Environmental barrier materials and coatings containing low melting temperature phases

By using EBC, a material with a low melting temperature, on Si-based ceramic matrix composites (CMC), the problems of rapid oxidant diffusion caused by microstructural defects and fast TGO growth rate were solved, achieving a more durable oxidant protection effect.

CN118891328APending Publication Date: 2024-11-01OERLIKON METCO (USA) CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380028062.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-11
Filing Date
2023-04-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing environmental barrier coatings (EBCs) for Si-based ceramic matrix composites (CMCs) have microstructural defects in high-temperature oxidizing environments, leading to rapid diffusion of oxidants and fast growth rate of thermally grown oxides (TGOs), resulting in a high risk of peeling and failing to effectively protect the CMC substrate.

Method used

The EBC using low melting temperature material is formed by in-situ melting, diffusion and filling of microstructural defects during high-temperature coating of thermal spray material raw materials, resulting in a dense and crack-free EBC. This process includes powder mixing of low melting temperature material and high melting temperature matrix material, agglomeration, sintering and plasma densification treatment.

Benefits of technology

It significantly reduces microstructural defects, provides an enhanced oxidant diffusion barrier, slows TGO growth rate by more than half, and improves coating durability and protective effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891328A_ABST
    Figure CN118891328A_ABST
Patent Text Reader

Abstract

Environmental barrier materials and coatings containing low melting temperature materials are provided. The materials and coatings include high melting temperature materials, such as rare earth silicate, mullite, hafnium stone, zircon, HfO2, rare earth stabilized ZrO2, HfB2, HfC, ZrB2, ZrC, and SiC. The melting temperature of the low-melting-temperature material is lower than 1500 DEG C. The low melting temperature material in the coating melts, diffuses, and fills the microstructure defects in situ after post-heat treatment. Due to reduced microstructure defects, the EBC containing the low melting temperature material provides an enhanced barrier against oxidant diffusion and slows the TGO growth rate by more than two times compared to coatings not containing the low melting temperature material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Patent Application No. 63 / 329,575, filed on April 11, 2022, under 35 U.S.C. §119(e), the disclosure of which is expressly incorporated herein by reference in its entirety. Technical Field

[0003] The present disclosure relates to an environmental barrier coating (EBC) on a Si-based ceramic matrix composite (CMC) that is capable of protecting the CMC in a high temperature oxidizing environment. In an exemplary embodiment, a thermal spray material feedstock containing a low melting temperature material melts, diffuses, and fills the EBC microstructural defects in situ under high temperature coating conditions. Due to the reduction in microstructural defects, the EBC containing the low melting temperature material provides an enhanced barrier to prevent the diffusion of oxidants (water vapor and oxygen) compared to a coating without the low melting temperature material, and makes the growth rate of thermally grown oxide (TGO) more than two times slower. For example, in some preferred embodiments, the TGO growth rate in the EBC coating containing the low melting temperature material is five times (or more) slower than that in the EBC coating without the low melting temperature material. In a more preferred embodiment, the TGO growth rate in the EBC coating containing the low melting temperature material is 10 times (or more) slower than that in the EBC coating without the low melting temperature material. Background Art

[0004] Rare earth silicates and mullite are commonly used in environmental barrier coatings (EBCs) applied to Si-based ceramic matrix composites (CMCs) to protect the CMCs from oxidation and water vapor corrosion. Conventional EBCs contain a Si-bond coat and an ytterbium silicate top coat. Air plasma spray (APS) is a commonly used process for EBC deposition. However, the coatings treated with APS usually contain at least a certain degree of porosity and microstructural defects, such as splat boundaries and microcracks. In the high-temperature gas turbine engine environment, these microstructural defects provide a fast diffusion path for oxidants (water vapor and oxygen) to reach the Si-bond coat and accelerate the oxidation of the Si-bond coat. When exposed to the high-temperature oxidizing environment in the gas turbine engine, the Si-bond coat will also be oxidized to form a thermally grown oxide (TGO) SiO2 layer. When the TGO layer reaches a threshold thickness, the EBC will peel off. Therefore, a new dense and crack-free EBC is needed to protect the Si-bond coat and the CMC substrate from oxidation, reduce the TGO growth rate, and improve the coating durability. Summary of the invention

[0005] The object of the present disclosure is to obtain a dense and crack-free EBC capable of preventing oxidants (water vapor and oxygen) from reaching underlying components (e.g., silicon bond coat and / or CMC substrate). In some embodiments, such an EBC can be obtained from a thermal spray material feedstock comprising: a first powder comprising at least one low melting temperature material having a melting temperature of less than 1500° C., and a second powder comprising at least one environmental barrier coating substrate material (typically a high melting temperature substrate material).

[0006] In some embodiments, the at least one low melting temperature material is a single oxide compound, a binary oxide, a ternary oxide, or multiple oxides. For example, in some embodiments, the low melting temperature material may include at least four oxides having a melting temperature less than 1300°C.

[0007] In some embodiments, the at least one environmental barrier coating matrix material (typically a high melting temperature matrix material) includes at least one material selected from the group consisting of rare earth silicates, rare earth oxides, mullite, alkali silicates, HfO2, HfSiO4, HfTiO4, ZrTiO4, ZrSiO4, rare earth oxide-stabilized zirconium oxide, rare earth oxide-stabilized hafnium oxide, HfB2, HfC, ZrB2, ZrC and SiC.

[0008] In some embodiments, the first and second powders are mixed, agglomerated, agglomerated and sintered, plasma densified, or fused and crushed.

[0009] In some specific embodiments, the at least one low melting temperature material includes: CaO, MgO, Al2O3, SiO2, Na2O, K2O and Fe2O3. In other embodiments, the at least one low melting temperature material is Li2O.

[0010] In some embodiments, the EBC may include: an EBC top coating, comprising: an EBC substrate (typically a high melting temperature substrate material), the EBC substrate comprising a material selected from the group consisting of rare earth silicates, rare earth oxides, mullite, alkali silicates, HfO2, HfSiO4, HfTiO4, ZrTiO4, ZrSiO4, rare earth oxide-stabilized zirconia, rare earth oxide-stabilized hafnium oxide, HfB2, HfC, ZrB2, ZrC, SiC and combinations thereof, and at least one low melting temperature material having a melting temperature less than 1500°C embedded in the EBC substrate; and a Si-based bonding coating.

[0011] In some embodiments, the at least one low melting temperature material of the EBC may include: CaO, MgO, Al2O3, SiO2, Na2O, K2O, and Fe2O3. In other embodiments, the at least one low melting temperature material of the EBC is Li2O.

[0012] In some embodiments, the EBC matrix includes at least one rare earth silicate including at least one rare earth element selected from the group consisting of Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. In other embodiments, the EBC matrix includes at least one rare earth oxide including at least one rare earth element selected from the group consisting of Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In the following detailed description, the present disclosure is further described by way of non-limiting examples of preferred embodiments of the present disclosure, with reference to the indicated several figures of the drawings.

[0014] Figure 1 Schematic diagram of the as-deposited coating microstructure.

[0015] Figure 2A is a schematic diagram of a mixed powder including a base powder and a low melting temperature powder.

[0016] Figure 2B is a schematic diagram of an agglomerated powder including a base powder and a low melting temperature powder.

[0017] Figure 3 Scanning electron microscope (SEM) images of the high melting temperature matrix powder and the first low melting temperature powder are shown.

[0018] Figure 4A is an illustration of a SEM image of an as-sprayed APS Yb2Si2O7 coating showing microcracks and sheet boundaries.

[0019] Figure 4B is an illustration of a SEM image of a heat treated APS Yb2Si2O7 coating showing microcracks and sheet boundaries.

[0020] Figure 4C is a graphic representation of the SEM image of the as-sprayed APS Yb2Si2O7-sodium calcium magnesium aluminum silicate coating.

[0021] Figure 4D is a graphic representation of a SEM image of a heat treated APS Yb2Si2O7-sodium calcium magnesium aluminum silicate coating.

[0022] Figure 5A is a graphic representation of an SEM image of a Yb2Si2O7 coating evaluated after exposure to 90 vol% H2O-10 vol% air at 1316°C for 170 hours.

[0023] Figure 5B is a graphic representation of an SEM image of a Yb2Si2O7 coating evaluated after exposure to 90 vol% H2O-10 vol% air at 1316°C for 510 hours.

[0024] Figure 5C is a graphic representation of an SEM image of a Yb2Si2O7-sodium calcium magnesium aluminum silicate coating evaluated after exposure to 90 vol% H2O-10 vol% air at 1316°C for 170 hours.

[0025] Figure 5D is a graphic representation of an SEM image of a Yb2Si2O7-sodium calcium magnesium aluminum silicate coating evaluated after exposure to 90 vol% H2O-10 vol% air at 1316°C for 510 hours.

[0026] Figure 6 is a graph showing TGO thickness as a function of exposure (time) for Yb2Si2O7 coating and APS Yb2Si2O7-sodium calcium magnesium aluminosilicate coating.

[0027] Figure 7 is a graphic representation of SEM images of a high melting temperature matrix powder and a second low melting temperature powder.

[0028] Fig. 8A is a graphic representation of the SEM image of the as-sprayed APS Yb2Si2O7-0.4wt%Li2O coating.

[0029] Figure 8B is a graphic representation of the SEM image of the heat-treated APS Yb2Si2O7-0.4wt%Li2O coating.

[0030] Fig. 9A is a graphic representation of an SEM image of a Yb2Si2O7 coating evaluated after exposure to 90 vol% H2O-10 vol% air at 1316°C for 410 hours.

[0031] Fig. 9B is a graphic representation of an SEM image of a Yb2Si2O7-0.4wt%Li2O coating evaluated after exposure to 90vol%H2O-10vol% air at 1316°C for 410 hours. DETAILED DESCRIPTION

[0032] In the following description, various embodiments of the present disclosure will be described with reference to the accompanying drawings. Detailed embodiments of the present disclosure are discussed herein as needed; however, it is to be understood that the disclosed embodiments are merely examples of embodiments of the present disclosure, which may be embodied in various alternative forms. The figures are not necessarily drawn to scale, and certain features may be exaggerated or reduced to show the details of a particular component. Therefore, the specific structural and functional details disclosed herein should not be interpreted as limiting, but only as a representative basis for teaching those skilled in the art to adopt the present disclosure in different ways.

[0033] As used herein, the singular forms "a", "an", and "the" include plural references unless the context clearly indicates otherwise. For example, reference to a "powder material" would also mean that there may be a mixture of one or more powder materials unless specifically excluded. As used herein, the indefinite article "a" means one, as well as more than one, and does not necessarily limit the noun it refers to to the singular.

[0034] Unless otherwise indicated, all numbers used in the specification and claims to indicate quantities should be understood as being modified by the term "about" in all instances. Accordingly, unless otherwise indicated, the numerical parameters set forth in the specification and claims are approximate values ​​that may vary depending on the desired properties sought to be obtained by the embodiments of the present disclosure. At a minimum, and without being construed as an attempt to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should be interpreted in light of the number of significant digits and ordinary rounding conventions.

[0035] In addition, the listing of numerical ranges in this specification is considered to be the disclosure of all numerical values ​​and ranges within the range (unless otherwise expressly indicated). For example, if the range is from about 1 to about 40, it is considered to include, for example, 1, 7, 23.7, 34, 36.1, 40 or any other value or range within the range.

[0036] As used herein, the terms "about" and "approximately" indicate that the amount or value in question may be the specified specific value or some other value in the vicinity thereof. Generally, the terms "about" and "approximately" indicating a value are intended to indicate a range within ±5% of that value. As an example, the phrase "about 100" indicates a range of 100±5, i.e., a range from 95 to 105. Generally, when the terms "about" and "approximately" are used, it can be expected that similar results or effects according to the present disclosure can be obtained within a range of ±5% of the indicated value.

[0037] The term "at least partially" is intended to mean that the subsequent property is satisfied to a certain extent (such as 25% or 50%) or completely.

[0038] The terms "substantially" and "essentially" are used to indicate that the subsequent characteristic, property or parameter is fully (entirely) achieved or satisfied, or to a large extent (eg, 90%, 95% or 99%) without adversely affecting the expected result.

[0039] As used herein, the term "comprising" is intended to be non-exclusive and open. Thus, for example, a composition comprising oxide A may include other oxides in addition to A. However, the term "comprising" also encompasses the more restrictive meanings of "consisting essentially of" and "consisting of", such that, for example, a "composition comprising oxide A" may also consist (essentially) of oxide A.

[0040] In the present disclosure, unless otherwise stated, all weight percentages referring to elements / components of a composition / material / layer are based on the total weight of the composition / material / layer, which includes any unavoidable impurities that may be present.

[0041] The present disclosure relates to EBCs (e.g., EBCs including an EBC topcoat and a Si-based bond coat), and methods of applying the EBCs to substrates (and articles formed by applying the EBCs to substrates), such as substrates selected from Si-based ceramic matrix composites (CMCs). In embodiments, the EBC coating compositions and structural arrangements of the EBCs disclosed herein can achieve excellent environmental barrier coating bond coat adhesion, oxidation resistance and fatigue resistance, and environmental performance, as well as self-healing capabilities to ensure long-term durability of the CMCs.

[0042] In an embodiment, the EBC of the present disclosure includes a substrate (i.e., an environmental barrier coating substrate) comprising a high melting temperature substrate material selected from the group consisting of rare earth silicates (including one or more rare earth elements selected from the following: Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu), rare earth oxides (including one or more rare earth elements selected from the following: Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, and Lu), , Dy, Ho, Er, Tm, Yb and Lu), mullite (3Al2O3-2SiO2), alkali silicates, HfO2, HfSiO4, HfTiO4, ZrTiO4, ZrSiO4, rare earth oxide stabilized zirconia, rare earth oxide stabilized hafnium oxide, HfB2, HfC, ZrB2, ZrC, SiC and combinations thereof; and at least one low melting temperature material embedded in the environmental barrier coating substrate (high melting temperature substrate material) having a melting temperature less than 1500°C.

[0043] In some embodiments, at least one low melting temperature material having a melting temperature less than 1500°C may be embedded in the environmental barrier coating substrate (high melting temperature substrate material), and the content of the low melting temperature material (relative to the total weight of the at least one low melting temperature material and the environmental barrier coating substrate (high melting temperature substrate material)) is in the range of 0.1wt% to 10wt%, preferably, the content of the low melting temperature material is in the range of 0.1wt% to 5wt%, or more particularly, the content of the low melting temperature material is in the range of 0.3wt% to 4wt%.

[0044] like Figure 1 As shown, in some embodiments, EBC 110 is composed of multiple layers directly adjacent to substrate 100 (e.g., SiC / SiC ceramic matrix composite substrate, etc.), which can provide enhanced environmental protection. In these embodiments, EBC 110 can include Si-based bonding coating 120 and EBC top coating 130.

[0045] When present, the Si-based bond coating 120 can have any desired coating thickness or coating thickness range, for example, such as a coating thickness ranging from 5 μm to 200 μm. In an embodiment, the Si-based bond coating may include a Si-based metal. In some embodiments, the Si-based bond coating may be composed of one or more of: MoSi2 or HfSi2, or Si-Al2O3, Si-Al2O3-RE2O3 (wherein RE is a rare earth element).

[0046] The EBC top coating 130 can have any desired coating thickness or coating thickness range, such as, for example, a coating thickness ranging from 50 μm to 1000 μm. In an embodiment, the EBC top coating 130 may include a high melting temperature matrix material 132 and a low melting temperature material 134 embedded within the high melting temperature matrix material 132 . Figure 1 Microcracks 136 that may be present throughout the EBC top coating 130 are also schematically shown.

[0047] In some embodiments, the low melting temperature material is at least one oxide compound shown in Table 1 (below) (ie, wherein the corresponding powder particles or phases are made of a single oxide compound).

[0048] Table 1

[0049] Material Melting temperature(℃) <![CDATA[P2O5]]> 340 <![CDATA[K2O]]> 350 <![CDATA[B2O3]]> 510 KF 858 <![CDATA[BaB8O 13 ]]> 890 <![CDATA[Co2O3]]> 895 <![CDATA[Co3O4]]> 900 <![CDATA[Ba2B 10 THE 17 ]]> 905 <![CDATA[BaB4O7]]> 910 <![CDATA[Li2B4O7]]> 917 <![CDATA[Zn3B2O6]]> 980 <![CDATA[Fe2B2O5]]> 980 <![CDATA[CaB4O7]]> 986 <![CDATA[MgB2O4]]> 988 <![CDATA[LiNiO2]]> 1000 <![CDATA[Ba2B2O5]]> 1050 <![CDATA[Na2SiO3]]> 1088 <![CDATA[BaB2O4]]> 1095 <![CDATA[LiCoO2]]> 1100 <![CDATA[BaB2O4]]> 1100 <![CDATA[Fe3BO5]]> 1100 <![CDATA[NaAlSi3O8]]> 1100 <![CDATA[GeO2]]> 1115 <![CDATA[Nd(BO2)3]]> 1120 <![CDATA[Na2O]]> 1132 <![CDATA[Fe2SiO4]]> 1200 <![CDATA[Nd4B2O9]]> 1200 <![CDATA[MgB2O4]]> 1200 <![CDATA[Li3PO4]]> 1205 <![CDATA[Li4SiO4]]> 1258 <![CDATA[MgF2]]> 1263 <![CDATA[Mg2B2O5]]> 1310 CuO 1326 <![CDATA[Mg3B2O6]]> 1340 <![CDATA[BaTi2O5]]> 1375 FeO 1377 <![CDATA[Ba3B2O6]]> 1383 <![CDATA[CaAl2O4]]> 1390 <![CDATA[CaF2]]> 1418 <![CDATA[Ba4Ti 13 THE 30 ]]> 1430 <![CDATA[Li2O]]> 1438

[0050] In another embodiment, the low melting temperature material is at least one binary oxide shown in Table 2 (below).

[0051] Table 2

[0052]

[0053] In yet another embodiment, the low melting temperature material is at least one ternary oxide shown in Table 3 (below).

[0054] Table 3

[0055] Ternary materials Melting temperature(℃) <![CDATA[(0.2-0.5mol)MgO–(0.1-0.3mol)Al2O3–(0.2-0.5mol)B2O3]]> 1200-1500 <![CDATA[(0.2-0.5mol)CaO-(0.05-0.5mol)Al2O3-(0.4-0.8mol)SiO2]]> 1170-1500 <![CDATA[(0.2-0.5mol)CaO-(0.2-0.5mol)MgO-(0.4-0.7mol)SiO2]]> 1300-1500 <![CDATA[(0.1-0.4mol)MgO-(0.2-0.4mol)Al2O3-(0.5-0.7mol)SiO2]]> 1300-1500 <![CDATA[(0.05-0.2mol)Na2O-(0.05-0.2mol)Al2O3-(0.6-0.8mol)SiO2]]> 1000-1400 <![CDATA[(0.1-0.6mol))BaO-(0.05-0.3mol)B2O3-(0.3-0.8mol)SiO2]]> 850-1400 <![CDATA[(0.1-0.7mol)B2O3-(0.05-0.25mol)Al2O3-(0.1-0.8mol)SiO2]]> 1200-1500 <![CDATA[(0.05-0.9mol)Li2O-(0.05-0.9mol)B2O3-(0.05-0.9mol)Y2O3]]> 900-1500

[0056] In yet another embodiment, the low melting temperature material is a mixture of at least one of the multi-oxides shown in Table 4 (below).

[0057] Table 4

[0058] Multi-element oxide materials Melting temperature(℃) <![CDATA[Na2O-CaO-Al2O3-SiO2]]> 900-1300 <![CDATA[CaO-MgO-FeO-SiO2]]> 900-1300 <![CDATA[CaO-Al2O3-FeO-SiO2]]> 900-1300 <![CDATA[B2O3-Al2O3-BaO-SiO2]]> 900-1300 <![CDATA[B2O3-Al2O3-Na2O-SiO2]]> 900-1300 <![CDATA[CaO-MgO-Al2O3-SiO2]]> 900-1300 <![CDATA[Na2O-Al2O3-K2O-SiO2]]> 900-1300 <![CDATA[P2O5–CaO-TiO2–Na2O]]> 900-1300 <![CDATA[P2O5-Li2O–Al2O3–TiO2]]> 900-1300 <![CDATA[CaO-MgO-Al2O3-FeO-SiO2]]> 900-1300 <![CDATA[SiO2-Al2O3-Fe2O3-CaO-Na2O-K2O]]> 900-1300 <![CDATA[SiO2-Al2O3-CaO-MgO-Na2O-K2O]]> 900-1300 <![CDATA[SiO2-Al2O3-Fe2O3-CaO-MgO-Na2O-K2O]]> 900-1300 <![CDATA[CaO-MgO-Al2O3-SiO2-Na2O-K2O-Fe2O3]]> 900-1300 <![CDATA[SiO2-Al2O3-CaO-Fe2O3-MgO-Na2O-K2O-TiO2]]> 900-1300 <![CDATA[P2O5-Na2O-Al2O3-Fe2O3-Cr2O3-SrO]]> 900-1300

[0059] In some embodiments, the low melting temperature material can be formed from calcium-magnesium-aluminum-silicate (CMAS) powder (having a melting temperature less than 1500°C), such as a CMAS powder comprising: 29wt% to 39wt% quartz (SiO2), 25wt% to 35wt% gypsum (CaSO4 x 2H2O), 12wt% to 23wt% fine quartz (SiO2+KAlSi3O8), 9wt% to 19wt% dolomite (CaMg(Co3)2) and 3wt% to 7wt% salt (NaCl).

[0060] In other embodiments, the low melting temperature material may be formed of CMAS powder (having a melting temperature of less than 1500° C.), wherein the CMAS powder is selected from one of the following compositions:

[0061] Composition 1: 60.0 mol% to 70.0 mol% SiO2, 15.0 mol% to 31.0 mol% CaO,

[0062] 6.0 mol% to 10.0 mol% MgO, 2.0 mol% to 5.0 mol% Al2O3, 0.5 mol% to 5.0 mol% Na2O, and 0.1 mol% to 1.0 mol% K2O;

[0063] Composition 2: 50.0 mol% to 65.0 mol% SiO2, 25.0 mol% to 40.0 mol% CaO,

[0064] 1.0 mol% to 6.0 mol% MgO, 1.0 mol% to 3.5 mol% Al2O3, 3.0 mol% to 5.0 mol% Na2O, and 0.01 mol% to 0.5 mol% K2O; and

[0065] Composition 3: 25.0 mol% to 55.0 mol% SiO2, 35.0 mol% to 60.0 mol% CaO,

[0066] 0.5 mol% to 5.0 mol% MgO, 0.5 mol% to 3.0 mol% Al2O3, 1.0 mol% to 5.0 mol% Na2O and 0.0 mol% to 0.2 mol% K2O.

[0067] In some embodiments, the high melting temperature matrix material is composed of the following components: rare earth silicates (including rare earth elements Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu), rare earth oxides (including rare earth elements Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu), mullite (3Al2O3-2SiO2), alkali silicates (BaO-SrO-Al2O3-SiO2), HfO2, HfSiO4, HfTiO4, ZrTiO4, ZrSiO4, rare earth oxide-stabilized zirconium oxide, rare earth oxide-stabilized hafnium oxide, HfB2, HfC, ZrB2, ZrC, SiC and combinations thereof. In some embodiments, the material of the high melting temperature matrix can be selected so that the matrix has a melting temperature that is at least 350° C. higher than the melting temperature (melting point) of the low melting temperature material. In some embodiments, the matrix formed of the high melting temperature matrix material can have a melting temperature in the range of from 1800° C. to 3900° C., particularly in the range of from 2200° C. to 3400° C., and more particularly in the range of from 2500° C. to 3000° C.

[0068] In some embodiments, the EBC of the present disclosure may be formed from a thermal spray material feedstock comprising: (i) a first powder comprising a low melting temperature material having a melting temperature less than 1500° C., and (ii) a second powder comprising a high melting temperature matrix material.

[0069] Figure 2A A schematic diagram of an exemplary embodiment of a thermal spray material feedstock is shown, wherein the thermal spray material feedstock includes a mixed powder including a high melting temperature matrix material powder 220 and a low melting temperature material powder 230 .

[0070] In some embodiments, the particle size distribution (in terms of particle size) of the high melting temperature matrix material powder can range from 11 μm to 200 μm. In a preferred embodiment, the particle size distribution of the high melting temperature matrix material powder can range from 11 μm to 150 μm. In a more preferred embodiment, the particle size distribution of the high melting temperature matrix material powder can range from 11 μm to 125 μm.

[0071] In some embodiments, the high melting temperature matrix material powder may have an average particle size (diameter) ranging from 25 μm to 125 μm, preferably in the range of from 25 μm to 90 μm.

[0072] In some embodiments, the particle size distribution (in terms of particle size) of the low melting temperature material powder can range from 1 μm to 125 μm. In a preferred embodiment, the particle size distribution of the low melting temperature material powder can range from 2.5 μm to 75 μm, such as from 5 μm to 62 μm. In a more preferred embodiment, the particle size distribution of the low melting temperature material powder can range from 5 μm to 55 μm.

[0073] In some embodiments, the low melting temperature material powder may have an average particle size (diameter) ranging from 5 μm to 40 μm, preferably in the range of from 5 μm to 25 μm.

[0074] In some embodiments, the low melting temperature material powder has an average particle size smaller than the average particle size (diameter) of the high melting temperature matrix material powder (for example, an average particle size at least 30% smaller (preferably at least 50% smaller) than the average particle size of the high melting temperature matrix material powder).

[0075] In some embodiments, the EBC of the present disclosure may be formed from a thermal spray material feedstock including an agglomerated powder. Figure 2B 2 is a schematic diagram of an exemplary embodiment of a thermal spray material feedstock, wherein the thermal spray material feedstock includes agglomerated powder particles, the agglomerated powder particles including a high melting temperature matrix material powder 220 and a low melting temperature material powder 230 .

[0076] In some embodiments, the particle size distribution of the agglomerated powder may range from 11 μm to 125 μm. In a preferred embodiment, the particle size distribution of the agglomerated powder may range from 11 μm to 90 μm. In a more preferred embodiment, the particle size distribution of the agglomerated powder may range from 11 μm to 62 μm.

[0077] In some embodiments, the high melting temperature matrix material powder and the low melting temperature material powder in the thermal spray material feedstock are manufactured by one or more of the following methods: mixing, agglomeration, agglomeration and sintering, plasma densification, or fusion and fragmentation.

[0078] In an embodiment, the Si-based bond coating and EBC top coating on the Si-based ceramic matrix composite (CMC) can be deposited by one of the following methods (using conditions known to those skilled in the art): air plasma spraying (APS), high velocity oxygen fuel spraying (High Velocity Oxy-Fuel, HVOF), combustion spraying, vacuum plasma spraying or suspension thermal spraying. For example, in an embodiment where the Si-based bond coating and EBC top coating are deposited on the Si-based ceramic matrix composite (CMC) by APS, the conditions shown in Table 5 (below) can be used.

[0079] Table 5

[0080] Si Bond Coating Top coating Current A 450 500 Voltage V 96.6 97 Power kW 44.3 50 Ar nlpm 75 70 <![CDATA[H2 nlpm]]> 5 5 Powder feeding rate g / min 10-50 10-50 Coating thickness (μm) 150 200

[0081] In some embodiments, the low melting temperature material may be specifically selected and provided in the EBC in an amount effective to enable at least some of the selected low melting temperature material to melt, diffuse, and at least partially fill microstructural defects that occur during EBC deposition, such as microcracks and sheet boundaries, at or below a predetermined heat treatment temperature. In a preferred embodiment, the low melting temperature material may be specifically selected and provided in the EBC in an amount effective to enable at least some of the selected low melting temperature material to melt, diffuse, and substantially fill microstructural defects that occur during EBC deposition (e.g., fill at least 90% or at least 95% of the volume of the initially existing microstructural defects), such as microcracks and sheet boundaries, at or below a predetermined heat treatment temperature. Due to the reduction in microstructural defects, some embodiments of the present disclosure include EBCs containing low melting temperature materials that provide an enhanced oxidant diffusion barrier and have a TGO growth rate that is more than two times slower (e.g., more than five times slower or more than 10 times slower (e.g., the amount is in the range of from five to 20 times)) compared to coatings that do not contain low melting temperature materials.

[0082] In some embodiments, the content of the low melting temperature material in the EBC top coating is 0.1wt% to 40wt% based on the total weight of the EBC top coating. In another embodiment, the content of the low melting temperature material in the EBC top coating is 0.5wt% to 10wt% based on the total weight of the EBC top coating. In yet another embodiment, the content of the low melting temperature material in the EBC top coating is 1.0wt% to 5.0wt% based on the total weight of the EBC top coating.

[0083] In some embodiments, the EBC of the present disclosure may be prepared by a method including a post-coating heat treatment process. In these embodiments, the heat treatment temperature may be an effective (i.e., sufficiently high) temperature to melt and diffuse the low melting temperature material within the matrix structure of the EBC (e.g., a matrix structure formed by a high melting temperature matrix material), such as a temperature equal to or at least 50°C higher than the melting temperature of the low melting temperature material, or a temperature in the range of 50°C to 150°C higher than the melting temperature of the low melting temperature material. In some embodiments, the heat treatment temperature may be a temperature equal to or higher than a temperature sufficient to ensure that 100% of the low melting temperature material is completely melted to form a liquid phase. For example, the heat treatment temperature may be a temperature equal to or higher than the melting temperature of the low melting temperature material by at least 100°C to ensure that the low melting temperature material is completely melted to form a liquid phase in the environmental barrier coating matrix (EBC matrix, which is formed by a high melting temperature matrix material) and fill the microcracks in the EBC.

[0084] The present invention is further illustrated by the following non-limiting examples, in which all parts, percentages, ratios and proportions are by weight, all temperatures are in ° C., and all pressures are atmospheric pressure unless otherwise indicated:

[0085] Example

[0086] Several specific EBCs were prepared as exemplary embodiments of the innovations disclosed herein. These examples are included herein for illustrative purposes.

[0087] In the example, Metco 4810Si powder was used for bond coat deposition and M6157 Yb2Si2O7 powder was used for baseline top coat deposition. Yb2Si2O7 / Si baseline EBC and Yb2Si2O7 / Si containing low melting temperature phase were deposited onto SiC substrate using a SinplexPro plasma torch with a 9 mm nozzle.

[0088] All the as-sprayed coatings were further annealed at 1300°C for 10 hours in an air atmosphere. The heat-treated EBCs were isothermally evaluated in a steam furnace at 1316°C to study the growth behavior of thermally grown oxide (TGO). Water was injected into the furnace along with air using a peristaltic pump. The amount of water and air was controlled to create an environment with about 90 vol% H2O(g) and about 10 vol% air, with a hot zone gas velocity of 4 cm / s in the furnace chamber. The thickness of thermally grown oxide (TGO) at different exposure times was measured using a scanning electron microscope (SEM).

[0089] Example 1: Figure 3Scanning electron microscope (SEM) images of a high melting temperature matrix powder 320 composed of Metco 6157Yb2Si2O7 having a high melting temperature of about 1850°C and a low melting temperature powder 330 composed of sodium calcium magnesium aluminum silicate powder having a melting temperature of about 1140°C are shown. Figure 3 In the figure, the bright phase is Yb2Si2O7 and the dark phase is sodium calcium magnesium aluminum silicate powder.

[0090] Comparative Example 1A: Figure 4A The SEM image of the sprayed APS Yb2Si2O7 coating is shown. Figure 4A , SEM images show microcracks and flake boundaries in the as-sprayed APS Yb2Si2O7 coating (e.g., a flake boundary is a boundary between two flakes where remelting and / or recrystallization of material near the flake surface (during the thermal spray production process) results in an interface (between flakes) having a different morphology than the material inside the flakes).

[0091] Comparative Example 1B: Figure 4B Shows the SEM image of the heat-treated APS Yb2Si2O7 coating. Figure 4B In Figure 2, SEM images show microcracks and sheet boundaries in an APS Yb2Si2O7 coating heat treated at 1300°C for 10 hours.

[0092] Example 1A: Figure 4C The SEM image of the sprayed APS Yb2Si2O7-sodium calcium magnesium aluminum silicate coating is shown. Figure 4C In the figure, the SEM image shows the microcracks and sheet boundaries in the as-sprayed APSYb2Si2O7-sodium calcium magnesium aluminosilicate coating. Figure 4C The distribution of the sodium calcium magnesium aluminum silicate phase 410 in the Yb2Si2O7 matrix 420 is also shown.

[0093] Example 1B: Figure 4D SEM images of heat-treated APS Yb2Si2O7-sodium calcium magnesium aluminum silicate coatings are shown. Figure 4D In Figure 2, the SEM image shows the disappearance of microcracks and platelet boundaries in the APS Yb2Si2O7-sodium calcium magnesium aluminum silicate coating after 10 hours of heat treatment at 1300°C, as well as the disappearance of the low melting temperature sodium calcium magnesium aluminum silicate phase.

[0094] Comparative Example 1C: Figure 5A Shown is a SEM image of a Yb2Si2O7 coating evaluated after exposure to 90 vol% H2O-10 vol% air at 1316°C for 170 h. Figure 5A In the SEM image, it is shown that the thickness of TGO in the Yb2Si2O7 coating is about 6 μm.

[0095] Comparative Example 1D: Figure 5B Shown is a SEM image of a Yb2Si2O7 coating evaluated after exposure to 90 vol% H2O-10 vol% air at 1316°C for 510 h. Figure 5B In the SEM image, it is shown that the thickness of TGO in the Yb2Si2O7 coating is about 13.5 μm.

[0096] Example 1C: Figure 5C Shown is a SEM image of a Yb2Si2O7-sodium calcium magnesium aluminum silicate coating evaluated after exposure to 90 vol% H2O-10 vol% air at 1316°C for 170 h. Figure 5C In the SEM image, it is shown that the thickness of TGO in the Yb2Si2O7-sodium calcium magnesium aluminum silicate coating is about 0.67 μm.

[0097] Example 1D: Figure 5D Shown is a SEM image of a Yb2Si2O7-sodium calcium magnesium aluminum silicate coating evaluated after exposure to 90 vol% H2O-10 vol% air at 1316°C for 510 h. Figure 5D In the SEM image, it is shown that the TGO thickness in the Yb2Si2O7-sodium calcium magnesium aluminum silicate coating is about 1.1 μm.

[0098] Figure 6 is a graph showing the TGO thickness of Yb2Si2O7 coating and APSYb2Si2O7-sodium calcium magnesium aluminum silicate coating as a function of exposure (time) at 1316°C in 90 vol% H2O-10 vol% air. Figure 6 The TGO growth rate in the EBC containing low melting temperature sodium calcium magnesium aluminum silicate is about 10 times slower than that in the Yb2Si2O7 coating.

[0099] Example 2: Figure 7 SEM images of a high melting temperature matrix powder 720 composed of Metco 6157Yb2Si2O7 having a high melting temperature of about 1850°C and a low melting temperature powder 730 composed of Li2O having a melting temperature of about 1438°C are shown. Figure 7 In the figure, the bright phase is Yb2Si2O7 and the dark phase is Li2O powder.

[0100] Example 2A: Fig. 8A The SEM image of the sprayed APS Yb2Si2O7-0.4wt%Li2O coating is shown. Fig. 8A , the SEM image shows microcracks 810 . Fig. 8A The distribution of Li2O 820 in the Yb2Si2O7 matrix is ​​also shown.

[0101] Example 2B: Figure 8B SEM images of heat-treated APS Yb2Si2O7-0.4wt%Li2O coatings are shown. Figure 8B In Figure 2, the SEM images show that the microcracks disappear and the coating becomes densified in the APS Yb2Si2O7-0.4wt%Li2O coating after heat treatment at 1300℃ for 10 hours.

[0102] Comparative Example 2A: Fig. 9A Shown is a SEM image of a Yb2Si2O7 coating evaluated after exposure to 90 vol% H2O-10 vol% air at 1316°C for 410 h. Fig. 9A In the SEM image, it is shown that the thickness of TGO in the Yb2Si2O7 coating is about 11.3 μm.

[0103] Example 2C: Fig. 9B Shown is a SEM image of a Yb2Si2O7-0.4wt%Li2O coating evaluated after exposure to 90vol%H2O-10vol% air at 1316°C for 410 hours. Fig. 9B In the SEM image, it is shown that the thickness of TGO in the Yb2Si2O7-0.4wt%Li2O coating is about 6.5μm.

[0104] Further, at least because the invention is disclosed herein in a manner that enables it to be made and used with the aid of the disclosure of specific exemplary embodiments, the invention can be implemented in the absence of any additional elements or additional structures not specifically disclosed herein, for example, for simplicity or efficiency.

[0105] It should be noted that the foregoing examples are provided for the purpose of explanation only and are in no way to be construed as limitations on the present invention. Although the present invention has been described with reference to exemplary embodiments, it should be understood that the words used herein are descriptive and illustrative, rather than restrictive. Within the scope of the appended claims, changes as currently described and as modified may be made without departing from the scope and spirit of the present disclosure in its various aspects. Although the present invention has been described herein with reference to specific means, materials, and embodiments, the present invention is not intended to be limited to the details disclosed herein; on the contrary, the present invention extends to all functionally equivalent structures, methods, and uses, such as within the scope of the appended claims.

Claims

1. A thermal spraying material raw material, comprising: (a) a first powder comprising at least one low melting temperature material having a melting temperature of less than 1500° C.; and (b) A second powder comprising at least one environmental barrier coating matrix material.

2. The thermal spraying material raw material according to claim 1, wherein: The at least one low melting temperature material is a single oxide compound, a binary oxide, a ternary oxide, or a multi-element oxide.

3. The thermal spray material feedstock according to any one of the preceding claims, wherein: The low melting temperature material is a multi-component oxide including at least four oxides having a melting temperature lower than 1300°C.

4. The thermal spray material feedstock according to any one of the preceding claims, wherein: The at least one environmental barrier coating matrix material includes at least one high melting temperature matrix material selected from the group consisting of rare earth silicates, rare earth oxides, mullite, alkali silicates, HfO2, HfSiO4, HfTiO4, ZrTiO4, ZrSiO4, rare earth oxide-stabilized zirconium oxide, rare earth oxide-stabilized hafnium oxide, HfB2, HfC, ZrB2, ZrC and SiC.

5. The thermal spray material feedstock according to any one of the preceding claims, wherein: The first powder and the second powder are mixed, agglomerated, agglomerated and sintered, plasma densified, or fused and crushed.

6. The thermal spray material feedstock according to any one of the preceding claims, wherein: The at least one low melting temperature material includes: CaO, MgO, Al2O3, SiO2, Na2O, K2O and Fe2O3.

7. The thermal spray material raw material according to any one of claims 1, 2, 4 and 5, wherein: The at least one low melting temperature material is Li2O.

8. An environmental barrier coating (EBC), comprising: (I) EBC top coating, comprising: (i) an EBC matrix comprising at least one selected from the group consisting of rare earth silicates, rare earth oxides, mullite, alkali silicates, HfO2, HfSiO4, HfTiO4, ZrTiO4, ZrSiO4, rare earth oxide-stabilized zirconia, rare earth oxide-stabilized hafnium oxide, HfB2, HfC, ZrB2, ZrC, and SiC; and (ii) at least one low melting temperature material having a melting temperature of less than 1500° C. embedded in the EBC matrix; and (II) Si-based bond coating.

9. The environmental barrier coating of claim 8, wherein: The at least one low melting temperature material includes: CaO, MgO, Al2O3, SiO2, Na2O, K2O and Fe2O 3。 10. The environmental barrier coating of claim 8, wherein: The at least one low melting temperature material is Li2O.

11. The environmental barrier coating according to any one of claims 8 to 10, wherein The EBC matrix includes at least one rare earth silicate, which includes at least one rare earth element selected from the group consisting of Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu.

12. The environmental barrier coating according to any one of claims 8 to 10, wherein The EBC matrix includes at least one rare earth oxide, which includes at least one rare earth element selected from the group consisting of Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu.

13. The environmental barrier coating according to any one of claims 8 to 12, wherein The concentration of the at least one low melting temperature material in the EBC matrix is ​​in a range of 0.1 wt % to 40 wt % based on the total weight of the EBC top coating layer.

14. The environmental barrier coating according to any one of claims 8 to 13, wherein The concentration of the at least one low melting temperature material in the EBC matrix is ​​in a range of 0.4 wt % to 10 wt % based on the total weight of the EBC top coating layer.

15. The environmental barrier coating according to any one of claims 8 to 14, wherein The concentration of the at least one low melting temperature material in the EBC matrix is ​​in a range of 0.4 wt % to 5.0 wt % based on the total weight of the EBC top coating layer.

16. A method for applying an EBC on a Si-based CMC, comprising: The EBC of claim 8 is deposited on the Si-based CMC.

17. The method according to claim 16, wherein: The deposition is performed by air plasma spraying (APS), high velocity oxy-fuel spraying (HVOF), combustion spraying, vacuum plasma spraying or suspension thermal spraying.

18. An EBC top coating comprising: (i) an EBC matrix comprising at least one selected from the group consisting of rare earth silicates, rare earth oxides, mullite, alkali silicates, HfO2, HfSiO4, HfTiO4, ZrTiO4, ZrSiO4, rare earth oxide-stabilized zirconia, rare earth oxide-stabilized hafnium oxide, HfB2, HfC, ZrB2, ZrC, and SiC; and (ii) at least one low melting temperature material having a melting temperature less than 1500°C embedded in the EBC matrix.

Citation Information

Cited By

  • Ceramic coating for high-level radioactive nuclide glass curing smelting furnace and preparation method of ceramic coating

    CN121517226A