Method for preparing carboxyalkylated polysaccharide and method for preparing biodegradable superabsorbent polymer using same

By performing carboxylic alkylation reaction of polysaccharides under high torque and specific water content conditions, avoiding the use of organic solvents, the economic and environmental problems of polysaccharide carboxylic alkylation reaction in the prior art are solved, and high efficiency preparation and high water retention capacity are achieved Biodegradable superabsorbent polymers.

CN118891291APending Publication Date: 2024-11-01LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028250.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-23
Filing Date
2023-12-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, the carboxylic alkylation reaction of polysaccharides uses alcohol-based organic solvents, which leads to high economic costs and great environmental impact, and makes it difficult to achieve large-scale production.

Method used

The gelatinization and carboxylic alkylation reaction of polysaccharides under specific water content and high torque conditions, avoid the use of alcohol-based organic solvents, carboxylic alkylation using hydroxides and metal salts of halogenated alkylcarboxylic acids, and then make the preparation Carboxylic alkylated polysaccharides are self-crosslinked to prepare superabsorbent polymers.

Benefits of technology

Efficient and economical preparation of carboxylic alkylated polysaccharides is achieved, reducing the environmental impact and producing biodegradable superabsorbent polymers with high water retention capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891291A_ABST
    Figure CN118891291A_ABST
Patent Text Reader

Abstract

The present disclosure relates to a method for preparing a carboxyalkylated polysaccharide and a method for preparing a biodegradable superabsorbent polymer using the same. More specifically, the present disclosure relates to a method for preparing a carboxyalkylated polysaccharide having high substitution efficiency by performing a carboxyalkylation reaction at a high torque caused by gelatinization while using a specific content of water. In addition, the present disclosure relates to a method for preparing a biodegradable superabsorbent polymer capable of producing a superabsorbent polymer having a high water retention capacity by self-crosslinking the carboxyalkylated polysaccharide prepared by the method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Korean Patent Application No. 10-2022-0183169 filed in the Korean Intellectual Property Office on December 23, 2022, the disclosure of which is incorporated herein by reference in its entirety.

[0003] The present disclosure relates to methods for preparing carboxyalkylated polysaccharides and methods of using the same to prepare biodegradable superabsorbent polymers. Background Art

[0004] Recently, as interest in biomass materials has increased due to environmental issues, interest in biodegradable materials such as polysaccharides, polyaspartic acid, and polyglutamic acid has increased.

[0005] In particular, polysaccharides are widely present in nature as components of plants and animals, and have emerged as important biodegradable materials due to their cost-effectiveness and ease of use. However, in order to be used in various industrial fields, it is necessary to replace the hydroxyl groups (-OH) present in polysaccharides with other functional groups, and methods for producing modified polysaccharides substituted with various substituents have been considered.

[0006] Among these modified polysaccharides, carboxyalkylated polysaccharides with carboxyl groups introduced into the end groups can be applied to various applications that need to contain acidic groups. In particular, carboxyalkylated polysaccharides can be used as the main raw material of biodegradable superabsorbent polymers. Superabsorbent polymers (SAP) are synthetic polymer materials that can absorb 500 to 1000 times of their own weight of water, and in addition to sanitary products such as children's diapers, they are also widely used in gardening water-retaining soil products, civil engineering and construction water-stopping materials, seedling-raising sheets, food circulation field preservatives, poultice materials, or electrical insulation. Therefore, it is necessary to study the method for industrially producing carboxyalkylated polysaccharides in large quantities while causing minimal environmental impact.

[0007] However, conventional carboxyalkylation of polysaccharides faces challenges in economic feasibility due to the alcohol-based organic solvents used during the carboxyalkylation reaction, and there are process problems for large-scale production. In addition, when a large amount of alcohol-based organic solvents are used, expensive solvent recovery equipment is also required to recover and reuse the solvent after the reaction.

[0008] Therefore, there is still a need for an economically feasible and large-scale preparation method of carboxyalkylated polysaccharides for producing biodegradable super absorbent polymers. As a result of research on this method, it was determined that these requirements can be met when carboxyalkylation of polysaccharides is carried out under high torque and temperature conditions caused by gelatinization while using a specific amount of water as the only solvent, thereby completing the present invention. Summary of the invention

[0009] Technical issues

[0010] The present disclosure relates to a method for preparing a carboxyalkylated polysaccharide and a method for preparing a biodegradable superabsorbent polymer using the same. More specifically, the present disclosure relates to a method for preparing a carboxyalkylated polysaccharide having a high substitution efficiency by carrying out a carboxyalkylation reaction under a high torque caused by gelatinization while using a specific amount of water. In addition, the present disclosure relates to a method for preparing a biodegradable superabsorbent polymer capable of producing a superabsorbent polymer having a high water retention capacity by self-crosslinking the carboxyalkylated polysaccharide prepared by the method.

[0011] Technical Solution

[0012] In order to solve the above problems, a method for preparing carboxyalkylated polysaccharides is provided, which comprises the following steps: mixing polysaccharides, hydroxides, metal salts of halogenated alkyl carboxylic acids and water in a reactor, and performing gelatinization and carboxyalkylation of the polysaccharide, wherein water is used in an amount of 0.35 to 1.0 times the weight of the polysaccharide, and after gelatinization of the polysaccharide, the torque in the reactor is maintained at 7 to 18 Nm.

[0013] In addition, a method for preparing a biodegradable superabsorbent polymer is provided, the method comprising the steps of:

[0014] Dissolving the carboxyalkylated polysaccharide prepared according to the preparation method in water of 5 to 15 times its weight (step 1); and

[0015] The product of step 1 is allowed to self-crosslink while drying at pH 6 to 8 (step 2).

[0016] Beneficial Effects

[0017] The above method for preparing carboxyalkylated polysaccharide has the advantage of improving the substitution efficiency of carboxyalkyl while using only a small amount of water as a solvent during the carboxyalkylation reaction. In addition, the above preparation method does not use an alcohol-based organic solvent as a reaction solvent, so it is environmentally friendly and economical, and is suitable for large-scale production of carboxyalkylated polysaccharide.

[0018] Furthermore, when the carboxyalkylated polysaccharide prepared by the above preparation method is self-crosslinked, a biodegradable super absorbent polymer having a high water retention capacity can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The internal torque and temperature in the reactor of Examples 1-2 are shown.

[0020] Figure 2 The internal torque and temperature in the reactors of Comparative Examples 1-3 are shown.

[0021] Figure 3 The internal torque and temperature in the reactor of Reference Example 1-1 are shown.

[0022] Figure 4 The internal torque and temperature in the reactor of Reference Examples 1-2 are shown.

[0023] Figure 5 The internal torque and temperature in the reactors of Reference Examples 1-3 are shown.

[0024] Figure 6 The carboxymethylated starch prepared in Example 1-1 is shown 1 H NMR spectrum.

[0025] Figure 7 The carboxymethylated starch prepared in Example 1-2 is shown 1 H NMR spectrum.

[0026] Figure 8 The carboxymethylated starch prepared in Reference Example 1-1 is shown 1 H NMR spectrum.

[0027] Fig. 9 The carboxymethylated starch prepared in Reference Example 1-2 is shown. 1 H NMR spectrum.

[0028] Fig.10 The carboxymethylated starch prepared in Reference Examples 1-3 is shown. 1 H NMR spectrum. DETAILED DESCRIPTION

[0029] The terms used herein are only used for the purpose of describing specific embodiments and are not intended to limit the present invention. Unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. It should also be understood that the terms "comprise", "include" or "have" when used in the present disclosure indicate the presence of the features, steps, components or combinations thereof, but do not exclude the presence or addition of one or more other features, steps, components or combinations thereof.

[0030] Furthermore, as used herein, when it is mentioned that a layer or an element is formed “on” a layer or an element, the layer or element may be directly formed on the layer or element, or other layers or elements may be additionally formed between layers, on an object, or on a substrate.

[0031] Since the present invention can be modified in various ways and has various forms, its specific embodiments are shown by way of example and will be described in detail. However, it is not intended to limit the present invention to the specific forms disclosed, but it should be understood that the present invention includes all modifications, equivalents and alternatives within the concept and technical scope of the present invention.

[0032] Furthermore, unless explicitly stated otherwise, the technical terms are used only to refer to specific embodiments and are not intended to limit the present disclosure. Unless the context clearly indicates otherwise, the singular form is intended to include the plural form as well.

[0033] Meanwhile, conventionally used super absorbent polymers are prepared by polymerizing acrylic acid-based monomers with a crosslinking agent in the presence of a polymerization initiator. In the case of super absorbent polymers prepared in this manner, they do not have biodegradability, thereby causing environmental problems.

[0034] Therefore, super absorbent polymers capable of showing biodegradability have been developed, and materials such as polysaccharides, polyaspartic acid and polyglutamic acid have been discussed as biodegradable materials capable of preparing such biodegradable resins. However, they reduce absorbency, which is an important physical property of super absorbent polymers, or are not easy to produce on a large scale, making it difficult to replace super absorbent polymers prepared from acrylic acid-based monomers.

[0035] Therefore, modified polysaccharides in which multiple functional groups are introduced into biodegradable and easily available polysaccharides such as starch are being used. However, there is a problem that these modified polysaccharides are not environmentally friendly and are not economical due to the organic solvents used during production.

[0036] Therefore, the present inventors devised a method of gelatinizing a polysaccharide such as starch using a small amount of water while stirring to induce torque in the polysaccharide, and performing carboxyalkylation at a torque above a certain level. Under such circumstances, it was determined that the reaction can be performed in a short time without using an alcohol-based solvent separately, and that the reaction efficiency (RE) can be improved compared to the case of using an alcohol-based solvent separately, thereby completing the present invention.

[0037] Furthermore, the present inventors have determined that when the carboxyalkylated polysaccharide prepared as above is self-crosslinked under specific pH conditions without using an internal crosslinking agent, a biodegradable superabsorbent polymer having high absorption properties can be prepared.

[0038] Hereinafter, various inventions will be described in detail.

[0039] (Method for preparing carboxyalkylated polysaccharide)

[0040] The method for preparing a carboxyalkylated polysaccharide with improved reaction efficiency (RE) comprises the following steps: mixing a polysaccharide, a hydroxide, a metal salt of a halogenated alkyl carboxylic acid and water in a reactor, and performing gelatinization and carboxyalkylation of the polysaccharide. Herein, water is used in an amount of 0.35 to 1.0 times the weight of the polysaccharide, and after gelatinization of the polysaccharide, the torque in the reactor is maintained at 7 to 18 Nm.

[0041] More specifically, in the above steps, when the polysaccharide is mixed with hydroxide and water, gelatinization of the polysaccharide is first performed, and then the carboxyalkylation reaction of the gelatinized polysaccharide is performed with the metal salt of the halogenated alkyl carboxylic acid.

[0042] At this time, by measuring the internal torque in the reactor from the start of mixing to the completion of mixing using a torque sensor set in the reactor, the time when the gelatinization of the polysaccharide is completed can be determined as the time when the torque is stable. More specifically, when the polysaccharide is gelatinized with water and hydroxide, the torque and temperature increase with the internal heat energy generation due to the load caused during gelatinization. Thereafter, when the gelatinization is completed, the torque and temperature in the reactor remain constant. Therefore, the carboxyalkylation of the polysaccharide can be carried out under constant torque conditions in the reactor, and thus a carboxyalkylated polysaccharide with a uniform degree of substitution and an improved substitution efficiency can be produced.

[0043] Therefore, when the torque in the reactor after gelatinization of the polysaccharide is less than 7 Nm, there is a problem that the substitution efficiency of the carboxyalkyl group decreases. When the torque exceeds 18 Nm, the internal temperature may excessively increase and water used as a solvent may evaporate, which may deteriorate processability.

[0044] More specifically, the torque (Nm) in the above steps can be 7 or greater, 7.5 or greater, or 8 or greater, and 18 or less, 16 or less, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, or 9 or less.

[0045] Polysaccharides refer to polymeric carbohydrate molecules composed of glucose repeating units. In this case, polysaccharides are also referred to as polymeric molecules composed of glucosamine units in which an amino group is introduced into a hydroxyl group bonded to the carbon atom at position 2 in a glucose repeating unit and / or N-acetylglucosamine units in which an N-acetylamino group is introduced into a hydroxyl group bonded to the carbon atom at position 2 in a glucose repeating unit. These polysaccharides can be divided into storage polysaccharides used as general energy sources, structural polysaccharides that form structural components of plants and animals (e.g., cell walls of plants or exoskeletons of arthropods), or capsular polysaccharides that form bacterial capsules. Storage polysaccharides include starch, dextrin, glycogen, inulin, etc., and structural polysaccharides include cellulose, chitin, chitosan, pectin, arabinoxylan, carrageenan, agar, etc. Capsular polysaccharides include alginate, xanthan gum, guar gum, gellan gum, dextran, welan gum, etc. Among them, those that can be gelatinized are suitable for the method of preparing carboxyalkylated polysaccharides. More specifically, starch, dextrin, glycogen, inulin, cellulose, chitosan, pectin, agar, carrageenan, alginate, xanthan gum, guar gum, gellan gum, or a combination thereof may be used as the polysaccharide.

[0046] In this article, the gelatinization of polysaccharides refers to the phenomenon that the physical properties of polysaccharides are changed by hydration, swelling and collapse when polysaccharide particles are heated with water or mixed with water and alkali. More specifically, when the micelle structure in the polysaccharide particles absorbs water molecules, the polysaccharide particles swell, and then the micelle structure in the polysaccharide particles collapses due to thermal energy or alkali. In other words, in the above preparation method, hydroxide (which is an alkali that promotes gelatinization) is used together with the polysaccharide, and water is used in a small amount compared to the polysaccharide, thereby causing torque during the gelatinization process, and thus continuously supplying thermal energy in the polysaccharide, thereby further promoting gelatinization.

[0047] Therefore, in the above preparation method, the polysaccharide capable of such gelatinization may not have reactive functional groups other than hydroxyl groups. For example, it is preferred to use at least one selected from starch, dextrin, glycogen, cellulose, pectin, inulin, agar and guar gum as the polysaccharide. More preferably, starch or its hydrolyzate dextrin may be used as the polysaccharide.

[0048] In particular, starch is contained in foods such as potatoes, wheat, corn, rice and cassava in large quantities, and is therefore easily available, which is desirable. This starch comprises amylose and amylopectin, and amylose and amylopectin can be contained in starch in a weight ratio of 1:99 to 80:20. In terms of processability and solubility, it is advantageous that amylopectin content is greater than amylose content. Starch can be selected from potato starch, corn starch, rice starch, wheat starch, cassava starch and sweet potato starch, and potato starch with high amylopectin content can be more preferred.

[0049] In addition, the gelatinized polysaccharide prepared by the above steps is not in a flowable liquid state dissolved or suspended in water, but in a semisolid colloidal state. Since the gelatinized polysaccharide in the colloidal state is mixed by the shearing action of the two screws arranged in the reactor and the chamber wall, the torque and heat energy in the reactor can be maintained above a certain level.

[0050] In order to keep the torque above a certain level after gelatinization of the polysaccharide, it is important to control the amount of water used. Therefore, in order to produce a carboxyalkylated polysaccharide having a uniform degree of substitution while maintaining the torque so that the carboxyalkylation reaction in the reactor can proceed smoothly, water needs to be used in an amount of 0.35 to 1.0 times the weight of the polysaccharide.

[0051] On the other hand, when water is used in an amount less than 0.35 times the weight of the polysaccharide, during the gelatinization process of the polysaccharide, the water evaporates due to the increased torque, which causes process problems and makes it difficult to prepare a carboxyalkylated polysaccharide with a uniform degree of substitution. When water is used in an amount exceeding 1.0 times the weight of the polysaccharide, the torque decreases during the gelatinization process of the polysaccharide, resulting in reduced reaction efficiency and yield. In addition, the cost of drying the water increases, and the amount of by-products such as sodium chloride (NaCl) generated during the reaction increases, which may reduce the absorption performance of the superabsorbent polymer.

[0052] More specifically, water can be used in an amount of 0.35 times or more, 0.4 times or more, 0.45 times or more, 0.5 times or more, 0.6 times or more, or 0.7 times or more, as well as 1.0 times or less, 0.9 times or less, 0.8 times or less, 0.75 times or less, 0.74 times or less, 0.73 times or less, or 0.72 times or less, based on the weight of the polysaccharide.

[0053] Preferably, water may be used in an amount of 0.45 to 0.75 times the weight of the polysaccharide.

[0054] As water, ordinary water such as tap water, distilled water, deionized water, purified water, etc. can be used without limitation, but distilled water can be preferably used.

[0055] In addition, the hydroxide and the metal salt of the haloalkyl carboxylic acid are not dissolved in water before being mixed with the polysaccharide. In addition, unlike the commonly known methods, the polysaccharide is not mixed with an organic solvent before being mixed with the hydroxide. In contrast, in the above method, all the reactants for the carboxyalkylation reaction are added to the reactor together with the solvent, thereby shortening the production process and improving production efficiency.

[0056] Furthermore, when the polysaccharide is mixed with the hydroxide, the metal salt of the halogenated alkyl carboxylic acid and water, no solvent other than water is used. Other commonly used solvents other than water include, for example, alcohol-based solvents such as ethanol, methanol or isopropanol; and water-miscible solvents such as acetone, 1,4-dimethoxybenzene, and the like. Alkane, dimethylformamide or dimethyl sulfoxide. When water is not used at all as a solvent for the gelatinization and carboxyalkylation reaction of polysaccharides, there is a problem that the reaction will not proceed because the metal salts of hydroxides and halogenated alkyl carboxylic acids are difficult to mix with polysaccharides. If a solvent other than water is mixed with water and then used, there may be environmental problems and cost problems associated with recovery, as well as safety problems such as evaporation caused by low boiling points. In addition, if a solvent other than water is mixed with water and then used in a reactor, it interferes with the gelatinization of polysaccharides, causing caking and mixing problems. However, in the above preparation method, these problems can be overcome by using only water as a solvent in the gelatinization and carboxyalkylation of polysaccharides.

[0057] Meanwhile, the polysaccharide used in the above preparation method includes an anhydroglucose unit (AGU) represented by the following Chemical Formula 1, and the molecular weight of the anhydroglucose unit (AGU) is 162.14.

[0058] [Chemical formula 1]

[0059]

[0060] At this time, the numbering in Chemical Formula 1 refers to the position of each carbon, and carboxyalkylation can occur on the hydroxyl group of the second carbon (C2), the third carbon (C3), or the sixth carbon (C6) in the anhydroglucose unit (AGU). For example, the carboxymethylated polysaccharide has a structure in which one or more hydroxyl groups (OH) in the anhydroglucose unit (AGU) are replaced by carboxymethyl groups (OCH 2 COOH / OCH 2 COO-) substituted structure.

[0061] Therefore, for example, when an alkali metal salt of a haloacetic acid is used as the metal salt of a haloalkyl carboxylic acid, the carboxyalkylated polysaccharide finally prepared by the above preparation method comprises a carboxymethylated glucose unit represented by the following Chemical Formula 2:

[0062] [Chemical formula 2]

[0063]

[0064] In chemical formula 2,

[0065] Each R is independently hydrogen, CH 2 COO - M+ or CH 2 COOH,

[0066] Provided that at least one R is CH 2 COO - M + or CH 2 COOH, and

[0067] M is an alkali metal.

[0068] The degree of substitution (DS) of the carboxyalkyl group in the carboxyalkylated polysaccharide prepared by the above method may be 0.6 to 1.1. When the degree of substitution (DS) of the carboxyalkyl group is too low, there is a problem that the water retention capacity of the superabsorbent polymer is reduced because of insufficient dissolution in water required for preparing the superabsorbent polymer. When the degree of substitution (DS) of the carboxyalkyl group is too high, the generation of by-products increases, which is undesirable because the reaction efficiency and biodegradability are reduced.

[0069] More specifically, the degree of substitution (DS) of the carboxyalkyl group may be 0.6 or more, 0.62 or more, or 0.64 or more, and 1.1 or less, 1.05 or less, 1.0 or less, 0.96 or less, 0.9 or less, 0.8 or less, 0.7 or less, or 0.65 or less.

[0070] Herein, the degree of substitution (DS) of carboxyalkyl refers to the average number of hydroxyl groups (-OH) substituted by carboxyalkyl groups per anhydroglucose unit. That is, since each glucose unit has 3 hydroxyl groups, the theoretical maximum degree of substitution is 3. When the degree of substitution is 0.1, 3 hydroxyl groups are substituted for every 10 glucose units. In addition, the degree of substitution of these acidic groups can be determined by the final prepared carboxyalkylated polysaccharide. 1 1H NMR analysis was used for calculation.

[0071] In this case, the carboxyalkylated polysaccharide may be carboxymethylated. Therefore, the degree of substitution (DS) of the carboxyalkyl group in the carboxyalkylated polysaccharide may be regarded as meaning the degree of substitution of the carboxymethyl group in the carboxymethylated polysaccharide.

[0072] In addition, the hydroxide may be one or more selected from sodium hydroxide, potassium hydroxide, and lithium hydroxide. At this time, sodium hydroxide (NaOH) is most preferred because it is easily available.

[0073] In addition, the hydroxide may be used in an amount of 0.5 to 1.5 equivalents relative to the mole number obtained by dividing the weight (g) of the polysaccharide by the molecular weight of the anhydroglucose unit (AGU). Specifically, the equivalent of the hydroxide may be obtained by dividing the weight (g) of the hydroxide used by the molecular weight to obtain the mole number, and then dividing the obtained mole number of the hydroxide by the mole number of the polysaccharide obtained by dividing the weight (g) of the polysaccharide used by 162.14, which is the molecular weight of the anhydroglucose unit (AGU).

[0074] More preferably, the hydroxide may be used in an amount of 0.5 equivalents or more and less than 1.2 equivalents relative to the molar number obtained by dividing the weight (g) of the polysaccharide by the molecular weight of the anhydroglucose unit (AGU). If the equivalent of the hydroxide is too low, the reaction may not proceed because there is not enough hydroxide, and the degree of substitution of the carboxyalkyl group in the final carboxyalkylated polysaccharide may be reduced. If the equivalent of the hydroxide is too high, a process of neutralizing the high pH caused by the unreacted hydroxide is required, and therefore, there may be a problem of generating a by-product that reduces absorbency.

[0075] More specifically, the hydroxide can be used in an amount of 0.5 equivalents or more, 0.6 equivalents or more, or 0.7 equivalents or more, and 1.15 equivalents or less, 1.1 equivalents or less, 1.0 equivalents or less, 0.9 equivalents or less, or 0.8 equivalents or less, relative to the mole number obtained by dividing the weight (g) of the polysaccharide by the molecular weight of the anhydroglucose unit (AGU).

[0076] In addition, the metal salt of the halogenated alkyl carboxylic acid is a metal salt of an alkyl carboxylic acid (alkanoic acid, R-COOH, wherein R is an alkyl) with at least one halogen substituent, that is, a compound in which an anion of an alkyl carboxylic acid with at least one halogen substituent is bonded to a metal cation. In this article, the metal salt can be an alkali metal salt, an alkaline earth metal salt or a divalent transition metal salt. In addition, the halogen substituent can be preferably chlorine or bromine. In addition, the alkyl can be linear or branched, and the number of carbon atoms is not particularly limited, but can be 1 to 20 or 1 to 10. Specific examples of the alkyl group include methyl, ethyl, propyl, n-propyl, isopropyl, butyl, n-butyl, isobutyl, tert-butyl, sec-butyl, 1-methyl-butyl, 1-ethylbutyl, pentyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, 1-ethyl-propyl, 1,1-dimethylpropyl, hexyl, n-hexyl, 1-methylpentyl, 2-methylpentyl, 4-methyl-2-pentyl, 3,3-dimethylbutyl, 2-ethylbutyl The invention also includes, but is not limited to, 1-methylhexyl, 2-methylhexyl, 3-methylhexyl, 4-methylhexyl, 5-methylhexyl, cyclopentylmethyl, cyclohexylmethyl, octyl, n-octyl, tert-octyl, 1-methylheptyl, 2-ethylhexyl, 2,4,4-trimethyl-1-pentyl, 2,4,4-trimethyl-2-pentyl, 2-propylpentyl, n-nonyl, 2,2-dimethylheptyl and the like.

[0077] The metal salt of a halogenated alkyl carboxylic acid may be an alkali metal salt of a halogenated alkyl carboxylic acid.

[0078] In one embodiment, when the carboxyalkylated polysaccharide is carboxymethylated, the metal salt of the haloalkylcarboxylic acid may be an alkali metal salt of a haloacetic acid.

[0079] In another embodiment, the metal salt of a haloalkyl carboxylic acid may be an alkali metal salt of an alkyl carboxylic acid substituted with at least one chlorine.

[0080] In another embodiment, the metal salt of a haloalkyl carboxylic acid may be an alkali metal salt of acetic acid substituted with at least one chlorine.

[0081] Preferably, the metal salt of the halogenated alkyl carboxylic acid may be an alkali metal salt of chloroacetic acid in consideration of reactivity.

[0082] The alkali metal salt of chloroacetic acid may be one or more selected from sodium monochloroacetate (SMCA), potassium monochloroacetate and lithium monochloroacetate. Preferably, sodium monochloroacetate (SMCA) is used in consideration of its easy availability and reactivity.

[0083] As an example, when sodium monochloroacetate is used as the metal salt of the halogenated alkyl carboxylic acid, the finally prepared carboxymethylated polysaccharide comprises a repeating unit represented by the following Chemical Formula 2-1:

[0084] [Chemical formula 2-1]

[0085]

[0086] In chemical formula 2-1,

[0087] Each R 1 are independently hydrogen, CH 2 COO - Na + or CH 2 COOH,

[0088] The condition is that at least one R 1 CH 2 COO - Na + or CH 2 COOH.

[0089] At this time, the metal salt of a halogenated alkyl carboxylic acid may be used in an amount of 0.5 to 1.5 equivalents relative to the mole number obtained by dividing the weight (g) of the polysaccharide by the molecular weight of anhydroglucose unit (AGU). Specifically, the equivalent of the metal salt of a halogenated alkyl carboxylic acid may be obtained by dividing the weight (g) of the metal salt of the halogenated alkyl carboxylic acid used by the molecular weight to obtain the mole number, and then dividing the obtained mole number of the metal salt of the halogenated alkyl carboxylic acid by the mole number of the polysaccharide obtained by dividing the weight (g) of the polysaccharide used by 162.14, which is the molecular weight of anhydroglucose unit (AGU).

[0090] More preferably, the metal salt of the haloalkyl carboxylic acid can be used in an amount of 0.5 equivalents or more and less than 1.2 equivalents relative to the molar number obtained by dividing the weight (g) of the polysaccharide by the molecular weight of the anhydroglucose unit (AGU). If the equivalent of the metal salt of the haloalkyl carboxylic acid is too low, there may be a problem that the hydroxyl groups of the polysaccharide are not sufficiently replaced by carboxymethyl groups. If the equivalent of the metal salt of the haloalkyl carboxylic acid is too high, there may be a problem that chloroacetic acid or glycolic acid is formed as a byproduct of a side reaction during the reaction, which reduces the reaction efficiency of the production of the carboxymethylated polysaccharide due to the neutralization reaction with the hydroxide. In addition, if the pH is reduced due to the neutralization reaction, a cross-linking reaction may also be carried out during the reaction, thereby reducing absorbency.

[0091] More specifically, the metal salt of a halogenated alkyl carboxylic acid can be used in an amount of 0.5 equivalents or more, 0.6 equivalents or more, or 0.7 equivalents or more, and 1.15 equivalents or less, 1.1 equivalents or less, 1.0 equivalents or less, 0.9 equivalents or less, or 0.8 equivalents or less, relative to the mole number obtained by dividing the weight (g) of the polysaccharide by the molecular weight of the anhydroglucose unit (AGU).

[0092] In addition, based on 1mol of hydroxide, the metal salt of haloalkyl carboxylic acid can be used in an amount of 1mol to 1.29mol. When the metal salt of haloalkyl carboxylic acid is used too much or too little based on hydroxide, the substitution reaction of carboxyalkyl may not be sufficiently carried out to reach the degree of substitution (DS) of carboxyalkyl within the above range. In addition, the content of sodium chloride (NaCl) by-products that may be produced during the reaction may increase. In addition, the excessive production of haloalkyl carboxylic acid or glycolic acid may cause the problem of partially forming a cross-linked structure. More specifically, the metal salt of haloalkyl carboxylic acid and hydroxide can be used in a mol ratio of 1:1.

[0093] In addition, mixing can be performed in a state where 70% to 95% of the total volume in the reactor is filled. When the total volume of the reactants loaded in the reactor is too small, the torque may not increase enough to allow the carboxyalkylation reaction to proceed during gelatinization. When the total volume of the reactants loaded in the reactor is too large, it is difficult to introduce them into the reactor, and the carboxyalkylation substitution reaction may not occur uniformly.

[0094] More specifically, mixing can be carried out when 70% or more, 75% or more, 76% or more, or 77% or more, and 95% or less, 94% or less, 93% or less, or 92% or less of the total volume in the reactor is filled.

[0095] In addition, any kneading machine equipped with two screws or wing rotors that can generate torque and heat energy can be used without limitation as a reactor for preparing the above-mentioned carboxyalkylated polysaccharide. For example, a closed mixer such as a Banbury mixer or an Intermix mixer, a double roll mill, etc. can be used.

[0096] Preferably, an internal mixer can be used as the reactor.

[0097] In addition, mixing can be carried out for 5 minutes to 15 minutes. At this time, the two screws or wing rotors arranged in the reactor can rotate at 30 rpm to 100 rpm. More preferably, mixing can be carried out for 10 minutes.

[0098] In this article, the gelatinization of the polysaccharide can be completed within 2 / 5 of the total mixing time from the start of mixing. By measuring the internal torque in the reactor from the start of mixing to the completion of mixing using a temperature and torque sensor set in the reactor as described above, the time when the gelatinization of the polysaccharide is completed can be determined as the time when the torque is stable. For example, when the total mixing time is 10 minutes, the gelatinization of the polysaccharide can be completed within 4 minutes.

[0099] Meanwhile, after gelatinization of the polysaccharide, the temperature in the reactor can be maintained at 90°C to 110°C. When the internal heat energy increases due to the load caused during gelatinization, the internal temperature in the reactor rises until the gelatinization is completed. However, after the gelatinization is completed, no additional load is caused, and the temperature is maintained within a certain range. Therefore, since not only the torque but also the temperature are maintained above a certain level after the gelatinization of the polysaccharide, the substitution efficiency of the carboxyalkyl group of the polysaccharide can be further improved.

[0100] More specifically, after gelatinization of the polysaccharide, the temperature in the reactor can be 90°C or higher, 92°C or higher, 94°C or higher, or 96°C or higher, and 110°C or lower, 105°C or lower, 100°C or lower, below 100°C, 99°C or lower, 98°C or lower, or 97°C or lower.

[0101] When an internal mixer is used as the reactor as described above, the temperature and torque in the reactor can be measured by temperature and torque sensors between the two screws.

[0102] In addition, after the above steps, the preparation method may further include the following steps: dissolving the prepared product in water and then precipitating it in an alcohol-based organic solvent. This is to purify the prepared product, i.e., the carboxyalkylated polysaccharide, to obtain the carboxyalkylated polysaccharide from which impurities have been removed.

[0103] Herein, the alcohol-based organic solvent may be one or more selected from methanol, ethanol, and isopropanol.

[0104] In addition, the alcohol-based organic solvent may be used in a volume (ml / g) of 10 to 60 times the weight of the product. Among them, methanol is most preferred in terms of purification efficiency and cost.

[0105] In addition, after the above steps, the preparation method may further include the following steps: a step of recovering the precipitate by filtering under reduced pressure; and a step of drying the recovered precipitate. After these steps, the carboxyalkylated polysaccharide from which residual hydroxide and generated by-products are effectively removed can be obtained.

[0106] (Method for preparing biodegradable superabsorbent polymer)

[0107] The method for preparing a biodegradable superabsorbent polymer having improved water retention capacity comprises the following steps:

[0108] Dissolving the carboxyalkylated polysaccharide prepared according to the above preparation method in water of 5 to 15 times its weight (step 1); and

[0109] The product of step 1 is allowed to self-crosslink while drying at pH 6 to 8 (step 2).

[0110] Step 1

[0111] First, step 1 is a step of dissolving the carboxyalkylated polysaccharide prepared according to the above method in water in an amount of 5 to 15 times its weight. Through the above steps, self-crosslinking in step 2 to be described later can occur sufficiently in the solution.

[0112] Herein, when the carboxyalkylated polysaccharide is dissolved in less than 5 times its weight of water, the precipitate may clump together, thereby causing a problem of by-product removal. When the carboxyalkylated polysaccharide is dissolved in more than 15 times its weight of water, there may be a problem of increased cost due to excessive use of solvent.

[0113] The dissolution in step 1 can be performed under standard temperature and pressure conditions. Herein, standard temperature means a temperature of about 21° C. to about 23° C., and standard pressure means atmospheric pressure without any applied pressure.

[0114] Step 2

[0115] Step 2 is a step of self-crosslinking the product of step 1 while drying at pH 6 to 8. The pH can be adjusted, for example, using an aqueous hydrochloric acid solution, an aqueous sodium hydroxide solution, or an aqueous potassium hydroxide solution, and can be adjusted using an acid / base solution generally used for pH adjustment. Through the above steps, a crosslinked polymer in which the polysaccharide is crosslinked and polymerized by an esterification reaction in the carboxyalkylated polysaccharide is produced.

[0116] In particular, the crosslinking reaction in step 2 is a self-crosslinking reaction, and a crosslinking agent commonly used in the production of crosslinked polymers of super absorbent polymers is not used. More specifically, meth(acrylate)-based compounds such as polyethylene glycol (meth)acrylate and ethylene glycol di(meth)acrylate and epoxy-based compounds such as ethylene glycol diglycidyl ether, propylene glycol and glycerol are commonly used as crosslinking agents, but such crosslinking agents are not used in the above preparation method. When a crosslinking agent is used, the content of biomass-based raw materials in the final super absorbent polymer is reduced, making it more advantageous to self-crosslink the carboxyalkylated polysaccharide without a separate crosslinking agent in terms of improving biodegradability.

[0117] Furthermore, during the cross-linking reaction, a reaction catalyst and / or a heat stabilizer may be additionally used to promote the esterification reaction.

[0118] The catalyst for esterification may include 4-dimethylaminopyridine (DMAP), magnesium acetate, tetra-n-butyl titanate (TBT), lead acetate, sodium acetate, potassium acetate, antimony trioxide, N-methylimidazole, or a mixture thereof. In order to shorten the reaction time and obtain the desired degree of crosslinking, the catalyst may be used in an amount of 0.1 mol to 5 mol based on 1 mol of the carboxyalkylated polysaccharide. Specifically, the reaction catalyst may be used in an amount of 0.1 mol or more, 0.5 mol or more, 1 mol or more, or 2 mol or more, and 4.5 mol or less, 4 mol or less, or 3.5 mol or less based on 1 mol of the carboxyalkylated polysaccharide.

[0119] In addition, an organic or inorganic phosphorus compound can be used as a heat stabilizer. The organic or inorganic phosphorus compound can be, for example, phosphoric acid, an organic ester of phosphoric acid, phosphorous acid, or an organic ester of phosphorous acid. More specifically, as a commercially available material of a heat stabilizer, phosphoric acid, an alkyl phosphate ester, or an aryl phosphate ester can be used.

[0120] Furthermore, during the crosslinking reaction, additional additives such as a thickener, a plasticizer, a storage stabilizer and an antioxidant may be used, if necessary.

[0121] In addition, the self-crosslinking reaction in step 2 is performed at a pH of 6 to 8. When the pH in the self-crosslinking reaction is less than 6, the crosslinking reaction may proceed rapidly, and there is a risk that the water retention capacity of the super absorbent polymer may be reduced. When the pH in the self-crosslinking reaction exceeds 8, crosslinking may proceed very slowly or may hardly react, which is undesirable.

[0122] In addition, the drying in step 2 can be performed at a temperature of 100° C. to 130° C. The drying method can be selected and used without limitation in terms of constitution as long as it is a method generally used in the art. Specifically, the drying step can be performed by methods such as hot air supply, infrared radiation, microwave radiation, UV ray radiation, etc.

[0123] Specifically, the drying may be performed under vacuum. Meanwhile, in consideration of process efficiency, etc., the drying may be performed for about 30 minutes to about 4 hours, or about 2 hours to 3 hours.

[0124] In addition, the drying method can be selected and used without limitation in terms of composition, as long as it is a method commonly used in the art. Specifically, the drying step can be performed by methods such as hot air supply, infrared radiation, microwave radiation, UV ray radiation, etc. The water content of the cross-linked polymer prepared after drying can be about 5% by weight to about 10% by weight.

[0125] Additional Steps

[0126] In addition, the preparation method may further include, after step 2, the step of crushing and classifying the cross-linked polymer prepared in step 2.

[0127] However, before pulverizing the cross-linked polymer, a coarse pulverization step may be optionally performed.

[0128] The coarse pulverization step is a step for improving the drying efficiency in the subsequent drying step and controlling the particle size of the superabsorbent polymer powder to be finally prepared. At this time, the pulverizer used herein may include, but its configuration is not limited to, any one selected from the following: a vertical pulverizer, a turbine cutter, a turbine grinder, a rotary cutter mill, a cutter mill, a disc mill, a chip crusher, a crusher, a meat grinder, and a disc cutter.

[0129] In the coarse pulverization step, the cross-linked polymer may be pulverized to have a weight average particle size of about 2 mm to 10 mm. Due to the high water content of the cross-linked polymer, it is technically difficult to pulverize it to have a diameter of less than 2 mm, and there may be a phenomenon that the pulverized particles adhere to each other. At the same time, when the polymer is pulverized to have a diameter greater than 10 mm, the efficiency improvement effect in the subsequent drying step may not be significant.

[0130] Subsequently, a step of pulverizing and classifying the roughly pulverized cross-linked polymer may be performed.

[0131] The pulverizing step may be performed so that the particle size of the cross-linked polymer powder (i.e., the base resin) is about 150 μm to about 850 μm. In order to pulverize the polymer to such a diameter, a pin mill, a hammer mill, a spiral mill, a roller mill, a disc mill, or an inching mill may be used as a pulverizer, but the present disclosure is not limited thereto.

[0132] Furthermore, in order to control the physical properties of the super absorbent polymer finally prepared after the pulverization step as described above, a step of classifying the pulverized polymer powder according to particle size may be further performed.

[0133] Therefore, the finally prepared super absorbent polymer may be in the form of a powder having a particle size of 150 μm to 850 μm. The particle size may be measured according to the EDANA WSP 220.3 method (European Disposables and Nonwovens Association).

[0134] In addition, the superabsorbent polymer can meet the centrifuge retention capacity (CRC) of 30 g / g to 45 g / g measured according to EDANA WSP 241.3. More specifically, the centrifuge retention capacity (CRC) of the superabsorbent polymer can be 30 g / g or more, 35 g / g or more, 37 g / g or more, 39 g / g or more, 39.2 g / g or more, 40 g / g or more, 41 g / g or more, or 41.2 g / g or more, and 45 g / g or less, 44 g / g or less, or 43.5 g / g or less.

[0135] Hereinafter, the present invention will be described in more detail by the following examples. However, these examples are for illustrative purposes only, and the present invention is not intended to be limited by these examples.

[0136] Example - Preparation of Carboxymethylated Starch

[0137] Measurement of moisture content of potato starch

[0138] The water content of potato starch is the moisture content in the gross weight of the potato starch obtained, and can be obtained as the percentage obtained by the value of the weight of dry potato starch subtracted from the gross weight of potato starch divided by the gross weight of potato starch.At this moment, the weight of dry potato starch is obtained by using a moisture analyzer to measure the weight change in 0.001g during drying at 125 ℃ and the weight remains unchanged for more than 30 seconds.The water content of the potato starch used in the embodiment, comparative example and reference example is measured using the above method, and it is found to be 17 weight %.Therefore, it is found that the actual starch content included in the potato starch is 83 weight %.

[0139] Example 1-1

[0140] In a closed mixer reactor, 28 g (actual starch content considering the water content: 23.24 g, 0.143 mol) of potato starch (manufactured by Daesang, with a water content of 17 wt %), 4.01 g (0.1 mol, 0.7 equivalent relative to the molar number of starch) of NaOH, 11.69 g (0.1 mol, 0.7 equivalent relative to the molar number of starch) of SMCA and 12 g of distilled water were charged to 77% of the reactor volume and mixed at 50 rpm for 10 minutes to carry out gelatinization and carboxymethylation of starch.

[0141] At this time, the internal torque and temperature in the reactor during mixing were measured using a temperature and torque sensor positioned between two screws provided in the internal mixer reactor. As a result of the measurement, it was determined that the gelatinization of starch was completed within 3 minutes from the start of mixing, and after the gelatinization of starch, the torque and temperature in the reactor were maintained at 7Nm to 9Nm and 96.3±1°C, respectively.

[0142] The prepared carboxymethyl starch was recovered, dissolved in distilled water, precipitated in methanol in an amount 40 times the volume (ml / g) of the carboxymethyl starch, and then filtered and dried under reduced pressure to obtain purified carboxymethylated starch.

[0143] Example 1-2

[0144] (Step 1)

[0145] In a closed mixer reactor, 33.4 g (actual starch content considering the water content: 27.72 g, 0.171 mol) of potato starch (manufactured by Daesang, with a water content of 17 wt %), 4.79 g (0.12 mol, 0.7 equivalent relative to the molar number of starch) of NaOH, 13.94 g (0.12 mol, 0.7 equivalent relative to the molar number of starch) of SMCA and 14.31 g of distilled water were charged to 92% of the reactor volume and mixed at 50 rpm for 10 minutes to carry out gelatinization and carboxymethylation of starch.

[0146] At this time, the internal torque and temperature in the reactor during mixing were measured using a temperature and torque sensor positioned between two screws provided in the internal mixer reactor, and a graph of the measurement is shown in Figure 1 As a result of the measurement, it was determined that the gelatinization of the starch was completed within 3 minutes from the start of mixing, and after the gelatinization of the starch, the torque and the temperature in the reactor were maintained at 8 Nm to 10 Nm and 96.4±1° C., respectively.

[0147] Thereafter, an additional purification step was performed in the same manner as in Example 1-1 to obtain purified carboxymethylated starch.

[0148] Comparative Example 1-1

[0149] 200L of isopropyl alcohol (IPA) was added to the flask, and 20g (actual starch content considering water content: 16.60g, starch content: 0.102mol) of potato starch (manufactured by Daesang, water content of 17% by weight) and 4.34g (0.109mol, 1.06 equivalents relative to the number of moles of starch) of NaOH were dispersed therein and kept at a temperature of 70°C. Thereafter, 20g of distilled water and 12.65g of SMCA (0.109mol, 1.06 equivalents relative to the number of moles of starch) were added thereto and reacted for 5 hours to prepare carboxymethylated starch. In the case of Comparative Example 1-1, gelatinization and carboxymethylation of starch were performed in the presence of an excess solvent in the flask, so that torque in the flask was not sufficiently caused.

[0150] Thereafter, an additional purification step was performed in the same manner as in Example 1-1 to obtain purified carboxymethylated starch.

[0151] Comparative Example 1-2

[0152] 400L of isopropyl alcohol (IPA) was added to the flask, and 200g (actual starch content considering water content: 166g, starch content: 1.02mol) of potato starch (manufactured by Daesang, water content of 17% by weight) and 30.71g (0.768mol, 0.75 equivalents relative to the number of moles of starch) of NaOH were dispersed therein and kept at a temperature of 70°C. Thereafter, 77g of distilled water and 89.44g of SMCA (0.768mol, 0.75 equivalents relative to the number of moles of starch) were added thereto and reacted for 5 hours to prepare carboxymethylated starch. In the case of Comparative Example 1-2, gelatinization and carboxymethylation of starch were performed in the flask, so that torque in the flask was not sufficiently caused.

[0153] Thereafter, an additional purification step was performed in the same manner as in Example 1-1 to obtain purified carboxymethylated starch.

[0154] Comparative Examples 1-3

[0155] In a closed mixer reactor, 28 g (actual starch content considering the water content: 23.24 g, 0.143 mol) of potato starch (manufactured by Daesang, with a water content of 17 wt %), 6.91 g (0.173 mol, 1.2 equivalents relative to the molar number of starch) of NaOH, 20.11 g (0.173 mol, 1.2 equivalents relative to the molar number of starch) of SMCA, 3 g of distilled water and 9 g of IPA were charged to 95% of the reactor volume and mixed at 50 rpm for 10 minutes to perform gelatinization and carboxymethylation of the starch.

[0156] At this time, the internal torque and temperature in the reactor during mixing were measured using a temperature and torque sensor positioned between two screws provided in the internal mixer reactor, and a graph of the measurement is shown in Figure 2 As a result of the measurement, it was determined that the gelatinization of the starch was completed within 3 minutes from the start of mixing, and after the gelatinization of the starch, the torque and the temperature in the reactor continued to increase to 90 Nm or more and 130° C. or more, respectively. Therefore, it was difficult to perform carboxymethylation, making it impossible to obtain carboxymethylated starch having a uniform degree of substitution.

[0157] Reference example 1-1

[0158] In a closed mixer reactor, 28 g (actual starch content considering the water content: 23.24 g, 0.143 mol) of potato starch (manufactured by Daesang, with a water content of 17 wt %), 6.91 g (0.173 mol, 1.2 equivalents relative to the molar number of starch) of NaOH, 20.11 g (0.173 mol, 1.2 equivalents relative to the molar number of starch) of SMCA and 12 g of distilled water were charged to 90% of the reactor volume and mixed at 50 rpm for 10 minutes to carry out gelatinization and carboxymethylation of starch.

[0159] At this time, the internal torque and temperature in the reactor during mixing were measured using a temperature and torque sensor positioned between two screws provided in the internal mixer reactor, and a graph of the measurement is shown in Figure 3 As a result of the measurement, it was determined that the gelatinization of the starch was completed within 3 minutes from the start of mixing, and after the gelatinization of the starch, the torque and the temperature in the reactor were maintained at 8 Nm to 10 Nm and 96.9±1° C., respectively.

[0160] Thereafter, an additional purification step was performed in the same manner as in Example 1-1 to obtain purified carboxymethylated starch.

[0161] Refer to Example 1-2

[0162] In a closed mixer reactor, 28 g (actual starch content considering the water content: 23.24 g, 0.143 mol) of potato starch (manufactured by Daesang, with a water content of 17 wt %), 6.91 g (0.173 mol, 1.2 equivalents relative to the molar number of starch) of NaOH, 20.11 g (0.173 mol, 1.2 equivalents relative to the molar number of starch) of SMCA, 6 g of distilled water and 6 g of glycerol were charged to 93% of the reactor volume and mixed at 50 rpm for 10 minutes to carry out gelatinization and carboxymethylation of starch.

[0163] At this time, the internal torque and temperature in the reactor during mixing were measured using a temperature and torque sensor positioned between two screws provided in the internal mixer reactor, and a graph of the measurement is shown in Figure 4 As a result of the measurement, it was determined that the gelatinization of the starch was completed within 4 minutes from the start of mixing, and after the gelatinization of the starch, the torque and the temperature in the reactor were maintained at 16 Nm to 18 Nm and 102.5±1° C., respectively.

[0164] Thereafter, an additional purification step was performed in the same manner as in Example 1-1 to obtain purified carboxymethylated starch.

[0165] Refer to Example 1-3

[0166] In a closed mixer reactor, 28 g (actual starch content considering the water content: 23.24 g, 0.143 mol) of potato starch (manufactured by Daesang, with a water content of 17 wt %), 6.91 g (0.173 mol, 1.2 equivalents relative to the molar number of starch) of NaOH, 20.11 g (0.173 mol, 1.2 equivalents relative to the molar number of starch) of SMCA, 6 g of distilled water and 6 g of IPA were charged to 88% of the reactor volume and mixed at 50 rpm for 10 minutes to perform gelatinization and carboxymethylation of starch.

[0167] At this time, the internal torque and temperature in the reactor during mixing were measured using a temperature and torque sensor positioned between two screws provided in the internal mixer reactor, and a graph of the measurement is shown in Figure 5 As a result of the measurement, it was determined that the gelatinization of the starch was completed within 4 minutes from the start of mixing, and after the gelatinization of the starch, the torque and the temperature in the reactor were maintained at 12 Nm to 15 Nm and 98.4±1° C., respectively.

[0168] Thereafter, an additional purification step was performed in the same manner as in Example 1-1 to obtain purified carboxymethylated starch.

[0169] The starch content in the potato starch used in the Examples, Comparative Examples and Reference Examples, the water content in the potato starch, the total water input, the amount of water and additional solvent used relative to the weight of starch, and the equivalents of NaOH and SMCA used are shown in Table 1 below.

[0170] Example - Preparation of Superabsorbent Polymer

[0171] Example 2-1

[0172] (Step 1)

[0173] The carboxymethylated starch prepared in Example 1-1 was dissolved in water in an amount 10 times its weight.

[0174] (Step 2)

[0175] Thereafter, the product of step 1 having a pH of 7.5 to 8 was adjusted to pH 6.5 using a 3% hydrochloric acid aqueous solution and dried for 2 to 3 hours in an oven capable of changing wind direction up and down at the above pH while supplying 120° C. hot air, and then self-crosslinked to prepare a crosslinked polymer.

[0176] (Additional steps)

[0177] Thereafter, the cross-linked polymer was pulverized and classified with a pulverizer to select a size of 150 μm to 850 μm, which was used as a final super absorbent polymer.

[0178] Example 2-2, Comparative Example 2-1, Comparative Example 2-2, and Reference Examples 2-1 to 2-3

[0179] A super absorbent polymer was prepared in the same manner as in Example 2-1, except that the carboxymethylated starch prepared in one of Example 1-2, Comparative Example 1-1, Comparative Example 1-2, and Reference Examples 1-1 to 1-3 was used instead of the carboxymethylated starch prepared in Example 1-1.

[0180] Test Example 1: Measurement of Degree of Substitution of Carboxymethylated Starch

[0181] (1) Measurement of actual degree of substitution

[0182] First, prepare the carboxymethylated starch prepared in one of the embodiments, comparative examples and reference examples. 1 HNMR analysis of the samples and obtained 1 H NMR spectrum. Specifically, for 1 The samples for H NMR analysis were prepared by dissolving them in H 2 The carboxymethylated starch in 0.05% ethanol was added to MeOH, then stirred, filtered and dried. Then, 50 mg of the sample was prepared and dissolved in 0.75 mL of D 2 O and 0.25 mL D 2 SO 4 (these are NMR measurement solvents), and stirred at 90° C. for 1 hour. It was confirmed that the color of the sample changed to dark yellow.

[0183] Thereafter, the carboxymethylated starch prepared in one of Example 1-1, Example 1-2, Reference Example 1-1, Reference Example 1-2 and Reference Example 1-3 1 H NMR spectra are shown in Figures 6 to 10 middle.

[0184] More specifically, the degree of substitution of the carboxymethylated starch prepared in Example 1 was measured as follows.

[0185] 1) in obtaining the carboxymethylated starch prepared in Example 1 1 After the H NMR spectrum, the sum of the integrations of 2.57 ppm, 2.58 ppm, 2.60 ppm, 2.64 ppm, 2.66 ppm, 3.15 ppm, 3.16 ppm, 3.33 ppm, and 3.34 ppm (peaks within 2.5 ppm to 3.6 ppm) was set to 1.

[0186] 2) Next, the degree of substitution at the second carbon position (2-DS) is obtained as the sum of the integrals at the peaks of 3.34 ppm, 3.33 ppm (double peak, 0.23) and 2.57 ppm, 2.58 ppm (double peak, 0.20), the degree of substitution at the third carbon position (3-DS) is obtained by dividing the integral value at the peaks of 2.39 ppm, 2.41 ppm (0.20) by 2, and the degree of substitution at the sixth carbon position (6-DS) is obtained by dividing the integral value at the peaks of 2.14 ppm, 2.15 ppm (0.19) by 2.

[0187] 3) Then, the degree of substitution at the second carbon position (2-DS), the degree of substitution at the third carbon position (3-DS), and the degree of substitution at the sixth carbon position (6-DS) are all added together to obtain the degree of substitution (DS) of the carboxymethyl group.

[0188] In the same manner, the degree of substitution of the carboxymethyl groups of the carboxymethylated starches prepared in other examples, comparative examples and reference examples was obtained. 1 A slight shift may have occurred in the H NMR spectrum, so the results of the degree of substitution measurement compared with the spectrum of Example 1 are shown in Table 2.

[0189] (2) Measurement of reaction efficiency (RE, %)

[0190] The reaction efficiency (RE, %) was calculated according to the following Equation 1, and the results are shown in Table 2.

[0191] [Equation 1]

[0192] Reaction efficiency (RE, %) = (actual substitution degree) / (predicted substitution degree) * 100

[0193] In equation 1,

[0194] The estimated degree of substitution refers to the equivalent amount of SMCA added relative to the moles of starch.

[0195] Test Example 2: Measurement of centrifuge retention capacity (CRC) of superabsorbent polymers

[0196] The centrifuge retention capacity of the superabsorbent polymer prepared in one of Examples, Comparative Examples and Reference Examples was measured by water absorption capacity under no load conditions according to EDANA WSP 241.3 (European Disposables and Nonwovens Association) and is shown in Table 3.

[0197] Specifically, the super absorbent polymers prepared in the examples, comparative examples and reference examples were classified using a sieve of #30 to #50 to obtain only super absorbent polymers having a particle size of 300 μm to 600 μm. 0 After the superabsorbent polymer (g, about 0.17 g) was uniformly inserted into the nonwoven fabric envelope and sealed, it was immersed in physiological saline (0.9 wt % sodium chloride aqueous solution) at room temperature. After 30 minutes, the envelope was centrifuged at 250G for 3 minutes to drain water, and the weight of the envelope was measured. 2 (g). In addition, after the same operation was performed without using the polymer, the weight W of the encapsulated material was measured. 1 (g).

[0198] Then, CRC (g / g) was calculated according to the following Equation 2 using the obtained weight value.

[0199] [Equation 2]

[0200] CRC(g / g)={[W 2 (g)-W 1 (g)] / W 0 (g)}-1

[0201] [Table 1]

[0202]

[0203] * The amount of water and other solvents used: by weight relative to the weight of starch

[0204] [Table 2]

[0205]

[0206] [Table 3]

[0207]

[0208] Referring to Tables 1 to 3 above, it is determined that the preparation method of the embodiment in which starch gelatinization and carboxymethylation are performed using a specific content of water and a predetermined torque is maintained after gelatinization of the starch exhibits significantly improved reaction efficiency compared to the preparation method of Comparative Example 1-1 in which starch gelatinization and carboxymethylation are performed using an excess amount of solvent according to a known preparation method.

[0209] In addition, in the case of the carboxymethylated starch prepared in Comparative Example 1-2, a similar equivalent of SMCA as in the example was used, and thus the degree of substitution was also similar, but the water retention capacity of the final superabsorbent polymer was significantly lower than that of the superabsorbent polymer produced using the carboxymethylated starch of the example. This is considered to be because, unlike the example, torque was not sufficiently induced in the flask reactor, and the torque could not be maintained at a certain level after gelatinization of the starch, so the carboxymethyl group was not uniformly substituted compared to the carboxymethylated starch of the example.

[0210] Furthermore, it was determined from Comparative Examples 1-3 that when too little water was used during gelatinization and carboxymethylation of starch, the internal torque in the reactor continued to increase after gelatinization, making it impossible to produce uniformly substituted carboxymethylated starch.

[0211] Furthermore, it was confirmed from Reference Examples 1-1 to 1-3 that when the equivalent amount of the reactants was adjusted to an appropriate amount while performing carboxymethylation using water as the only solvent, the carboxymethylation efficiency could be further improved.

Claims

1. A method for preparing a carboxyalkylated polysaccharide, comprising the following steps: The polysaccharide, hydroxide, metal salt of halogenated alkyl carboxylic acid and water are mixed in a reactor, and the polysaccharide is gelatinized and carboxyalkylated. wherein the water is used in an amount of 0.35 to 1.0 times the weight of the polysaccharide, and After gelatinization of the polysaccharide, the torque in the reactor was maintained at 7 to 18 Nm.

2. The method according to claim 1, No solvents other than water are used.

3. The method according to claim 1, The water is used in an amount of 0.45 to 0.75 times the weight of the polysaccharide.

4. The method according to claim 1, The polysaccharide is one or more selected from starch, dextrin, glycogen, cellulose, pectin, inulin, agar and guar gum.

5. The method according to claim 1, The degree of substitution (DS) of the carboxyalkyl group in the prepared carboxyalkylated polysaccharide is 0.6 to 1.

1.

6. The method according to claim 1, The carboxyalkylated polysaccharide is carboxymethylated.

7. The method according to claim 1, The mixing is performed in a state where 70% to 95% of the total volume of the reactor is filled.

8. The method according to claim 1, The reactor is a closed mixer.

9. The method according to claim 1, The hydroxide is at least one selected from the group consisting of sodium hydroxide, potassium hydroxide and lithium hydroxide.

10. The method according to claim 1, wherein the hydroxide is used in an amount of 0.5 equivalents or more and less than 1.2 equivalents relative to the number of moles obtained by dividing the weight (g) of the polysaccharide by the molecular weight of anhydroglucose unit (AGU).

11. The method according to claim 1, The metal salt of the halogenated alkyl carboxylic acid is an alkali metal salt of chloroacetic acid.

12. The method according to claim 11, The alkali metal salt of chloroacetic acid is at least one selected from sodium monochloroacetate (SMCA), potassium monochloroacetate and lithium monochloroacetate.

13. The method according to claim 1, wherein the metal salt of the halogenated alkyl carboxylic acid is used in an amount of 1 mol to 1.29 mol based on 1 mol of the hydroxide.

14. The method according to claim 1, The mixing is performed for 5 to 15 minutes.

15. The method according to claim 1, The gelatinization of the polysaccharide is completed within 2 / 5 of the total mixing time from the start of mixing.

16. The method according to claim 1, Wherein after gelatinization of the polysaccharide, the temperature in the reactor is maintained at 90°C to 110°C.

17. The method according to claim 1, The method further includes dissolving the prepared product in water and then precipitating it in an alcohol-based organic solvent.

18. The method according to claim 17, The alcohol-based organic solvent is at least one selected from methanol, ethanol and isopropanol.

19. A method for preparing a biodegradable superabsorbent polymer, comprising the steps of: Dissolving the carboxyalkylated polysaccharide prepared according to the preparation method according to any one of claims 1 to 18 in water in an amount of 5 to 15 times its weight (step 1); and The product of step 1 is allowed to self-crosslink while drying at pH 6 to 8 (step 2).

20. The method according to claim 19, The super absorbent polymer prepared therein satisfies a centrifuge retention capacity (CRC) of 30 g / g to 45 g / g measured according to EDA NAWSP 241.

3.

21. The method according to claim 19, The dissolution in step 1 is carried out under standard temperature and pressure conditions.

22. The method according to claim 19, The drying in step 2 is carried out at a temperature of 100°C to 130°C.

23. The method according to claim 19, After step 2, The method further comprises the step of pulverizing and classifying the cross-linked polymer prepared in step 2.