Photocatalyst member

By using cerium oxide as the base layer and titanium oxide as the photocatalyst layer, the problem of photocatalyst shedding and low productivity during the substrate fixation process is solved, and high productivity and efficient photocatalytic performance is achieved, which is suitable for a variety of applications.

CN118891099APending Publication Date: 2024-11-01DEXERIALS CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380027226.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-24
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

During the fixation process of substrate, existing photocatalysts are prone to fall off due to the powdering of the bonding agent, and increasing the bonding agent ratio to enhance binding will reduce catalytic performance. It is difficult for existing methods to achieve titanium oxide crystallization at room temperature and High productivity.

Method used

Using cerium oxide as the base layer, a crystalline cerium oxide layer is formed by high film formation speed and extremely thin film thickness, and a titanium oxide layer with high photocatalytic performance can be achieved without heating treatment. The layer structure of cerium oxide and titanium oxide is preferably The thickness and film formation speed of the base layer and the photocatalyst layer are used to improve industrial productivity.

Benefits of technology

The photocatalyst member with high productivity and high photocatalytic properties without heat treatment is achieved, which can effectively decompose organic matter and maintain optical properties, and is suitable for applications such as virus sterilization and anti-fog films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891099A_ABST
    Figure CN118891099A_ABST
Patent Text Reader

Abstract

According to one aspect of the present invention, provided is a photocatalyst member in which a photocatalyst layer is formed on a base material with an underlayer interposed therebetween, the underlayer comprising at least cerium oxide, and the photocatalyst layer comprising at least titanium oxide. Here, the underlayer may be constituted only of cerium oxide, or may be constituted of cerium oxide and at least one other element in an amount of 10 atomic% or less in terms of the cerium element ratio. According to the present invention, a photocatalyst having high industrial productivity can be produced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a photocatalyst structure.

[0002] This application claims priority based on Japanese Patent Application No. 2022-056768 filed in Japan on March 30, 2022, the contents of which are incorporated herein by reference. Background Art

[0003] Photocatalysts that produce catalytic effects through light such as ultraviolet rays and visible light have various effects and are now attracting attention. As the effects brought about by photocatalysts, hydrogen / oxygen generation brought about by the photolysis of water, strong oxidizing properties brought about by the generation of active oxygen on the surface, and super hydrophilicity brought about by the generation of multiple hydroxyl groups on the surface are known, as seen in the Honda-Fujishima effect. Photocatalysts can be used in various applications, especially sterilizing viruses such as coronaviruses and pathogens that have become popular in recent years by light irradiation, decomposing formaldehyde that is the cause of disease in residential areas, and applying super hydrophilic anti-fog films.

[0004] In addition, when a photocatalyst is applied to an anti-reflection film, it is expected that fingerprints attached to the surface of the anti-reflection film can be effectively decomposed. In particular, since the anti-reflection film formed by a dielectric multilayer film in which inorganic substances with different refractive indices are alternately stacked with a thickness of less than 1 μm uses interference of light, even if transparent foreign matter such as tiny fingerprints is attached to the surface, the interference effect is destroyed and the transparent foreign matter is easily visible. In the past, anti-reflection films were covered with substances with low surface energy such as fluorine compounds to suppress the attachment of transparent foreign matter such as fingerprints, but the effect was not sufficient and wiping and other cleaning were also required. In view of such a problem, if transparent foreign matter as an organic substance can be decomposed by a photocatalyst, cleaning is not required, so photocatalysts are highly expected.

[0005] Titanium oxide is known as a material having photocatalytic ability. As a method of forming titanium oxide on the surface of certain substrates, vacuum thin film forming methods such as sputtering are known. However, in order for titanium oxide to exert its photocatalytic performance, it needs to be crystallized into anatase or rutile type, and for crystallization, a heat treatment of more than 300°C is required during or after film formation. Therefore, it is difficult to apply photocatalysts to components such as plastics with low heat resistance. As another method, a method of applying crystallized titanium oxide fine powder together with a binder to a substrate for fixation has been proposed. This coating method is widely used because it does not require treatment such as heating and can be used for large-area treatment. Currently, almost all commercialized photocatalysts are based on this coating method.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2007-308729

[0009] Patent Document 2: Japanese Patent Application Publication No. 2007-314835

[0010] Patent Document 3: Japanese Patent No. 5217023

[0011] Patent Document 4: Japanese Patent Application Publication No. 2000-345320

[0012] Patent Document 5: Japanese Patent No. 4460537 Summary of the invention

[0013] Problems to be solved by the invention

[0014] However, most of the binders used for fixing to the substrate are organic substances, and the binders decompose due to contact with the photocatalyst, which is called powdering, and there is a problem that the photocatalyst itself also falls off. In addition, if the ratio of the binder is increased in order to enhance the bonding between the substrate and the photocatalyst, there is also a problem that the ratio of the photocatalyst is relatively reduced and the catalytic performance becomes lower.

[0015] Therefore, it is hoped that a titanium oxide thin film can be formed by a vacuum thin film formation method without a binder, but how to achieve photocatalytic performance by film formation at room temperature becomes a problem.

[0016] As a method for obtaining titanium oxide crystallized at room temperature, Patent Document 1 discloses a method of using a single cathode or a dual cathode to set the duty ratio of voltage application to a fixed value or less. Patent Document 1 describes that titanium oxide crystallized by this method is obtained, but the inventors were unable to confirm crystallization during a reproduction experiment, which may depend on the structure of the device, etc.

[0017] Patent Documents 2 and 3 disclose methods of promoting crystallization by performing the formation of a titanium metal film and oxidation treatment separately. However, this requires a complex structure for the equipment, and is difficult to implement with a general-purpose sputtering device.

[0018] As an example of using a general-purpose sputtering device, a method of adding water during film formation and performing a relatively low temperature (200° C. or higher) heat treatment to crystallize the film has been attempted, as shown in Patent Document 4. However, although it is low-temperature crystallization, heating at 200° C. or higher is required, so many plastic substrates will deform. Therefore, there is a problem of lack of versatility.

[0019] As a method of obtaining photocatalytic performance by film formation at room temperature using a general-purpose sputtering device, there is a method of forming a film of zirconium oxide as a base layer and then forming a film of titanium oxide, as shown in Patent Document 5. This method can be said to be a method that can achieve excellent photocatalytic performance without performing a heat treatment.

[0020] However, the film formation rate of zirconium oxide is extremely slow, and the degree of crystallization of zirconium oxide is also low. Therefore, in order to fully function as a base layer, a certain film thickness is required. Combined with the low film formation rate, the productivity is low.

[0021] The present invention has been made to solve the above problems, and an object of the present invention is to explore an underlayer different from zirconium oxide and to provide a photocatalyst with high industrial productivity.

[0022] Methods for solving problems

[0023] The inventors have conducted intensive research on this subject and have completed the present invention. That is, by using cerium oxide as a base layer, a cerium oxide layer crystallized at a high film formation rate and an extremely thin film thickness is formed, and a very high photocatalytic performance can be imparted without heating the titanium oxide layer formed thereon.

[0024] Specifically, for example, a base layer containing cerium oxide (CeO2) or other elements not exceeding 10 atomic % of cerium element relative to cerium oxide is formed. Then, a photocatalyst layer containing titanium oxide (TiO2) or other elements not exceeding 10 atomic % of titanium element relative to titanium oxide is formed. It can be seen that the photocatalyst layer exhibits photocatalytic performance without heat treatment.

[0025] The base layer of the present invention is preferably composed of cerium oxide only, but as long as the crystallinity of cerium oxide can be maintained, other elements may also be contained. Particularly during sputtering, in order to achieve stable discharge, cerium oxide is sometimes mixed with other metals to make a composite target. In this case, metal sometimes enters the film during film formation, but as long as the crystallinity of cerium oxide can be maintained. The thickness of the base layer is not particularly limited, and it is known that for example, even if it is 10nm, it has an effect. However, in the case where the substrate is a plastic film, the surface is sometimes not smooth, so the thickness of the base layer is preferably more than 20nm. If the thickness of the base layer is more than 20nm, the continuity of the base layer can be ensured, and sufficient crystallinity can be maintained. However, when the thickness of the base layer is more than 100nm, not only a heat load is applied to the substrate, but also there is no efficiency in industry, so it is preferably less than 100nm.

[0026] The photocatalyst layer of the present invention is composed of titanium oxide (TiO2), but as long as it exhibits photocatalytic performance, it may contain other elements in addition to titanium oxide. For example, the band gap of titanium oxide is in the ultraviolet region, and ultraviolet rays are required to work as a photocatalyst, but there are examples of adding nitrogen to make it respond to visible light. In the present invention, nitrogen can also be added to make a visible responsive photocatalyst. In addition, in order to improve the conductivity of the photocatalyst layer, metal elements such as niobium can also be added. The thickness of the photocatalyst layer is not particularly limited, and is preferably above 20nm to clearly exhibit photocatalytic performance. In addition, even if the thickness of the photocatalyst layer is thick, the effect of the present invention can be obtained, but it is ideal in the industry to be less than 200nm.

[0027] Furthermore, the present invention may also have layers other than the base layer and the photocatalytic layer. For example, in order to maintain the superhydrophilicity of the photocatalyst, a silicon oxide film may be formed on the surface of the photocatalyst layer. In addition, as shown in the Honda-Fujishima effect, in order to use the present invention as a photocatalyst electrode, a conductive layer may be formed before forming the base layer.

[0028] In summary, the present invention was accomplished by forming a photocatalyst layer containing titanium oxide on the side opposite to the substrate with respect to an underlayer containing cerium oxide. The gist of the present invention is as follows.

[0029] According to one aspect of the present invention, there is provided a photocatalytic member characterized in that a photocatalytic layer is formed on a substrate via an underlayer, the underlayer contains at least cerium oxide, and the photocatalytic layer contains at least titanium oxide.

[0030] Here, the underlayer may be composed of cerium oxide alone, or may be composed of cerium oxide and at least one other element in an amount of 10 atomic % or less in terms of the cerium element ratio.

[0031] The photocatalyst layer may be composed of titanium oxide alone, or may be composed of titanium oxide and at least one other element in an amount of 10 atomic % or less in terms of the titanium element ratio.

[0032] In addition, the thickness of the base layer may be 10 nm or more.

[0033] In addition, the thickness of the photocatalytic layer may be 20 nm or more.

[0034] Furthermore, a hydrophilic retaining layer made of silicon oxide or a composite oxide of silicon oxide and other metals may be provided on the photocatalytic layer.

[0035] Alternatively, the substrate may be transparent.

[0036] Alternatively, the substrate may be a polymer film.

[0037] Effects of the Invention

[0038] According to the present invention, a photocatalyst with high industrial productivity can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] [ Figure 1 ] is a diagram showing an example of an XRD spectrum.

[0040] [ Figure 2 ] is a cross-sectional view showing an outline of the photocatalyst component of the present invention. DETAILED DESCRIPTION

[0041] <1. Comparison between cerium oxide and zirconium oxide>

[0042] The cerium oxide used in the present invention is shown in comparison with the zirconium oxide used in Patent Document 5. First, the crystallinity of each material during film formation is compared.

[0043] The film is formed using an RF sputtering device. The exhaust system consists of a turbomolecular pump and a rotary pump, capable of exhausting up to 5×10 - 4 Pa or less. Four cathodes are arranged in the vacuum tank, and target materials with a diameter of 2 inches can be set on each of them. A baffle mechanism is arranged between each cathode, and the opening and closing time can be controlled by a timer. Therefore, if the film forming speed is known in advance, the thickness of the film can be precisely controlled by controlling the opening time of the baffle. The vacuum tank is connected to the gas supply piping, and argon, oxygen, and nitrogen can be supplied. The flow rate of each gas can be precisely controlled by a mass flow meter arranged between the gas storage bottle and the vacuum tank. A conduction valve is arranged between the turbomolecular pump and the vacuum tank, and the exhaust speed can be adjusted to any film forming pressure. The substrate can be set on a workbench opposite to the target. The workbench can rotate to make the thickness of the film uniform, and can also be heated to 300°C. In addition, the distance between the workbench and the target can be adjusted.

[0044] After the silicon substrate was placed on the workbench in the RF sputtering apparatus, the evacuation was performed to 5×10 -4 Argon and oxygen are introduced below Pa. The ratio of argon to oxygen is determined by previously investigating the conditions under which no absorption occurs in the visible light region.

[0045] The cerium oxide film is formed by sintering cerium oxide and forming it into a target shape. Zirconium oxide uses metal zirconium as a target. It is known that the film forming speed of a metal target is generally faster than that of an oxide target.

[0046] 200W of RF power was applied to a 2-inch target, and a film was formed on a silicon substrate for a certain period of time. The film thickness was evaluated using a spectroscopic ellipsometer (M-2000 manufactured by J.A. Woollam). In the ellipsometer, the amplitude ratio Ψ and the phase difference Δ of p-polarized light and s-polarized light are obtained at each wavelength. However, if an appropriate optical model is applied to them and the film thickness is also included as a parameter for fitting, the optical constant and the film thickness are obtained. The measurement result based on the center of the silicon substrate is taken as the film thickness. The result of dividing the film thickness by the film formation time is shown in Table 1.

[0047] [Table 1]

[0048] As can be seen from Table 1, cerium oxide has a film forming speed more than twice that of zirconium oxide.

[0049] Furthermore, in order to compare the crystallinity of each material, a film was formed on a glass substrate and evaluated by XRD. In order to avoid the influence of the substrate on the crystallization of the thin film, an alkali-free glass (OA-10G manufactured by Nippon Electric Glass Co., Ltd.) was used. The substrate was washed with a neutral detergent, ultrasonically cleaned in an ethanol solution for 10 minutes, and after being lifted out of the liquid, the droplets were immediately removed with an air gun to prevent the generation of dry spots.

[0050] The cleaned alkali-free glass was placed on a workbench in the above-mentioned RF sputtering device, and the film formation time was adjusted to a film thickness of 50 nm based on the film formation speed in Table 1, and the crystallinity was evaluated by XRD. XRD was measured using X'Pert PRO MPD (manufactured by PANalytical) with Cuα as the radiation source and an incident angle of 1°. The results of XRD are shown in Figure 1 .

[0051] like Figure 1 As shown in FIG. 1 , a slight peak is observed in zirconium oxide at around 28°. In contrast, in cerium oxide, in addition to having a sharp peak at the same position, peaks are also confirmed at 33°, 47°, and 56°. Therefore, it can be said that cerium oxide has an advantage in crystallinity. Figure 1 The results of hafnium oxide are also shown for comparison. Hafnium oxide is located just below zirconium on the periodic table and is expected to have similar properties to zirconium, but it did not crystallize.

[0052] The main reason for the photocatalytic performance of titanium oxide by forming a base layer is believed to be partial heteroepitaxial growth. It is believed that the base layer forms a lattice, and the titanium oxide grows in a manner consistent with its crystallites. Therefore, it is believed that if the base layer side is significantly crystallized with a thin film thickness, the titanium oxide of the photocatalyst layer formed later will also promote crystallization.

[0053] Based on the above results, preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0054] <2. Photocatalyst member of this embodiment>

[0055] Figure 2 It is a cross-sectional view schematically showing the structure of the photocatalyst member 1 of the present invention.

[0056] The photocatalyst member 1 of the present embodiment is a photocatalyst member in which a photocatalyst layer 4 is formed on a substrate 2 via an underlayer 3 . The underlayer 3 contains at least cerium oxide, and the photocatalyst layer 4 contains at least titanium oxide.

[0057] <3. Base material>

[0058] The substrate 2 of the present invention can be made of any material. If the material of the substrate 2 is exemplified, it is glass, metal, resin, ceramic, etc. In particular, the resin film that makes the thickness of the resin thinner is lightweight and can be attached to various places, etc., and has many advantages. Furthermore, due to industrial reasons, it has the advantage of being able to use a roll-to-roll sputtering device and continuously perform film forming treatment in mass production. Furthermore, when used in places where light needs to be transmitted, such as window glass and displays, transparent resin (polymer) films are sometimes used.

[0059] The material of the transparent resin film is not particularly limited, and for example, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyaramid, polyimide, polycarbonate, polyethylene, polypropylene, triacetyl cellulose (TAC), polycycloolefin (COC, COP), etc. can be used.

[0060] The thickness of the substrate 2 is not particularly limited. When the substrate 2 is a resin film, it is preferably set to be 20 μm or more and 200 μm or less in consideration of the ease of handling during manufacturing and the thinning of the component. It should be noted that, from the viewpoint of improving the scratch resistance of the substrate 2, a coating film such as an acrylic resin may be formed on at least one surface of the substrate 2 by, for example, solution coating. In addition, in order to improve the haze and film running properties, a material in which organic or inorganic particles are dispersed inside the above-mentioned acrylic resin may also be used.

[0061] <4. Basal layer>

[0062] The base layer 3 is a layer that promotes the crystallization of the photocatalyst layer 4, which is the purpose of this embodiment. The base layer 3 contains cerium oxide. More specifically, the base layer 3 is composed only of cerium oxide, or is composed of cerium oxide and at least one other element whose total cerium element ratio is less than 10 atomic %. However, this composition is just an example, as long as the base layer 3 contains cerium oxide. The elements contained in the base layer 3 can be measured, for example, by an X-ray microanalyzer (XMA), fluorescent X-ray analysis (XRF), etc.

[0063] As for the method for preparing the base layer 3, any method can be used. However, from the perspective of stacking of heterogeneous materials used to form a multilayer film, sputtering is effective. The preferred minimum thickness is 10 nm or more. In addition, considering the influence of the surface roughness of the substrate 2, it is preferably 20 nm or more. Regarding the thickness of the base layer 3, for example, a cross-sectional slice of the sample can be made by a slicing method and measured by a transmission electron microscope. If the thickness of the base layer 3 is 20 nm or more, even if the surface of the substrate 2 is rough, the continuity of the base layer 3 can be more reliably ensured. On the other hand, film formation of more than 100 nm not only imposes a heat load on the substrate 2, but is also inefficient in industry, so it is preferably less than 100 nm. The base layer 3 is preferably composed of cerium oxide alone, but other elements may also be contained as long as its crystallinity can be maintained. In particular, when sputtering, in order to achieve stable discharge, cerium oxide is mixed with other metals to form a composite target, and sometimes metals are mixed into the film during film formation. Even in such a case, as long as the crystallinity of the base layer 3 can be maintained. If other metals are exemplified, Zn, Al, etc. can be cited.

[0064] <5. Photocatalyst layer>

[0065] The photocatalyst layer 4 is a layer that functions as a photocatalyst. The photocatalyst layer 4 contains titanium oxide as a photocatalyst. More specifically, the photocatalyst layer 4 is composed only of titanium oxide, or is composed of titanium oxide and at least one other element whose total content is less than 10 atomic % in terms of the titanium element ratio. However, this composition is only an example, and it is sufficient as long as titanium oxide is contained in the photocatalyst layer 4 to the extent that the effect of the present embodiment can be obtained. The elements contained in the photocatalyst layer 4 can be measured, for example, by an X-ray microanalyzer (XMA) or fluorescent X-ray analysis (XRF).

[0066] The method for preparing the photocatalyst layer 4 may be any method. However, from the perspective of stacking heterogeneous materials used to form a multilayer film, a sputtering method is effective. In order for the photocatalyst layer 4 to function as a photocatalyst, the thickness of the photocatalyst layer 4 is preferably at least 20 nm. Regarding the thickness of the photocatalyst layer 4, for example, a cross-sectional slice of a sample can be prepared by a slicing method and measured with a transmission electron microscope. There is no particular upper limit to the thickness, but the film formation speed of titanium oxide is also slow. From the perspective of industrial productivity, it is preferably less than 200 nm. In the photocatalyst layer 4, other elements may also be contained as long as photocatalytic performance is exhibited. For example, the band gap of titanium oxide is in the ultraviolet region, and ultraviolet rays are required to work as a photocatalyst, but there are examples of adding nitrogen to make it respond in visible light. In the present invention, nitrogen can also be added to make a visible response photocatalyst. In addition, in order to improve the conductivity of the photocatalyst layer, metal elements such as niobium can also be added.

[0067] <6. Other layers>

[0068] Here, in order to make the photocatalyst component 1 conductive, one or more layers of conductive material may be stacked between the substrate 2 and the base layer 3. As such conductive materials, for example, indium-tin composite oxide (ITO), aluminum-zinc composite oxide (AZO), etc. may be cited. In addition, metal materials may also be stacked. Furthermore, in order to suppress oxidation caused by plasma when the base layer 3 is formed on the metal material, different oxides may also be stacked. Furthermore, in order to ensure the close adhesion between the substrate 2 and the base layer 3, a close adhesion layer may also be formed. Furthermore, in the case where the substrate 2 is a transparent substrate, in order to improve the transparency of the photocatalyst component 1, a transparent material may also be formed into a film. Furthermore, in order to make the surface of the substrate 2 smooth, a smoothing layer may also be formed.

[0069] Furthermore, a transparent material may be formed on the surface of the photocatalytic layer 4. In particular, a hydrophilic retaining layer made of silicon oxide or a composite oxide of silicon oxide and other metals may be formed on the photocatalytic layer 4 so that super-hydrophilicity can be maintained for a long time even in a dark place. In addition, titanium oxide used in the photocatalyst layer is a high refractive index material, so in order to reduce the reflectivity of the surface, a low refractive index material such as silicon oxide may be stacked on the photocatalyst layer.

[0070] As described above, according to this embodiment, since cerium oxide is used for the base layer 3, the photocatalyst layer 4 can function as a photocatalyst even without heating the photocatalyst layer 4. Furthermore, cerium oxide has a high film forming speed, so a photocatalyst with high industrial productivity can be manufactured.

[0071] Example

[0072] Hereinafter, the present invention will be specifically described with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0073] <Example 1>

[0074] As a substrate, alkali-free glass (OA-10G manufactured by Nippon Electric Glass Co., Ltd.) was used. After the substrate was washed with a neutral detergent, ultrasonic cleaning was performed in an ethanol solution for 10 minutes. After being lifted from the liquid, the droplets were immediately removed with an air gun and dried. The substrate was set in an RF sputtering device, and film formation was performed after exhausting. As a base layer, cerium oxide was film-formed with a thickness of 50 nm, and then 50 nm of titanium oxide was stacked thereon as a photocatalyst layer and then taken out to prepare a sample.

[0075] <Example 2>

[0076] A sample was prepared under the same conditions as in Example 1 except that the thickness of cerium oxide was set to 10 nm.

[0077] <Example 3>

[0078] A sample was prepared under the same conditions as in Example 1 except that the thickness of cerium oxide was 100 nm.

[0079] <Example 4>

[0080] A sample was prepared under the same conditions as in Example 1 except that the thickness of titanium oxide was set to 20 nm.

[0081] <Example 5>

[0082] A sample was prepared under the same conditions as in Example 1 except that the thickness of cerium oxide was set to 200 nm.

[0083] <Example 6>

[0084] After the sample was prepared under the same conditions as in Example 1, a silicon oxide film was formed into a thickness of 5 nm using a sputtering device.

[0085] <Example 7>

[0086] As a substrate, a cycloolefin polymer (COP) was used. Before placing the substrate in a sputtering device, the surface of the COP was exposed to argon plasma at 5W for 60 seconds using a vacuum device capable of plasma treatment, and the substrate was immediately placed in the sputtering device after removing surface contamination. Then, a sample was prepared under the same conditions as in Example 1.

[0087] <Comparative Example 1>

[0088] As a substrate, alkali-free glass (OA-10G manufactured by Nippon Electric Glass Co., Ltd.) was used. The substrate was washed with a neutral detergent, ultrasonically cleaned in an ethanol solution for 10 minutes, and immediately removed from the liquid with an air gun and dried to prepare a sample.

[0089] <Comparative Example 2>

[0090] As a substrate, alkali-free glass (OA-10G manufactured by Nippon Electric Glass Co., Ltd.) was used. The substrate was washed with a neutral detergent, ultrasonically cleaned in an ethanol solution for 10 minutes, and immediately removed from the liquid with an air gun and dried. The substrate was placed in an RF sputtering device, vented, and titanium oxide was formed into a 50 nm film and then taken out to prepare a sample.

[0091] <Comparative Example 3>

[0092] A sample prepared under the same conditions as in Comparative Example 2 was heated to 300° C. in an electric furnace and maintained at that temperature for 2 hours. The heating of the electric furnace was then stopped, and the sample was taken out after being cooled in the furnace to room temperature.

[0093] <Comparative Example 4>

[0094] A sample was prepared under the same conditions as in Example 1 except that cerium oxide was changed to zirconium oxide.

[0095] <Comparative Example 5>

[0096] A sample was prepared under the same conditions as in Comparative Example 4 except that the thickness of zirconium oxide was set to 10 nm.

[0097] <Comparative Example 6>

[0098] A sample was prepared under the same conditions as in Example 1 except that cerium oxide was changed to hafnium oxide.

[0099] <Evaluation>

[0100] <Superhydrophilicity evaluation>

[0101] The prepared samples were left in a dark place for 48 hours to remove the influence of external light. Then, they were taken out and placed in a xenon-promoted weathering tester Q-SUN Xe-3 (manufactured by Q-Lab Corp.). Xenon light is close to the spectrum of sunlight, and the amount of light can also be controlled, so the effect of the photocatalyst can be accurately verified. Illuminance 64W / m 2 (0.55W / m 2 / nm@340nm), filter using Daylight-B / B, irradiate for 1 hour at black panel temperature 70℃, temperature 47℃, relative humidity 50%. After taking out, evaluate the contact angle of water within 30 minutes to evaluate whether it is super hydrophilic. The contact angle of water is measured by using a fully automatic contact angle meter DMo-702 (manufactured by Kyowa Interface Science Co., Ltd.), drop 1.5μL of pure water, and measure the contact angle. Repeat the measurement 3 times, and take the average value as the contact angle after irradiation.

[0102] <Evaluation Results>

[0103] <Examples 1 to 3>

[0104] As can be seen from Table 2, when the thickness of cerium oxide is set to 10 nm to 100 nm and the thickness of titanium oxide is set to 50 nm, the contact angle after xenon light irradiation is 10° or less, which is a superhydrophilic state and functions as a photocatalyst.

[0105] <Examples 4 to 5>

[0106] Compared with Examples 1 to 3, it can be seen that even when the thickness of titanium oxide was set to 20 nm and 200 nm, respectively, the contact angle after xenon light irradiation was 10° or less, and the superhydrophilic state was achieved, and the titanium oxide functioned as a photocatalyst.

[0107] <Example 6>

[0108] It was found that even if a silicon oxide layer as a hydrophilic retaining layer was formed on the surface, the contact angle after xenon light irradiation was 10° or less, and the film was in a super-hydrophilic state, and functioned as a photocatalyst.

[0109] <Example 7>

[0110] It is known that the glass transition temperature of COP is 150°C, but the sample after film formation does not deform, etc., and is not exposed to high temperature. It is known that the contact angle after xenon light irradiation is 10° or less, and it is in a super-hydrophilic state, and functions as a photocatalyst.

[0111] <Comparative Example 1>

[0112] It was found that in the case of the glass substrate alone, the contact angle after xenon light irradiation was not less than 10°, and that no photocatalytic performance was exhibited.

[0113] <Comparative Example 2>

[0114] When titanium oxide is formed into a film at room temperature without heat treatment, the contact angle after xenon light irradiation is not less than 10°, and photocatalytic performance is not exhibited. This shows that photocatalytic performance is not exhibited simply by forming titanium oxide.

[0115] <Comparative Example 3>

[0116] When the film formed under the same conditions as in Comparative Example 2 was heat treated and irradiated with xenon light, the contact angle was 10° or less, and the film became super-hydrophilic and had photocatalytic performance. However, it was clear that a high temperature heat treatment of 300°C was required.

[0117] <Comparative Example 4>

[0118] When zirconium oxide is used as the base layer instead of cerium oxide, the contact angle is less than 10° when irradiated with xenon light, and the film is super-hydrophilic, and photocatalytic performance is obtained. However, as shown in Table 1, the film formation speed of zirconium oxide is slower than that of cerium oxide, and the productivity is poor.

[0119] <Comparative Example 5>

[0120] If zirconium oxide is thinned to 10 nm to reduce the effect of slow film formation, the contact angle after xenon light irradiation will not be less than 10°, and no photocatalytic performance is shown. In contrast, as shown in Example 2, cerium oxide shows photocatalytic performance even in a thin film thickness, showing its superiority over zirconium oxide.

[0121] <Comparative Example 6>

[0122] When hafnium oxide was used as the underlayer instead of cerium oxide, the contact angle after xenon light irradiation did not become 10° or less, and photocatalytic performance was not exhibited. This shows that cerium oxide of the present invention is suitable for an underlayer exhibiting photocatalytic performance.

[0123] As described above, according to this embodiment, a photocatalyst member showing high productivity without heat treatment can be provided. According to this embodiment, a photocatalyst member for sterilization of viruses and pathogens, decomposition of formaldehyde causing sick house syndrome, anti-fogging film, etc. can be provided.

[0124] Furthermore, by applying the present embodiment to an optical film utilizing the light interference effect, a function of decomposing organic matter such as sweat can be imparted, and excellent optical characteristics can be always maintained.

[0125] [Table 2]

[0126]

[0127] The preferred embodiment of the present invention is described in detail with reference to the accompanying drawings, but the present invention is not limited to this example. It is obvious that anyone with common knowledge in the technical field to which the present invention belongs can think of various variations or modifications within the scope of the technical ideas described in the claims, and these are of course understood to belong to the technical scope of the present invention.

Claims

1. A photocatalyst component, characterized in that The present invention is a photocatalyst member in which a photocatalyst layer is formed on a substrate via an underlayer, wherein the underlayer contains at least cerium oxide and the photocatalyst layer contains at least titanium oxide.

2. The photocatalyst member according to claim 1, wherein The underlayer is composed of the cerium oxide alone, or is composed of the cerium oxide and at least one other element in an amount of 10 atomic % or less in terms of the cerium element ratio.

3. The photocatalyst member according to claim 1 or 2, characterized in that The photocatalyst layer is composed of the titanium oxide alone, or is composed of the titanium oxide and at least one other element in an amount of 10 atomic % or less in terms of the titanium element ratio.

4. The photocatalyst member according to any one of claims 1 to 3, characterized in that The thickness of the base layer is greater than 10 nm.

5. The photocatalyst member according to any one of claims 1 to 4, characterized in that The photocatalyst layer has a thickness of 20 nm or more.

6. The photocatalyst member according to any one of claims 1 to 5, characterized in that A hydrophilic retaining layer made of silicon oxide or a composite oxide of silicon oxide and other metals is provided on the photocatalyst layer.

7. The photocatalyst member according to any one of claims 1 to 6, characterized in that The substrate is transparent.

8. The photocatalyst member according to any one of claims 1 to 7, wherein The substrate is a polymer film.

Citation Information

Patent Citations

  • Method for forming thin film of amorphous titanium oxide, and photocatalytic composite thin film

    JP2006104541A