Method for producing polymer, varnish, and method for producing varnish
By controlling the molar ratio of diamine to tetracarboxylic acid dianhydride and tert-butanol ratio during the polymerization process, a polymer with high molecular weight and excellent storage stability is formed, and the problem of viscosity change of polyimide resin is solved, and the High strength and long-term stability of polyimide films.
Patent Information
- Application Number
- CN202380028248.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-01
AI Technical Summary
Existing polyimide resins are prone to viscosity changes under high molecular weight and different resin concentrations, which are difficult to maintain stability, especially during storage and use, which leads to difficult to control the viscosity increase and affects its application performance.
By polymerizing diamine and tetracarboxylic dianhydride in the presence of tert-butanol and solvent during the polymerization process, the molar ratio of diamine/tetracarboxylic dianhydride is controlled to be above 1.00 and less than 1.03 to ensure the weight uniformity of the polymer. The molecular weight reaches more than 300,000, and a specific monomer ratio and tert-butanol ratio are used to form a polymer with excellent storage stability.
It has achieved a polymer with less viscosity increase and excellent storage stability in high molecular weight resins. It is suitable for the manufacture of various polyimide films, and has improved the mechanical strength and service life of the polyimide film.
Smart Images

Figure BDA0005046734210000031 
Figure BDA0005046734210000032 
Figure BDA0005046734210000061
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a polymer, a varnish, and a method for producing the varnish. Background Art
[0002] Polyimide resins have excellent mechanical properties and heat resistance, and therefore are being studied for various applications in the fields of electrical and electronic components. For example, since it is expected that glass substrates used in image display devices such as liquid crystal displays and OLED displays will be replaced by polyimide film substrates, polyimide resins that meet the performance requirements of optical materials are being developed.
[0003] As a raw material for producing polyimide molded products including such polyimide films, varnishes are used, which are solutions of polyimide or polyimide precursor dissolved in a solvent. Varnishes have also been studied in order to improve the performance of the obtained polyimide molded products and to facilitate the production of the molded products.
[0004] For example, Patent Document 1 discloses a varnish containing a polymer such as polyamic acid and a solvent, and a compound such as a monovalent primary amine and a monohydric alcohol in specific amounts for the purpose of improving storage stability.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2021-014564 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] Although polyimide resin has excellent properties as mentioned above, higher strength and heat resistance are gradually required recently. Therefore, the high molecular weight of polyimide resin is gradually needed. In addition, according to the shape, thickness and purpose of the target polyimide film, varnishes of various resin concentrations are needed. On the other hand, the varnish comprising high molecular weight polyimide or polyimide precursor has the problem of viscosity rising easily during storage. And then, if the resin concentration changes, the viscosity changes greatly, but according to the purpose, the required resin concentration is different. Like this, it is difficult to suppress the viscosity change of varnish and maintain stability under various resin concentrations. Especially seek a varnish comprising high molecular weight polyimide or polyimide precursor and excellent storage stability.
[0010] The present invention has been made in view of such a situation, and an object of the present invention is to provide a method for producing a polymer, a varnish containing the polymer, and a method for producing a varnish, wherein the method for producing a polymer can produce a varnish having a small viscosity increase in a wide viscosity range and excellent storage stability even if it contains a high molecular weight resin.
[0011] Solutions for solving problems
[0012] The present inventors have found that the above-mentioned problems can be solved by setting the monomer ratio to a specific range when obtaining a polyimide or a polymer which is a polyimide precursor, and performing polymerization in the presence of tert-butyl alcohol, thereby completing the invention.
[0013] That is, the present invention relates to the following [1] to
[14] .
[0014] [1] A method for producing a polymer, comprising a step 1 of polymerizing a diamine and a tetracarboxylic dianhydride to obtain a polymer, wherein the molar ratio of the diamine to the tetracarboxylic dianhydride in the step 1 (diamine / tetracarboxylic dianhydride) is 1.00 or more and less than 1.03, and the step 1 is a step of polymerizing the diamine and the tetracarboxylic dianhydride in the presence of tert-butyl alcohol and a solvent, and the polymer has at least one selected from the group consisting of an amic acid unit and an imide unit as a repeating unit, and has a weight average molecular weight of 300,000 or more.
[0015] [2] The method for producing a polymer according to [1], wherein the polymer is at least one selected from the group consisting of polyamic acid, polyimide, and imide-amic acid copolymer.
[0016] [3] The method for producing a polymer according to [1] or [2], wherein the polymer is a polyamic acid, and step 1 is a step of mixing a solution containing a diamine and a solvent with tetracarboxylic dianhydride and tert-butyl alcohol to perform polymerization.
[0017] [4] The method for producing a polymer according to any one of [1] to [3], wherein the polymer is a polyamic acid, the tetracarboxylic dianhydride includes a compound represented by the following formula (a1), and the diamine includes a compound represented by the following general formula (b1).
[0018]
[0019] (In formula (b1), R 1 , R 2 , R 3 Each independently represents an organic group having 1 to 20 carbon atoms. h, i, j, and k are integers of 0 to 4.
[0020] [5] The method for producing a polymer according to the above [1] or [2], wherein the above polymer is an imide-amic acid copolymer, the above tetracarboxylic dianhydride comprises a first tetracarboxylic dianhydride and a second tetracarboxylic dianhydride, the above diamine comprises a first diamine and a second diamine, and the above step 1 comprises the following step 1-1 and the following step 1-2.
[0021] Step 1-1: a step of reacting the first tetracarboxylic dianhydride with the first diamine in the presence of a solvent to obtain an imide oligomer
[0022] Step 1-2: A step of mixing the imide oligomer obtained in step 1-1, the second tetracarboxylic dianhydride, the second diamine and tert-butyl alcohol to polymerize
[0023] [6] A method for producing a polymer according to the above [5], wherein the above polymer is an imide-amic acid copolymer, the above first tetracarboxylic dianhydride comprises a compound represented by the following formula (a1), the above second tetracarboxylic dianhydride comprises a compound represented by the following formula (a2), and the above first diamine and the above second diamine comprise a compound represented by the following formula (b1).
[0024]
[0025] (In formula (b1), R 1 , R 2 , R 3 Each independently represents an organic group having 1 to 20 carbon atoms. h, i, j, and k are integers of 0 to 4.
[0026] [7] The method for producing a polymer according to any one of [1] to [6], wherein the amount of tert-butyl alcohol in step 1 is 2 mol% or more relative to the total amount of tetracarboxylic dianhydride in step 1.
[0027] [8] A varnish comprising a polymer obtained by the production method according to any one of [1] to [7] above and a solvent.
[0028] [9] A method for producing a varnish, comprising a step 1 of polymerizing a diamine and a tetracarboxylic dianhydride to obtain a polymer, wherein the molar ratio of the diamine to the tetracarboxylic dianhydride in the step 1 (diamine / tetracarboxylic dianhydride) is 1.00 or more and less than 1.03, the step 1 is a step of polymerizing the diamine and the tetracarboxylic dianhydride in the presence of tert-butyl alcohol and a solvent, the polymer has at least one selected from the group consisting of an amic acid unit and an imide unit as a repeating unit, and has a weight average molecular weight of 300,000 or more, and the varnish contains the polymer and a solvent.
[0029]
[10] A varnish obtained by the production method described in [9] above.
[0030]
[11] The varnish according to [8] or
[10] , wherein the rate of increase in viscosity on the 7th day after storage at 23°C is 15% or less relative to the viscosity on the 0th day.
[0031]
[12] The varnish according to [8],
[10] or
[11] above, wherein the solvent contains at least one selected from the group consisting of cyclic amides, chain amides and cyclic esters.
[0032]
[13] The varnish according to any one of [8] or
[10] to
[12] above, wherein the solvent contains N-methylpyrrolidone.
[0033]
[14] A method for producing a polyimide film, comprising: a step of casting the varnish described in any one of [8] or
[10] to
[13] above onto a substrate; and a step of drying the cast varnish to form a polymer film.
[0034] Effects of the Invention
[0035] According to the present invention, a method for producing a polymer, a varnish containing the polymer, and a method for producing the varnish can be provided, wherein the method for producing the polymer can obtain a varnish having a small viscosity increase and excellent storage stability even if a high molecular weight resin is contained. In addition, a method for producing a polyimide film using the varnish can also be provided. DETAILED DESCRIPTION
[0036] [Method for producing polymer]
[0037] The method for producing a polymer of the present invention comprises a step 1 of polymerizing a diamine and a tetracarboxylic dianhydride to obtain a polymer, wherein the molar ratio of the diamine to the tetracarboxylic dianhydride in the step 1 (diamine / tetracarboxylic dianhydride) is 1.00 or more and less than 1.03, and the step 1 is a step of polymerizing the diamine and the tetracarboxylic dianhydride in the presence of tert-butyl alcohol and a solvent, and the polymer has at least one selected from the group consisting of an amic acid unit and an imide unit as a repeating unit, and has a weight average molecular weight of 300,000 or more.
[0038] <Polymer>
[0039] First, the polymer produced by the above-mentioned production method will be described.
[0040] The polymer has at least one selected from the group consisting of amic acid units and imide units as a repeating unit, preferably an amic acid unit as a structural unit, and more preferably both amic acid units and imide units as repeating units from the viewpoint of improving storage stability.
[0041] Here, "using an amic acid unit as a repeating unit" means a unit having an amic acid structure in which one tetracarboxylic dianhydride and one diamine are bonded to each other, and refers to the smallest unit repeated in the aforementioned polymer. In addition, "using an imide unit as a repeating unit" means a unit having an imide structure in which one tetracarboxylic dianhydride and one diamine are bonded to each other, and refers to the smallest unit repeated in the aforementioned polymer.
[0042] The aforementioned polymer is preferably at least one selected from the group consisting of polyamic acid, polyimide and imide-amic acid copolymer, more preferably at least one selected from the group consisting of polyamic acid and imide-amic acid copolymer, from the viewpoint of obtaining a high molecular weight polymer, polyamic acid is further preferred, and from the viewpoint of improving storage stability, imide-amic acid copolymer is further preferred.
[0043] From the viewpoint of the mechanical strength of the obtained polyimide film, the weight average molecular weight (Mw) of the above-mentioned polymer is 300,000 or more, preferably 400,000 or more, and more preferably 500,000 or more. In addition, there is no upper limit, but it is preferably 1,000,000 or less, and more preferably 700,000 or less. In addition, from the same viewpoint, the number average molecular weight is preferably 50,000 to 500,000. In addition, the weight average molecular weight and number average molecular weight of the polymer can be obtained by the standard polystyrene (PS) conversion value measured based on gel permeation chromatography.
[0044] As described above, in the step 1, since diamine and tetracarboxylic dianhydride are polymerized in the presence of tert-butyl alcohol, the polymer has a tert-butyloxy group derived from tert-butyl alcohol at a part of the terminals.
[0045] (Structural units of polymers)
[0046] The aforementioned polymer has a structural unit A derived from tetracarboxylic dianhydride and a structural unit B derived from a diamine.
[0047] It should be noted that, when the polymer is polyamic acid, structural unit A and structural unit B form an amic acid structure, when the polymer is polyimide, structural unit A and structural unit B form an imide structure, and when the polymer is an imide-amic acid copolymer, structural unit A and structural unit B simultaneously form an imide structure and an amic acid structure. The structural units derived from tetracarboxylic dianhydride are collectively referred to as structural units A, and the structural units derived from diamines are collectively referred to as structural units B.
[0048] (Structural unit A)
[0049] The structural unit A is a structural unit derived from tetracarboxylic dianhydride. There are no particular limitations on the structural unit as long as it is derived from tetracarboxylic dianhydride. It preferably contains a structural unit derived from aromatic tetracarboxylic dianhydride, and more preferably a structural unit derived from aromatic tetracarboxylic dianhydride.
[0050] Examples of the aromatic tetracarboxylic dianhydride that imparts a structural unit derived from an aromatic tetracarboxylic dianhydride include biphenyltetracarboxylic dianhydride (BPDA), 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), pyromellitic dianhydride, 3,3',4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, and 2,2',3,3'-benzophenonetetracarboxylic dianhydride.
[0051] Among these, from the viewpoint of achieving a high molecular weight, at least one selected from the group consisting of a compound represented by the following formula (a1) and a compound represented by the following formula (a2) is preferred, and a compound represented by the following formula (a1) is more preferred.
[0052] That is, the structural unit A preferably contains at least one selected from the group consisting of a structural unit (A1) derived from a compound represented by the following formula (a1) and a structural unit (A2) derived from a compound represented by the following formula (a2), and more preferably contains a structural unit (A1) derived from a compound represented by the following formula (a1).
[0053]
[0054] The compound represented by formula (a1) is biphenyltetracarboxylic dianhydride (BPDA), and specific examples thereof include: 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA) represented by the following formula (a1s), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA) represented by the following formula (a1a), and 2,2',3,3'-biphenyltetracarboxylic dianhydride (i-BPDA) represented by the following formula (a1i). Among them, 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA) represented by the following formula (a1s) is preferred.
[0055]
[0056] The compound represented by formula (a2) is 9,9′-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF).
[0057] When the polymer is a polyamic acid, it preferably contains the structural unit (A1).
[0058] When the polymer is an imide-amic acid copolymer, it is preferred that the polyimide unit contains the structural unit (A2), and the polyamic acid unit contains the structural unit (A1).
[0059] The structural unit A may contain structural units other than aromatic tetracarboxylic dianhydride. Although it does not specifically limit as tetracarboxylic dianhydride which provides such a structural unit, alicyclic tetracarboxylic dianhydride and aliphatic tetracarboxylic dianhydride are mentioned.
[0060] Examples of the alicyclic tetracarboxylic dianhydride that imparts a structural unit derived from an alicyclic tetracarboxylic dianhydride include 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, dicyclohexyltetracarboxylic dianhydride, 5,5'-(1,4-phenylene)-bis[hexahydro-4,7-methanoisobenzofuran-1,3-dione], 5,5'-bis-2-norbornene-5,5',6,6'-tetracarboxylic acid-5,5',6,6'-dianhydride, and positional isomers thereof.
[0061] As an aliphatic tetracarboxylic dianhydride which provides the structural unit derived from an aliphatic tetracarboxylic dianhydride, 1,2,3,4-butanetetracarboxylic dianhydride etc. are mentioned.
[0062] The structural unit optionally contained in the structural unit A may be one type or two or more types.
[0063] In the present specification, aromatic tetracarboxylic dianhydride refers to a tetracarboxylic dianhydride containing one or more aromatic rings, alicyclic tetracarboxylic dianhydride refers to a tetracarboxylic dianhydride containing one or more alicyclic rings and no aromatic ring, and aliphatic tetracarboxylic dianhydride refers to a tetracarboxylic dianhydride containing neither an aromatic ring nor an alicyclic ring.
[0064] (Structural unit B)
[0065] The structural unit B is a structural unit derived from a diamine. There are no particular limitations on the structural unit as long as it is a structural unit derived from a diamine. However, it preferably includes a structural unit derived from an aromatic diamine, and more preferably includes a structural unit derived from an aromatic diamine.
[0066] Examples of the aromatic diamine to which the structural unit derived from the aromatic diamine is added include 4-aminophenyl-4-aminobenzoate (4-BAAB), 2,2'-bis(trifluoromethyl)benzidine (TFMB), 3,5-diaminobenzoic acid (3,5-DABA), 9,9-bis(4-aminophenyl)fluorene (BAFL), 1,4-phenylenediamine, p-phenylenediamine, 1,5-diaminonaphthalene, 2,2'-dimethylbiphenyl-4,4'-diamine, 4,4'-diaminodiphenylmethane, 1,4- Bis[2-(4-aminophenyl)-2-propyl]benzene, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-diaminobenzanilide, 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-inden-5-amine, α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, N,N'-bis(4-aminophenyl)terephthalamide, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 1,4-bis(4-aminophenoxy)benzene, etc.
[0067] From the viewpoint of achieving a high molecular weight, a compound represented by the following formula (b1) is preferred among the aromatic diamines.
[0068]
[0069] (In formula (b1), R 1 , R 2 , R 3 Each independently represents an organic group having 1 to 20 carbon atoms. h, i, j, and k are integers of 0 to 4.
[0070] That is, the structural unit B preferably includes a structural unit (B1) derived from the compound represented by the above formula (b1).
[0071] R 1 , R 2 , R 3 Each independently represents an organic group having 1 to 20 carbon atoms, preferably R 1 , R 2 , R 3 Each is independently methyl or trifluoromethyl.
[0072] h, i, j, and k are integers of 0 to 4, and h, i, j, and k are each preferably 0.
[0073] It should be noted that, when the structural unit B includes the structural unit (B1) derived from the compound represented by the aforementioned formula (b1), it is preferred that the structural unit A includes the structural unit (A1) derived from the compound represented by the aforementioned formula (a1). That is, it is preferred that the structural unit A of the aforementioned polymer includes the structural unit (A1) derived from the compound represented by the aforementioned formula (a1), and the structural unit B of the aforementioned polymer includes the structural unit (B1) derived from the compound represented by the aforementioned formula (b1). By setting the combination of the above structural units, a high molecular weight polymer with excellent film properties can be obtained, and the effect of the present invention, namely, storage stability, can be more clearly manifested.
[0074]
[0075] Among the compounds represented by the above formula (b1), the compound represented by the formula (b11) (4-aminophenyl-4-aminobenzoate (4-BAAB)) is particularly preferred.
[0076] That is, it is particularly preferred that the structural unit B includes a structural unit (B11) derived from a compound represented by the above formula (b11).
[0077] It should be noted that, when the structural unit B includes the structural unit (B11) derived from the compound represented by the aforementioned formula (b11), it is preferred that the structural unit A includes the structural unit (A1) derived from the compound represented by the aforementioned formula (a1). That is, it is preferred that the structural unit A of the aforementioned polymer includes the structural unit (A1) derived from the compound represented by the aforementioned formula (a1), and the structural unit B of the aforementioned polymer includes the structural unit (B11) derived from the compound represented by the aforementioned formula (b11). By setting the combination of the above structural units, a high molecular weight polymer with excellent film properties can be obtained, and the effect of the present invention, namely, storage stability, can be particularly clearly manifested.
[0078] The structural unit B may contain structural units other than aromatic diamines. The diamine that provides such structural units is not particularly limited, and examples thereof include alicyclic diamines and aliphatic diamines.
[0079] As an alicyclic diamine which provides the structural unit derived from an alicyclic diamine, 1, 3- bis (aminomethyl) cyclohexane, 1, 4- bis (aminomethyl) cyclohexane, etc. are mentioned.
[0080] Examples of the aliphatic diamine for providing the structural unit derived from the aliphatic diamine include ethylenediamine and hexamethylenediamine.
[0081] The structural unit optionally contained in the structural unit B may be one kind or two or more kinds.
[0082] In the present specification, aromatic diamine refers to a diamine containing one or more aromatic rings, alicyclic diamine refers to a diamine containing one or more alicyclic rings and no aromatic ring, and aliphatic diamine refers to a diamine containing neither an aromatic ring nor an alicyclic ring.
[0083] (Method for producing polymer and method for producing varnish)
[0084] As described above, the method for producing the polymer comprises step 1 of polymerizing a diamine and a tetracarboxylic dianhydride to obtain a polymer, wherein the molar ratio of the diamine to the tetracarboxylic dianhydride in the step 1 (diamine / tetracarboxylic dianhydride) is greater than 1.00 and less than 1.03, and the step 1 is a step of polymerizing a diamine and a tetracarboxylic dianhydride in the presence of tert-butyl alcohol and a solvent, and is preferably carried out by the following method.
[0085] The aforementioned polymer contains either or both of an imide unit and an amic acid unit, and these can be adjusted by changing the production method.
[0086] Specifically, in the manufacturing method (manufacturing method of imide-amic acid copolymer) containing both imide units and amic acid units, a polymer (polyimide) substantially composed of imide units can be obtained by using only a process for manufacturing a portion mainly containing imide units (polyimide portion), and a polymer (polyamic acid) substantially composed of amic acid units can be obtained by using only a process for manufacturing a portion mainly containing amic acid units (polyamic acid portion).
[0087] If the above method is used, a polymer solution containing a polymer dissolved in a solvent can be obtained. The varnish of the present invention can be obtained by further adding a solvent to the above polymer solution, or by concentrating the solution to reduce the solvent. Therefore, the manufacturing method of the varnish of the present invention includes the manufacturing method of the above polymer.
[0088] In other words, the method for producing a varnish of the present invention comprises a step 1 of polymerizing a diamine and a tetracarboxylic dianhydride to obtain a polymer, wherein the molar ratio of the diamine to the tetracarboxylic dianhydride in the step 1 (diamine / tetracarboxylic dianhydride) is 1.00 or more and less than 1.03, the step 1 is a step of polymerizing the diamine and the tetracarboxylic dianhydride in the presence of tert-butyl alcohol and a solvent, the polymer has at least one selected from the group consisting of an amic acid unit and an imide unit as a repeating unit, and has a weight average molecular weight of 300,000 or more, and the varnish comprises the polymer and a solvent.
[0089] The varnish may be the polymer solution obtained in the above-mentioned method for producing the polymer, or may be a solution obtained by further adding a solvent, or may be a solution obtained by reducing the solvent by concentration, etc. That is, the method for producing the varnish may be any of a method having only the above-mentioned step 1, a method having a step of adding a solvent after the above-mentioned step 1, or a method having a step of reducing the solvent after the above-mentioned step 1.
[0090] As described above, when the polymer obtained by the manufacturing method of the present invention is an imide-amic acid copolymer, a polyimide or a polyamic acid, the conditions of the suitable process 1 are different, but the molar ratio of the aforementioned diamine in process 1 to the aforementioned tetracarboxylic dianhydride (diamine / tetracarboxylic dianhydride) is 1.00 or more and less than 1.03. The molar ratio of the aforementioned diamine in process 1 to the aforementioned tetracarboxylic dianhydride (diamine / tetracarboxylic dianhydride) is preferably 1.005 or more, more preferably 1.010 or more. In addition, it is preferably 1.025 or less, more preferably 1.020 or less. By setting the molar ratio of the aforementioned diamine in process 1 to the aforementioned tetracarboxylic dianhydride to the aforementioned range, a high molecular weight polymer can be obtained, and even if a high molecular weight polymer is included, a varnish with less viscosity increase and excellent storage stability can be obtained.
[0091] In addition, the amount of tert-butyl alcohol used in step 1 is preferably 2 mol% or more, more preferably 2.5 mol% or more, and further preferably 3 mol% or more relative to the total amount of tetracarboxylic dianhydride in step 1. In addition, it is preferably 5 mol% or less, more preferably 4 mol% or less, and further preferably 3.5 mol% or less. By setting the amount of tert-butyl alcohol in step 1 to the above range, even if a high molecular weight polymer is included, the viscosity increase is small and the varnish with excellent storage stability can be obtained.
[0092] The reason why a varnish having excellent storage stability and little viscosity increase can be obtained by setting the molar ratio of the diamine to the tetracarboxylic dianhydride to the above range and using tert-butyl alcohol is not clear, but it is considered that the reaction between the diamine and the acid dianhydride is suppressed by the reaction between the acid dianhydride and tert-butyl alcohol.
[0093] Hereinafter, the polymer obtained by the above-mentioned production method is divided into the case where the polymer is an imide-amic acid copolymer, the case where the polymer is a polyimide, and the case where the polymer is a polyamic acid, and will be described in detail.
[0094] (Method for producing imide-amic acid copolymer)
[0095] In a preferred production method for a polymer containing both an imide unit and an amic acid unit (hereinafter also referred to as an imide-amic acid copolymer), the tetracarboxylic dianhydride contains a first tetracarboxylic dianhydride and a second tetracarboxylic dianhydride, the diamine contains a first diamine and a second diamine, and step 1 includes the following steps 1-1 and 1-2.
[0096] Step 1-1: a step of reacting the first tetracarboxylic dianhydride with the first diamine in the presence of a solvent to obtain an imide oligomer
[0097] Step 1-2: A step of mixing the imide oligomer obtained in step 1-1, the second tetracarboxylic dianhydride, the second diamine, and tert-butyl alcohol to perform polymerization.
[0098] The preferred tetracarboxylic dianhydride and diamine used in each process are stated in the description of each process, but when the polymer obtained by the production method of the present invention is an imide-amic acid copolymer, it is preferred that the first tetracarboxylic dianhydride contains a compound represented by the following formula (a1), the second tetracarboxylic dianhydride contains a compound represented by the following formula (a2), and the first diamine and the second diamine contain a compound represented by the following formula (b1).
[0099]
[0100] (In formula (b1), R 1 , R 2 , R 3 Each independently represents an organic group having 1 to 20 carbon atoms. h, i, j, and k are integers of 0 to 4.
[0101] R 1 , R 2 , R 3 Each independently represents an organic group having 1 to 20 carbon atoms, preferably R 1 , R 2 , R 3 Each is independently methyl or trifluoromethyl.
[0102] h, i, j, and k are integers of 0 to 4, and h, i, j, and k are each preferably 0.
[0103] [Process 1-1]
[0104] Step 1-1 is a step of reacting the first tetracarboxylic dianhydride constituting the imide portion with the first diamine in the presence of a solvent to obtain an imide oligomer.
[0105] The first tetracarboxylic dianhydride used in step 1-1 preferably contains an aromatic tetracarboxylic dianhydride, and more preferably contains an aromatic tetracarboxylic dianhydride. In addition, it is preferred to contain a compound represented by the above formula (a2). The first tetracarboxylic dianhydride may contain tetracarboxylic dianhydrides other than aromatic tetracarboxylic dianhydrides.
[0106] The first diamine used in step 1-1 preferably contains an aromatic diamine, more preferably an aromatic diamine. In addition, it preferably contains a compound represented by the above formula (b1), more preferably a compound represented by the above formula (b11). The first diamine may contain a diamine other than an aromatic diamine.
[0107] In step 1-1, the amount of diamine is preferably 1.01 to 2 mol, more preferably 1.05 to 1.9 mol, and even more preferably 1.1 to 1.7 mol, based on tetracarboxylic dianhydride.
[0108] The method for reacting the first tetracarboxylic dianhydride and the first diamine to obtain the imide oligomer in step 1-1 is not particularly limited, and a known method can be used.
[0109] Specific reaction methods include: (1) a method in which tetracarboxylic dianhydride, a diamine and a solvent are placed in a reactor, stirred at 10 to 110° C. for 0.5 to 30 hours, and then the temperature is increased to carry out an imidization reaction; (2) a method in which a diamine and a solvent are placed in a reactor and dissolved, and then tetracarboxylic dianhydride is placed in the reactor, stirred at 10 to 110° C. for 0.5 to 30 hours as required, and then the temperature is increased to carry out an imidization reaction; (3) a method in which tetracarboxylic dianhydride, a diamine and a solvent are placed in a reactor, and the temperature is immediately increased to carry out an imidization reaction, etc.
[0110] In the imidization reaction, it is preferred to use a Dean-Stark apparatus or the like to carry out the reaction while removing water generated during the production. By carrying out such an operation, the degree of polymerization and the imidization ratio can be further increased.
[0111] In the above-mentioned imidization reaction, a known imidization catalyst can be used. Examples of the imidization catalyst include a base catalyst and an acid catalyst.
[0112] Examples of the base catalyst include organic base catalysts such as pyridine, quinoline, isoquinoline, α-methylpyridine, β-methylpyridine, 2,4-lutidine, 2,6-lutidine, trimethylamine, triethylamine, tripropylamine, tributylamine, triethylenediamine, imidazole, N,N-dimethylaniline, and N,N-diethylaniline; and inorganic base catalysts such as potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, potassium hydrogen carbonate, and sodium hydrogen carbonate.
[0113] Examples of the acid catalyst include crotonic acid, acrylic acid, trans-3-hexenoic acid, cinnamic acid, benzoic acid, methylbenzoic acid, hydroxybenzoic acid, terephthalic acid, benzenesulfonic acid, p-toluenesulfonic acid, and naphthalenesulfonic acid. The above imidization catalysts may be used alone or in combination of two or more.
[0114] Among the above, from the viewpoint of operability, a base catalyst is preferred, an organic base catalyst is more preferred, at least one selected from triethylamine and triethylenediamine is further preferred, and triethylamine is further preferred.
[0115] From the viewpoint of reaction rate and suppression of gelation, the temperature of the imidization reaction is preferably 120 to 250° C., more preferably 160 to 200° C. The reaction time is preferably 0.5 to 10 hours after the start of distillation of generated water.
[0116] The solution containing the imide oligomer dissolved in the solvent is obtained by the above method. The solution containing the imide oligomer obtained in step 1-1 may contain at least a part of the components used as the first tetracarboxylic dianhydride and the first diamine in step 1-1 as unreacted monomers within the range not impairing the effects of the present invention.
[0117] [Process 1-2]
[0118] Step 1-2 in the production method of the present invention is a step of mixing the imide oligomer obtained in step 1-1, the second tetracarboxylic dianhydride, the second diamine, and tert-butyl alcohol to perform polymerization.
[0119] The second tetracarboxylic dianhydride used in step 1-2 preferably contains an aromatic tetracarboxylic dianhydride, and more preferably contains an aromatic tetracarboxylic dianhydride. In addition, it is preferred to contain a compound represented by the above formula (a1). The second tetracarboxylic dianhydride may contain tetracarboxylic dianhydrides other than aromatic tetracarboxylic dianhydrides.
[0120] The second diamine used in step 1-2 preferably contains an aromatic diamine, more preferably an aromatic diamine. In addition, it preferably contains a compound represented by the above formula (b1), more preferably a compound represented by the above formula (b11). The second diamine may contain a diamine other than an aromatic diamine.
[0121] Since the molar ratio of diamine to tetracarboxylic dianhydride in the whole process 1-1 and process 1-2 (diamine / tetracarboxylic dianhydride) is 1.00 or more and less than 1.03, the molar ratio of diamine to tetracarboxylic dianhydride in process 1-2 is determined in such a manner that the ratio of the whole process 1-1 and process 1-2 is 1.00 or more and less than 1.03, taking into account the respective amounts used in the above-mentioned process 1-1. Among them, the molar ratio of diamine to tetracarboxylic dianhydride in process 1-2 is preferably 0.70 to 1.00 mol, more preferably 0.80 to 0.95 mol, and even more preferably 0.85 to 0.90 mol.
[0122] In operation 1-2, in addition to the aforementioned imide oligomer, the second tetracarboxylic dianhydride, and the second diamine, tert-butyl alcohol is also mixed. The amount of tert-butyl alcohol used in operation 1-2 is not limited, and the total amount of tetracarboxylic dianhydride relative to the entirety of operation 1-1 and operation 1-2 is preferably 2 mol% or more, more preferably 2.5 mol% or more, and further preferably 3 mol% or more. In addition, it is preferably 5 mol% or less, more preferably 4 mol% or less, and further preferably 3.5 mol% or less. By setting the amount of tert-butyl alcohol in operation 1-2 to the aforementioned range, even if a high molecular weight polymer is included, a varnish having a low viscosity rise and excellent storage stability can be obtained.
[0123] In step 1-2, the method for polymerizing the imide oligomer obtained in step 1-1, the second tetracarboxylic dianhydride, and the second diamine is not particularly limited, and a known method can be used.
[0124] Specific reaction methods include: (1) a method in which an imide oligomer, a second tetracarboxylic dianhydride, a second diamine and tert-butanol are introduced into a reactor and stirred at a temperature in the range of 0 to 120° C., preferably 5 to 80° C., for 1 to 72 hours; (2) a method in which an imide oligomer and a solvent are introduced into a reactor and dissolved, and then a second tetracarboxylic dianhydride, a second diamine and tert-butanol are introduced and stirred at a temperature in the range of 0 to 120° C., preferably 5 to 80° C., for 1 to 72 hours.
[0125] In addition, in any method, it is preferable to dissolve the diamine in a solvent in advance.
[0126] When the reaction is conducted at 80° C. or lower, the molecular weight of the copolymer obtained in step 1-2 does not vary depending on the temperature history during polymerization, and the progress of thermal imidization can be suppressed, so the copolymer can be produced stably.
[0127] The concentration of the copolymer in the obtained solution is usually in the range of 1 to 50% by mass, preferably 3 to 35% by mass, and more preferably 5 to 30% by mass.
[0128] From the viewpoint of the mechanical strength of the obtained polyimide film, the weight average molecular weight (Mw) of the imide-amic acid copolymer obtained by the above-mentioned manufacturing method is 300,000 or more, preferably 400,000 or more, and more preferably 500,000 or more. In addition, there is no upper limit, preferably 1,000,000 or less, more preferably 700,000 or less. In addition, from the same viewpoint, the number average molecular weight is preferably 50,000 to 500,000. It should be noted that the weight average molecular weight and number average molecular weight of the copolymer can be obtained by the standard polystyrene (PS) conversion value measured by gel permeation chromatography.
[0129] (Method for producing polyamic acid)
[0130] In the case of a polymer containing an amic acid unit (also referred to as a polyamic acid), in a preferred production method, the step 1 is a step of mixing a solution containing a diamine and a solvent with tetracarboxylic dianhydride and tert-butyl alcohol to perform polymerization.
[0131] As described above, the tetracarboxylic dianhydride used in step 1 preferably contains aromatic tetracarboxylic dianhydride, and more preferably contains aromatic tetracarboxylic dianhydride. In addition, it is preferred to contain a compound represented by the above formula (a1). The tetracarboxylic dianhydride may contain tetracarboxylic dianhydride other than aromatic tetracarboxylic dianhydride.
[0132] As the diamine used in step 1, as described above, an aromatic diamine is preferably included, and an aromatic diamine is more preferred. In addition, a compound represented by the aforementioned formula (b1) is preferably included, and a compound represented by the aforementioned formula (b11) is more preferred. The diamine may include a diamine other than an aromatic diamine.
[0133] That is, when the polymer obtained by the production method of the present invention is a polyamic acid, it is preferred that the tetracarboxylic dianhydride contains a compound represented by the following formula (a1), and the diamine contains a compound represented by the following general formula (b1).
[0134]
[0135] (In formula (b1), R 1 , R 2 , R 3 Each independently represents an organic group having 1 to 20 carbon atoms. h, i, j, and k are integers of 0 to 4.
[0136] R 1 , R 2 , R 3 Each independently represents an organic group having 1 to 20 carbon atoms, preferably R 1 , R 2 , R 3 Each is independently methyl or trifluoromethyl.
[0137] h, i, j, and k are integers of 0 to 4, and h, i, j, and k are each preferably 0.
[0138] As described above, the molar ratio of the diamine to the tetracarboxylic dianhydride in step 1 (diamine / tetracarboxylic dianhydride) is 1.00 or more and less than 1.03. The molar ratio of the aforementioned diamine to the aforementioned tetracarboxylic dianhydride in step 1 (diamine / tetracarboxylic dianhydride) is preferably 1.005 or more, more preferably 1.010 or more. In addition, it is preferably 1.025 or less, more preferably 1.020 or less. By setting the molar ratio of the aforementioned diamine to the aforementioned tetracarboxylic dianhydride in step 1 to the aforementioned range, a high molecular weight polymer can be obtained, and even if a high molecular weight polymer is included, a varnish with little viscosity increase and excellent storage stability can be obtained.
[0139] In step 1, a solution containing a diamine and a solvent is mixed with tetracarboxylic dianhydride and tert-butyl alcohol to perform polymerization. The amount of tert-butyl alcohol used in step 1 is not limited. As described above, it is preferably 2 mol% or more, more preferably 2.5 mol% or more, and further preferably 3 mol% or more relative to the total amount of tetracarboxylic dianhydride in step 1. In addition, it is preferably 5 mol% or less, more preferably 4 mol% or less, and further preferably 3.5 mol% or less. By setting the amount of tert-butyl alcohol in step 1 to the above range, a varnish having excellent storage stability and little viscosity increase can be obtained even if a high molecular weight polymer is included.
[0140] In step 1, the method for polymerizing tetracarboxylic dianhydride and diamine is not particularly limited, and a known method can be used.
[0141] Specific examples of the reaction method include a method in which a solution containing a diamine and a solvent, tetracarboxylic dianhydride, and tert-butyl alcohol are charged into a reactor and stirred at 0 to 120° C., preferably 5 to 80° C., for 1 to 72 hours.
[0142] When the reaction is performed at 80° C. or lower, the molecular weight of the polyamic acid obtained in step 1 does not vary depending on the temperature history during polymerization, and the progress of thermal imidization can be suppressed, so the polyamic acid can be stably produced.
[0143] The concentration of the polyamic acid in the obtained solution is usually in the range of 1 to 50% by mass, preferably 3 to 35% by mass, and more preferably 5 to 30% by mass.
[0144] From the viewpoint of the mechanical strength of the obtained polyimide film, the weight average molecular weight (Mw) of the polyamic acid obtained by the aforementioned manufacturing method is 300,000 or more, preferably 400,000 or more, and more preferably 500,000 or more. In addition, the upper limit is not limited, but is preferably 1,000,000 or less, and more preferably 700,000 or less. In addition, from the same viewpoint, the number average molecular weight is preferably 50,000 to 500,000. In addition, the weight average molecular weight and number average molecular weight of the polyamic acid can be obtained by the standard polystyrene (PS) conversion value measured based on gel permeation chromatography.
[0145] (Method for producing polyimide)
[0146] In a preferred production method in the case of a polymer containing an imide unit (also referred to as a polyimide), the step 1 is a step of mixing a solution containing a diamine and a solvent with tetracarboxylic dianhydride and tert-butyl alcohol to perform polymerization.
[0147] As described above, the tetracarboxylic dianhydride used in step 1 preferably contains aromatic tetracarboxylic dianhydride, and more preferably contains aromatic tetracarboxylic dianhydride. In addition, it is preferred to contain a compound represented by the above formula (a1). The tetracarboxylic dianhydride may contain tetracarboxylic dianhydride other than aromatic tetracarboxylic dianhydride.
[0148] As the diamine used in step 1, as described above, an aromatic diamine is preferably included, and an aromatic diamine is more preferred. In addition, a compound represented by the aforementioned formula (b1) is preferably included, and a compound represented by the aforementioned formula (b11) is more preferred. The diamine may include a diamine other than an aromatic diamine.
[0149] As described above, the molar ratio of the diamine to the tetracarboxylic dianhydride in step 1 (diamine / tetracarboxylic dianhydride) is 1.00 or more and less than 1.03. The molar ratio of the aforementioned diamine to the aforementioned tetracarboxylic dianhydride in step 1 (diamine / tetracarboxylic dianhydride) is preferably 1.005 or more, more preferably 1.010 or more. In addition, it is preferably 1.025 or less, more preferably 1.020 or less. By setting the molar ratio of the aforementioned diamine to the aforementioned tetracarboxylic dianhydride in step 1 to the aforementioned range, a high molecular weight polymer can be obtained, and even if a high molecular weight polymer is included, a varnish with little viscosity increase and excellent storage stability can be obtained.
[0150] In step 1, a solution containing a diamine and a solvent is mixed with tetracarboxylic dianhydride and tert-butyl alcohol to perform polymerization. The amount of tert-butyl alcohol used in step 1 is not limited. As described above, it is preferably 2 mol% or more, more preferably 2.5 mol% or more, and further preferably 3 mol% or more relative to the total amount of tetracarboxylic dianhydride in step 1. In addition, it is preferably 5 mol% or less, more preferably 4 mol% or less, and further preferably 3.5 mol% or less. By setting the amount of tert-butyl alcohol in step 1 to the above range, a varnish having a small viscosity increase and excellent storage stability can be obtained even if a high molecular weight polymer is included.
[0151] In step 1, the method for polymerizing tetracarboxylic dianhydride and diamine is not particularly limited, and a known method can be used.
[0152] Specific reaction methods include: (1) a method in which a solution containing a diamine and a solvent, tetracarboxylic dianhydride and tert-butanol are introduced into a reactor, stirred at 10 to 110° C. for 0.5 to 30 hours as required, and then the temperature is raised to carry out an imidization reaction; (2) a method in which a solution containing a diamine and a solvent, tetracarboxylic dianhydride and tert-butanol are introduced into a reactor, and the temperature is immediately raised to carry out an imidization reaction.
[0153] In the imidization reaction, it is preferred to use a Dean-Stark apparatus or the like to carry out the reaction while removing water generated during the production. By carrying out such an operation, the degree of polymerization and the imidization ratio can be further increased.
[0154] In the above-mentioned imidization reaction, a known imidization catalyst can be used. Examples of the imidization catalyst include a base catalyst and an acid catalyst.
[0155] Examples of the base catalyst include organic base catalysts such as pyridine, quinoline, isoquinoline, α-methylpyridine, β-methylpyridine, 2,4-lutidine, 2,6-lutidine, trimethylamine, triethylamine, tripropylamine, tributylamine, triethylenediamine, imidazole, N,N-dimethylaniline, and N,N-diethylaniline; and inorganic base catalysts such as potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, potassium hydrogen carbonate, and sodium hydrogen carbonate.
[0156] Examples of the acid catalyst include crotonic acid, acrylic acid, trans-3-hexenoic acid, cinnamic acid, benzoic acid, methylbenzoic acid, hydroxybenzoic acid, terephthalic acid, benzenesulfonic acid, p-toluenesulfonic acid, and naphthalenesulfonic acid. The above imidization catalysts may be used alone or in combination of two or more.
[0157] Among the above, from the viewpoint of operability, a base catalyst is preferred, an organic base catalyst is more preferred, at least one selected from triethylamine and triethylenediamine is further preferred, and triethylamine is further preferred.
[0158] From the viewpoint of reaction rate and suppression of gelation, the temperature of the imidization reaction is preferably 120 to 250° C., more preferably 160 to 200° C. The reaction time is preferably 0.5 to 10 hours after the start of distillation of generated water.
[0159] The concentration of the polyimide in the obtained solution is usually in the range of 1 to 50% by mass, preferably 3 to 35% by mass, and more preferably 5 to 30% by mass.
[0160] From the viewpoint of mechanical strength, especially elongation, of the obtained polyimide film, the weight average molecular weight (Mw) of the polyimide obtained by the above-mentioned manufacturing method is 300,000 or more, preferably 400,000 or more, and more preferably 500,000 or more. In addition, there is no upper limit, but it is preferably 1,000,000 or less, and more preferably 700,000 or less. In addition, from the same viewpoint, the number average molecular weight is preferably 50,000 to 500,000. In addition, the weight average molecular weight and number average molecular weight of the polyimide can be obtained by the standard polystyrene (PS) conversion value measured by gel permeation chromatography.
[0161] Next, the raw materials and the like used in the method for producing the polymer (imide-amic acid copolymer, polyamic acid, polyimide) and the method for producing the varnish of the present invention will be described.
[0162] [Tetracarboxylic dianhydride]
[0163] The tetracarboxylic dianhydride used as a raw material in the present production method is not particularly limited as long as it is tetracarboxylic dianhydride, but preferably contains aromatic tetracarboxylic dianhydride, and more preferably contains aromatic tetracarboxylic dianhydride.
[0164] From the viewpoint of achieving a high molecular weight, at least one selected from the group consisting of the compound represented by the above formula (a1) and the compound represented by the above formula (a2) is preferred, and the compound represented by the above formula (a1) is more preferred.
[0165] When the polymer is a polyamic acid, it preferably contains a compound represented by the above formula (a1).
[0166] When the polymer is an imide-amic acid copolymer, it is preferred that the raw material of the polyimide unit contains the compound represented by the above formula (a2), and the raw material of the polyamic acid unit contains the compound represented by the above formula (a1).
[0167] As tetracarboxylic dianhydride, acid dianhydride can be cited, but it is not limited thereto, and derivatives thereof can be cited as long as they can provide the structural unit A in the above-mentioned polymer. As the derivative, tetracarboxylic acid (free acid) and alkyl esters of the tetracarboxylic acid can be cited. Among them, acid dianhydride is preferred.
[0168] 〔Diamine〕
[0169] The diamine used as a raw material in the present production method is not particularly limited as long as it is a diamine, but preferably contains an aromatic diamine, more preferably contains an aromatic diamine, further preferably contains a compound represented by the aforementioned formula (b1), and further preferably contains a compound represented by the aforementioned formula (b11).
[0170] Examples of the diamine include diamines, but are not limited thereto, and derivatives thereof may be used as long as they are within the range that can provide the structural unit B in the above-mentioned polymer. Examples of the derivatives include diisocyanates corresponding to the diamines. Among them, diamines are preferred.
[0171] 〔Capping agent〕
[0172] In the production of the polymer, a terminal blocking agent may be used in addition to the aforementioned tetracarboxylic dianhydride, diamine and tert-butyl alcohol. In the production of the aforementioned imide-amic acid copolymer, the terminal blocking agent is preferably used in step 1-2.
[0173] As the end-capping agent, monoamines or dicarboxylic acids are preferred. The amount of the introduced end-capping agent is preferably 0.0001 to 0.1 moles relative to 1 mole of the tetracarboxylic acid component, and particularly preferably 0.001 to 0.06 moles. As monoamine end-capping agents, for example, methylamine, ethylamine, propylamine, butylamine, benzylamine, 4-methylbenzylamine, 4-ethylbenzylamine, 4-dodecylbenzylamine, 3-methylbenzylamine, 3-ethylbenzylamine, aniline, 3-methylaniline, 4-methylaniline, etc. are recommended. Among them, benzylamine and aniline can be suitably used. As dicarboxylic acid end-capping agents, dicarboxylic acids are preferred, and a part of them can also be closed-looped. For example, phthalic acid, phthalic anhydride, 4-chlorophthalic acid, tetrafluorophthalic acid, 2,3-benzophenone dicarboxylic acid, 3,4-benzophenone dicarboxylic acid, cyclopentane-1,2-dicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, etc. are recommended. Among them, phthalic acid and phthalic anhydride can be used preferably.
[0174] 〔Solvent〕
[0175] The solvent used in the method for producing a polymer can be any solvent that can dissolve the generated polymer. Examples include aprotic solvents, phenolic solvents, ether solvents, carbonate solvents, etc., preferably at least one selected from the group consisting of aprotic solvents, phenolic solvents, ether solvents, and carbonate solvents.
[0176] Specific examples of the aprotic solvent include cyclic amides, chain amides, that is, amide-based solvents, phosphorus-containing amide-based solvents, sulfur-containing solvents, ketone-based solvents, and ester-based solvents including cyclic esters.
[0177] Among these, the solvent preferably contains at least one selected from the group consisting of cyclic amides, chain amides, and cyclic esters, and more preferably contains cyclic amides.
[0178] Examples of the cyclic amide include N-methylpyrrolidone, N-methylcaprolactam, and 1,3-dimethylimidazolidinone, and N-methylpyrrolidone is preferred.
[0179] Examples of the chain amide include N,N-dimethylformamide, N,N-dimethylacetamide, and tetramethylurea.
[0180] Examples of the cyclic ester include γ-butyrolactone and γ-valerolactone.
[0181] As other ester solvents, 2-methoxy-1-methylethyl acetate and the like can be mentioned.
[0182] Examples of the phosphorus-containing amide solvent include hexamethylphosphoramide and hexamethylphosphorus triamide.
[0183] Examples of the sulfur-containing solvent include dimethyl sulfone, dimethyl sulfoxide, and sulfolane.
[0184] Examples of the ketone solvent include acetone, methyl ethyl ketone, cyclohexanone, and methylcyclohexanone.
[0185] Specific examples of the phenolic solvent include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol.
[0186] Specific examples of the ether solvent include 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, bis[2-(2-methoxyethoxy)ethyl]ether, tetrahydrofuran, and 1,4-dioxane.
[0187] Specific examples of the carbonate-based solvent include diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, and propylene carbonate.
[0188] The solvent preferably contains at least one selected from the group consisting of cyclic amides, chain amides and cyclic esters, more preferably contains cyclic amides, and further preferably contains N-methylpyrrolidone. The above solvents may be used alone or in combination of two or more.
[0189] [Varnish]
[0190] The varnish of the present invention comprises the polymer obtained by the above-mentioned production method and a solvent.
[0191] The solvent is not particularly limited as long as it can dissolve the polymer, and the above-mentioned compound used as the solvent in the manufacture of the polymer is preferably used alone or in a mixture of two or more. The above-mentioned solvent preferably contains at least one selected from the group consisting of cyclic amides, chain amides and cyclic esters, more preferably contains cyclic amides, and further preferably contains N-methylpyrrolidone.
[0192] The varnish of the present invention may be the polymer solution itself obtained by the above-mentioned method for producing a polymer, may be one in which a solvent is further added, or may be one in which the solvent is reduced by concentration or the like.
[0193] The polymer contained in the varnish of the present invention is a polyamic acid or an imide-amic acid copolymer, and when the varnish contains an amic acid portion, from the viewpoint of making the imidization efficiency of the amic acid portion good, the varnish of the present invention may further contain an imidization catalyst and a dehydration catalyst. As an imidization catalyst, as long as it is an imidization catalyst with a boiling point of more than 40°C and less than 180°C, an amine compound with a boiling point of less than 180°C can be cited as a preferred one. If it is an imidization catalyst with a boiling point of less than 180°C, after the film is formed, the film does not have concerns about coloring and damaged appearance during drying at high temperatures. In addition, if the boiling point is an imidization catalyst of more than 40°C, the possibility of volatilization before imidization can be fully avoided.
[0194] Examples of the amine compound preferably used as the imidization catalyst include pyridine and picoline. The above-mentioned imidization catalysts may be used alone or in combination of two or more.
[0195] Examples of the dehydration catalyst include acid anhydrides such as acetic anhydride, propionic anhydride, n-butyric anhydride, benzoic anhydride, and trifluoroacetic anhydride; and carbodiimide compounds such as dicyclohexylcarbodiimide. These may be used alone or in combination of two or more.
[0196] The polymer contained in the varnish of the present invention has solvent solubility, so it can be made into a high-concentration varnish. The varnish of the present invention preferably contains 3 to 40% by mass of the polymer, more preferably 5 to 40% by mass, and further preferably 10 to 30% by mass. The viscosity of the varnish is preferably 1 to 200 Pa·s, more preferably 2 to 20 Pa·s. The viscosity of the varnish is a value measured at 25°C using an E-type viscometer.
[0197] In addition, the varnish of the present invention may also contain various additives such as inorganic fillers, adhesion promoters, release agents, flame retardants, ultraviolet stabilizers, surfactants, leveling agents, defoaming agents, fluorescent brighteners, crosslinking agents, polymerization initiators, and photosensitizers, within the range that the required properties of the polyimide film are not impaired.
[0198] The varnish of the present invention has a small viscosity increase in a wide viscosity range and excellent storage stability even if it contains a high molecular weight resin. Therefore, the increase rate of the viscosity on the 7th day after storage at 23° C. is preferably 20% or less, more preferably 15% or less, further preferably 12% or less, and further preferably 9% or less relative to the viscosity on the 0th day.
[0199] [Method for producing polyimide film]
[0200] The varnish can be used to manufacture a polyimide film. The varnish can manufacture a high-strength film because it contains a high-molecular-weight resin. In addition, even if the varnish contains a high-molecular-weight resin, the viscosity rise is small in a wide viscosity range and the storage stability is excellent, so a high-strength film can be stably manufactured even after long-term storage.
[0201] The method for producing a polyimide film using the varnish of the present invention is not particularly limited, but is preferably carried out by the following method.
[0202] That is, a suitable method for producing a polyimide film comprises the steps of casting the above-mentioned varnish on a substrate; and drying the cast varnish to form a polymer film.
[0203] Examples of the substrate include smooth plate-like objects, such as smooth glass plates, metal plates, and plastic plates.
[0204] “Casting on a substrate” means “applying on a substrate”, and the varnish is poured onto the substrate to form a thin film.
[0205] After the varnish is cast on the substrate, the solvent contained in the varnish is removed by heating and dried to form a polymer film. Preferably, the polyimide film is produced by further drying the polymer film at a temperature higher than the boiling point of the solvent used.
[0206] The polyimide film can be obtained by drying the polymer film at a temperature above the boiling point of the solvent after peeling the polymer film from the substrate, or by drying the polymer film at a temperature above the boiling point of the solvent before peeling the polymer film from the substrate and then peeling the polymer film from the substrate. In addition, when the polymer in the aforementioned polymer film has an amic acid portion, the polyimide film can also be obtained by heating at a temperature above the boiling point of the solvent to imidize (dehydrated ring closure).
[0207] From the viewpoint of the mechanical strength of the polyimide film, especially the elongation, the weight average molecular weight (Mw) of the polyimide contained in the polyimide film obtained by the above-mentioned manufacturing method is 300,000 or more, preferably 400,000 or more, and more preferably 500,000 or more. In addition, there is no upper limit, but it is preferably 1,000,000 or less, and more preferably 700,000 or less. In addition, from the same viewpoint, the number average molecular weight is preferably 50,000 to 500,000. In addition, the weight average molecular weight and number average molecular weight of the polyimide can be obtained by the standard polystyrene (PS) conversion value measured by gel permeation chromatography.
[0208] The heating temperature when drying the varnish of the present invention to obtain a polymer film is preferably 50 to 150° C. The heating time is usually 1 minute to 6 hours, preferably 5 minutes to 2 hours, and more preferably 15 minutes to 1 hour.
[0209] The process preferably includes the following step: drying the polymer film after removing the solvent contained in the varnish by heating at a temperature above the boiling point of the solvent used. When the polymer in the polymer film has an amic acid moiety, it can be imidized by chemical imidization or the like and then dried at a temperature above the boiling point of the solvent, but it is preferred to perform thermal imidization (dehydration ring closure) in this drying step to produce a polyimide film.
[0210] The heating temperature when further drying the polymer film is preferably 100 to 500° C., more preferably 200 to 450° C., and even more preferably 300 to 430° C. The heating time is usually 1 minute to 6 hours, preferably 5 minutes to 2 hours, and more preferably 15 minutes to 1 hour.
[0211] When the polymer film is dried at a temperature above the boiling point of the solvent, the heating may be divided into two or more stages. When the heating is divided into two or more stages, it is preferably two or more stages. There is no upper limit, but it is preferably five or less stages.
[0212] Although not particularly limited, for example, when divided into two or more stages, the heating temperature of the initial stage is preferably 100 to 300° C., and the heating time is preferably 1 minute to 6 hours. The heating temperature of the final stage is preferably 300 to 500° C., and the heating time is preferably 1 minute to 6 hours. When divided into two stages, the heating temperature of the first stage is preferably 100 to 300° C., and the heating time is preferably 1 minute to 6 hours. The heating temperature of the second stage is preferably 300 to 500° C., and the heating time is preferably 1 minute to 6 hours.
[0213] The atmosphere when the polymer film is further dried may include air, nitrogen, oxygen, hydrogen, nitrogen / hydrogen mixed gas, etc. However, in order to suppress the coloration of the obtained polyimide film, nitrogen with an oxygen concentration of 100 ppm or less and nitrogen / hydrogen mixed gas containing hydrogen with a hydrogen concentration of 0.5% or less are preferred.
[0214] The thickness of the polyimide film of the present invention can be appropriately selected depending on the application, and is preferably 1 to 250 μm, more preferably 5 to 100 μm, and even more preferably 5 to 50 μm. A thickness of 1 to 250 μm enables practical use as a self-supporting film.
[0215] The thickness of the polyimide film can be easily controlled by adjusting the solid content concentration and viscosity of the varnish and the amount of the varnish during casting.
[0216] The polyimide film of the present invention can be suitably used as a film for various members such as color filters, flexible displays, semiconductor components, optical members, etc. The polyimide film of the present invention is particularly suitably used as a substrate for image display devices such as liquid crystal displays and OLED displays.
[0217] Example
[0218] The present invention is specifically described below by way of examples, but the present invention is not limited to these examples.
[0219] Evaluation of the varnishes obtained in Examples and Comparative Examples was performed by the methods shown below.
[0220] (1) Polymer content
[0221] Take about 3 g of the varnish obtained in the examples and comparative examples and weigh it accurately. Then use a dryer to fully dry the varnish under nitrogen at 320°C, and weigh the mass of the varnish (polymer) after drying. The mass of the varnish before drying is set as (A), and the mass of the varnish (polymer) after drying is set as (B). Use the following formula to calculate the content (%) of the polymer in the varnish.
[0222] Polymer content (%) = (B) / (A) × 100
[0223] The content of the polymer in the varnish of each Example and each Comparative Example is shown in Table 1-1 and Table 1-2.
[0224] (2) Weight average molecular weight of polymer
[0225] The weight average molecular weight of the polymer contained in the varnish obtained in each example and each comparative example was determined by a standard polystyrene (manufactured by Tosoh Corporation) conversion value measured by gel permeation chromatography. The elution phase used was a mixture obtained by adding 24.8 mM of LiBr·H2O (manufactured by FUJIFILM Wako Pure Chemical Corporation, purity 99.5%) and 63.2 mM of phosphoric acid (manufactured by FUJIFILM Wako Pure Chemical Corporation, for high performance liquid chromatography) to DMF (manufactured by FUJIFILM Wako Pure Chemical Corporation, for high performance liquid chromatography). The apparatus was Shodex101 (manufactured by Showa Denko K.K.), the chromatographic column was KD-806M (manufactured by Showa Denko K.K.), the flow rate was set to 1.0 mL / min, and the column temperature was set to 40°C.
[0226] The molecular weights of the polymers contained in the varnishes of the Examples and Comparative Examples are shown in Table 1-1 and Table 1-2.
[0227] (3) Storage stability evaluation
[0228] The varnish obtained in each embodiment and each comparative example is diluted with NMP (N-methyl-2-pyrrolidone) in such a manner that the viscosity or polymer content (polymer concentration) shown in Table 1-1 and Table 1-2 is obtained. The viscosity of the solution just after dilution (before storage) is set as the viscosity on the 0th day of storage (A). The diluted solution is put into a glass screw tube, purged with nitrogen, and then stored at 23°C and 50% humidity. The viscosity is measured again on the 7th day of storage and is set as the viscosity on the 7th day of storage (B). The viscosity increase rate is calculated using the following formula.
[0229] Thickening rate (%) = [(B) - (A)] / (A) × 100
[0230] The results of the storage stability evaluation of the varnishes of each Example and each Comparative Example are shown in Table 1-1 and Table 1-2. The smaller the value of the viscosity increase ratio, the more excellent the storage stability.
[0231] (4) Evaluation of tensile elongation
[0232] The polyimide films obtained by the method described in the following production of polyimide film using the varnishes obtained in Examples and Comparative Examples were evaluated for tensile elongation as a film physical property.
[0233] The tensile elongation was measured in accordance with JIS K7127:1999 using a tensile tester "Strograph VG-1E" (manufactured by TOYO SEIKI CO., LTD.). The distance between the clamps was set to 50 mm, the test piece size was set to 10 mm × 70 mm, the test speed was set to 20 mm / min, and the number of tests was set to 5 times. The average value of the obtained elongation of 10% or more was set to A, and the value of less than 10% was set to B. The larger the average value of the elongation, the better the tensile elongation, and the better the physical properties of the film.
[0234] The evaluation results are shown in Tables 1-1 and 1-2.
[0235] The tetracarboxylic acid component and the diamine component used in Examples and Comparative Examples, and their abbreviations and the like are as follows.
[0236] <Tetracarboxylic dianhydride>
[0237] BPAF: 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (manufactured by JFE Chemical Corporation; compound represented by formula (a2))
[0238] s-BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride (manufactured by Mitsubishi Chemical Corporation; compound represented by formula (a1s))
[0239] <Diamine>
[0240] 4-BAAB: 4-aminophenyl-4-aminobenzoate (manufactured by Nipponjunryo Chemicals Co., Ltd.; compound represented by formula (b11))
[0241] The abbreviations of the solvents and catalysts used in Examples and Comparative Examples are as follows.
[0242] NMP: N-methyl-2-pyrrolidone (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0243] TEA: triethylamine (manufactured by Kanto Chemical Co., Ltd.)
[0244] <Example 1: Production of polyamic acid varnish>
[0245] In a 500 mL 5-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet pipe, a Dean-Stark apparatus equipped with a cooling tube, a thermometer, and a glass end cap, 26.101 g (0.114 mol) of 4-BAAB and 192.000 g of NMP were added, and the temperature in the system was set to 70° C. under a nitrogen atmosphere, and the mixture was stirred at a rotation speed of 200 rpm to obtain a solution.
[0246] To this solution, 0.254 g (0.003 mol) of tert-butyl alcohol and 24.000 g of NMP were added, and further 33.645 g (0.114 mol) of s-BPDA and 24.000 g of NMP were added, and stirred at 70° C. for 4 hours to obtain a solution containing polyamic acid. NMP was added thereto to adjust the viscosity at 25° C. to 3 Pa·s, thereby preparing a varnish for storage stability evaluation.
[0247] <Example 2: Preparation of imide-amic acid copolymer varnish>
[0248] In a 500 mL 5-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet pipe, a Dean-Stark apparatus equipped with a cooling tube, a thermometer, and a glass end cap, 7.449 g (0.033 mol) of 4-BAAB and 49.695 g of NMP were added, and the temperature in the system was set to 70° C. under a nitrogen atmosphere, and the mixture was stirred at a rotation speed of 200 rpm to obtain a solution.
[0249] After adding 9.974 g (0.022 mol) of BPAF and 15.000 g of NMP at once to the solution, 0.110 g of TEA and 5.000 g of NMP as an imidization catalyst were added, and the mixture was heated with a mantle heater to raise the temperature in the reaction system to 190° C. over about 20 minutes. While collecting the distilled components, the temperature in the reaction system was maintained at 190° C. and refluxed for 1 hour. Thereafter, 135.065 g of NMP was added, and the temperature in the reaction system was cooled to 50° C. to obtain a solution containing an oligomer having an imide repeating structural unit.
[0250] To the obtained solution, 17.754 g (0.078 mol) of 4-BAAB and 15.000 g of NMP were added, followed by 0.242 g (0.003 mol) of tert-butyl alcohol and 5.000 g of NMP, and then 25.606 g (0.087 mol) of s-BPDA and 15.000 g of NMP were added, and the mixture was stirred at 70° C. for 4 hours to obtain a solution containing an imide-amic acid copolymer. NMP was added thereto to adjust the viscosity at 25° C. to 3 Pa·s, thereby preparing a varnish for storage stability evaluation.
[0251] <Example 3: Preparation of imide-amic acid copolymer varnish>
[0252] A solution containing an imide-amic acid copolymer was obtained in the same manner as in Example 2 except that the amount of 4-BAAB was changed as shown in Table 1-1. NMP was added thereto so that the viscosity at 25° C. became 3 Pa·s to prepare a varnish for storage stability evaluation.
[0253] <Examples 4 and 5: Production of imide-amic acid copolymer varnish>
[0254] A solution containing an imide-amic acid copolymer was obtained in the same manner as in Example 3. NMP was added thereto so that the solid content (polymer concentration in the varnish) became 15% by mass and 20% by mass, respectively, to prepare a varnish for storage stability evaluation.
[0255] <Comparative Example 1: Production of polyamic acid varnish>
[0256] A solution containing a polyamic acid was obtained in the same manner as in Example 1 except that tert-butyl alcohol was not used. NMP was added thereto so that the viscosity at 25° C. became 3 Pa·s, thereby preparing a varnish for evaluating storage stability.
[0257] <Comparative Example 2: Production of polyamic acid varnish>
[0258] A solution containing a polyamic acid was obtained in the same manner as in Comparative Example 1. NMP was added thereto so that the solid content (polymer concentration in the varnish) became 15% by mass, thereby preparing a varnish for storage stability evaluation.
[0259] <Comparative Examples 3 and 4: Production of polyamic acid varnish>
[0260] A solution containing polyamic acid was obtained in the same manner as in Example 1 except that methanol or ethanol was used instead of tert-butyl alcohol. NMP was added thereto so that the viscosity at 25° C. was 3 Pa·s, thereby preparing a varnish for storage stability evaluation.
[0261] <Comparative Example 5: Production of imide-amic acid copolymer varnish>
[0262] A solution containing an imide-amic acid copolymer was obtained in the same manner as in Example 2 except that tert-butyl alcohol was not used. NMP was added thereto so that the viscosity at 25° C. became 3 Pa·s, thereby preparing a varnish for evaluating storage stability.
[0263] <Comparative Examples 6 and 7: Production of Imide-Amide Acid Copolymer Varnish>
[0264] A solution containing an imide-amic acid copolymer was obtained in the same manner as in Comparative Example 5. NMP was added thereto so that the solid content (polymer concentration in the varnish) became 15% by mass and 20% by mass, respectively, to prepare a varnish for storage stability evaluation.
[0265] <Comparative Example 8: Production of imide-amic acid copolymer varnish>
[0266] A solution containing an imide-amic acid copolymer was obtained in the same manner as in Comparative Example 5 except that the amount of s-BPDA was changed as shown in Table 1-2. NMP was added thereto so that the viscosity at 25° C. became 3 Pa·s to prepare a varnish for storage stability evaluation.
[0267] <Comparative Example 9: Production of imide-amic acid copolymer varnish>
[0268] A solution containing an imide-amic acid copolymer was obtained in the same manner as in Example 3 except that tert-butyl alcohol was not used. NMP was added thereto so that the viscosity at 25° C. became 3 Pa·s, thereby preparing a varnish for evaluating storage stability.
[0269] <Comparative Example 10: Production of imide-amic acid copolymer varnish>
[0270] A solution containing an imide-amic acid copolymer was obtained in the same manner as in Comparative Example 5 except that the amount of 4-BAAB was changed as shown in Table 1-2. NMP was added thereto so that the viscosity at 25° C. became 3 Pa·s to prepare a varnish for storage stability evaluation.
[0271] 〈Manufacturing of polyimide film〉
[0272] The polyimide film used in the above-mentioned tensile elongation evaluation was produced as follows.
[0273] The varnish prepared in the aforementioned embodiments and comparative examples is applied onto a glass plate by a spin coater, maintained at 80°C for 20 minutes using a heating plate, then transferred to a hot air dryer, heated to 420°C at a heating rate of 5°C / min in a nitrogen atmosphere, and heated at 420°C in the hot air dryer for 60 minutes in a nitrogen atmosphere to evaporate the solvent and perform thermal imidization to obtain a polyimide film.
[0274] [Table 1-1]
[0275] Table 1-1
[0276]
[0277] *) The numbers described for the imide part, the amic acid part and the alcohols represent the molar ratio.
[0278] [Table 1-2]
[0279] Table 1-2
[0280]
[0281] *) The numbers described for the imide part, the amic acid part and the alcohols represent the molar ratio.
[0282] As shown in Tables 1-1 and 1-2, it can be seen that the varnish containing the polymer obtained by the production method of the present invention can obtain a varnish having a small viscosity increase in a wide viscosity range and excellent storage stability even if it contains a high molecular weight resin (polyimide precursor). It should be noted that the molecular weight of the resin in Comparative Examples 8 and 10 is low.
Claims
1. A method for producing a polymer, comprising step 1 of polymerizing a diamine and a tetracarboxylic dianhydride to obtain a polymer, The molar ratio of the diamine to the tetracarboxylic dianhydride in the step 1 (diamine / tetracarboxylic dianhydride) is 1.00 or more and less than 1.03, The step 1 is a step of polymerizing diamine and tetracarboxylic dianhydride in the presence of tert-butyl alcohol and a solvent. The polymer includes at least one selected from the group consisting of an amic acid unit and an imide unit as a repeating unit, and has a weight average molecular weight of 300,000 or more.
2. The method for producing a polymer according to claim 1, in, The polymer is at least one selected from the group consisting of polyamic acid, polyimide, and imide-amic acid copolymer.
3. The method for producing a polymer according to claim 1 or 2, in, The polymer is polyamic acid, and step 1 is a step of mixing a solution containing a diamine and a solvent with tetracarboxylic dianhydride and tert-butyl alcohol to perform polymerization.
4. The method for producing a polymer according to any one of claims 1 to 3, in, The polymer is a polyamic acid, the tetracarboxylic dianhydride includes a compound represented by the following formula (a1), and the diamine includes a compound represented by the following general formula (b1), In formula (b1), R 1 , R 2 , R 3 Each independently represents an organic group having 1 to 20 carbon atoms; h, i, j, and k are integers of 0 to 4.
5. The method for producing a polymer according to claim 1 or 2, in, The polymer is an imide-amic acid copolymer, the tetracarboxylic dianhydride includes a first tetracarboxylic dianhydride and a second tetracarboxylic dianhydride, the diamine includes a first diamine and a second diamine, and the step 1 includes the following step 1-1 and the following step 1-2, Step 1-1: a step of reacting the first tetracarboxylic dianhydride with the first diamine in the presence of a solvent to obtain an imide oligomer Step 1-2: A step of mixing the imide oligomer obtained in step 1-1, the second tetracarboxylic dianhydride, the second diamine, and tert-butyl alcohol to perform polymerization.
6. The method for producing a polymer according to claim 5, in, The polymer is an imide-amic acid copolymer, the first tetracarboxylic dianhydride comprises a compound represented by the following formula (a1), the second tetracarboxylic dianhydride comprises a compound represented by the following formula (a2), the first diamine and the second diamine comprise a compound represented by the following formula (b1), In formula (b1), R 1 , R 2 , R 3 Each independently represents an organic group having 1 to 20 carbon atoms; h, i, j, and k are integers of 0 to 4.
7. The method for producing a polymer according to any one of claims 1 to 6, in, The amount of tert-butyl alcohol in step 1 is 2 mol% or more based on the total amount of tetracarboxylic dianhydride in step 1. 8 . A varnish comprising a polymer obtained by the production method according to claim 1 and a solvent.
9. A method for producing a varnish, comprising step 1 of polymerizing a diamine and a tetracarboxylic dianhydride to obtain a polymer, The molar ratio of the diamine to the tetracarboxylic dianhydride in the step 1 (diamine / tetracarboxylic dianhydride) is 1.00 or more and less than 1.03, The step 1 is a step of polymerizing diamine and tetracarboxylic dianhydride in the presence of tert-butyl alcohol and a solvent. The polymer has at least one selected from the group consisting of an amic acid unit and an imide unit as a repeating unit, and has a weight average molecular weight of 300,000 or more. The varnish comprises the polymer and a solvent. 10 . A varnish obtained by the production method according to claim 9 .
11. The varnish according to claim 8 or 10, in, The rate of increase in viscosity on the 7th day after storage at 23°C was 15% or less relative to the viscosity on the 0th day.
12. The varnish according to claim 8, 10 or 11, in, The solvent contains at least one selected from the group consisting of cyclic amides, chain amides, and cyclic esters.
13. The varnish according to any one of claims 8 or 10 to 12, in, The solvent contained N-methylpyrrolidone.