Thermally conductive polymer composition, material for forming thermally conductive polymer composition, and thermally conductive polymer
The composition of liquid rubber, solvent and curing agent is solved, and the problem that the existing thermally conductive materials are difficult to maintain the fluidity and shape following when improving thermal conductivity is improved, and a thermally conductive polymer composition with excellent thermal conductivity and construction properties is achieved. , the thermal conductivity reaches 10W/(m·K or above, and no solvent removal is required.
Patent Information
- Application Number
- CN202380028480.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-03-17
- Publication Date
- 2024-11-01
AI Technical Summary
When existing thermal conductivity improves thermal conductivity, it is difficult to maintain fluidity and shape following, and it is difficult to remove solvents after construction, resulting in the thermal resistance problem not being completely solved.
Using a composition of liquid rubber, solvent and curing agent, the solvent components are introduced into the cured thermally conductive polymer through chemical bonding, increasing the filler volume to improve thermal conductivity, while maintaining fluidity and shape following, avoiding the need to remove solvents .
A thermal conductivity polymer composition with high thermal conductivity, low viscosity, good shape following and excellent construction properties is achieved, with a thermal conductivity of 10W/(m·K or above, and no solvent removal is required.
Smart Images

Figure BDA0005048588110000101 
Figure BDA0005048588110000111
Abstract
Description
Technical Field
[0001] The present invention relates to a thermally conductive polymer composition, a material for forming the thermally conductive polymer composition and a thermally conductive polymer.
[0002] This application claims priority based on patent application No. 2022-048886 filed in Japan on March 24, 2022, and its contents are incorporated herein. Background Art
[0003] Regarding the heat-conducting material that is disposed between the heating element and the heat-dissipating component and transfers heat, various forms of heat-conducting materials are known, such as grease type, gap filler type, sheet type, etc. By using these heat-conducting materials, for example, the heat generated in the heating element can be effectively dissipated from heat-dissipating components such as metal frames or radiators. Such a heat-conducting material can reduce the thermal resistance between the heating element and the heat-dissipating component by being disposed between the heating element and the heat-dissipating component.
[0004] In recent years, with the development of high performance and integration of various electronic devices, a structure with improved heat dissipation is required to effectively dissipate the heat generated by the operation of the components (heating element) to the outside. Therefore, a thermal conductive material is required that can further reduce the thermal resistance between the heating element and the heat dissipation component.
[0005] In order to reduce the thermal resistance between the heating element and the heat dissipation component, it is possible to consider increasing the thermal conductivity of the thermally conductive material itself or increasing the close contact between the thermally conductive material and the heating element or heat dissipation component connected to the thermally conductive material to reduce the thermal resistance generated at their interface (interface thermal resistance).
[0006] Conventionally, as a general thermally conductive material, a thermally conductive material obtained by filling silicone resin or the like with a filler having high thermal conductivity, such as alumina, is known (for example, refer to Patent Document 1).
[0007] Furthermore, there is also known a thermally conductive material which improves adhesion to the surface of each component by reducing hardness to reduce thermal resistance generated at the interface between the thermally conductive material and each component in contact therewith (see, for example, Patent Document 2).
[0008] Furthermore, there is also known a two-liquid curing gap filler or putty-like thermally conductive material that can reduce the thermal resistance generated at the interface between the thermally conductive material and the components connected thereto by mixing and curing a plurality of fluids with high fluidity (for example, see Patent Documents 3 and 4).
[0009] Patent Document 1: Japanese Patent Application Publication No. 2005-006428
[0010] Patent Document 2: Japanese Patent Application Publication No. 2019-011423
[0011] Patent Document 3: Japanese Patent Application Publication No. 2020-050701
[0012] Patent Document 4: Japanese Patent Application Publication No. 2020-157554
[0013] However, the thermally conductive materials disclosed in Patent Documents 1 to 4 all increase the amount of filler added to improve thermal conductivity, and as a result, the hardness increases, making it difficult for the thermally conductive material to follow the surface shape of each component and adhere to it without gaps. Therefore, when ensuring high thermal conductivity, if it is a sheet-like thermally conductive material, the sheet will become hard, and if it is a fluid-like thermally conductive material, the fluidity will decrease. Therefore, in any form, it is difficult to arrange the thermally conductive material without gaps along the surface shape of each component to reduce the thermal resistance generated at the interface.
[0014] Furthermore, when the thermally conductive material is diluted with a solvent or the like to reduce the hardness of the thermally conductive material during construction, there is a concern that voids may be generated in the thermally conductive material when the solvent is removed after construction, or that it may be difficult to remove the solvent by heating or the like depending on the location of the thermally conductive material. Summary of the invention
[0015] The present invention has been made in view of the above background, and an object of the present invention is to provide a thermally conductive polymer composition having high thermal conductivity, low viscosity, high shape-conforming properties, and high workability, which does not require solvent removal during curing, a thermally conductive polymer composition-forming material, and a thermally conductive polymer obtained therefrom.
[0016] In order to achieve the above-mentioned object, the present invention is constructed as follows.
[0017] That is, a thermally conductive polymer composition according to one embodiment of the present invention is characterized in that it contains: a liquid rubber having two or more hydroxyl groups in one molecule; a solvent having one or more hydroxyl groups in one molecule; a curing agent having two or more functional groups in one molecule that can react with both the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent; and a filler.
[0018] According to the present invention, the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent are reacted with the functional groups contained in the curing agent and chemically bonded, so that the solvent component is introduced into the cured thermally conductive polymer as a constituent material. Thus, even if the filler content that causes the decrease in fluidity before curing is increased to improve thermal conductivity, the fluidity before curing can be kept high by the solvent component. Therefore, a thermally conductive polymer composition with high shape followability to the surface of each component, excellent workability, and high thermal conductivity can be achieved.
[0019] In the thermally conductive polymer composition according to one aspect of the present invention, the filler may have a thermal conductivity of 10 W / (m·K) or more.
[0020] In the thermally conductive polymer composition according to one aspect of the present invention, the liquid rubber may include at least one of polybutadiene, polyisoprene, and polyolefin having a plurality of hydroxyl groups.
[0021] In the thermally conductive polymer composition according to one embodiment of the present invention, the solvent may include at least one of n-butyl carbitol, glycerol, polyethylene glycol monomethyl ether, butylene glycol, propylene glycol, ethylene glycol, and tetraethylene glycol monomethyl ether.
[0022] In the thermally conductive polymer composition according to one aspect of the present invention, the curing agent may be an isocyanate compound.
[0023] In the thermally conductive polymer composition according to one aspect of the present invention, the thermally conductive polymer composition may further contain a thickening material.
[0024] A thermally conductive polymer composition forming material according to one embodiment of the present invention is used to form the thermally conductive polymer composition described in the above items, wherein the thermally conductive polymer composition forming material comprises a liquid A containing the liquid rubber and the solvent, and a liquid B containing the curing agent, and at least one of the liquid A or the liquid B further contains the filler.
[0025] The thermally conductive polymer according to one embodiment of the present invention is characterized in that the thermally conductive polymer is a thermally conductive polymer obtained by curing the thermally conductive polymer composition according to any of the above items, and the terminal group of the thermally conductive polymer contains -[(C2H4-O) m -C n H 2n+1 ](where m and n are arbitrary natural numbers).
[0026] In the thermally conductive polymer according to one aspect of the present invention, the thermal conductivity of the thermally conductive polymer may be 1.5 W / (m·K) or more.
[0027] According to the present invention, there can be provided a thermally conductive polymer composition having high thermal conductivity, low viscosity, high shape-conforming properties, and high workability without removing a solvent during curing, a thermally conductive polymer composition forming material, and a thermally conductive polymer obtained therefrom. DETAILED DESCRIPTION
[0028] Hereinafter, a thermally conductive polymer composition, a thermally conductive polymer composition forming material, and a thermally conductive polymer obtained therefrom according to an embodiment of the present invention will be described with reference to the accompanying drawings. In addition, each embodiment shown below is specifically described for better understanding of the gist of the invention, and is not intended to limit the present invention unless otherwise specified.
[0029] (Thermal conductive polymer composition)
[0030] The thermally conductive polymer composition of the present embodiment contains a liquid rubber, a solvent, a curing agent, and a filler having thermal conductivity. The thermally conductive polymer composition of the present embodiment is a composition in a state before curing (polymerization reaction).
[0031] The liquid rubber may be any liquid rubber having fluidity at room temperature, and may have two or more hydroxyl groups (—OH) in one molecule in its composition formula. The hydroxyl groups are preferably located at the ends of the molecules.
[0032] A part of the hydroxyl groups in such a liquid rubber reacts with the functional groups of the curing agent to form a chemical bond during the curing of the thermally conductive polymer composition described later.
[0033] Specific examples of liquid rubbers having two or more hydroxyl groups in one molecule at the terminal group include hydroxyl-containing polybutadiene, hydroxyl-containing polyisoprene, hydroxyl-containing polyolefin, etc. Among them, hydroxyl-containing polybutadiene is preferred from the viewpoint of good filler filling properties. These hydroxyl groups may be located at the ends of the molecule.
[0034] For example, the hydroxyl-containing polybutadiene may be Poly bd (registered trademark) series (hydroxyl number: 0.83 to 1.83 mol / kg, manufactured by Idemitsu Kosan Co., Ltd.), G series (hydroxyl number: 0.48 to 1.39 mol / kg, manufactured by Nippon Soda Co., Ltd.), Krasol LBH series (hydroxyl number: undisclosed, manufactured by Total Cray Valley Co., Ltd.). Furthermore, the hydroxyl-containing polyisoprene may be Poly ip (registered trademark) (hydroxyl number: 0.83 mol / kg, manufactured by Idemitsu Kosan Co., Ltd.).
[0035] The number average molecular weight of the liquid rubber is not particularly limited, and for example, a liquid rubber having a number average molecular weight in the range of 1000 to 3000 can be used. In addition, the hydroxyl value of the liquid rubber is preferably in the range of 0.5 to 2.0. In addition, the viscosity of the liquid rubber is not particularly limited, and for example, it can be in the range of 1.0 Pa·s to 1000 Pa·s.
[0036] The solvent is a component that improves the plasticity of the thermally conductive polymer composition, and in the composition formula, it only needs to have one or more hydroxyl groups (-OH) in one molecule. The hydroxyl group may be located at the end of the molecule.
[0037] The hydroxyl group in such a solvent reacts with the functional group of the curing agent to form a chemical bond during curing of the thermally conductive polymer composition described below.
[0038] In addition, it is preferred that the solvent has a molecular weight of 50 to 450, a boiling point of 100 to 250° C., and a viscosity of 500 mPa·s or less (25° C.).
[0039] The solvent may be a polyol.
[0040] In addition, the solvent may be a solvent compatible with the liquid rubber. The solvent compatible with the liquid rubber refers to a liquid substance that maintains a mixed state to the extent that phase separation does not occur after the liquid rubber and the solvent are mixed in any proportion and left to stand for more than 10 minutes to the naked eye.
[0041] Specific examples of the solvent having one or more hydroxyl groups in one molecule include n-butyl carbitol (diethylene glycol monobutyl ether), glycerol, polyethylene glycol monomethyl ether, butanediol, propylene glycol, ethylene glycol, and tetraethylene glycol monomethyl ether.
[0042] Regarding the solvent contained in the conventional thermally conductive polymer composition, curing is performed by volatilizing and removing the solvent, so that the cured thermally conductive polymer contains almost no solvent components. On the other hand, the solvent contained in the thermally conductive polymer composition of the present embodiment is chemically bonded to the liquid rubber through the curing agent during curing, thereby becoming a part of the constituent of the thermally conductive polymer. In other words, the thermally conductive polymer has a solvent-curing agent-liquid rubber bond. In addition, the curing agent will also bond with the solvent or bond with the liquid polymer, so it also has a solvent-curing agent-solvent or liquid rubber-curing agent-liquid rubber bond. Furthermore, when the curing agent is a multifunctional type, there are multiple bonds formed between the solvent and the liquid polymer via the curing agent, so it is more preferred.
[0043] For the above reasons, the solvent does not need to be a low-boiling-point solvent with high volatility, and a solvent having a wide boiling point range from a low-boiling-point solvent to a high-boiling-point solvent can be used according to the application. In particular, from the perspective of ease of construction work of the thermally conductive polymer composition, a medium-boiling-point solvent or a high-boiling-point solvent is preferred. Specifically, the boiling point of the solvent is preferably 100° C. or higher, more preferably 150° C. or higher, and further preferably 180° C. or higher.
[0044] The appropriate content ratio of the solvent to the liquid rubber may be, for example, in the range of 50 parts by mass or more and 600 parts by mass or less relative to 100 parts by mass of the liquid rubber. By setting the content ratio of the solvent to the liquid rubber within such a range, the fluidity can be ensured and the workability can be improved during the construction of the thermally conductive polymer composition, and the curing of the liquid rubber component can be prevented from being hindered.
[0045] The appropriate ratio of the solvent to the liquid rubber is preferably in the range of 100 parts by mass or more and 300 parts by mass or less relative to 100 parts by mass of the liquid rubber.
[0046] The curing agent only needs to have two or more functional groups that can react with the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent molecules in one molecule. The curing agent of this embodiment only needs to chemically bond with the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent, respectively. The multiple hydroxyl groups of the liquid rubber are preferably located at the ends of the molecule.
[0047] Specific examples of the curing agent having two or more functional groups reactive with a hydroxyl group in one molecule include isocyanate compounds, acid anhydrides, carboxylic acids, and amines.
[0048] The method for curing the thermally conductive polymer composition with such a curing agent is not particularly limited, and examples thereof include a curing method in which the curing is carried out by polymerization reaction at room temperature or a method in which the curing is accelerated by increasing the reaction rate by heating.
[0049] The appropriate content ratio of the curing agent to the liquid rubber is, for example, within a range of 50 parts by mass or more and 400 parts by mass or less relative to 100 parts by mass of the liquid rubber. By setting the content ratio of the curing agent to the liquid rubber within such a range, the curing agent can be polymerized sufficiently with the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent to form a thermally conductive polymer with appropriate hardness, and the situation in which the brittleness is increased due to excessive hardness can be prevented.
[0050] The content ratio of the curing agent in the liquid rubber is preferably 50 parts by mass or more and 360 parts by mass or less, and more preferably 90 parts by mass or more and 200 parts by mass or less, based on 100 parts by mass of the liquid rubber.
[0051] The filler is a component that improves the thermal conductivity of the cured thermally conductive polymer, and metals, metal oxides, metal hydroxides, metal nitrides, carbon, etc. can be used. Examples of the metal include gold (319), silver (428), copper (403), aluminum (236), tungsten (177), titanium (22), nickel (94), iron (84), and alloys formed by using two or more of these metals. In addition, the numerical values in parentheses of the above metals are examples of thermal conductivity expressed in units of W / (m·K). The thermal conductivity of these metals is 10 W / (m·K) or more.
[0052] Examples of metal oxides used as fillers include aluminum oxide (20-35), magnesium oxide (45-60), beryllium oxide (272), zinc oxide (54), silicon oxide (2), and titanium oxide (8). Examples of metal hydroxides include aluminum hydroxide. Examples of metal nitrides include aluminum nitride (150-250), boron nitride (30-50), and silicon nitride (20-90). The values in parentheses of the above oxides are thermal conductivities expressed in units of W / (m·K).
[0053] Further, examples of carbon include graphite (100), carbon fiber (94 to 149), fullerene (0.4 in the case of C60), graphene (3000 to 5300), carbon nanotube (650 to 830 in the case of multilayer), etc. The numerical values in parentheses of the above carbon are thermal conductivity expressed in units of W / (m·K).
[0054] Among them, aluminum oxide is particularly preferred as a constituent material of the filler from the viewpoint of being cheap and readily available. Moreover, among these metal oxides, metal hydroxides, and carbon, the thermal conductivity of materials other than silicon oxide, titanium oxide, and fullerene is 10 W / (m·K) or more. In addition, the thermal conductivity of materials other than fullerene is 2 W / (m·K) or more.
[0055] The filler preferably includes one or two or more of the above-mentioned material examples, more preferably includes one or two or more of metal oxides, metal hydroxides and metal nitrides, and particularly preferably includes aluminum oxide.
[0056] The filler may be in the form of particles, but spherical particles, disc-shaped particles, or rounded particles with few edges and corners (round particles) are preferably used from the viewpoint of providing the thermally conductive elastomer composition with excellent shape conformability and high thermal conductivity after curing.
[0057] Regarding the particle size distribution of the filler, from the perspective of ensuring both filling and processability, it can have multiple peaks. Therefore, the filler can include a plurality of filler particles with different average particle sizes (d50) (analysis method: laser diffraction scattering particle size distribution measurement, measuring device: particle size distribution measuring device (Microtrac MT3300EX II), measurement conditions: ultrasonic (US) dispersion using sodium hexametaphosphate for 1 minute). In the case where the filler includes two filler particles with different average particle sizes (d50), it is preferred that, for example, the peak on the small particle size side is within the range of 0.3 μm or more and 10 μm or less and the peak on the large particle size side is within the range of 20 μm or more and 100 μm or less.
[0058] In the thermally conductive polymer composition of the present embodiment, a composition containing any one or more of a liquid rubber, a solvent, and a curing agent can be used as a base material. In this case, the appropriate content ratio of the filler relative to the base material is as long as it is within the range of 200 mass parts or more and 3000 mass parts or less relative to 100 mass parts of the base material. By setting the content ratio of the filler within such a range, the viscosity increase of the thermally conductive polymer composition can be suppressed, and the thermal conductivity of the cured thermally conductive polymer can be further improved. In addition, the appropriate content ratio of the filler relative to the base material is preferably within the range of 200 mass parts or more and 2500 mass parts or less relative to 100 mass parts of the base material.
[0059] In the thermally conductive polymer composition of this embodiment, in addition to the above-mentioned liquid rubber, solvent, curing agent, and filler, a lubricant, an antioxidant, a flame retardant, a thickening material, etc. can be further added. For example, by further adding a flame retardant, it can also be used as a flame-retardant thermally conductive component between a battery cell and a casing (heat sink) of a lithium ion secondary battery.
[0060] According to the thermally conductive polymer composition of the present embodiment having the above-described structure, the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent are chemically bonded and cured by polymerization reaction with the functional groups in the curing agent, respectively, so that the solvent component is introduced into the cured thermally conductive polymer as a constituent material. Thus, even if the filler content that causes the hardness to increase is increased to improve the thermal conductivity, the hardness can be kept low by the solvent component. Therefore, a thermally conductive polymer composition having high shape followability, excellent workability, and high thermal conductivity can be realized.
[0061] The thermally conductive polymer of the present embodiment may be a thermally conductive polymer composition having a thermal conductivity of 1.5 W / (m·K) or more after curing.
[0062] (Thermal Conductive Polymer Composition Forming Material)
[0063] The thermally conductive polymer composition forming material of this embodiment is a two-liquid mixed type thermally conductive polymer material for forming the above-mentioned thermally conductive polymer composition, and includes a liquid A containing the above-mentioned liquid rubber and a solvent, and a liquid B containing a curing agent. In addition, at least one of the liquid A or the liquid B, or both of them, further contains a filler.
[0064] In addition, as long as the filling amount of the filler reaches 2000 parts by mass, the density of liquid A and liquid B is similar. A lubricant, antioxidant, flame retardant, thickening material, etc. listed in the thermally conductive polymer composition of this embodiment may be further added to at least one or both of liquid A and liquid B.
[0065] When using the thermally conductive polymer composition forming material of the present embodiment, liquid A and liquid B are mixed, and the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent of liquid A are contacted with the curing agent contained in liquid B to chemically bond and cure. As a construction method, for example, a method can be used in which a two-liquid mixing dispenser is used to dispense the liquid A and liquid B in equal volumes, mix them, and form a thermally conductive polymer composition, and the thermally conductive polymer composition is directly applied to the surface of a component on which a thermally conductive polymer is provided.
[0066] The method for manufacturing the thermally conductive polymer composition forming material of the present embodiment is not particularly limited, and a known method can be applied. For example, a method of mixing a base material obtained by mixing materials other than fillers in the above-mentioned constituent materials of liquid A and liquid B and a filler contained in at least one or both of liquid A and liquid B can be cited. The mixing order of the constituent materials of the base material is not particularly limited and can be appropriately determined. As a method for mixing the materials, a method using a mixing device such as a stirring type, a rotating type, and a vibrating type can be cited.
[0067] Thus, according to the thermally conductive polymer composition forming material of the present embodiment, by separating the liquid A containing the liquid rubber and the solvent and the liquid B containing the curing agent from each other, the liquid A and the liquid B can be mixed and cured at any time to form a thermally conductive polymer, and a thermally conductive polymer composition forming material with excellent storage properties can be achieved.
[0068] (Thermal Conductive Polymer)
[0069] The thermally conductive polymer of this embodiment can be obtained by curing the thermally conductive polymer composition. In such a thermally conductive polymer, for example, the terminal group is -[(C2H4-O) m -C n H 2n+1 ] (wherein m and n are arbitrary natural numbers). m is preferably 1 to 20,000. n is preferably 1 to 5.
[0070] In the thermally conductive polymer obtained by curing the thermally conductive polymer composition of the present embodiment, for example, the liquid rubber is polymerized through the urethane bond, so that the cohesive fracture is suppressed and the adhesion to the parts is improved. The thermal conductivity of such a thermally conductive polymer measured by a conventional method is, for example, in the range of 1 W / (m·K) or more and 5 W / (m·K) or less.
[0071] Above, an embodiment of the present invention has been described, but this embodiment is only an example and is not intended to limit the scope of the invention. This embodiment can be implemented in various other ways, and various omissions, substitutions, and changes can be made without departing from the scope of the main purpose of the invention. This embodiment or its modification is included in the scope or main purpose of the invention, and is included in the invention described in the scope of the claims and its equivalent.
[0072] Example
[0073] Next, the A liquid and the B liquid of the thermally conductive polymer composition forming materials of Examples 1 to 6 of the present invention and Comparative Example 1 prepared as samples were mixed in equal volumes to form a thermally conductive polymer composition, which was then cured to obtain a thermally conductive polymer. The specific gravity of the A liquid and the B liquid was almost the same as that of the liquid due to the blending, and was 3 g / cm 3 Then, the thermal conductivity of each thermally conductive polymer was measured.
[0074] The thermal conductivity was measured by a single-direction heat flow steady-state comparison method (SCHF, sample temperature: 50° C.) using a resin material thermal resistance measuring device (manufactured by Hitachi Technologies and Services, Ltd.) in accordance with ASTM D5470.
[0075] The compositions of liquid A and liquid B and the thermal conductivities of the obtained thermally conductive polymers are summarized in Table 1 (Inventive Examples 1 to 4) and Table 2 (Inventive Examples 5 and 6, Comparative Example 1).
[0076] In addition, the details of each component are as follows.
[0077] [Liquid rubber]
[0078] Hydroxyl-containing polybutadiene: Polybd (registered trademark) series (manufactured by Idemitsu Kosan Co., Ltd.), G series (manufactured by Nippon Soda Co., Ltd.), Krasol LBH series (manufactured by Total Cray Valley Co., Ltd.)
[0079] Hydroxyl-containing polyisoprene: Poly ip (registered trademark) (manufactured by Idemitsu Kosan Co., Ltd.)
[0080] [Solvent]
[0081] n-Butyl carbitol: (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0082] · Naphthenic processing oil: SUNTHENE series (manufactured by JAPAN SUN OIL COMPANY, LTD.)
[0083] [filler]
[0084] ·Spherical alumina: AS series, AS-C series (all d50 = 5 to 50 μm (analysis method: laser diffraction scattering particle size distribution measurement, measurement device: particle size distribution measurement device Microtrac MT3300EX II, measurement conditions: ultrasonic (US) dispersion using sodium hexametaphosphate for 1 minute)) (manufactured by Showa Denko KK)
[0085] Spherical, tri-dispersed alumina: DAB series (manufactured by Denka Company Limited)
[0086] [Curing agent (cross-linking agent)]
[0087] ·Difunctional isocyanate: MILLIONATE MTL series, HDI, TDI series (all manufactured by TOSOH CORPORATION), Lupranate (registered trademark) MI (manufactured by BASF INOAC Polyurethanes Ltd.)
[0088] · Polyfunctional isocyanate: MILLIONATE MR series (manufactured by TOSOH CORPORATION), Lupranate (registered trademark) series (manufactured by BASF INOAC Polyurethanes Ltd.)
[0089] [Thickening material]
[0090] Terpene resins: CLEARON series, YS POLYSTER series, YS RESIN series (all manufactured by YASUHARA CHEMICAL CO., LTD.), TAMANOL 901 (manufactured by ARAKAWA CHEMICAL INDUSTRIES, LTD.)
[0091] [Antioxidant]
[0092] Hindered phenol antioxidants: ADK STAB AO series (manufactured by ADEKA CO., LTD.), Irganox series (manufactured by BASF Japan Ltd.), KEMINOX series (manufactured by Chemipro Kasei Kaisha, Ltd.)
[0093] [Flame retardant]
[0094] Phosphorus-based flame retardants: CR series, PX series, DAIGUARD series, TMP, TEP, TPP, TCP, TXP, CDP (all manufactured by DAIHACHI CHEMICAL INDUSTRY CO., LTD.), REOFOS series (manufactured by Ajinomoto Fine-Techno Co., Inc.), Exolit OP 500 series (manufactured by Clariant chemicals Ltd.)
[0095]
[0096]
[0097] According to the results shown in Tables 1 and 2, the thermal conductivity of the thermally conductive polymers of Examples 1 to 6 of the present invention, which were obtained by chemically bonding the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent to the functional groups in the curing agent, was 1.95 to 3.51 W / (m·K), and excellent thermal conductivity was obtained. On the other hand, the thermal conductivity of the thermally conductive polymer of Comparative Example 1, in which the solvent and the curing agent were not chemically bonded, was 1.40 W / (m·K), which was a low value. Therefore, it can be confirmed that the thermally conductive polymer obtained by curing the thermally conductive polymer composition obtained by mixing the thermally conductive polymer composition forming material of the present invention has excellent thermal conductivity.
[0098] Industrial Applicability
[0099] According to the present invention, there can be provided a thermally conductive polymer composition having high thermal conductivity, low viscosity, high shape-conforming property, and high workability without removing a solvent during curing, a thermally conductive polymer composition forming material, and a thermally conductive polymer obtained therefrom.
Claims
1. A thermally conductive polymer composition, characterized in that contain: Liquid rubber, with two or more hydroxyl groups in one molecule; Solvents, which have more than one hydroxyl group in one molecule; a curing agent having two or more functional groups in one molecule that can react with both the hydroxyl groups of the liquid rubber and the hydroxyl groups of the solvent; and filler.
2. The thermally conductive polymer composition according to claim 1, characterized in that The thermal conductivity of the filler is greater than 10 W / (m·K).
3. The thermally conductive polymer composition according to claim 1 or 2, characterized in that: The liquid rubber includes at least one of polybutadiene, polyisoprene, and polyolefin having a plurality of hydroxyl groups.
4. The thermally conductive polymer composition according to any one of claims 1 to 3, characterized in that The solvent comprises at least one of n-butyl carbitol, glycerol, polyethylene glycol monomethyl ether, butanediol, propylene glycol, ethylene glycol and tetraethylene glycol monomethyl ether.
5. The thermally conductive polymer composition according to any one of claims 1 to 4, characterized in that The curing agent is an isocyanate compound.
6. The thermally conductive polymer composition according to any one of claims 1 to 5, characterized in that The thermally conductive polymer composition further contains a thickening material.
7. A thermally conductive polymer composition forming material, characterized in that: Used to form the thermally conductive polymer composition according to any one of claims 1 to 6, The thermally conductive polymer composition forming material includes a liquid A containing the liquid rubber and the solvent and a liquid B containing the curing agent, and at least one of the liquid A or the liquid B further contains the filler.
8. A thermally conductive polymer, characterized in that The thermally conductive polymer is a thermally conductive polymer obtained by curing the thermally conductive polymer composition according to any one of claims 1 to 6, The terminal group of the thermally conductive polymer comprises -[(C2H4-O) m -C n H 2n+1 ], where m and n are any natural numbers.
9. The thermally conductive polymer according to claim 8, characterized in that The thermal conductivity of the thermally conductive polymer is 1.5 W / (m·K) or more.