue application.
8. The method for improving uniformity and reducing surface damage after p-GaN etching according to claim 1, characterized in that: In step S5, the GaN etching solution uses a hot solution of phosphoric acid, and an 85 wt % phosphoric acid solution is used for etching during the etching process, and the solution temperature is maintained at 100° C.
9. The method for improving uniformity and reducing surface damage after p-GaN etching according to claim 1, characterized in that: In the step S6, when an inductively coupled plasma etcher is used for etching, O2 gas is introduced after the vacuum degree in the chamber reaches 5.5mTorr, with an oxygen flow rate of 20sccm, an ICP power of 400W, an RF power of 300W, and an oxidation etching time of 5min; after etching, BCl3 gas is introduced with a BCl3 flow rate of 5sccm, an ICP power of 500W, an RF power of 60W, and an etching time of 2min to oxidize GaN, and then BCl3 gas is introduced to etch away the generated oxide layer without causing too much damage to the GaN surface, and this cycle is repeated to reduce the surface unevenness and damage caused by wet etching.
Citation Information
Cited By
Method and equipment for accurately removing post-aluminum corrosion product based on wet pretreatment and atomic layer etching
CN122438531A
A method and equipment for precise removal of post-corrosion products in aluminum based on wet pretreatment and atomic layer etching.
CN122438531B