Alkali metal silicate aqueous solution and method for producing same
By filtration and adsorption of the alkali metal silicate aqueous solution from plant ash, the low whiteness and environmental problems of the wet-type silica of plant ash-type silica are solved, and high-quality and low-energy consumption are achieved.
Patent Information
- Application Number
- CN202380027179.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-05
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-03-09
AI Technical Summary
The alkali metal silicate aqueous solution from plant ash has many impurities and foreign matters when making wet silica, resulting in low whiteness. The prior art treatment methods consume high energy and are unfriendly in the environment, making it difficult to provide high functions and high quality. Quality wet silica.
By filtration and adsorption of alkali metal silicate aqueous solution from plant ash with high transmittance, the P2O5/SiO2 ratio is controlled to be above 1.0×10-3, the SiO2 concentration is between 8.9% and 16.7%, and the transmittance is above 65%. The K2O/Na2O ratio is 0.03-0.30, and the solid component on the filter is less than 100ppm. A filter with a mesh less than 50μm and an adsorbent material was processed to prepare a high-quality alkali metal silicate aqueous solution.
The production of high-quality wet-process silica with the same degree of whiteness as the sand-derived sodium silicate aqueous solution is achieved, reducing impurities and foreign matter content, promoting the reuse of plant ash, and meeting environmentally friendly requirements.
Smart Images

Figure CN118891229A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an aqueous solution of an alkali metal silicate (of plant origin) produced using plant ash and a method for producing the same.
[0002] Cross-references of related applications
[0003] This application claims the benefit of priority from Japanese Patent Application No. 2022-062996, filed on April 5, 2022, the contents of which are incorporated herein by reference. Background Art
[0004] Sodium silicate is also known as "water glass". As a raw material for wet-process silicon dioxide and synthetic zeolite, it is widely used in fields related to foundation curing agents for civil engineering, cleaning agents, fibers and pulp, etc. As general methods for producing sodium silicate, there are widely known methods: a wet method (chemical formula A) in which natural sand (silica sand, silica, silicate clay, etc.) with a large amount of silicon dioxide (SiO2) is dissolved in a sodium hydroxide aqueous solution; or a dry method (chemical formula B) in which sand is mixed with soda ash and placed in a melting furnace, heated and melted, and taken out when it becomes a transparent body and cooled and solidified.
[0005] Chemical formula A
[0006] 2NaOH+nSiO2→Na2O·nSiO2+H2O n: molar ratio
[0007] (Sodium silicate aqueous solution)
[0008] Chemical formula B
[0009] Na2CO3+nSiO2→Na2O·nSiO2+CO2 n: molar ratio
[0010] (Sodium silicate cullet)
[0011] Conventional wet-process silica made from sand-derived sodium silicate has a high BET specific surface area and micropores to mesopores, and is therefore widely used as a reinforcing filler for industrial rubber, tires, silicone rubber, etc., a filler for paper, a matting agent for coatings, an abrasive for tooth powder, etc., and an anti-blocking agent for films.
[0012] In recent years, there has been a demand for a sustainable and regenerative society to protect the global environment. As one of the specific measures for this purpose, the popularization of biomass technologies that do not use fossil fuels, such as biomass boilers and biomass power generation, is being promoted in various places. In the equipment using such technologies, plants with high silica content (grape plants such as rice husks, rice straw, wheat straw, bagasse, and bamboo) are mostly used as fuel. However, in these equipment, the disposal of combustion ash (plant ash) with high silica content has become a problem.
[0013] Therefore, as one of the methods to solve this problem, the following attempts have been made in the past: plant ash (especially rice husk ash) containing a large amount of silica components is dissolved in an aqueous sodium hydroxide solution to produce an aqueous silicic acid solution containing an alkali component, and wet-process silica is produced from the alkali metal silicate aqueous solution (for example, Patent Document 1 and Patent Document 2).
[0014] It should be noted that the silicic acid aqueous solution using plant ash as a raw material generally contains potassium as an alkali component in addition to sodium. Therefore, in the following description, except for the case where the alkali component is particularly limited to sodium, the silicic acid containing the alkali component is referred to as "alkali metal silicate" instead of the commonly used term "sodium silicate" (Na2O·nSiO2). In the present invention and this specification, the meaning of alkali metal silicate includes sodium silicate.
[0015] Patent Document 1: Japanese Patent Application No. 2007-510613
[0016] Patent Document 2: Japanese Patent Application No. 2007-522069
[0017] The entire descriptions of Patent Documents 1 and 2 are incorporated herein by reference. Summary of the invention
[0018] Problems to be solved by the invention
[0019] Based on the known technologies such as Patent Document 1 and Patent Document 2, it is not impossible to produce wet-process silica by producing an alkali metal silicate aqueous solution from rice husk ash or other plant ash.
[0020] However, the aqueous alkali metal silicate solution derived from plant ash contains more impurities and foreign matter that cause coloration than the one made from sand, and the wet-process silica produced from these colored aqueous alkali metal silicate solutions can only be low-quality wet-process silica that has many impurities and foreign matter and is colored (low in whiteness). Therefore, conventional wet-process silica produced from aqueous alkali metal silicate solutions derived from plant ash can only be used for limited purposes and methods: for inexpensive and general purposes; or for mixing a small amount of aqueous alkali metal silicate solution derived from plant ash with aqueous alkali metal silicate solution derived from sand for use; etc.
[0021] The quality of natural sand is constant in each place of production, so if the alkali metal silicate used to be the source of sand, the quality of impurities can be addressed by changing the origin of the sand according to the intended use. However, when using plant ash, since the plant ash itself contains a large amount of impurities and foreign matter and the quality is unstable, it is difficult to find a solution to the problems of impurities, foreign matter, and coloration.
[0022] For these reasons, wet-process silica produced from aqueous alkali metal silicate solutions derived from plant ash has not become as widespread as expected.
[0023] In addition, the conventional methods involve long-term contact with oxygen (Patent Document 1) and combustion at high temperatures (Patent Document 2), which generate a large amount of carbon dioxide and consume a lot of energy. These methods are not appropriate in view of recent environmental issues.
[0024] Furthermore, consumers of wet-process silica are demanding the supply of high-performance and high-quality wet-process silica while using an environmentally friendly raw material (alkali metal silicate).
[0025] The present invention has been accomplished in view of the above-mentioned problems, and an object of the present invention is to provide an aqueous solution of alkali metal silicate derived from plant ash, which can produce high-quality wet-process silica having the same degree of whiteness as when using a conventional aqueous solution of alkali metal silicate derived from sand.
[0026] In addition, a second object of the present invention is to provide a method for producing an alkali metal silicate aqueous solution, which can produce such an alkali metal silicate aqueous solution of sufficient quality.
[0027] Means for solving problems
[0028] The present inventors have discovered that by producing wet-process silica using an aqueous alkali metal silicate solution derived from plant ash having a high transmittance as a raw material, it is possible to produce high-quality wet-process silica having the same degree of whiteness as when using a conventional aqueous alkali metal silicate solution derived from sand, thereby completing the present invention.
[0029] The present invention is constructed as follows. [1]
[0031] An alkali metal silicate aqueous solution, wherein, expressed in mass %, the ratio of P2O5 concentration to SiO2 concentration (P2O5 / SiO2) is 1.0×10 -3 In the above, the SiO2 concentration is 8.9 mass % to 16.7 mass %, and the transmittance (%T) at an optical path length of 1 cm and a wavelength of 500 nm is 65% or more. [2]
[0033] An alkali metal silicate aqueous solution as described in [1], wherein the ratio of SiO2 concentration to (Na2O+K2O) concentration SiO2 / (Na2O+K2O), expressed in mol %, is 2.8 to 3.5. [3]
[0035] The alkali metal silicate aqueous solution as described in [1] or [2], wherein the ratio of K2O concentration to Na2O concentration (K2O / Na2O) is 0.03 to 0.30, expressed in mol%. [4]
[0037] The alkali metal silicate aqueous solution according to any one of [1] to [3], wherein when the alkali metal silicate aqueous solution is filtered through a filter having a mesh size of 1 μm, the amount of solid matter captured on the filter is less than 100 ppm by mass relative to the mass of the alkali metal silicate aqueous solution before filtration. [5]
[0039] The alkali metal silicate aqueous solution according to any one of [1] to [4], which is used as a raw material for wet-process silica. [6]
[0041] A method for producing an alkali metal silicate aqueous solution, comprising: subjecting a raw material alkali metal silicate aqueous solution obtained by mixing plant ash containing a silicon dioxide component, sodium hydroxide and water to one or both of a filtration treatment using a filter with a mesh size of less than 50 μm and an adsorption treatment using an adsorbent to obtain an alkali metal silicate aqueous solution. [7]
[0043] The method for producing an alkali metal silicate aqueous solution according to [6], wherein the plant ash is rice husk ash.
[0044] Effects of the Invention
[0045] By using the aqueous alkali metal silicate solution derived from plant ash of the present invention as a raw material, it is possible to produce high-quality wet-process silica having the same degree of whiteness as when using a conventional aqueous sodium silicate solution derived from sand.
[0046] Furthermore, the production method of the present invention can provide an aqueous solution of alkali metal silicate derived from plant ash, which can produce high-quality wet-process silica having the same degree of whiteness as when using a conventional aqueous solution of alkali metal silicate derived from sand.
[0047] Furthermore, in the present invention, since plant ash that is usually discarded can be reused, it is possible to produce an alkali metal silicate aqueous solution in consideration of the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is an image showing a filtration residue in rough filtration of an alkali metal silicate aqueous solution.
[0049] Figure 2 It is the transmittance spectrum of the alkali metal silicate aqueous solution (Example 4, Comparative Example 1, Comparative Example 4) in the wavelength range of 200 nm to 800 nm.
[0050] Figure 3 It is the transmittance spectrum of the alkali metal silicate aqueous solution (Example 1, Example 5, Reference Example 1) in the wavelength range of 200 nm to 800 nm.
[0051] Figure 4 This is the transmittance spectrum of the alkali metal silicate aqueous solution (Comparative Example 3) in the wavelength range of 200 nm to 800 nm. DETAILED DESCRIPTION
[0052] <Alkali Metal Silicate Aqueous Solution>
[0053] The alkali metal silicate aqueous solution of the present invention is an alkali metal silicate aqueous solution in which, expressed in mass %, the ratio of the P2O5 concentration to the SiO2 concentration (P2O5 / SiO2) is 1.0×10 -3 In the above, the SiO2 concentration is 8.9 mass % to 16.7 mass %, and the transmittance (%T) at an optical path length of 1 cm and a wavelength of 500 nm is 65% or more.
[0054] The alkali metal silicate aqueous solution of the present invention is produced using plant ash, which is the combustion ash of plants containing silicon dioxide. Plant ash contains phosphorus, and phosphoric acid (P2O5) when converted into oxides is a component inherently contained in plant ash. In the alkali metal silicate aqueous solution of the present invention using plant ash as the main silicon dioxide source, the ratio of P2O5 concentration to SiO2 concentration, expressed in mass %, is higher than that of the alkali metal silicate aqueous solution derived from sand, and the ratio P2O5 / SiO2 is 1.0×10 -3 Generally speaking, the ratio P2O5 / SiO2 in the alkali metal silicate aqueous solution using only sand as the silica source will not be 1.0×10 -3 Therefore, by the presence of P2O5 based on the ratio P2O5 / SiO2, it can be determined that the alkali metal silicate aqueous solution is derived from plant ash (that is, at least a portion of the silica source is plant ash). In the alkali metal silicate aqueous solution of the present invention, the ratio P2O5 / SiO2 can be 1.5×10 -3 Above, 1.8×10 -3 Above, or 2.0×10 -3 The upper limit of the ratio of P2O5 / SiO2 is not particularly limited and depends on the type of plant ash, for example, 20×10 -3 From the perspective of reducing impurities, the ratio of P2O5 / SiO2 is preferably 15×10 -3 Below, more preferably 13×10 -3 Below, more preferably 10×10 -3 the following.
[0055] In the alkali metal silicate aqueous solution of the present invention, the transmittance (%T) at an optical path length of 1 cm and a wavelength of 500 nm is 65% or more.
[0056] Generally, plant ash contains a large amount of impurities and foreign matter. When the alkali metal silicate aqueous solution is manufactured using plant ash with a lot of impurities and foreign matter by the conventional method, the impurities and foreign matter are mixed into the alkali metal silicate aqueous solution, and the above transmittance (%T) is reduced. In the alkali metal silicate aqueous solution of the present invention, the above transmittance is made 65% or more by reducing the amount of impurities and foreign matter. By making the above transmittance 65% or more, it is easy to manufacture wet-process silica with high whiteness. In the alkali metal silicate aqueous solution of the present invention, the above transmittance is preferably 70% or more, more preferably 80% or more, and further preferably 90% or more. In particular, if the transmittance is 80% or more, it is easy to manufacture wet-process silica with a whiteness of 90 or more.
[0057] Transmittance (%T) refers to the value measured at a wavelength of 500nm using a 10mm square cuvette (standard type, optical path length 1cm) made of borosilicate glass and pure water as a reference. The wavelength of 500nm is near the boundary between blue and green in the visible light wavelength (380nm to 780nm), and is a wavelength that is easily correlated with the whiteness of silica.
[0058] The SiO2 concentration in the alkali metal silicate aqueous solution of the present invention is 8.9 mass % to 16.7 mass %. Generally speaking, the SiO2 concentration of the alkali metal silicate aqueous solution used as a raw material for wet-process silica is within the above range. Therefore, by making the SiO2 concentration within the above range, it is easy to use the alkali metal silicate aqueous solution of the present invention in the same use as the existing alkali metal silicate aqueous solution.
[0059] The alkali metal silicate aqueous solution of the present invention contains a sodium component and a potassium component derived from plant ash. In the alkali metal silicate aqueous solution of the present invention, the ratio of SiO2 concentration to (Na2O+K2O) concentration SiO2 / (Na2O+K2O) is preferably 2.8 to 3.5, expressed in mole %. Generally speaking, in the alkali metal silicate aqueous solution used as a raw material for wet-process silica, the molar ratio SiO2 / (Na2O+K2O) (usually, the amount of K2O is very small) is in the range of 2.8 to 3.5. Therefore, by making the molar ratio SiO2 / (Na2O+K2O) within the above range, it is easy to use the alkali metal silicate aqueous solution of the present invention in the same use as the existing alkali metal silicate aqueous solution.
[0060] In the alkali metal silicate aqueous solution of the present invention, the ratio of K2O concentration to Na2O concentration K2O / Na2O is preferably 0.03 to 0.30, expressed in mol%. By making the molar ratio K2O / Na2O less than 0.30, it is not easy to produce deviations in the neutralization reaction during the neutralization synthesis of wet-process silica, and it is not easy to cause problems in the quality stability of wet-process silica. In addition, if the molar ratio K2O / Na2O is more than 0.03, it is easy to adjust the molar ratio K2O / Na2O by mixing with other types of alkali metal silicates such as sand-derived alkali metal silicates. The molar ratio K2O / Na2O is preferably in the range of 0.04 to 0.20, and more preferably in the range of 0.05 to 0.15.
[0061] The molar ratio K2O / Na2O in the alkali metal silicate can be one of the criteria for determining whether the alkali metal silicate is derived from plant ash. Generally, in the alkali metal silicate derived from sand, the molar ratio K2O / Na2O is less than 0.01. Therefore, when the molar ratio K2O / Na2O is 0.01 or more, except for the case where the K2O concentration is clearly adjusted in the post-treatment, it can be said that the alkali metal silicate aqueous solution contains plant ash in most cases.
[0062] The total of the Na2O concentration and the K2O concentration (Na2O+K2O) can be, for example, 3.5 mass % to 5.0 mass %. Generally speaking, in the alkali metal silicate aqueous solution used as the raw material of wet-process silica, the total concentration of Na2O+K2O (usually, the amount of K2O is very small) is in the range of 3.5 mass % to 5.0 mass %. Therefore, by making the total concentration of Na2O+K2O in the above range, it is easy to use the alkali metal silicate aqueous solution of the present invention in the same use as the existing alkali metal silicate aqueous solution.
[0063] In the alkali metal silicate aqueous solution of the present invention, when the alkali metal silicate aqueous solution is filtered using a filter with a mesh (particle retention capacity) of 1 μm, the amount of solid content captured on the filter is preferably less than 100 mass ppm relative to the mass of the alkali metal silicate aqueous solution before filtration. The above-mentioned solid content is preferably less than 90 mass ppm, more preferably less than 80 mass ppm relative to the mass of the alkali metal silicate aqueous solution before filtration. In particular, when the adsorption treatment and filtration described later are performed, the above-mentioned solid content can also be less than 50 mass ppm, preferably less than 40 mass ppm, and more preferably less than 30 mass ppm.
[0064] The material of the filter used is not particularly limited as long as the mesh size is 1 μm. For example, filter with test filter paper (e.g., specification 5C, ADVANTEC), fully wash the filter paper with pure water, and dry at 105° C. for 2 hours. Based on the mass of the solid content remaining on the filter paper (the mass of the undissolved residue) and the mass of the alkali metal silicate aqueous solution for filtration, the mass % concentration of the undissolved residue can be calculated by the following formula.
[0065] [Number 1]
[0066]
[0067] According to the experiment conducted by the present inventors, it is known that the cause of the coloration problem in the wet-process silica derived from plant ash in the past is the impurities and foreign matter in the alkali metal silicate aqueous solution derived from plant ash. That is, there are a large number of impurities and foreign matter in the alkali metal silicate aqueous solution derived from plant ash in the past, and the impurities and foreign matter make the alkali metal silicate aqueous solution turbid and colored. Moreover, the use of such an alkali metal silicate aqueous solution to manufacture wet-process silica will result in the mixing of impurities and foreign matter into the wet-process silica, resulting in the problem of reduced whiteness of the wet-process silica.
[0068] As described later, the plant ash contains carbon components remaining due to unburning, as well as insoluble foreign matter such as graphite-based foreign matter and vitrified silica components, which easily produce undissolved residues in the alkali metal silicate aqueous solution derived from the plant ash. When the alkali metal silicate aqueous solution with a lot of undissolved residues is directly used as a raw material to manufacture wet-process silica, a large amount of impurities and foreign matter will be mixed into the wet-process silica. For example, in matte applications, such foreign matter is scattered on the surface after coating and becomes a protrusion, which becomes a reason for reducing the matte performance and damaging the appearance. In addition, in order to reduce the quality of the product, it is not preferred that impurities and foreign matter are mixed into the wet-process silica in applications such as industrial rubber, tires and toothpaste. Therefore, in order to obtain wet-process silica with high whiteness, the mass% concentration of the undissolved residue in the alkali metal silicate aqueous solution is adjusted to the above range, thereby suppressing the mixing of impurities and foreign matter into the wet-process silica.
[0069] The alkali metal silicate aqueous solution of the present invention can be obtained by the method for producing an alkali metal silicate aqueous solution of the present invention (the method for producing an alkali metal silicate aqueous solution described later) by performing one or both of the prescribed filtration treatment and adsorption treatment. In addition, as shown in the examples, plant ash with high whiteness can also be obtained by the method for producing an alkali metal silicate aqueous solution by mixing the plant ash, sodium hydroxide and water.
[0070] For comparison, for example, in the methods of Patent Documents 1 and 2, the obtained alkali metal silicate aqueous solution is not subjected to purification treatment such as filtration treatment. Therefore, due to the presence of impurities and foreign matter in the plant ash, the above-mentioned conventional alkali metal silicate aqueous solution is not transparent and wet-process silica with high whiteness cannot be produced. This is confirmed by the results of Comparative Example 3 described in the Examples.
[0071] <Method for producing an aqueous alkali metal silicate solution>
[0072] The method for producing an alkali metal silicate aqueous solution of the present invention comprises: subjecting a raw material alkali metal silicate aqueous solution obtained by mixing plant ash containing a silicon dioxide component, sodium hydroxide and water to one or both of a filtration treatment using a filter having a mesh size of less than 50 μm and an adsorption treatment using an adsorbent to obtain an alkali metal silicate aqueous solution. By this production method, the alkali metal silicate aqueous solution of the present invention can be obtained.
[0073] <Plant ash containing silica>
[0074] The plant ash used in the manufacture of the alkali metal silicate aqueous solution of the present invention is the combustion ash of plant materials containing silicon dioxide components. The type and part of the plant material are not particularly limited as long as they are plants and parts containing silicon dioxide components. As plants containing silicon dioxide components, for example, plants of the grass family such as rice (rice straw, rice husk), wheat, sugar cane, and bamboo can be cited. For reasons such as less pollution such as sludge adhesion, aggregation in the aggregation site, and easy availability, threshed rice husks (rice husks) are most preferred.
[0075] The quality of the plant ash used in the present invention is not particularly limited. From the perspective of industrially efficiently producing an alkali metal silicate aqueous solution with few impurities and foreign matter, it is preferred to use plant ash with a low carbon content and high whiteness. The carbon content in the plant ash is preferably 2% by mass or less, and preferably 1% by mass or less. The lower limit of the carbon content in the plant ash is not particularly limited, and is actually 0.05% by mass or more, and can be 0.1% by mass or more. The whiteness of the plant ash is preferably 30 or more, more preferably 40 or more, and further preferably 50 or more. The upper limit of the whiteness of the plant ash is not particularly limited, and is actually 90 or less, and can also be 70 or less.
[0076] In order to obtain plant ash with high whiteness and few impurities and foreign matter as described above, it is preferable to use a combustion furnace capable of burning the plant material at 550°C to 900°C while flowing. The combustion temperature is more preferably 600°C to 800°C, and even more preferably 650°C to 750°C.
[0077] Here, the relationship between the above-mentioned combustion method of causing the plant material containing silica components to flow while burning at 550°C to 900°C and the impurities and foreign matter in the plant ash is described. In order to produce plant ash with high whiteness, the inventors have investigated in detail the types of impurities and foreign matter in the plant ash and the causes of their generation. As a result, it can be seen that: in the case of combustion at a temperature below 550°C and in the case of uneven combustion due to insufficient material flow, the plant material is easily unburned, and the water-soluble hydrocarbon components are easy to remain in the plant ash. The water-soluble hydrocarbon components are dissolved in the alkali metal silicate aqueous solution and are difficult to remove by filtration, which becomes the cause of the coloring of the aqueous solution. In addition, it is known that when sufficient oxygen is not supplied during combustion, the hydrocarbon components in the plant material are carbonized, and insoluble graphite-based foreign matter is generated in the plant ash. In addition, it is known that when the plant material is burned at a combustion temperature of 700°C or above, the vitrified silica component is easily generated as an insoluble foreign matter in the plant ash. In this case, it is known that the silica component on the surface of the material is vitrified, and the material is easily unburned and oxygen-deficient inside, and water-soluble hydrocarbon components and insoluble graphite-based foreign matter are also easily generated. If the plant ash obtained by one-time combustion at high temperature is used to manufacture the alkali metal silicate aqueous solution, in addition to the vitrified silica component, the water-soluble hydrocarbon component and the insoluble graphite-based foreign matter are also mixed into the alkali metal silicate aqueous solution, and the quality reduction of the alkali metal silicate aqueous solution becomes significant. In addition, it is confirmed that even if the ash looks white at first glance, there are a certain amount of impurities and foreign matter such as water-soluble hydrocarbon components, insoluble graphite-based foreign matter and vitrified silica components in the plant ash. If the above-mentioned generation process of impurities and foreign matter in the plant ash is taken into account, in order to obtain plant ash with high whiteness, it is effective to uniformly burn the plant material under sufficient oxygen while suppressing the vitrification of the silica component by the above-mentioned combustion method.
[0078] In the above-mentioned combustion method, the combustion of the plant material preferably uses a combustion furnace. The model of the combustion furnace is not particularly limited. As mentioned above, in order to obtain plant ash with high whiteness and few impurities and foreign matter, it is preferred to use a combustion furnace equipped with a flow device that allows the plant material to flow during combustion, and capable of causing the plant material to flow while burning at 550°C to 900°C. For example, the combustion furnace can be a direct combustion furnace that uses oxygen to burn the plant material, or it can be a gasification combustion furnace that heats the plant material in an oxygen-free or low-oxygen state to generate organic gas and then burns the material. In addition, in the case where the plant ash contains a large amount of graphite-based foreign matter, for example, the carbon component can be removed by secondary combustion in the same combustion furnace while reusing the heat of the primary combustion.
[0079] According to such a method, the quality of plant ash is easily stabilized, and thus the plant ash is more excellent as a silica source for the alkali metal silicate aqueous solution of the present invention.
[0080] <Sodium hydroxide aqueous solution>
[0081] The sodium hydroxide and water used in the manufacture method of the present invention can use known sodium hydroxide and water. In the mode of mixing the sodium hydroxide aqueous solution with the plant ash, the concentration of the sodium hydroxide aqueous solution is not particularly limited, and a known concentration can be used. In general, from the aspect of the productivity of the alkali metal silicate aqueous solution, it is preferred to mix the sodium hydroxide aqueous solution with the plant ash at a concentration as high as possible, and then dilute it with water to the desired SiO2 concentration. On the other hand, the apparent density of plant ash is very small, so if the concentration of the sodium hydroxide aqueous solution is too high, it is sometimes difficult to put the plant ash into the sodium hydroxide aqueous solution. From the aspect of easily mixing the plant ash and the sodium hydroxide aqueous solution, the concentration of the sodium hydroxide aqueous solution is actually less than 20% by mass, and can also be less than 15% by mass or less than 10% by mass.
[0082] <Detailed Production Conditions of Alkali Metal Silicate Aqueous Solution>
[0083] The alkali metal silicate aqueous solution of the present invention is obtained by mixing plant ash containing a silicon dioxide component, sodium hydroxide and water. The mixing order of plant ash, sodium hydroxide and water is not particularly limited. Plant ash and sodium hydroxide may be added to water simultaneously or separately, a mixture of plant ash and sodium hydroxide may be added to water, plant ash may be added to a sodium hydroxide aqueous solution obtained by dissolving sodium hydroxide in water, or sodium hydroxide may be added to an aqueous solution obtained by dissolving plant ash in water.
[0084] The amount and mixing ratio of water, sodium hydroxide and plant ash used can be appropriately adjusted according to the type of plant ash and the target SiO2 concentration and application of the alkali metal silicate aqueous solution. The silica component after vitrification is difficult to dissolve, so it is not necessary to dissolve all the silica components in the plant ash in the aqueous solution. If the method is to dissolve about 90% to 95% by mass of the silica component in the plant ash, the alkali metal silicate aqueous solution can be produced with good productivity in terms of energy consumption and time.
[0085] For example, assuming that 90% of the silica content contained in plant ash is dissolved in an aqueous solution, if plant ash in an amount approximately 3 times the mass of sodium hydroxide in the aqueous solution is added to dissolve the ash, the ratio of SiO2 concentration to (Na2O+K2O) concentration SiO2 / (Na2O+K2O) can be easily adjusted to 2.8 to 3.5, expressed in mole %.
[0086] In the production method of the present invention, other conditions for mixing and dissolving plant ash, sodium hydroxide and water are not particularly limited.
[0087] The mixed dissolution is carried out, for example, in a dissolution tank (container) with stirring, at normal pressure (atmospheric pressure) or under pressure, at 60° C. to 100° C. and for 1 to 5 hours, as appropriate.
[0088] The manufacturing method of the present invention comprises: subjecting the above-mentioned raw material alkali metal silicate aqueous solution to one or both of a filtration treatment using a filter with a mesh of less than 50 μm and an adsorption treatment using an adsorbent material to obtain an alkali metal silicate aqueous solution. As described above, the conventional plant ash is mixed with impurities such as graphite-based foreign matter, foreign matter formed by vitrification of the silica component, and water-soluble hydrocarbon compounds. If these impurities and foreign matter are mixed into the alkali metal silicate aqueous solution and wet-process silica, they become the cause of their coloration. Therefore, for example, the target quality of wet-process silica of the present invention cannot be obtained by simply dissolving the conventional plant ash in a sodium hydroxide aqueous solution. In the present invention, impurities and foreign matter in the alkali metal silicate aqueous solution are removed by subjecting the raw material alkali metal silicate aqueous solution to one or both of the above-mentioned filtration treatment and adsorption treatment.
[0089] In order to remove insoluble foreign matter, the mesh of the filter used in the filtration process is less than 50μm. From the perspective of more fully removing foreign matter, the mesh of the filter is preferably less than 40μm, more preferably less than 30μm, and further preferably less than 20μm. When the mesh of the filter is less than 10μm, the filterability (productivity) is significantly deteriorated, so the mesh of the filter can be appropriately selected while considering productivity and quality. There is no particular restriction on the material of the filter, and various filters such as filter paper, filter cloth and membrane filter can be used. From the perspective of more fully removing foreign matter, the filtration process using a filter with a mesh less than 50μm can be implemented multiple times. When the filtration process is implemented multiple times, it is usually implemented in the order of mesh size from large to small.
[0090] In addition, in the manufacturing method of the present invention, before the filtration treatment using a filter with a mesh size of less than 50 μm, the filtration treatment using a filter with a mesh size of 50 μm or more may be performed. The filtration treatment using a filter with a mesh size of 50 μm or more may be appropriately performed as needed when there are many undissolved coarse particles.
[0091] Adsorption treatment can remove water-soluble impurities that are difficult to remove by filtration treatment.
[0092] Whether or not to perform the adsorption treatment is appropriately determined according to the amount and type of impurities in the alkali metal silicate aqueous solution. For example, it is preferred to perform both filtration and adsorption treatment on the alkali metal silicate aqueous solution having the transmittance (%T) at a wavelength of 500 nm of less than 10%.
[0093] In contrast, as long as the transmittance (%T) of 65% or more can be achieved after any treatment (for example, when there are few impurities and foreign matter in the plant ash), only one of the filtration and adsorption treatments may be used. Specifically, when it is sufficient to remove insoluble foreign matter, only filtration may be performed, and when it is sufficient to remove water-soluble impurities, only adsorption treatment may be performed. In addition, for the alkali metal silicate aqueous solution having the transmittance (%T) of 65% or more, in order to further improve the transmittance, one or both of filtration and adsorption treatment may be performed, and adsorption treatment may be performed after filtration, and filtration may be performed again to remove the residual adsorbent.
[0094] The adsorbent material used in the adsorption treatment is not particularly limited, and known adsorbent materials can be used. Examples of the adsorbent material include diatomaceous earth, clay minerals, activated carbon, zeolite, silica gel, and activated alumina. The adsorbent material is preferably activated carbon. The time of the adsorption treatment can be appropriately adjusted according to the amount of impurities and foreign matter in the alkali metal silicate aqueous solution, for example, 12 hours to 40 hours, preferably 15 hours to 30 hours. The amount of the adsorbent used in the adsorption treatment can be appropriately adjusted according to the amount of impurities in the alkali metal silicate aqueous solution, for example, 5g to 20g relative to 1,000g of the alkali metal silicate aqueous solution, or 8g to 15g.
[0095] The silica content and alkali content in plant ash are not fixed, so the concentrations of K2O and SiO2 in the alkali metal silicate aqueous solution are prone to deviation. Therefore, as needed, after one or both of the above-mentioned filtration treatment and adsorption treatment are performed, the final concentration adjustment and the adjustment of each molar ratio are performed. The adjustment of the mass % of SiO2 can be carried out by dilution with water or additional addition of silica material (such as commercially available silica powder). The ratio of SiO2 concentration to (Na2O+K2O) expressed in mole % can be adjusted by adding sodium hydroxide.
[0096] <Other conditions for the alkali metal silicate aqueous solution>
[0097] The alkali metal silicate aqueous solution of the present invention can use a silica material derived from sand (silica sand, silica, silicate clay, etc.) as a part of the silica source. When the quality of wet-process silica is important, the proportion of silica materials derived from sand can be increased, and when environmental considerations (recycling of plant ash) are important, the proportion of plant ash can be increased. From the perspective of environmental considerations, it is preferred to use as much plant ash as possible. The proportion of plant ash in the silica source is preferably 60% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more. In the preparation of the raw alkali metal silicate aqueous solution, it is also possible not to use a silica material derived from sand as the silica source, so that the amount of plant ash is 100% by mass.
[0098] The sand-derived silica material can be added as a part of the silica source when preparing the above-mentioned alkali metal silicate aqueous solution. In addition, the sand-derived silica material can also be used in a form in which the plant ash-derived alkali metal silicate aqueous solution and the sand-derived sodium silicate aqueous solution are prepared separately and mixed before using these aqueous solutions.
[0099] The alkali metal silicate aqueous solution of the present invention may contain additives as needed. There are no particular restrictions on the additives, and known additives may be used. For example, an aluminum oxide (Al2O3) source such as sodium aluminate may be added. Wet-process silica produced from an alkali metal silicate aqueous solution containing such additives has the effect of improving the reinforcing performance as a reinforcing agent for silicone rubber, industrial rubber, and tires.
[0100] As described above, according to the production method of the present invention, it is possible to fully remove impurities and foreign matters such as graphite-based foreign matters, foreign matters formed by vitrification of the silica component, and water-soluble hydrocarbon compounds in the plant ash from the alkali metal silicate aqueous solution. As a result, it is possible to provide an alkali metal silicate aqueous solution derived from plant ash that can produce high-quality wet-process silica having the same degree of whiteness as when using an alkali metal silicate aqueous solution derived from sand.
[0101] In addition, in the present invention, plant ash that is usually discarded can be reused, so that the alkali metal silicate aqueous solution can be supplied in consideration of the environment. In addition, the alkali metal silicate aqueous solution obtained by the production method of the present invention has a small content of impurities and foreign matter, so high-quality wet-process silica can be produced.
[0102] <Use of Alkali Metal Silicate Aqueous Solution>
[0103] The alkali metal silicate aqueous solution of the present invention can be used as a raw material for the production of wet-process silica. Although the alkali metal silicate aqueous solution of the present invention is derived from plant ash, the above-mentioned transmittance (%T) is 65% or more, and the content of impurities and foreign matter that cause coloring is small. By using the alkali metal silicate aqueous solution of the present invention as a raw material, high-quality wet-process silica having the same degree of whiteness as when using the conventional alkali metal silicate aqueous solution derived from sand can be produced, even though it is produced using plant ash. In addition, since the alkali metal silicate aqueous solution of the present invention has a small content of impurities and foreign matter, it is possible to produce high-quality wet-process silica with less impurities and foreign matter.
[0104] The type of wet-process silica produced using the alkali metal silicate aqueous solution of the present invention as a raw material is not particularly limited, and may be, for example, precipitated silica (white carbon black) or gel-process silica. The reason is that, in the case of wet-process silica, the process of precipitating silica from the alkali metal silicate aqueous solution basically shows the same tendency. An example of a synthesis process of wet-process silica is shown below (chemical formula C).
[0105] Chemical formula C (Example of the synthesis process of wet-process silica)
[0106] M2O·nSiO2+H2SO4→nSiO2+M2SO4+H2O
[0107] Here, M represents a base including sodium and potassium, and n represents a molar ratio.
[0108] The wet-process silica produced using the alkali metal silicate aqueous solution of the present invention as a raw material has high whiteness and little foreign matter, and therefore has sufficient reinforcing properties as a reinforcing filler for industrial rubber or tires. Furthermore, it can be used in applications where transparency and whiteness are important, such as reinforcing fillers for silicone rubber, fillers for paper (anti-see-through agents), matting agents for coatings, abrasives for toothpastes, and anti-blocking agents for films, in the same manner as the known alkali metal silicate aqueous solution derived from sand.
[0109] In addition, the alkali metal silicate aqueous solution of the present invention contains few impurities and foreign matter, so the alkali metal silicate aqueous solution of the present invention can also be used for known purposes other than wet-process silica, such as raw materials for synthesizing zeolite, foundation curing agents and cleaning agents for civil engineering, additives for fibers and pulp, etc. By using the alkali metal silicate aqueous solution of the present invention, the problem of foreign matter being mixed into the above-mentioned materials and products is less likely to occur compared with the conventional alkali metal silicate aqueous solution derived from plant ash.
[0110] Example
[0111] The following examples are given to illustrate the present invention, but are not intended to be limiting.
[0112] <Combustion conditions of plant ash>
[0113] Rice husk and rice straw are used as plant materials for making plant ash. Rice husk and rice straw are fully dried at 125°C for 2 hours. 500g of rice husk (apparent density: about 110g / L) or 250g of rice straw cut into about 10cm is placed in a 2mm thick stainless steel sagger (300mm×300mm×115mm (height)) with air holes and a lid, and it is stacked in 2 layers and burned in an air atmosphere using a table-top muffle furnace (model: KDF S100G, made by DENKEN Co., Ltd.). Plant ash can only be obtained at most 200g at a time, so multiple combustion treatments are carried out under the same conditions until the required amount of plant ash is obtained, and finally mixed. In addition, when burning at 900°C, a mullite sagger (external dimensions 210mm×210mm×70mm (height), internal dimensions 194mm×194mm×56mm (height)) with air holes and a lid is used instead of a stainless steel sagger.
[0114] Six types of plant ashes, ash a to ash f, were obtained by the above method. The combustion conditions of each sample are shown in Table 1 below. In Table 1, the combustion conditions of multiple combustion treatments are shown as follows: pre-combustion is performed at 500°C (more than once), the taken out ash is stirred, and then the next combustion treatment is carried out. For example, in Table 1, the combustion conditions of ash b "500°C, 2 hours, 600°C, 2 hours" means that after a pre-combustion of 2 hours at 500°C, a combustion treatment is carried out at 600°C for 2 hours. Plant ash f is ash obtained by burning rice husks at 700°C for 2 hours without allowing the material to flow in a state of excess air according to the method described in Patent Document 1.
[0115] <Analysis of plant ash>
[0116] ●Whiteness of plant ash
[0117] The measurement was performed using a whiteness meter (model: NW-12 manufactured by Nippon Denshoku Industries Co., Ltd.).
[0118] ●Carbon content in plant ash (mass %)
[0119] The carbon content was measured by heating the sample at a temperature of 1,350°C, an oxygen inflow pressure of 0.24 MPa, and a measurement time of 50 seconds using a carbon analyzer (model: CS744, manufactured by LECO JAPAN CORPORATION) using a combustion-non-dispersive infrared absorption method in an oxygen flow, and quantifying CO gas and CO2 gas using an infrared detector (NDIR) in the device. As a pretreatment, the plant ash was dried at 105°C for 2 hours.
[0120] ●Inorganic components other than carbon in plant ash (mass %)
[0121] Using a scanning fluorescent X-ray analyzer (model: ZSX PrimusII, manufactured by Rigaku), firstly, qualitative analysis of elements other than carbon was performed to confirm the types of inorganic impurities detected. Then, quantitative analysis of the detected inorganic impurities was performed. The test sample was a sample made by placing plant ash into a ring-shaped mold and press-molding. For the quantitative inorganic component composition (excluding carbon), the oxide conversion was performed using the analysis software attached to the device to calculate the concentration (mass %).
[0122] ●Ashing rate (mass %)
[0123] The mass % of the combustion ash after the combustion relative to the mass of the plant such as rice husk which was fully dried at 125° C. for 2 hours was measured.
[0124] [Number 2]
[0125]
[0126] ●Apparent density of plant ash (bulk density) (g / L)
[0127] The apparent density of plant ash is determined based on JIS K5101-12-1:2004 (pigment test method - apparent density or apparent specific volume - static method) using a dedicated measuring device (0.5 mm mesh sieve, funnel, 30 mL cylindrical receiver, receiver stand and funnel stand). The sample (plant ash) is dropped from above the sieve into the funnel with bristles, and the peak portion of the sample piled up in the receiver in a mountain shape is scraped off with a scraper, and then the mass of the sample is measured. Based on this mass, the apparent density (bulk specific gravity) of the plant ash in g / L is calculated by the following formula.
[0128] [Number 3]
[0129]
[0130] ●Bulk density of plant ash (apparent specific gravity) (g / mL)
[0131] The bulk density of plant ash is measured based on the item "7.8 Bulk density" of JIS K6220-1:2015 (Rubber Compounding - Organic Chemicals - Test Methods - Part 1: All) using a special measuring instrument (a cylinder made of ordinary steel with an inner diameter of 22.00±0.05mm and an inner depth of 100mm, and a piston with an outer diameter of 21.80±0.05mm, a length of 115mm, a mass of 190g and a hollow inside). The piston is allowed to fall naturally into the cylinder before the sample (plant ash) is loaded, and the height of the piston protruding from the upper part of the cylinder is measured. Next, a weighed sample of about 1g is placed in the cylinder, and the piston is slowly dropped over 5 seconds. The side wall of the cylinder is tapped with a piece of wood to make the piston fully fit, and the height of the piston protruding from the upper part of the cylinder is measured. The bulk density (apparent specific gravity) in g / mL is calculated using the change in the height of the piston protruding from the upper part of the cylinder and the bottom area inside the cylinder by the following formula.
[0132] [Number 4]
[0133]
[0134] Table 1 shows the carbon content and inorganic component composition other than carbon in the plant ash of each sample.
[0135] Combustion conditions and ingredients of ash a to ash f:
[0136] [Table 1]
[0137]
[0138] <Method for preparing aqueous alkali metal silicate solution>
[0139] ● Primary processing (mixing and filtering of materials)
[0140] 1,740 g of an aqueous sodium hydroxide solution adjusted to 5.8% by mass was added to a 3L stainless steel container equipped with a stirring device and heated to 85°C. Next, 300 g of plant ash was added to the sample solution while continuing to stir, and dissolved in 2 hours while maintaining 85°C, and the sample solution was cooled to room temperature. Here, it is assumed that 90% of the SiO2 contained in the plant ash is dissolved in the aqueous sodium hydroxide solution, and the target SiO2 concentration is set to 12.0% by mass. A 150 mm Φ magnetic Buchner funnel (suction filter) was installed on a 3L suction flask, and a polyester plain cloth (mesh size of about 50 μm × 400 μm) was used to coarsely filter while sucking the sample solution to remove undissolved residues. Thus, an alkali metal silicate aqueous solution after a single treatment was obtained.
[0141] Undissolved residues were found in the total plant ash, and the amount thereof was 10 to 20% by mass on a wet basis, which corresponds to about 1 to 4% by mass when converted to a solid content after drying. Figure 1 The following are photos of the undissolved residues of plant ash a to plant ash d and plant ash f. Since the amount of undissolved residue contains water, it is difficult to make a quantitative evaluation, and the correlation between the total amount of undissolved residue and the final combustion temperature cannot be confirmed. In contrast, the color of the undissolved residue varies depending on the final combustion temperature. Specifically, the residue of plant ash d burned at 900°C is a light yellow to white residue with undissolved glass as the main component, and the others are gray to black residues. The lower the final combustion temperature, the darker the black of the undissolved residue. It should be noted that when the required amount of alkali metal silicate aqueous solution is not obtained after the above filtration, the treatment is repeated multiple times under the same conditions, and finally mixed to obtain a sample.
[0142] ●Measurement of alkali concentration and SiO2 concentration (simple measurement for concentration adjustment)
[0143] The alkali concentration (mass % concentration of Na 2 O + K 2 O) and the SiO 2 concentration (mass % concentration) of the alkali metal silicate aqueous solution after the primary treatment were measured by the titration method shown below.
[0144] Alkali concentration:
[0145] In a 300 mL conical beaker, add about 2 g of a sample weighed to 1 mg and about 100 mL of distilled water, add 2 to 3 drops of methyl orange (0.1 mass % aqueous solution) as an indicator to the sample solution, and titrate with 1N-HCl using a 50 mL burette. The point where one drop turns orange is taken as the end point, and the alkali concentration is calculated from the consumption of 1N-HCl at this time by the following formula.
[0146] [Number 5]
[0147]
[0148] SiO2 concentration:
[0149] Add 5.0 g of sodium fluoride reagent to the above-mentioned alkali concentration titration endpoint solution and shake thoroughly to mix. Then, add about 0.5 mL of methyl red xylene cyanol FF indicator to the sample solution and titrate with 1N-HCl. When the liquid turns red, add 2.0 mL of 1N-HCl and record the titration amount a (mL). Here, methyl red xylene cyanol FF indicator is prepared by dissolving 0.8 g of methyl red and 0.2 g of xylene cyanol FF in 1,000 mL of ethanol.
[0150] Next, use a 10mL burette to perform back titration with 1N-NaOH. When the color of the sample solution turns tea-orange, confirm that the pH is in the range of 5.8 to 6.0 and use this as the endpoint. Record the titration amount b (mL) and calculate the SiO2 concentration using the following formula.
[0151] [Number 6]
[0152]
[0153] ● Secondary treatment of alkali metal silicate aqueous solution (if necessary)
[0154] Based on the measurement results of the above titration method, one or both of wet-process silica and water are added in a manner that the SiO2 concentration when converted to oxide is close to the target SiO2 concentration of 12.0% by mass, and the components are slightly adjusted (additional dissolution or additional heating and dissolution). In the present embodiment and comparative example, the alkali metal silicate aqueous solution obtained using plant ash d, plant ash e and plant ash f, respectively, is subjected to secondary treatment. For the alkali metal silicate aqueous solution derived from plant ash d, only wet-process silica (silicon dioxide purity of about 93% by mass, Nipsil LP, manufactured by Tosoh Silica Chemical Co., Ltd.) is added, heated and dissolved, and the SiO2 concentration is adjusted. For the alkali metal silicate aqueous solution derived from plant ash e, water and the above-mentioned wet-process silica are added, heated and dissolved, and the SiO2 concentration is adjusted. For the alkali metal silicate aqueous solution derived from plant ash f, only the above-mentioned wet-process silica is added, heated and dissolved, and the SiO2 concentration is adjusted. Plant ash f is ash obtained by burning rice husk at 700°C for 2 hours without flowing the material in an excess air state according to the method described in Patent Document 1. In the case of plant ash f, the surface portion of the rice husk is first vitrified, and most of the vitrified components are removed as a residue of coarse filtration during the primary treatment. Therefore, a larger amount of wet-process silica is required when adjusting the SiO2 concentration compared to plant ash d and plant ash e.
[0155] The sample solution subjected to the primary treatment and the secondary treatment as needed is used as the stock solution of the alkali metal silicate aqueous solution used in the examples and comparative examples. In the following description, the stock solution obtained using plant ash a is referred to as "alkali metal silicate a", and similarly, the stock solutions obtained using plant ash b to plant ash f are referred to as "alkali metal silicate b" to "alkali metal silicate f".
[0156] Furthermore, as Reference Example 1, an alkali metal silicate aqueous solution was produced using commercially available silica sand as a raw material by the following method.
[0157] Sodium silicate aqueous solution from silica sand:
[0158] 3,000 g of water was added to a 5 L pressure vessel (autoclave), and 500 g of sodium silicate cullet (medium molar grade, Na2O: 24.51%, SiO2: 75.44%, purity 99.9% or more, manufactured by Tokuyama Co., Ltd.) made from commercially available silica sand was dissolved under the conditions of a pressure of 0.7 MPa and a temperature of 160°C for 60 minutes. 2,000 g of the sodium silicate aqueous solution was taken from the container, diluted to 2 times with water, and cooled to room temperature. Then, a 150 mm Φ magnetic Buchner funnel (suction filter) was installed on a 5 L suction flask, and coarse filtration was performed while suctioning using a polyester plain cloth (mesh size of about 50 μm × 400 μm). The undissolved residue components were removed by coarse filtration to obtain a sodium silicate (alkali metal silicate) aqueous solution derived from silica sand.
[0159] <Examples and Comparative Examples of Alkali Metal Silicate Aqueous Solutions>
[0160] Alkali metal silicate a to alkali metal silicate f were prepared using plant ash a to plant ash f, respectively, to obtain alkali metal silicate aqueous solutions of Examples 1 to 3 and Comparative Examples 1 to 3. The following measurements were performed on each aqueous solution including the alkali metal silicate aqueous solution of Reference Example 1.
[0161] ●Composition analysis and impurity determination
[0162] The alkali metal silicate aqueous solution sample drawn with a syringe equipped with a membrane filter having a mesh size of 1 μm was diluted with pure water. A high-resolution ICP emission spectrometer (model: PS3520DDII, manufactured by Hitachi High-Technologies Corporation) was used to perform quantitative analysis of the sample (unit: mass %) using a standard solution based on the calibration curve of each element. The dilution ratio was 10,000 times (calibration curve standard solution: 20 mass ppm) for the quantitative analysis of SiO2, Na2O, and K2O, and 1,000 times (calibration curve standard solution: 10 mass ppm) for the quantitative analysis of P2O5, CaO, MgO, Al2O3, Fe2O3, and MnO.
[0163] ●Molar ratio
[0164] The above-measured SiO2, Na2O and K2O mass concentrations were converted into molar amounts to obtain the SiO2 / (Na2O+K2O) molar ratio and the K2O / Na2O molar ratio. Specifically, the molar mass of each component was set to 60.08 (SiO2), 61.98 (Na2O) and 94.19 (K2O), and each molar ratio was calculated by the following formula.
[0165] [Number 7]
[0166]
[0167] ●Determination of transmittance (%T) of aqueous alkali metal silicate solution
[0168] The transmittance at a wavelength of 200 nm to 800 nm was measured using a commercially available ultraviolet-visible spectrophotometer (model: V-730, manufactured by JASCO Corporation). In the measurement, a spectrophotometric standard cuvette made of borosilicate glass and having an optical path length of 10 mm (model: S10-G-10, manufactured by GL Sciences) was used, and the measured value under pure water was used as a comparative reference. The transmittance (%T) at a wavelength of 500 nm (near the boundary between blue and green) where coloration is easily seen among the visible light wavelengths (wavelengths of 380 nm to 780 nm) was taken as the transmittance (%T) of the alkali metal silicate aqueous solution.
[0169] ●Determination of undissolved residue (ppm by mass) in aqueous alkali metal silicate solution
[0170] Determine the undissolved residue of the alkali metal silicate aqueous solution as the raw material of wet-process silica (the amount of solid content captured on the filter after filtering using a filter with a mesh of 1 μm). Install a 110 mm Φ magnetic Buchner funnel (suction filter) on a 2 L suction flask, and use a filter paper with a mesh of 1 μm (specification 5C, manufactured by ADVANTEC) to filter 1,000 g of the alkali metal silicate aqueous solution. After the filtration is completed, further wash with 1,000 g of pure water and dry at 105°C for 2 hours using a box-type dryer. Then, calculate the mass of the solid content captured on the filter paper, and calculate the mass ppm concentration of the undissolved residue using the following formula.
[0171] [Number 8]
[0172]
[0173] ●Specific gravity of alkali metal silicate aqueous solution (reference value)
[0174] An alkali metal silicate aqueous solution adjusted to 20±0.5° C. is added to a 250 mL measuring cylinder, and a hydrometer (liquid hydrometer) is placed in the cylinder to read the scale at the time of rest.
[0175] <Production and physical property evaluation of wet-process silica>
[0176] In the case of wet-process silica, the process of precipitating silica from an alkali metal silicate aqueous solution shows a basically identical tendency, so alkali metal silicate a to alkali metal silicate f are used respectively to produce precipitated silica in wet-process silica by the following method, and their physical properties are confirmed (Example 1 to Example 3, Comparative Example 1 to Comparative Example 3). In addition, precipitated silica is produced using an aqueous sodium silicate solution derived from silica sand, and the quality is confirmed as Reference Example 1. The sodium silicate cullet and its aqueous solution in Reference Example 1 contain almost no impurities and are generally widely used as raw materials for high-quality wet-process silica with high whiteness. The physical properties are shown in Table 2 below.
[0177] ●Production of wet-process silica
[0178] In a 2L stainless steel container equipped with a stirring device, 495mL of warm water and 36mL of the alkali metal silicate aqueous solution for the test were added in a manner that the pH became 11.8±0.2, and the temperature was raised to 75°C. While stirring continuously in a manner that maintains the temperature and pH, 366mL of the alkali metal silicate aqueous solution and about 108mL of 20% by mass dilute sulfuric acid were added dropwise at a certain flow rate for 60 minutes. Then, the addition of the alkali metal silicate aqueous solution was stopped, and after the pH reached 3, the addition of dilute sulfuric acid was also stopped to terminate the neutralization reaction. A 150mmΦ magnetic Buchner funnel (suction filter) was installed on a suction flask with a capacity of 2L, and the sample liquid was suction filtered using a filter paper with a mesh of 8μm (specification 5A, made by ADVANTEC), and then washed with 600mL of pure water, and dried at 125°C for 8 hours to obtain wet-process silica (precipitated silica).
[0179] ●Whiteness of wet-process silica
[0180] The obtained wet-process silica powder was gently pulverized in a mortar for about 3 minutes, and then the whiteness of the wet-process silica was measured by the same method as that of the whiteness of the plant ash. When the whiteness of the wet-process silica is 85 or more, the quality of the wet-process silica is met as a high-functional wet-process silica, and the alkali metal silicate aqueous solution as the raw material thereof is evaluated as good. When the whiteness of the wet-process silica is less than 85, the wet-process silica is judged to be a colored product (discolored product), and the alkali metal silicate aqueous solution as the raw material thereof is evaluated as bad.
[0181] ●BET specific surface area of wet-process silica (reference value)
[0182] The BET specific surface area of the wet-process silica powder was measured by a single-point method using a fully automatic specific surface area measuring device (model: Macsorb HMmodel-1210, manufactured by Mountech).
[0183] ●Carbon content in wet-process silica (reference value)
[0184] The carbon content in the wet-process silica was measured by the same method as that used to measure the carbon content in the plant ash.
[0185] The analysis results of Examples 1 to 3, Comparative Examples 1 to 3, and Reference Example 1 are shown in Table 2 below.
[0186] [Table 2]
[0187]
[0188] <Examples and Comparative Examples of Mixing an Alkali Metal Silicate Aqueous Solution Filtered and Adsorbed and an Alkali Metal Silicate Aqueous Solution Derived from Sand>
[0189] As described below, alkali metal silicate a and alkali metal silicate b were subjected to one or both of filtration and adsorption treatment to evaluate the effect on the quality of wet-process silica (Examples 4 and 5 of aqueous alkali metal silicate solutions and Comparative Example 4). Furthermore, the quality of aqueous alkali metal silicate solutions derived from plant ash and aqueous alkali metal silicate solutions derived from sand was confirmed when mixed (Examples 6 to 8 of aqueous alkali metal silicate solutions).
[0190] <Comparative Example 4>
[0191] A 110 mm Φ magnetic Buchner funnel (suction filter) was installed on a suction flask with a capacity of 3 L, and alkali metal silicate a (about 2,000 g) was filtered while being sucked using filter paper (mesh size 1 μm, specification 5C, manufactured by ADVANTEC). Hereinafter, the filtration using the above filter paper will be referred to as "5C filtration". That is, in Comparative Example 4, 5C filtration was performed on the alkali metal silicate a of Comparative Example 1 to remove solid foreign matter present in the alkali metal silicate aqueous solution. Furthermore, wet-process silica was manufactured using the alkali metal silicate a after 5C filtration as a raw material, and its quality was analyzed.
[0192] <Example 4>
[0193] 20 g of commercially available powdered activated carbon was added to alkali metal silicate a (about 2,000 g) and allowed to stand for 24 hours to perform adsorption treatment on the components in the sample. Then, a 150 mm Φ magnetic Buchner funnel (suction filter) was installed on a suction flask with a capacity of 3 L, and the sample was subjected to 5C filtration. That is, in Example 4, the alkali metal silicate a of Comparative Example 1 was subjected to adsorption treatment to remove impurities in the aqueous solution by adsorption, and 5C filtration was performed to remove solid foreign matter present in the alkali metal silicate aqueous solution. Furthermore, wet-process silica was manufactured using the alkali metal silicate a after 5C filtration as a raw material, and its quality was analyzed.
[0194] <Example 5>
[0195] A 110 mm Φ magnetic Buchner funnel (suction filter) was attached to a 3 L suction flask, and alkali metal silicate b (about 2,000 g) was subjected to 5C filtration. Wet-process silica was produced using the alkali metal silicate b after 5C filtration as a raw material, and its quality was analyzed.
[0196] <Example 6 to Example 8>
[0197] The alkali metal silicate aqueous solution obtained in Example 5 after 5C filtration and the alkali metal silicate aqueous solution of Reference Example 1 were mixed at a ratio of 4:6 (Example 6: the aqueous solution derived from plant ash was 40% by mass. The same shall apply hereinafter), 6:4 (Example 7) and 8:2 (Example 8) to produce an alkali metal silicate aqueous solution. Furthermore, wet-process silica was produced using these alkali metal silicate aqueous solutions as raw materials, and the quality thereof was analyzed.
[0198] The analysis results of Comparative Example 4 and Examples 4 to 8 are shown in Table 3 below.
[0199] [Table 3]
[0200]
[0201] <Result Description>
[0202] From the results of plant ash b to plant ash d shown in Table 1, it can be seen that by pre-combustion, the plant material is fully burned, and the carbon-containing impurities in the plant ash caused by non-combustion are reduced. In contrast, from the results of plant ash a and plant ash e, it can be seen that a large amount of carbon-containing impurities remain due to insufficient combustion temperature. In addition, from the results of plant ash f, it can be seen that a large amount of carbon-containing impurities remain even when burning at high temperature without pre-combustion. It is believed that this is because the surface of the plant material is vitrified due to high-temperature combustion, and the material becomes non-combustible due to reasons such as insufficient oxygen supply.
[0203] From the results of Examples 1 to 3 shown in Table 2, it can be seen that when pre-combustion is performed to fully burn the sample and the alkali metal silicate aqueous solution is produced using plant ash, even if the alkali metal silicate aqueous solution is not subjected to filtration and adsorption treatment, the amount of insoluble foreign matter and water-soluble carbon compounds in the alkali metal silicate aqueous solution is small due to the small amount of filtration residue and high transmittance. It can be further seen that when wet-process silica is produced using such plant ash as a raw material, the impurities in the wet-process silica are also reduced, and wet-process silica with sufficient whiteness can be obtained. In contrast, from the results of Comparative Examples 1, 2 and 3, it can be seen that when the alkali metal silicate aqueous solution is produced using plant ash with insufficient combustion temperature and plant ash that has only been burned at high temperature, a large amount of carbon-containing impurities remain. It can be further seen that when wet-process silica is produced using such plant ash as a raw material, the impurities in the wet-process silica are also increased, and wet-process silica with sufficient whiteness cannot be obtained.
[0204] From the results of Comparative Example 4, Example 4, and Example 5 shown in Table 3, it can be seen that the quality of the alkali metal silicate aqueous solution is dramatically improved by subjecting the alkali metal silicate aqueous solution to one or both of filtration and adsorption treatment.
[0205] In particular, from the comparison among Comparative Examples 1, 4 and Example 4, it is understood that the quality of an alkali metal silicate aqueous solution of insufficient quality can be improved to such an extent that wet-process silica having a whiteness exceeding 90 can be produced by subjecting the solution to adsorption treatment and filtration.
[0206] Figure 2 The transmittance spectra (wavelength 200nm to 800nm) of the alkali metal silicate aqueous solutions in Comparative Example 1, Comparative Example 4, and Example 4 are shown. The higher the transmittance (%T) at a wavelength of 500nm, the higher the transparency. The transmittance of the alkali metal silicate a (plant ash a burned at 500°C, only treated once) in Comparative Example 1 is 4.4% at a wavelength of 500nm, and the whiteness of the precipitated silica produced using the alkali metal silicate a as a raw material is 58. In Comparative Example 4, in which the alkali metal silicate a was subjected to 5C filtration, although the coloring components dissolved in the alkali metal silicate aqueous solution remained, the transmittance at a wavelength of 500nm was improved to 32.8%. The whiteness of the wet-process silica produced using the alkali metal silicate aqueous solution of Comparative Example 4 as a raw material was also improved to 75, but the quality as wet-process silica was insufficient. In contrast, in Example 4 in which the alkali metal silicate a was subjected to the above-mentioned adsorption treatment and 5C filtration, the transmittance at a wavelength of 500 nm was improved to 94.5%, and the whiteness of the wet-process silica was also improved to 94, thereby obtaining wet-process silica of sufficient quality.
[0207] Figure 3The transmittance spectra (wavelength 200nm to 800nm) of the alkali metal silicate aqueous solution in Example 1, Example 5 and Reference Example 1 are shown. Example 1 is a case where alkali metal silicate b is produced using plant ash b burned at a final temperature of 600°C, and then wet-process silica is produced using this as a raw material. Example 5 is a case where alkali metal silicate b is subjected to 5C filtration and then used as a raw material to produce wet-process silica. Reference Example 1 is a case where wet-process silica is produced using an alkali metal silicate aqueous solution derived from silica sand.
[0208] In alkali metal silicate b, the filtration residue as solid foreign matter is 0.41% by mass, but the coloring components dissolved in the alkali metal silicate aqueous solution are in a state that is almost undetectable to the naked eye, and the transmittance at a wavelength of 500nm is 65.7%. The whiteness of wet-process silica produced using alkali metal silicate b as a raw material is 85, which is sufficient whiteness as a highly functional wet-process silica. In Example 5, in which 5C filtration was performed on alkali metal silicate b, the transmittance at a wavelength of 500nm was improved to 94.4%, and the whiteness of precipitated silica was also improved to 91. The quality is equivalent to the whiteness of wet-process silica produced using sand-derived alkali metal silicate aqueous solution as a raw material.
[0209] The quality of the aqueous alkali metal silicate solution derived from plant ash is sometimes inferior to the quality of the aqueous alkali metal silicate solution derived from sand as in Reference Example 1. In such a case, the quality of the aqueous alkali metal silicate solution derived from plant ash can be further improved by mixing it with an aqueous alkali metal silicate solution derived from sand as needed (Examples 6 to 8).
[0210] Figure 4 The transmittance spectrum (wavelength 200nm to 800nm) of the alkali metal silicate aqueous solution in Comparative Example 3 is shown. The transmittance of the alkali metal silicate aqueous solution derived from plant ash f produced by the method described in Patent Document 1 is 55.4% at a wavelength of 500nm, and the whiteness of the wet-process silica produced using it as a raw material is 73, and wet-process silica with sufficient whiteness cannot be obtained.
[0211] Industrial Applicability
[0212] The wet-process silica synthesized using the alkali metal silicate aqueous solution of the present invention as a raw material can have high reinforcing properties in industrial rubber or tire applications, and can be used as a reinforcing filler for silicone rubber where transparency or whiteness is important, a filler for paper (anti-see-through agent), a matting agent for paint or an abrasive for toothpaste, an anti-blocking agent for films, etc. (similar to the conventional alkali metal silicate aqueous solution derived from sand), and is therefore useful as an alkali metal silicate aqueous solution that takes environmental considerations into account.
Claims
1. An alkali metal silicate aqueous solution, wherein: Expressed in mass %, the ratio of P2O5 concentration to SiO2 concentration, P2O5 / SiO2, is 1.0×10 -3 In the above, the SiO2 concentration is 8.9 mass % to 16.7 mass %, and the transmittance (%T) at an optical path length of 1 cm and a wavelength of 500 nm is 65% or more.
2. The alkali metal silicate aqueous solution according to claim 1, wherein Expressed in mol %, the ratio of SiO2 concentration to (Na2O+K2O) concentration, SiO2 / (Na2O+K2O), is 2.8 to 3.
5.
3. The alkali metal silicate aqueous solution according to claim 1 or 2, wherein The ratio of K2O concentration to Na2O concentration, K2O / Na2O, is 0.03 to 0.30, expressed in mol%.
4. The alkali metal silicate aqueous solution according to claim 1 or 2, wherein When the alkali metal silicate aqueous solution is filtered through a filter having a mesh size of 1 μm, the amount of solid components captured on the filter is less than 100 mass ppm based on the mass of the alkali metal silicate aqueous solution before filtration.
5. The alkali metal silicate aqueous solution according to claim 1 or 2, which is used as a raw material for wet-process silica.
6. A method for producing an alkali metal silicate aqueous solution, comprising: The raw material alkali metal silicate aqueous solution obtained by mixing plant ash containing silica components, sodium hydroxide and water is subjected to one or both of filtration treatment using a filter with a mesh size of less than 50 μm and adsorption treatment using an adsorbent to obtain an alkali metal silicate aqueous solution.
7. The method for producing an alkali metal silicate aqueous solution according to claim 6, wherein: The plant ash is rice husk ash.
Citation Information
Patent Citations
Improvement of silica airgel
JP2007510613A
Soluble biogenic silica and applications using same
JP2007522069A
Production method for water glass and active carbon by using rice husk ash
CN102020272A
Production of water glass and activated carbon from rice husk ash
CN1039000A
Novel process for the preparation of silicate and its use for the preparation of precipitated silica
CN108137331A