Preparation method of double-layer modified lithium-sulfur battery composite diaphragm
By employing a Co/CoN4@KB two-dimensional material bilayer composite membrane in lithium-sulfur batteries, the problems of polysulfide shuttle effect and reaction kinetics were solved, achieving efficient polysulfide adsorption and catalysis, and improving the electrochemical performance and stability of the batteries.
Patent Information
- Application Number
- CN202410923756.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The shuttle effect and poor reaction kinetics of polysulfides in lithium-sulfur batteries lead to the accumulation of low-activity sulfur and insufficient utilization of active materials. Existing modified materials cannot effectively limit the shuttle of polysulfides and improve battery capacity.
A two-dimensional material bilayer composite membrane, Co/CoN4@KB, is used to construct an adsorption-catalysis layer for polysulfides on the two-dimensional material. The synergistic effect of Co clusters and CoN4 enhances the adsorption and catalytic capacity of polysulfides. Combined with the physical confinement of MXene or graphene, the transport capacity of ions and electrons is enhanced.
It improves the rate performance and cycle stability of lithium-sulfur batteries, enhances the adsorption and catalytic ability of polysulfides, reduces the shuttle effect, and extends the battery's lifespan.
Smart Images

Figure CN118888970A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of battery diaphragm materials and relates to a method for preparing a double-layer modified lithium-sulfur battery composite diaphragm. Background Art
[0002] The rapid development of science and technology has led to an increasing demand for energy in society, while the use of traditional fossil energy will cause environmental pollution, so people's demand for green and clean energy is increasing. As a typical representative of green and clean energy, lithium-ion batteries have quickly dominated the markets of mobile communication devices, portable computers, digital cameras, electric vehicles, aerospace, etc. However, due to the limitation of the theoretical capacity of its own battery materials, the energy density of lithium-ion batteries is gradually approaching the limit, but it still cannot fully meet people's demand for long-lasting devices.
[0003] Lithium-sulfur batteries have a high theoretical energy density (2675Wh kg -1 ), high theoretical capacity based on sulfur (1675 mAhg -1 ), high natural abundance and environmental friendliness, has become a hot research topic in the next generation of battery systems. Despite this, the application of lithium-sulfur batteries is still subject to severe challenges. These include the low conductivity of sulfur and its discharge products (Li2S2 / Li2S), huge volume changes, the intermediate polysulfide dissolving in the electrolyte and shuttling between the lithium anode and the sulfur cathode, and the low electron transfer and multiphase transformation sluggishness of sulfur species. Among them, the shuttling effect of polysulfide intermediates and poor reaction kinetics are the main problems, which lead to the accumulation of low-activity sulfur and insufficient utilization of active materials, further shortening the service life.
[0004] At present, people use carbon fiber, carbon nanotubes, etc. as modification of polypropylene separators to improve electronic conductivity, but the cross-linked one-dimensional structure and poor adsorption capacity still cannot effectively restrict the shuttling of polysulfides. Two-dimensional materials, such as graphene and MXene, lead to a large number of nanosheets stacking due to the van der Waals force, which affects the migration of ions. In addition, the weak catalytic ability cannot further improve the reaction kinetics of lithium-sulfur batteries, resulting in limited improvement in battery capacity. Summary of the invention
[0005] In order to overcome the above technical problems, the present invention aims to provide a method for preparing a double-layer modified lithium-sulfur battery composite membrane, which is obtained by sequentially preparing a two-dimensional material, preparing a Co / CoN4@KB composite material, and preparing a Co / CoN4@KB-two-dimensional material double-layer composite membrane. The preparation method is simple, the process is easy to control, the synthesis conditions are mild, and the cost is low. A polysulfide adsorption-catalysis layer is further constructed on the two-dimensional material. The material has the ability of polysulfide step-by-step adsorption and conversion and abundant active sites, and improves the transport capacity of ions and electrons, thereby improving the rate performance and cycle stability of lithium-sulfur batteries.
[0006] To solve the above problems, the technical solution adopted by the present invention is:
[0007] A method for preparing a double-layer modified lithium-sulfur battery composite diaphragm is carried out in the following order:
[0008] (1) Preparation of two-dimensional materials
[0009] Weigh the two-dimensional material, and dilute the prepared MXene suspension with an ethanol diluent formed by ethanol and deionized water in a volume ratio of 1:1, which is recorded as solution A;
[0010] (2) Preparation of Co / CoN4@KB composites
[0011] Cobalt acetate tetrahydrate and phenanthroline were mixed in ethanol and stirred continuously at 50°C for 3 hours; then, Ketjen black was added to the above solution and stirred at 50°C for 3 hours to form a precursor, which was then transferred to a vacuum drying oven to evaporate the solvent, and finally the obtained product was calcined under argon protection to obtain a Co / CoN4@KB composite material;
[0012] (3) Preparation of Co / CoN4@KB-2D material double-layer composite membrane
[0013] Co / CoN4@KB was dispersed in a mixed solution of ethanol and water to obtain solution B, and then a vacuum filtration device was used with a polypropylene membrane as a filter membrane to drop solution A. After the solvent was completely separated, solution B was added. After the solvent was completely separated, the loaded membrane Co / CoN4@KB-two-dimensional material was transferred to a vacuum drying oven for drying, and finally a Co / CoN4@KB-two-dimensional material double-layer composite membrane was obtained.
[0014] As a limitation of the present invention:
[0015] (i) In step (1), the concentration of the hydrochloric acid is 9 M; the mass volume ratio of the lithium fluoride to the hydrochloric acid is 0.1 g / mL.
[0016] (ii) In step (1), the concentration of solution A is 0.3 mg / mL.
[0017] (iii) In step (2), the mass ratio of cobalt acetate tetrahydrate, phenanthroline and Ketjen black is (12-60):(17-34):48;
[0018] The mass volume ratio of the Ketjen black to ethanol is 16 mg / mL.
[0019] In step (2), the mass ratio of cobalt acetate tetrahydrate and phenanthroline will directly affect the generation of Co clusters and atomically dispersed CoN4. If the ratio is too high, it will affect the generation of single-atom Co, and if the ratio is too low, no Co clusters will be generated. It is worth noting that metal Co clusters have better adsorption and catalytic ability for long-chain polysulfides, while CoN4 has better adsorption ability for short-chain polysulfides and effectively reduces the conversion energy barrier between short-chain polysulfides. Therefore, the ratio of cobalt acetate tetrahydrate and phenanthroline should be strictly controlled to ensure the coexistence of Co clusters and single-atom CoN4, so that both have good adsorption and catalytic ability for polysulfides; the mass volume ratio of Ketjen black to ethanol will affect the loading amount of Co / CoN4 active sites on the conductive carbon structure, which will affect the synergy between the active sites and the adsorption and catalytic ability for long-chain and short-chain polysulfides, thereby further affecting the electrochemical performance of the battery.
[0020] (iv) In step (2), the temperature of the evaporating solvent is 80°C.
[0021] (V) In step (2), the calcination heating rate is 10°C / min, the calcination temperature is 650°C, and the calcination time is 2h.
[0022] The calcination heating rate and calcination temperature in the present invention have a certain influence on the morphology and structure formation of Co / CoN4@KB. When the calcination temperature is greater than 650°C and the heating rate is high (greater than 10°C / min), part of the Co will rapidly crystallize at high temperature and a large number of crystal structures will appear, which is not conducive to the generation and agglomeration of atomic-level Co; when the calcination temperature is less than 650°C and the heating rate is low (less than 10°C / min), the coordination between N atoms and atomically dispersed Co is insufficient, which is not conducive to its stable Co-4N cross-linking coordination to generate CoN4 configuration.
[0023] (vi) In step (3), the concentration of solution B is 0.5 mg / mL; the amount of solution A and solution B used is 2 mL.
[0024] The concentration of solution B and the amounts of solution A and solution B will affect the thickness of the double-layer material formed by filtration, thereby affecting the electrochemical performance and the mass energy density of the battery.
[0025] (VII) In step (1), the two-dimensional material is any one of graphene materials, MXene and the like; when the two-dimensional material is MXene material, the preparation process is carried out as follows:
[0026] Ti3AlC2 powder was slowly added to a mixed solution containing lithium fluoride and hydrochloric acid and stirred vigorously at 45 °C for 24 h. The mixture was then washed with deionized water by centrifugation at 3500 rpm until the pH value of the supernatant was about 6. Finally, the prepared neutral suspension was ultrasonically treated and centrifuged for 1 h to collect Ti3C2T x MXene supernatant.
[0027] The present invention also has a limitation. In step (3), the Co / CoN4@KB-two-dimensional material double-layer composite membrane has an upper layer of a Co / CoN4@KB layer and a lower layer of a two-dimensional material layer. The thickness of the Co / CoN4@KB layer is about 5 μm.
[0028] It is well known that the thickness of the diaphragm material affects the migration and diffusion of ions and polysulfides. A too large thickness of the Co / CoN4@KB layer is conducive to blocking polysulfides but will limit the diffusion path of ions. A too small thickness is not conducive to the interception of polysulfides. Therefore, selecting the appropriate thickness has a significant effect on improving the electrochemical performance.
[0029] The beneficial effects of the above technical solution of the present invention are:
[0030] (1) The present invention uses a simple annealing method to prepare a conductive Ketjen black loaded with clustered Co and single-atom dispersed CoN4 as a highly efficient adsorption and catalytic functional material for polysulfides. The Co cluster has a better capture and catalytic ability for long-chain polysulfides, while CoN4 has a stronger adsorption effect on short-chain polysulfides and better reduces the conversion energy barrier between short-chain solid polysulfides. Therefore, by constructing a coexistence of Co clusters and CoN4, the synergistic effect of the two is exerted to enable it to more efficiently realize the capture and conversion ability of polysulfides, reduce the shuttle effect, alleviate the loss of active substances, and improve the redox reaction kinetics of the electrochemical reaction.
[0031] (2) The two-dimensional material MXene or graphene used in the present invention can further intercept the polysulfides missed by the Co / CoN4@KB layer through chemical adsorption and physical confinement, further alleviating the shuttle effect of the battery.
[0032] (3) The preparation process of the double-layer modified lithium-sulfur battery composite membrane is simple, the synthesis conditions are mild, the cost is low, and it can be extended to other low-dimensional material systems. The material has excellent ionic conductivity when used as a lithium-sulfur battery membrane material. -1The initial discharge capacity at the current density is 1233 mAh g -1 After 100 cycles, the discharge capacity is 940 mAh g -1 .
[0033] The invention is suitable for preparing a double-layer modified lithium-sulfur battery composite diaphragm.
[0034] The present invention will be further described in detail below with reference to specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Ti3C2T prepared in Example 1 x Scanning electron microscope image of MXene;
[0036] Figure 2 This is a cross-sectional scanning electron microscope image of the Co / CoN4@KB-MXene double-layer modified composite membrane prepared in Example 1;
[0037] Figure 3 X-ray diffraction spectra of Co / CoN4@KB material and KB material prepared in Example 1 and Comparative Example;
[0038] Figure 4 This is a high-resolution electron microscope image of the Co / CoN4@KB material prepared in Example 1 corrected for high-angle annular dark field spherical aberration;
[0039] Figure 5 The ionic conductivity diagrams of different modified diaphragms prepared in Example 1 and Comparative Example;
[0040] Figure 6 ion diffusion activation energy diagram of different modified membranes prepared in Example 1 and Comparative Example;
[0041] Figure 7 This is a constant potential lithium sulfide deposition curve diagram of Co / CoN4@KB material prepared in Example 1;
[0042] Figure 8 This is a constant potential lithium sulfide deposition curve of MXene material;
[0043] Fig. 9 This is the constant potential lithium sulfide deposition curve of KB material;
[0044] Fig.10 The cycle performance diagram of lithium-sulfur batteries using different modified separators prepared in Example 1 and Comparative Example;
[0045] Fig.11 The figure is a rate performance diagram of lithium-sulfur batteries using different modified separators prepared in Example 1 and Comparative Example;
[0046] Fig.12 The cyclic voltammetry curves of lithium-sulfur batteries using different modified separators prepared in Example 1 and Comparative Example are shown. DETAILED DESCRIPTION
[0047] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0048] The reagents described in the following examples are all existing reagents unless otherwise specified, and the methods described in the following examples are all existing preparation and detection methods unless otherwise specified.
[0049] Example 1 A method for preparing a double-layer modified lithium-sulfur battery composite separator
[0050] This embodiment is a method for preparing a double-layer modified lithium-sulfur battery composite separator Co / CoN4@KB-MXene, which is carried out in the following steps:
[0051] (1) Ti3C2T x Preparation of MXene nanosheets
[0052] 1 g of Ti3AlC2 powder was slowly added to a mixed solution containing 1 g of lithium fluoride and 9 M hydrochloric acid and stirred vigorously at 45 °C for 24 h. The mixture was then washed by centrifugation with deionized water until the pH value of the supernatant was about 6. Finally, the prepared neutral suspension was ultrasonically treated and centrifuged at 3500 rpm for 1 h to collect Ti3C2T x The MXene supernatant was recorded as the MXene suspension; finally, the prepared MXene suspension was diluted to 0.3 mg / mL with ethanol and deionized water (volume ratio of 1:1), recorded as solution A;
[0053] (2) Preparation of Co / CoN4@KB composites
[0054] 24 mg of cobalt acetate tetrahydrate and 17.3 mg of phenanthroline were mixed in 3 mL of ethanol and stirred continuously at 50 °C for 3 h. Subsequently, 48 mg of Ketjen black was added to the above solution and stirred at 50 °C for 3 h to form a precursor, which was then transferred to a vacuum drying oven at 80 °C to evaporate the solvent; finally, the obtained product was heated to 650 °C at a heating rate of 10 °C / min under argon protection and calcined for 2 h to obtain a Co / CoN4@KB composite material;
[0055] (3) Preparation of Co / CoN4@KB-MXene double-layer composite membrane
[0056] Co / CoN4@KB was dissolved in a mixture of ethanol and water (volume ratio of 1:1) to obtain a solution B with a concentration of 0.5 mg / mL. Then, a vacuum filtration device was used with a polypropylene membrane as a filter membrane to drop 2 mL of solution A. After the solvent was completely separated, 2 mL of solution B was added. After the solvent was completely separated, the loaded membrane Co / CoN4@KB-MXene was transferred to a vacuum drying oven and dried at 60°C to obtain a Co / CoN4@KB-MXene double-layer composite membrane.
[0057] A series of morphology and electrochemical performance tests were performed on the diaphragm prepared in this example, and the specific results are as follows:
[0058] Figure 1 The Ti3C2T prepared in this example x Scanning electron microscope image of MXene. It shows distinct edges and typical two-dimensional nanosheet structure, which can physically hinder the migration of polysulfides.
[0059] Figure 2 This is a cross-sectional scanning electron microscope image of the Co / CoN4@KB-MXene double-layer modified composite membrane prepared in this embodiment. The upper layer is Co / CoN4@KB, and the lower layer is a MXene stacking layer, which can clearly distinguish the double-layer structure between Co / CoN4-KB and MXene. The thickness of the Co / CoN4@KB catalytic layer is ~5μm, which ensures an efficient electrochemical reaction interface, alleviates the accumulation of low-conductivity dead sulfur during charging and discharging, and the cross-linked conductive network rich in active sites promotes rapid electron transfer and reaction kinetics. Due to the interaction of van der Waals forces and hydrogen bonds, MXene nanosheets are well stacked into a two-dimensional layer with a thickness of only ~69.1nm. This unique two-dimensional MXene stacking layer has rich terminal functional groups and Lewis acidic surfaces, which can act as a micro-barrier to further physically block and chemically anchor polysulfides leaking from the pores and gaps of the upper Co / CoN4@KB layer.
[0060] Figure 3 The X-ray diffraction spectrum of the Co / CoN4@KB material obtained in this example is shown. Because the content of Co is low and exists in the form of clusters and single atoms, there is no obvious Co metal characteristic diffraction peak in the figure, and the two clear broad diffraction peaks belong to the (002) and (101) crystal planes of carbon.
[0061] Figure 4 The high-resolution electron microscopy image of the Co / CoN4@KB material obtained in this example with high-angle annular dark field and spherical aberration correction is shown. Abundant bright spots can be seen, which are atomically dispersed Co, marked with white circles. Black circles represent Co clusters, proving that isolated dispersed Co atoms and metallic Co atomic clusters coexist on the conductive Ketjen black.
[0062] Figure 5 The ionic conductivity of the Co / CoN4@KB-MXene double-layer modified composite membrane obtained in this example is shown. Due to the presence of the highly conductive and active Co / CoN4@KB layer, Co / CoN4@KB-MXene exhibits the highest ionic conductivity.
[0063] Figure 6 The diffusion activation energy of the Co / CoN4@KB-MXene double-layer modified composite membrane obtained in this example is shown. The results show that the activation energy of Co / CoN4@KB-MXene is 0.0341 eV.
[0064] Figure 7 The constant potential lithium sulfide deposition curve of the Co / CoN4@KB material obtained in this example is shown. The results show that the Co / CoN4@KB composite material prepared in the present invention makes lithium sulfide contribute 217.4 mAh g -1 capacity, promoting the kinetics of sulfur reduction reaction.
[0065] Fig.10 The cycling performance of the lithium-sulfur battery using Co / CoN4@KB-MXene obtained in this example is shown. The results show that at 0.2C (1C = 1675 mA g -1 The initial discharge capacity at the current density is 1233 mAh g -1 After 100 cycles, the discharge capacity is 940 mAh g -1 .
[0066] Fig.11 The rate performance of the lithium-sulfur battery using Co / CoN4@KB-MXene obtained in this embodiment is shown. The results show that the average discharge specific capacity at current densities of 0.2C, 0.5C, 1C, 2C, and 4C is 1297, 1086, 984, 853, and 709 mAh g, respectively. -1 , and then return to 0.2C with an average discharge capacity of 1168mAh g -1 .
[0067] Example 2
[0068] (1) Preparation of graphene
[0069] The purchased graphene was dispersed in ethanol and deionized water (volume ratio of 1:1) to form a 0.3 mg / mL suspension, which was recorded as solution A;
[0070] (2) Preparation of Co / CoN4@KB composites
[0071] 30 mg of cobalt acetate tetrahydrate and 25 mg of phenanthroline were mixed in 3 mL of ethanol and stirred continuously at 50 °C for 3 h. Subsequently, 48 mg of Ketjen black was added to the above solution and stirred at 50 °C for 3 h to form a precursor, which was then transferred to a vacuum drying oven at 80 °C to evaporate the solvent; finally, the obtained product was heated to 650 °C at a heating rate of 10 °C / min under argon protection and calcined for 2 h to obtain a Co / CoN4@KB composite material;
[0072] (3) Preparation of Co / CoN4@KB-graphene double-layer composite membrane
[0073] Co / CoN4@KB was dissolved in a mixture of ethanol and water (volume ratio of 1:1) to obtain a solution B with a concentration of 0.5 mg / mL. Then, a vacuum filtration device was used with a polypropylene membrane as a filter membrane to drop 2 mL of solution A. After the solvent was completely separated, 2 mL of solution B was added. After the solvent was completely separated, the loaded membrane Co / CoN4@KB-MXene was transferred to a vacuum drying oven and dried at 60°C to obtain a Co / CoN4@KB-graphene double-layer composite membrane.
[0074] The electrochemical performance of the membrane prepared in this example was tested, and the specific results are as follows:
[0075] The cycle performance test results of the lithium-sulfur battery using Co / CoN4@KB-graphene obtained in this example show that at 0.2C (1C = 1675mA g -1 The initial discharge capacity at the current density is 1216 mAh g -1 After 100 cycles, the discharge capacity is 882 mAh g -1 .
[0076] The rate performance test results of the lithium-sulfur battery using Co / CoN4@KB-graphene obtained in this embodiment show that the discharge specific capacities at current densities of 0.2C, 0.5C, 1C, 2C, and 4C are 1224, 973, 889, 774, and 677 mAh g, respectively. -1 , and then return to 0.2C discharge capacity is 1113mAh g -1 .
[0077] Embodiment 3-5
[0078] In Examples 3-5, a double-layer modified lithium-sulfur battery composite separator Co / CoN4@KB-MXene is prepared respectively. The specific preparation process is similar to that in Example 1, except that the technical parameters in the preparation process are different, as follows:
[0079]
[0080] Comparative Example
[0081] Preparation method of double-layer modified lithium-sulfur battery composite diaphragm without active sites in group A
[0082] This group prepared a double-layer modified lithium-sulfur battery composite diaphragm without active sites. The preparation process was similar to that of Example 1, except that in the preparation process, in step (2), ordinary Ketjen black was directly dissolved in a solution formed by ethanol and deionized water (volume ratio of 1:1) to obtain a solution C with a concentration of 0.5 mg / mL. Solution C was used instead of solution B to carry out the subsequent step (3). The prepared diaphragm was named KB-MXene.
[0083] A series of morphology and performance measurements were performed on the KB-MXene membrane prepared in this comparative example, and the specific results are as follows:
[0084] Figure 3 The X-ray diffraction spectrum of the KB material of this group is shown. The two clear broad diffraction peaks both belong to the (002) and (101) crystal planes of carbon.
[0085] Figure 5 The ionic conductivity of the KB-MXene double-layer modified composite membrane obtained in this group is shown. The results show that the ionic conductivity of KB-MXene is lower than that of Co / CoN4@KB-MXene.
[0086] Figure 6 The diffusion activation energy of the KB-MXene double-layer modified composite membrane obtained in this group is shown. The results show that the activation energy of KB-MXene is 0.04 eV.
[0087] Figure 8 The constant potential lithium sulfide deposition curve of the MXene material used in this group is shown. The results show that the MXene material makes lithium sulfide contribute 110.2mAh g in this deposition process. -1 capacity.
[0088] Fig. 9 The constant potential lithium sulfide deposition curve of the KB material used in this group is shown. The results show that the KB material makes lithium sulfide contribute 54.2 mAh g -1 capacity.
[0089] Fig.10 The cycling performance of the lithium-sulfur battery using KB-MXene obtained by this group is shown. The results show that the initial discharge capacity at a current density of 0.2C is 1169 mAh g -1 After 100 cycles, the discharge capacity is 761 mAh g -1 .
[0090] Fig.11 The results show that the average discharge capacity at current densities of 0.2C, 0.5C, 1C, 2C, and 4C is 1228, 987, 848, 688, and 521 mAh g, respectively. -1 , and then return to 0.2C with an average discharge capacity of 1048 mAh g -1 .
[0091] Group B MXene monolayer modified lithium-sulfur battery separator
[0092] This group prepared a MXene single-layer modified lithium-sulfur battery separator and explored the effect of the MXene layer on polysulfide. The material preparation process of this comparative example is similar to that of Example 1, except that step (2) is not performed and only solution A is added during the filtration process in step (3). The prepared separator is named MXene.
[0093] This group conducted performance tests on the prepared MXene single-layer modified lithium-sulfur battery separator, as follows:
[0094] Figure 5 The ionic conductivity of the MXene monolayer modified membrane obtained by this group is shown. The results show that MXene has the lowest ionic conductivity. Driven by van der Waals forces, the self-stacking effect of MXene nanosheets leads to the Li + The space is compressed, which is not conducive to the migration of ions. Therefore, the MXene-modified membrane has the lowest ionic conductivity.
[0095] Figure 6 The diffusion activation energy of the MXene monolayer modified membrane obtained in this group is shown. The results show that the activation energy of KB-MXene is 0.0426 eV.
[0096] Figure 8 The constant potential lithium sulfide deposition curve of the MXene material used in this group is shown. The results show that the MXene material makes lithium sulfide contribute 110.2mAh g in this deposition process. -1 capacity.
[0097] Fig.10 The cycling performance of the lithium-sulfur battery using MXene obtained by this group is shown. The results show that the initial discharge capacity at a current density of 0.2C is 992mAh g -1 After 100 cycles, the discharge capacity is 645 mAh g -1 .
[0098] Fig.11The results show that the average discharge capacity at current densities of 0.2C, 0.5C, 1C, 2C, and 4C is 929, 740, 659, 545, and 346 mAh g, respectively. -1 , and then return to 0.2C with an average discharge capacity of 795 mAh g -1 .
[0099] C group KB single layer modified lithium sulfur battery separator
[0100] This group prepared a MXene single-layer modified lithium-sulfur battery separator to explore the effect of the MXene layer on polysulfide. The preparation process is similar to that of Example 1, except that step (1) is not performed during the preparation process, and step (2) directly uses ordinary Ketjen black dissolved in a solution formed by ethanol and deionized water (volume ratio is 1:1) to obtain a solution C with a concentration of 0.5 mg / mL, and step (3) only adds solution C during the filtration process, and the resulting separator is named KB.
[0101] This group conducted performance tests on the prepared KB diaphragm, as follows:
[0102] Figure 5 The ionic conductivity of the KB monolayer modified membrane obtained by this group is shown. The results show that the ionic conductivity of KB is the highest than that of MXene.
[0103] Figure 6 The diffusion activation energy of the KB monolayer modified membrane obtained by this group is shown. The results show that the activation energy of KB is 0.0345 eV.
[0104] Fig. 9 The constant potential lithium sulfide deposition curve of the KB material used in this group is shown. The results show that the KB material makes lithium sulfide contribute 54.2 mAh g -1 capacity.
[0105] Fig.10 The cycling performance of the lithium-sulfur battery using KB obtained by this group is shown. The results show that the initial discharge capacity at a current density of 0.2C is 923 mAh g -1 After 100 cycles, the discharge capacity is 470 mAh g -1 .
[0106] Fig.11 The results show that the average discharge capacity at current densities of 0.2C, 0.5C, 1C, 2C, and 4C is 819, 596, 458, 336, and 273 mAh g, respectively. -1, and then return to 0.2C with an average discharge capacity of 645 mAh g -1 .
[0107] From the above results, it can be seen that the Co / CoN4@KB-MXene double-layer modified lithium-sulfur battery composite separator provided in Example 1 of the present invention has a good double-layer structure, Co / CoN4@KB has high conductivity, and the highly active catalytic sites can promote the conversion of long-chain and short-chain polysulfides, improve the kinetics of sulfur redox reactions, and have a strong chemical adsorption capacity for polysulfides. The MXene layer can adsorb polysulfides through Lewis acid-base interactions, and the stacking of two-dimensional nanosheets can serve as a micro-barrier for polysulfides, further alleviating the shuttling effect of polysulfides and avoiding a large loss of active substances.
[0108] Figures 5-6 The results show that the ionic conductivity of the Co / CoN4@KB-MXene double-layer modified lithium-sulfur battery (the composite material shown in the present invention) is better than that of other samples. This advantage is attributed to the fact that the highly conductive and active site-rich Co / CoN4@KB can reduce the energy barrier for lithium ion diffusion and enrich the ion transmission channels, while the MXene-modified separator compresses the ion migration space due to the dense stacking of nanosheets, and the lower activity leads to low ion diffusion capacity.
[0109] Figures 7 to 11 The results show that Co / CoN4@KB has the characteristics of targeted promotion of rapid conversion of sulfur intermediates of different lengths, thus improving the specific capacity of lithium-sulfur batteries. The excellent adsorption capacity and MXene barrier layer further reduce the loss of active substances, so that lithium-sulfur batteries show more stable cycle performance. Therefore, lithium-sulfur batteries using Co / CoN4@KB-MXene show excellent electrochemical performance.
[0110] from Fig.12 It can be seen from the comparison of the cyclic voltammetry curves that the battery using the Co / CoN4@KB-MXene membrane (the composite material shown in the present invention) has a stronger redox peak current, proving its higher redox kinetic activity. At the same time, the potential difference between the oxidation peak and the reduction peak is smaller, indicating good reversibility and smaller electrochemical polarization.
[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a double-layer modified lithium-sulfur battery composite diaphragm, It is characterized in that Follow the steps below in order: (1) Preparation of two-dimensional materials Weigh the two-dimensional material, and dilute the prepared MXene suspension with an ethanol diluent formed by ethanol and deionized water in a volume ratio of 1:1, which is recorded as solution A; (2) Co / CoN 4 Preparation of @KB composite materials Cobalt acetate tetrahydrate and phenanthroline were mixed in ethanol and stirred continuously at 50°C for 3 h. Subsequently, Ketjen black was added to the above solution and stirred at 50°C for 3 h to form a precursor. The precursor was then transferred to a vacuum drying oven to evaporate the solvent. Finally, the obtained product was calcined under argon protection to obtain Co / CoN 4 @KB Composites; (3) Co / CoN 4 @KB-Preparation of two-dimensional material double-layer composite membrane Co / CoN 4 @KB was dispersed in a mixed solution of ethanol and water to obtain solution B, and then a vacuum filtration device was used to add solution A using a polypropylene membrane as a filter membrane. After the solvent was completely separated, solution B was added. After the solvent was completely separated, the loaded membrane Co / CoN 4 @KB-The two-dimensional material was transferred to a vacuum drying oven for drying, and finally Co / CoN was obtained. 4 @KB-Two-dimensional material double-layer composite membrane.
2. A method for preparing a double-layer modified lithium-sulfur battery composite diaphragm according to claim 1, It is characterized in that In step (1), the concentration of the hydrochloric acid is 9 M; the mass volume ratio of the lithium fluoride to the hydrochloric acid is 0.1 g / mL.
3. A method for preparing a double-layer modified lithium-sulfur battery composite diaphragm according to claim 1, It is characterized in that In step (1), the concentration of solution A is 0.3 mg / mL.
4. A method for preparing a double-layer modified lithium-sulfur battery composite diaphragm according to claim 1, It is characterized in that In step (2), the mass ratio of cobalt acetate tetrahydrate, phenanthroline and Ketjen black is (24-60): (17-34): 48; The mass volume ratio of the Ketjen black to ethanol is 16 mg / mL.
5. A method for preparing a double-layer modified lithium-sulfur battery composite diaphragm according to claim 1, It is characterized in that In step (2), the temperature of the evaporating solvent is 80°C.
6. A method for preparing a double-layer modified lithium-sulfur battery composite diaphragm according to claim 1, It is characterized in that In step (2), the calcination heating rate is 10°C / min, the calcination temperature is 650°C, and the calcination time is 2h.
7. A method for preparing a double-layer modified lithium-sulfur battery composite diaphragm according to claim 1, It is characterized in that In step (3), the concentration of solution B is 0.5 mg / mL; the amount of solution A and solution B is 2 mL.
8. A method for preparing a double-layer modified lithium-sulfur battery composite diaphragm according to claim 1, It is characterized in that In step (1), the two-dimensional material is any one of two-dimensional materials such as graphene material, MXene, etc.
9. A method for preparing a double-layer modified lithium-sulfur battery composite separator according to any one of claims 1 to 8, It is characterized in that In step (3), the Co / CoN 4 @KB-Two-dimensional material double-layer composite membrane, the upper layer is Co / CoN 4 @KB layer, the lower layer is a two-dimensional material layer, the Co / CoN 4 @KB layer thickness is about 5μm.
Citation Information
Patent Citations
Diaphragm coating material of lithium-sulfur battery and preparation method of diaphragm coating material
CN114725614A
MXene-based composite material for improving performance of lithium-sulfur battery diaphragm and preparation method of MXene-based composite material
CN115504473A
Preparation method and application of MXene-based composite positive electrode material
CN118239489A
Cited By
MXene functionalized modified aramid paper-based battery diaphragm as well as preparation method and application thereof
CN122091915A
CoN4 catalyst modified battery diaphragm and application thereof
CN122638713A
A CoN4 catalyst-modified battery separator and its application
CN122638713B