Membrane electrode material, preparation method thereof and sodium ion battery
By generating two-dimensional layered MXene on the surface of Wood alloy, the problems of low sodium storage capacity and poor electrochemical stability of the negative electrode material of sodium ion battery are solved, and the effects of high energy density and long-term stable operation are achieved, which significantly improves the electrochemistry of the battery Performance and cycling performance.
Patent Information
- Application Number
- CN202411174827.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-01
AI Technical Summary
The existing sodium ion battery negative electrode materials have low sodium storage capacity and poor electrochemical stability, which easily create dendrite and safety hazards. The volume of the alloy material changes greatly during sodium embedding/desodium removal, resulting in electrode powdering and circulation performance. It is excellent and difficult to meet the needs of high energy density and long-term stable operation.
Two-dimensional layered MXene is generated on the surface of Wood alloy, and MXene modified Wood alloy thin-film electrode material is prepared. By adjusting the immersion time of MXene, its thickness is adjusted, the conductivity and structural stability of the material are improved, the electrochemical performance is improved, and the sodium ions are adjusted. Sodium-embedded/desodium pathway.
It improves the electrochemical performance and cycling performance of the battery, increases the capacity of the negative electrode, adapts to the needs of high energy density, and meets the needs of long-term and stable operation, avoids volume changes and electrode powdering, and significantly improves the rate performance and Coulomb efficiency.
Smart Images

Figure CN118888677A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries, and specifically relates to a thin film electrode material and a preparation method thereof, and a sodium ion battery. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] As an emerging energy storage technology, sodium-ion batteries are regarded as a strong competitor to lithium-ion batteries due to their abundant sodium resources, low cost and stable electrochemical performance. They have received widespread attention and in-depth research in recent years.
[0004] As an important component of sodium-ion batteries, negative electrode materials will directly affect the performance of batteries. At present, negative electrode materials for sodium-ion batteries mainly include carbon-based materials, pure metal materials and alloy materials. Among them, the sodium storage capacity of carbon-based materials is relatively low, which is difficult to meet the needs of high energy density. Pure metal materials have poor electrochemical stability and are prone to produce dendrites during the charging and discharging process, causing safety hazards. Alloy materials have received widespread attention due to their high theoretical capacity and stable structure. However, alloy materials are prone to severe volume changes during the sodium insertion / de-sodiumization process, resulting in powdering of electrode materials and capacity attenuation. At the same time, the cycle performance of alloy materials is poor, which is difficult to meet the needs of long-term stable operation. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a thin film electrode material, a preparation method thereof and a sodium ion battery. By generating a two-dimensional layered MXene on the surface of Wood's alloy, a MXene-modified Wood's alloy thin film electrode material is obtained, which improves the conductivity and stability of the material, thereby improving its electrochemical performance.
[0006] In order to achieve the above object, the technical solution of the present invention is:
[0007] In a first aspect, a method for preparing a thin film electrode material comprises the following steps:
[0008] S1, heating the Wood's alloy to a molten state at 80-100° C., and then coating a Wood's alloy layer with a thickness of 5-100 μm on a metal foil to obtain an electrode material;
[0009] S2. Prepare a MXene solution with a concentration of 1 to 2 mg / mL; the MXene includes: one or more of titanium-based MXene, niobium-based MXene, vanadium-based MXene and molybdenum-based MXene.
[0010] S3. Soak the electrode material obtained in S1 in the MXene solution obtained in S2 for 0.5 to 12 hours, take it out and dry it at 35 to 55° C. for 1 to 2 hours to obtain a thin film electrode material.
[0011] Optionally, in S1, the metal foil includes: copper foil, aluminum foil or silver foil; the thickness of the metal foil is 10 to 20 μm.
[0012] Optionally, in S1, the components and proportions of the Wood's alloy include: 50% bismuth (Bi), 25% lead (Pb), 12.5% tin (Sn) and 12.5% cadmium (Cd).
[0013] Optionally, in S2, the solvent of the MXene solution is water.
[0014] Optionally, in S2, the general formula of the MXene is M n+1 X n T x , n=1-3; wherein M represents a transition metal, including: one of Ti, Nb, V and Mo; X represents C or N; T represents a functional group, including: one of -OH, -F and -O.
[0015] Optionally, the MXene is one of Ti3AlC2, Nb2AlC, V2AlC or MO2TiC2.
[0016] Optionally, in S3, the MXene solution is maintained at room temperature.
[0017] In the second aspect, the thin film electrode material prepared by the above-mentioned method for preparing thin film electrode material has a two-dimensional layered MXene material covered on the surface of the Wood's alloy layer of the electrode material, and the thickness of the MXene material layer is 50nm to 1μm.
[0018] In a third aspect, a sodium ion battery comprises a battery negative electrode, wherein the battery negative electrode comprises the above-mentioned thin film electrode material.
[0019] Optionally, the working electrode of the sodium ion battery is metallic sodium; the electrolyte of the sodium ion battery includes: a diethylene glycol dimethyl ether solution of NaPF6, and the concentration of NaPF6 is 1 to 1.5M.
[0020] The beneficial effects of the present invention are:
[0021] The preparation method of the present invention is simple, Wood's alloy can be used to prepare electrodes by a scraping method, and the thickness of the two-dimensional layered MXene can be adjusted by changing the immersion time. The process is simple, efficient, safe and non-toxic. The present invention uses Wood's alloy as the negative electrode material. Wood's alloy, as an alloying material, includes a variety of metal components. It can utilize the influence of a variety of metal atoms in the alloy on the surface migration energy barrier of sodium atoms to improve the performance of the composite negative electrode, so that the capacity of the battery negative electrode is larger and meets the requirements of high energy density; a MXene layer is prepared on the surface of Wood's alloy. The hierarchical porous structure and good mechanical properties of the MXene layer have higher reaction activity, effectively improve the electrochemical performance of the battery, and can effectively adjust the sodium ion insertion / de-sodiumization path to avoid serious volume changes and improve the cycle performance of the electrode to meet the needs of long-term stable operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0023] Figure 1 This is a physical photo of the MXene-modified Wood's alloy thin film electrode material prepared in Example 1 of the present invention.
[0024] Figure 2 This is the locally enlarged SEM detection result of the MXene-modified Wood's alloy thin film electrode material prepared in Example 1 of the present invention.
[0025] Figure 3 These are the SEM test results of the MXene-modified Wood's alloy thin film electrode material prepared in Example 1 of the present invention.
[0026] Figure 4 This is a rate performance test diagram of the MXene-modified Wood's alloy thin film electrode material prepared in Example 1 of the present invention as a negative electrode material for a sodium ion battery.
[0027] Figure 5 This is a test diagram of the cycling performance of the MXene-modified Wood's alloy thin film electrode material prepared in Example 1 of the present invention as a negative electrode material for a sodium ion battery.
[0028] Figure 6 This is a physical photo of the Wood's alloy electrode material prepared in Comparative Example 1 of the present invention.
[0029] Figure 7 This is the locally enlarged SEM detection result of the Wood's alloy electrode material prepared in Comparative Example 1 of the present invention.
[0030] Figure 8 This is the SEM test result of the Wood's alloy electrode material prepared in Comparative Example 1 of the present invention.
[0031] Fig. 9 This is a rate performance test diagram of the Wood's alloy electrode material prepared in Comparative Example 1 of the present invention as a negative electrode material for a sodium ion battery. DETAILED DESCRIPTION
[0032] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0033] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0034] Example 1
[0035] A method for preparing a thin film electrode material of MXene-modified Wood's alloy comprises the following steps:
[0036] S1. After heating the Wood's alloy to a molten state at 100° C., a Wood's alloy layer with a thickness of 5 μm is scraped onto a copper foil, and the copper foil with the Wood's alloy attached is cut into a circular electrode piece with a diameter of 10 mm to obtain an electrode material;
[0037] S2. Select Ti3AlC2 from titanium-based MXene as raw material, prepare a Ti3AlC2 aqueous solution with a concentration of 1 mg / mL, and keep it at room temperature.
[0038] S3. Soak the electrode material in a MXene aqueous solution at room temperature for 0.5 h, take it out and dry it at 40° C. for 1 h to obtain a thin film electrode material.
[0039] The composition of Wood's alloy used in S1 is: 50% bismuth (Bi), 25% lead (Pb), 12.5% tin (Sn) and 12.5% cadmium (Cd), and the melting point is 70°C.
[0040] The actual photo of the thin film electrode material of MXene modified Wood's alloy prepared in this example is as follows: Figure 1 shown.
[0041] Example 2
[0042] The raw materials and raw material requirements in this embodiment are the same as those in Example 1.
[0043] In the preparation method, different immersion times are selected in S3, and other preparation methods are the same as those in Example 1, so as to obtain a series of thin film electrode materials.
[0044] The immersion times in S3 were: 1 h, 2 h, 4 h, 6 h and 12 h.
[0045] Example 3
[0046] In this embodiment, Nb2AlC in niobium-based MXene is selected as the preparation raw material, and the requirements for other raw materials are the same as those in Example 1.
[0047] In the preparation method, in S2, Nb2AlC in niobium-based MXene is selected as a preparation raw material to prepare a MXene aqueous solution with a concentration of 1 mg / mL;
[0048] In S3, the soaking time is 1 h.
[0049] The other preparation methods are the same as those in Example 1 to obtain a thin film electrode material.
[0050] Example 4
[0051] In this embodiment, V2AlC in vanadium-based MXene is selected as the preparation raw material, and the requirements for other raw materials are the same as those in Example 1.
[0052] In the preparation method, in S2, V2AlC in vanadium-based MXene is selected as a preparation raw material to prepare a MXene aqueous solution with a concentration of 1 mg / mL;
[0053] The other preparation methods are the same as those in Example 1 to obtain a thin film electrode material.
[0054] Example 5
[0055] In this embodiment, MO2TiC2 in molybdenum-based MXene is selected as the preparation raw material, and the requirements for other raw materials are the same as those in Example 1.
[0056] In the preparation method, in S2, MO2TiC2 in molybdenum-based MXene is selected as the preparation raw material to prepare a MXene aqueous solution with a concentration of 1 mg / mL;
[0057] The other preparation methods are the same as those in Example 1 to obtain a thin film electrode material.
[0058] Comparative Example 1
[0059] The difference between this comparative example and comparative example 1 is that after the Wood's alloy is scraped and cut into pieces, the thin film electrode material is not soaked in MXene solution. Figure 6 As shown, the surface of the un-immersed Wood alloy pole piece is silvery white.
[0060] The prepared electrode materials were subjected to performance testing, including SEM testing, MXene two-dimensional sheet thickness testing and electrochemical performance testing.
[0061] SEM inspection
[0062] The SEM test results of the surface of the thin film electrode material prepared in Example 1 are as follows: Figure 3 As shown, the SEM test results with a larger magnification are as follows Figure 2 As shown, it can be seen that MXene two-dimensional flakes are generated on the surface of Wood's alloy material and are distributed relatively evenly.
[0063] The SEM test results of the surface of the thin film electrode material prepared in Comparative Example 1 are as follows: Figure 8 As shown, the SEM test results with a larger magnification are as follows Figure 7 As shown, it can be seen that after scraping, the surface of pure Wood alloy is relatively smooth and has many nanopores distributed thereon.
[0064] Thickness detection
[0065] The thin film electrode materials of Example 1 and Example 2 with different immersion times were tested by observing the cross section through a scanning electron microscope.
[0066] The test results show that the thickness of the MXene two-dimensional sheet in Example 1 is 50 nm.
[0067] In Example 2, as the immersion time gradually increases, the thickness increases from 70 nm to 1 μm.
[0068] It can be seen that by adjusting the immersion time, the thickness of the MXene two-dimensional sheet on the surface of Wood's alloy can be effectively adjusted, and the longer the immersion time, the greater the thickness; accordingly, a thin film electrode material with a set MXene two-dimensional sheet thickness can be prepared.
[0069] Electrochemical performance testing
[0070] The MXene modified Wood alloy electrode sheet with a diameter of 10 mm prepared in Experimental Example 1 was used as the negative electrode of the sodium ion battery. Metallic sodium was used as the working electrode, 1M NaPF6 was dissolved in diethylene glycol dimethyl ether (Diglyme) (100 vol%) as the electrolyte, and a glass fiber membrane (Whatman GF / C) was used as the diaphragm. The button 2032 type sodium ion battery was assembled in an argon-filled glove box and tested after standing for 12 hours. The test temperature was 30°C and the test voltage range was 0.01 to 1.5V.
[0071] The test results are as follows: Figure 4As shown, it can provide a higher specific capacity at low rates. At the same time, it has high rate stability and can still provide a relatively ideal specific capacity at high rates; it shows that MXene-modified Wood alloy thin film electrode materials as negative electrode materials for sodium ion batteries show excellent rate performance and stability at different charge and discharge current densities, with a specific capacity of up to 340mAh / g and a coulombic efficiency stable at around 99%.
[0072] Cyclic performance test results are as follows Figure 5 As shown, after 1285 cycles at a current density of 1A / g, the specific capacity is 306mAh / g and the capacity retention rate is 96.6%, indicating that the specific capacity and coulombic efficiency of the MXene-modified Wood alloy thin film electrode material did not show a significant decrease in the cycle test.
[0073] It can be seen that the two-dimensional layered MXene covered on the surface of the MXene-modified Wood's alloy thin film electrode material improves the conductivity and structural stability of the material, and the prepared MXene-modified Wood's alloy thin film electrode material has excellent rate performance and cycle stability.
[0074] The rate performance of the electrode material obtained in Comparative Example 1 was tested in the same manner. Fig. 9 As shown, the rate performance of pure Wood's alloy is poor, and the specific capacity decays significantly with the rate change. When Wood's alloy material is used as the negative electrode material of sodium ion battery for rate testing, the specific capacity decays significantly at different current densities, and the coulombic efficiency cannot be stabilized, indicating that the electrochemical performance of the material is poor due to the lack of protection of the MXene layer.
[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a thin film electrode material, characterized in that: The following steps are involved: S1, heating the Wood's alloy to a molten state at 80-100° C., and then coating a Wood's alloy layer with a thickness of 5-100 μm on a metal foil to obtain an electrode material; S2. Prepare a MXene solution with a concentration of 1 to 2 mg / mL; the MXene includes one or more of titanium-based MXene, niobium-based MXene, vanadium-based MXene and molybdenum-based MXene; S3. Soak the electrode material obtained in S1 in the MXene solution obtained in S2 for 0.5 to 12 hours, take it out and dry it at 35 to 55° C. for 1 to 2 hours to obtain a thin film electrode material.
2. The method for preparing a thin film electrode material according to claim 1, characterized in that: In S1, the metal foil includes: copper foil, aluminum foil or silver foil; the thickness of the metal foil is 10 to 20 μm.
3. The method for preparing a thin film electrode material according to claim 1, characterized in that: In S1, the composition and mass ratio of the Wood's alloy are: 50% bismuth, 25% lead, 12.5% tin and 12.5% cadmium.
4. The method for preparing a thin film electrode material according to claim 1, characterized in that: In S2, the solvent of the MXene solution is water.
5. The method for preparing the thin film electrode material according to claim 1, It is characterized in that, in S2, the general formula of the MXene is M n+1 X n T x , n=1-3; wherein M represents a transition metal, including: one of Ti, Nb, V and Mo; X represents C or N; T represents a functional group, including: one of -OH, -F and -O.
6. The method for preparing a thin film electrode material according to claim 5, characterized in that, in S2, the MXene is one of Ti3AlC2, Nb2AlC, V2AlC or MO2TiC2.
7. The method for preparing a thin film electrode material according to claim 1, characterized in that: The MXene solution in S3 was kept at room temperature.
8. A thin film electrode material prepared by the method for preparing a thin film electrode material according to any one of claims 1 to 7, characterized in that: The surface of the Wood's alloy layer of the electrode material is covered with a two-dimensional layered MXene material, and the thickness of the MXene material layer is 50nm to 1μm.
9. A sodium ion battery, comprising a negative electrode, characterized in that: The battery negative electrode comprises the thin film electrode material as claimed in claim 8.
10. The sodium ion battery according to claim 9, characterized in that: The working electrode of the sodium ion battery is metallic sodium; the electrolyte of the sodium ion battery includes: a diethylene glycol dimethyl ether solution of NaPF6, and the concentration of NaPF6 is 1 to 1.5M.
Citation Information
Patent Citations
Negative-electrode-free lithium metal battery, negative electrode current collector of negative electrode-free lithium metal battery and preparation method
CN113013417A
Vanadium-based MXene zinc negative electrode protective coating and zinc ion battery thereof
CN116799216A
Alloy negative electrode material for sodium-ion battery, electrode and preparation method and application of sodium-ion battery
CN117758129A
Negative electrodes for non-aqueous secondary batteries composed of conjugated polymer and alkali metal alloying or inserting material
EP0199175A2
Lithium ion secondary battery positive electrode and lithium ion secondary battery
JP1999003708A
Cited By
Preparation method of thin-film battery positive electrode material