Vulcanization adhesive composition, vulcanization adhesive laminate composition, and laminate using same

By laminating compositions such as epihaloalcohol rubber, acrylate without hydroxyl groups and fluoroelastomer in the vulcanized bonding composition, the problem of poor adhesion under the vapor vulcanization method is solved, and the epihalogen is realized The firm bond between alcohol-solved rubber and fluoroelastomer is suitable for steam vulcanization process.

CN118891338APending Publication Date: 2024-11-01OSAKA SODA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026788.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-24
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, the vulcanized rubber laminate prepared by the vapor vulcanization method has poor adhesion and the increased use of alcohol-containing gasoline has resulted in poor bisphenol cross-linking system, making it difficult to achieve a firm bond between epihalogenated alcohol rubber and fluoroelastomer.

Method used

The vulcanized bonding composition and peroxide are used, including an epihaloalcohol rubber, acrylate with three or more functions and five or less functions without hydroxyl groups, an epoxy resin, a dibutyl dithiocarbamate, and a vulcanizing agent. The vulcanized adhesive laminate formed by a fluoro-rubber laminate is formed by a vulcanized agent, and the adhesiveness is improved by a co-crosslinking agent.

Benefits of technology

Even under the steam vulcanization molding method, firm bonding between the rubber layer and the fluoroelastic layer can be achieved, and the adhesion of the laminated body is improved, and it is suitable for steam vulcanization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005036754300000081
    Figure BDA0005036754300000081
  • Figure BDA0005036754300000211
    Figure BDA0005036754300000211
  • Figure BDA0005036754300000221
    Figure BDA0005036754300000221
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a composition for a vulcanization-bonded laminate in which an epichlorohydrin rubber and a fluororubber are firmly bonded; and a laminate using the composition. Disclosed is a composition for a vulcanized adhesive laminate, which is obtained by laminating a rubber layer (A) and a fluororubber layer (B), to obtain a laminate in which the rubber layer (A) and the fluororubber layer (B) are firmly adhered. The rubber layer (A) is formed from a vulcanization adhesive composition containing at least an epichlorohydrin rubber, a trifunctional to pentafunctional acrylate having no hydroxyl group, an epoxy resin, nickel dibutyldithiocarbamate, and a vulcanizing agent, and the fluororubber layer (B) is formed from a fluororubber composition containing at least a peroxide-based vulcanizing agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a vulcanization adhesive composition, a vulcanization adhesive laminate composition using the same, and a laminate using the same. Background Art

[0002] In recent years, due to the improvement of environmental awareness, the law for preventing fuel volatilization has been promoted and improved, especially in the automotive industry, with the United States as the center, the tendency of fuel volatilization suppression is significant, and the demand for materials with excellent fuel barrier properties is increasing. In order to make the fuel barrier property good, laminated hoses with fluororesin as barrier layers (rubber outside the barrier layer) are widely used, but fluororesin lacks flexibility and therefore cannot follow the flexibility of the laminated rubber, and there is a fear that the adhesion will be reduced. Such hoses are mostly formed by steam vulcanization. It is known that steam vulcanization usually has poor adhesion compared to pressurized vulcanization, and it is required to improve the adhesion based on steam vulcanization. In addition, in addition to evaporation restrictions, due to the increase in the use of alcohol-containing gasoline, it has also become a problem to cause adverse conditions in the bisphenol cross-linking system.

[0003] Therefore, in Patent Document 1, a vulcanized rubber laminate is provided, which is a vulcanized rubber laminate formed by heating and bonding an unvulcanized epihalohydrin rubber composition layer and an unvulcanized fluororubber composition layer, wherein the unvulcanized epihalohydrin rubber composition comprises a multifunctional (meth)acrylate compound having two or more (meth)acryloyl groups in the molecule and a vulcanizing agent, and the unvulcanized fluororubber composition contains an organic peroxide vulcanizing agent. In Patent Documents 2 to 4, a technology is provided for improving the adhesion of a laminate composition containing an epihalohydrin polymer and a compound having a vinyl group, a diazabicyclic compound, an epoxy resin, and a metal salt hydrate to a fluororesin, wherein epoxy resin and a metal salt hydrate are used as components for improving adhesion to the fluororesin.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 5499713

[0007] Patent Document 2: Japanese Patent No. 6954272

[0008] Patent Document 3: Japanese Patent No. 5955222

[0009] Patent Document 4: International Publication No. 2018 / 135367 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] An object of the present invention is to provide a vulcanization adhesive composition in which an epihalohydrin rubber and a fluororubber are firmly bonded to each other, a vulcanization adhesive laminate composition, and a laminate using the same.

[0012] Solutions for solving problems

[0013] The inventors of the present invention have conducted various studies to achieve the above-mentioned purpose, and found that a composition for vulcanized adhesive laminated body formed by laminating a rubber layer (A) formed by a vulcanized adhesive composition comprising at least (a1) epihalohydrin rubber, (a2) acrylate having more than 3 functions and less than 5 functions without hydroxyl groups, (a3) ​​epoxy resin, (a4) nickel dibutyl dithiocarbamate and (a5) a vulcanizing agent and a fluororubber layer (B) formed by a fluororubber composition comprising at least a peroxide-based vulcanizing agent, can obtain a laminated body in which the rubber layer (A) and the fluororubber layer (B) are firmly bonded, even when vulcanized by a steam vulcanization molding method known to have poor adhesion, thereby completing the present invention. In addition, when vulcanized by a steam vulcanization molding method, it is speculated that the adhesion between the epihalohydrin rubber and the fluororubber is poor due to the influence of steam in direct contact with the rubber.

[0014] That is, the aspects of the present invention are as follows.

[0015] Item 1. A vulcanized adhesive composition comprising, relative to 100 parts by mass of (a1) epihalohydrin rubber, at least 2 to 7 parts by mass of (a2) a trifunctional or higher and pentafunctional or lower acrylate having no hydroxyl group, 0.5 to 3 parts by mass of (a3) ​​an epoxy resin, 0.2 to 3 parts by mass of (a4) nickel dibutyl dithiocarbamate, and 0.1 to 10 parts by mass of (a5) a vulcanizing agent.

[0016] Item 2. The vulcanization adhesive composition according to Item 1, wherein the (a1) epihalohydrin rubber is at least one selected from the group consisting of an epihalohydrin-ethylene oxide copolymer, an epihalohydrin-propylene oxide copolymer, an epihalohydrin-allyl glycidyl ether copolymer, an epihalohydrin-ethylene oxide-allyl glycidyl ether terpolymer, an epihalohydrin-propylene oxide-allyl glycidyl ether terpolymer, and an epihalohydrin-ethylene oxide-propylene oxide-allyl glycidyl ether tetrapolymer.

[0017] Item 3. The vulcanization adhesive composition according to Item 1 or 2, wherein the (a2) trifunctional or higher and pentafunctional or lower acrylate having no hydroxyl group is at least one selected from the group consisting of trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and di(trimethylolpropane)tetraacrylate.

[0018] Item 4. The vulcanization adhesive composition according to any one of Items 1 to 3, wherein the epoxy resin (a3) ​​is a bisphenol A epoxy resin.

[0019] Item 5. The vulcanized adhesive composition according to any one of Items 1 to 4, wherein the (a5) vulcanizing agent is at least one selected from the group consisting of thiourea vulcanizing agents, quinoxaline vulcanizing agents, sulfur vulcanizing agents, peroxide vulcanizing agents, mercaptotriazine vulcanizing agents, and bisphenol vulcanizing agents.

[0020] Item 6. A composition for a vulcanizable adhesive laminate, comprising a laminate of a rubber layer (A) formed from the vulcanizable adhesive composition according to any one of Items 1 to 5 and a fluororubber layer (B) formed from a fluororubber composition containing at least a peroxide vulcanizing agent.

[0021] Item 7. A laminate obtained by vulcanizing the composition for a vulcanizable adhesive laminate according to Item 6.

[0022] Item 8. A catheter or a hose formed from the laminate according to Item 7.

[0023] Effects of the Invention

[0024] The vulcanization adhesive composition and the vulcanization adhesive laminate composition of the present invention can provide a laminate having high adhesive strength even in the case of a steam vulcanization molding method. DETAILED DESCRIPTION

[0025] <Composition for vulcanized adhesive laminate>

[0026] The composition for vulcanized adhesive laminated body of the present invention is composed of a layer formed by the composition for vulcanized adhesive (hereinafter referred to as rubber layer (A)) and a layer formed by a fluororubber composition (hereinafter referred to as fluororubber layer (B)), wherein the composition for vulcanized adhesive comprises at least an epihalohydrin rubber, an acrylate having more than 3 functions and less than 5 functions without a hydroxyl group, an epoxy resin, nickel dibutyl dithiocarbamate and a vulcanizing agent, and the fluororubber composition comprises at least a peroxide-based vulcanizing agent. Here, the composition for vulcanized adhesive laminated body is composed of a rubber layer (A) and a fluororubber layer (B), which means that, typically, a rubber layer (A) and a fluororubber layer (B) are stacked in the composition for vulcanized adhesive laminated body. It should be noted that, in the composition for vulcanized adhesive laminated body, as long as the rubber layer (A) and the fluororubber layer (B) are in contact at least partially, it may also have a layer other than the rubber layer (A) and the fluororubber layer (B).

[0027] The above-mentioned composition can obtain the above-mentioned effects. Although the reason why such effects are obtained is not necessarily clear, it is presumed as follows.

[0028] Usually, epihalohydrin rubber and fluororubber are incompatible on the bonding interface during vulcanization, so adhesion cannot be obtained.Therefore, by mixing co-crosslinking agent respectively in epihalohydrin rubber, these two rubber layers of fluororubber and crosslinking, adhesion can be shown.As co-crosslinking agent, polyfunctional acrylate such as pentaerythritol triacrylate, polyfunctional allyl compound such as triallyl isocyanurate are usually used, and these co-crosslinking agents play a role as the crosslinking point with two rubber layers.But, in the case of using acrylate with hydroxyl in the molecule such as pentaerythritol triacrylate as co-crosslinking agent, in the reaction between co-crosslinking agents in the bonding interface layer, if the anti-aging agent with the highest versatility in the rubber field, i.e. nickel dibutyl dithiocarbamate, is present in the rubber layer, then free radicals can be captured during reaction, and the hydroxyl of pentaerythritol triacrylate can work as chain transfer agent in addition, and the possibility of reducing the ability of co-crosslinking agent is high. Therefore, when using an acrylate having a hydroxyl group such as pentaerythritol triacrylate as a co-crosslinking agent, nickel dibutyl dithiocarbamate is not used or other antioxidants are used instead, but there is a concern that heat resistance may be reduced. In this regard, the present invention has found that a composition for a vulcanized adhesive laminate having sufficient adhesive strength can be obtained by using a polyfunctional acrylate having no hydroxyl group even when nickel dibutyl dithiocarbamate is used.

[0029] In addition, the acrylate with more than 3 functions and less than 5 functions of hydroxyl does not include the hydroxyl that may capture free radicals and consume, and then more than 3 functions, so the reactivity is very high, in addition, because it is less than 5 functions, it is also possible to prevent crosslinking from becoming too dense. And, by mixing epoxy resin with this acrylate, thus due to the influence of the compatibility of epihalohydrin rubber, epoxy resin, acrylate, acrylate is locally present on the composition surface. Like this, by epihalohydrin rubber, epoxy resin, acrylate with more than 3 functions and less than 5 functions of hydroxyl, the synergistic effect of these three, the acrylate with more than 3 functions and less than 5 functions of reactivity is very high, and is locally present on the composition surface, and plays the firm adhesion with fluororubber. It should be noted that such action function is the unique action function of the acrylate with more than 3 functions and less than 5 functions of hydroxyl, and surprisingly, the methacrylate with more than 3 functions and less than 5 functions of hydroxyl cannot play such action function.

[0030] As mentioned above, the composition for vulcanization bonding comprising (a1) epihalohydrin rubber, (a2) acrylates having more than 3 functions and less than 5 functions without hydroxyl groups, (a3) ​​epoxy resin, (a4) nickel dibutyl dithiocarbamate and (a5) vulcanizing agent exerts a strong adhesion with fluororubber. Therefore, the composition for vulcanization bonding laminate formed by the rubber layer (A) and the fluororubber layer (B) exerts a strong adhesion at the interface of the rubber layer (A) and the fluororubber layer (B), so even when vulcanized by a steam vulcanization molding method with poor known adhesion, a laminate having a strong adhesion of the rubber layer (A) and the fluororubber layer (B) can be obtained. In this way, the composition for vulcanization bonding of the present invention and the composition for vulcanization bonding laminate are suitable for steam vulcanization purposes.

[0031] In addition, usually, in the vulcanization of fluororubber, the method using peroxide vulcanizing agent and the method using bisphenol vulcanizing agent are known, and it is known that in the method using peroxide vulcanizing agent, the adhesion of epihalohydrin rubber to fluororubber is low. The composition for vulcanization bonding of the present invention is due to the strong adhesion with fluororubber, so for the fluororubber composition comprising peroxide vulcanizing agent, good adhesion can also be obtained. Of course, even when using the fluororubber composition comprising peroxide vulcanizing agent and vulcanizing by steam vulcanization molding method, strong adhesion with fluororubber can also be obtained.

[0032] <Rubber layer (A)>

[0033] The rubber layer (A) of the present invention is a layer formed of a vulcanization adhesive composition, wherein the vulcanization adhesive composition contains at least: (a1) epihalohydrin rubber, (a2) a trifunctional or higher and pentafunctional or lower acrylate having no hydroxyl group, (a3) ​​an epoxy resin, (a4) nickel dibutyl dithiocarbamate, and (a5) a vulcanizing agent.

[0034] The (a1) epihalohydrin rubber used in the present invention is not limited as long as it is a rubber having a binary copolymer or more of a structural unit derived from an epihalohydrin and a structural unit derived from other components. Examples of the structural unit derived from other components include: at least one structural unit derived from alkylene oxides such as ethylene oxide, propylene oxide, and n-butylene oxide, and glycidyls such as methyl glycidyl ether, ethyl glycidyl ether, n-glycidyl ether, allyl glycidyl ether, and phenyl glycidyl ether; more specifically, examples include: an epihalohydrin-ethylene oxide copolymer, an epihalohydrin-propylene oxide copolymer, an epihalohydrin-allyl glycidyl ether copolymer, an epihalohydrin-ethylene oxide-allyl glycidyl ether terpolymer, an epihalohydrin-propylene oxide-allyl glycidyl ether terpolymer, and an epihalohydrin-ethylene oxide-propylene oxide-allyl glycidyl ether tetrapolymer. Among them, preferably epihalohydrin-ethylene oxide copolymer, epihalohydrin-allyl glycidyl ether copolymer, epihalohydrin-ethylene oxide-allyl glycidyl ether terpolymer, more preferably epihalohydrin-allyl glycidyl ether copolymer, epihalohydrin-ethylene oxide-allyl glycidyl ether terpolymer. These copolymers can be used alone or in combination of two or more.

[0035] As epihalohydrin rubber, from the aspect of heat resistance, preferably contain more than the structural unit 10mol% that is derived from epihalohydrin, more preferably contain more than 20mol%, particularly preferably contain more than 25mol%.For the structural unit that is derived from epihalohydrin, can be calculated by the content of halogen atoms such as chlorine etc.The content of halogen atoms such as chlorine can be obtained by potentiometric titration according to the method for recording in JISK7229.

[0036] In the case of epihalohydrin-ethylene oxide copolymer, the lower limit of the structural unit derived from epihalohydrin is preferably more than 10mol%, more preferably more than 20mol%, particularly preferably more than 25mol%, and the upper limit is preferably below 95mol%, more preferably below 75mol%, and particularly preferably below 65mol%. The lower limit of the structural unit derived from ethylene oxide is preferably more than 5mol%, more preferably more than 25mol%, particularly preferably more than 35mol%, and the upper limit is preferably 90mol%, more preferably below 80mol%, and particularly preferably below 75mol%.

[0037] In the case of epihalohydrin-ethylene oxide-allyl glycidyl ether terpolymer, the lower limit of the structural unit derived from epihalohydrin is preferably 10mol% or more, more preferably 20mol% or more, particularly preferably 25mol% or more, and the upper limit is preferably 95mol% or less, more preferably 75mol% or less, and particularly preferably 65mol% or less. The lower limit of the structural unit derived from ethylene oxide is preferably 4mol% or more, more preferably 24mol% or more, particularly preferably 34mol% or more, and the upper limit is preferably 89mol% or less, more preferably 79mol% or less, and particularly preferably 74mol% or less. The lower limit of the structural unit derived from allyl glycidyl ether is preferably 1mol% or more, and the upper limit is preferably 10mol% or less, more preferably 8mol% or less, and particularly preferably 7mol% or less.

[0038] The copolymerization composition of epihalohydrin-ethylene oxide copolymer, epihalohydrin-ethylene oxide-allyl glycidyl ether terpolymer is obtained by the content of halogen atoms such as chlorine, iodine value.The content of halogen atoms such as chlorine is measured by potentiometric titration according to the method for recording in JIS K7229.The mole fraction of the structural unit based on epihalohydrin is calculated by the content of halogen atoms such as chlorine obtained.Iodine value is measured by the method based on JIS K6235.The mole fraction of the structural unit based on allyl glycidyl ether is calculated by the iodine value obtained.The mole fraction of the structural unit based on ethylene oxide is calculated by the mole fraction of the structural unit based on epihalohydrin, the mole fraction of the structural unit based on allyl glycidyl ether.

[0039] Examples of the epihalohydrin include epichlorohydrin and epibromohydrin, and epichlorohydrin is preferred.

[0040] As (a2) acrylates having three or more functions and five or less functions (preferably three or more functions and four or less functions) without hydroxyl groups, for example, trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, isocyanuric acid triacrylate, glycerol triacrylate, ethoxylated glycerol triacrylate, propoxylated glycerol triacrylate, pentaerythritol tetraacrylate, ethoxylated pentaerythritol tetraacrylate, propoxylated pentaerythritol tetraacrylate, di(trimethylolpropane) tetraacrylate, ethoxylated di(trimethylolpropane) tetraacrylate, propoxylated di(trimethylolpropane) tetraacrylate, etc. are listed. Among them, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and di(trimethylolpropane) tetraacrylate are preferably used, and trimethylolpropane triacrylate and pentaerythritol tetraacrylate are more preferred. These can be used alone, or two or more can be used in combination.

[0041] In the composition for vulcanization adhesive, the lower limit of the amount of the (a2) trifunctional or higher and pentafunctional acrylate having no hydroxyl group is preferably 2 parts by mass or more, more preferably 3 parts by mass or more, and further preferably 4 parts by mass or more, with respect to 100 parts by mass of the (a1) epihalohydrin rubber, and the upper limit is preferably 7 parts by mass or less, more preferably 6.5 parts by mass or less, and further preferably 6 parts by mass or less. When the amount is less than the lower limit, the effect as a co-crosslinking agent with the fluororubber layer (B) is small, and when the amount is more than the upper limit, crosslinking between the acrylates is dominant, and it may not function as a co-crosslinking agent.

[0042] (a3) Epoxy resin is preferably at least one resin selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, phenol novolac epoxy resin, o-cresol novolac epoxy resin, amine epoxy resin, hydrogenated bisphenol A epoxy resin and multifunctional epoxy resin. They can be used alone or in combination of two or more. Among them, bisphenol A epoxy resin is preferred from the perspective of good chemical resistance and adhesion.

[0043] More preferably, an epoxy resin represented by the following formula (1) is used: In the formula (1), n ​​is an average value, and is preferably 0.1 to 3, more preferably 0.1 to 0.5, and even more preferably 0.1 to 0.3.

[0044]

[0045] In the vulcanization adhesive composition, from the viewpoint of further improving the adhesion to the fluororubber layer (B), the lower limit of the amount of the epoxy resin (a3) ​​compounded relative to 100 parts by mass of the epihalohydrin rubber (a1) is preferably 0.3 parts by mass or more, more preferably 0.4 parts by mass or more, and even more preferably 0.5 parts by mass or more, and the upper limit is preferably 3 parts by mass or less, more preferably 2.5 parts by mass or less, and even more preferably 2 parts by mass or less.

[0046] In the composition for vulcanization bonding, the amount of nickel dibutyl dithiocarbamate (a4) is not limited as long as it is used as an anti-aging agent. The lower limit is preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, and further preferably 0.5 parts by mass or more, relative to 100 parts by mass of the epihalohydrin rubber (a1). The upper limit is preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and further preferably 1.5 parts by mass or less.

[0047] As (a5) vulcanizing agent, any vulcanizing agent commonly used in the rubber field can be used according to the application, and examples thereof include: polyamine vulcanizing agent, thiourea vulcanizing agent, thiadiazole vulcanizing agent, mercaptotriazine vulcanizing agent, pyrazine vulcanizing agent, quinoxaline vulcanizing agent, bisphenol vulcanizing agent, sulfur vulcanizing agent, peroxide vulcanizing agent, resin vulcanizing agent, quinonedioxime vulcanizing agent, etc. These can be used alone or in combination of two or more.

[0048] Examples of the polyamine vulcanizing agent include ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, hexamethylenetetramine, p-phenylenediamine, isopropylphenylenediamine, N,N′-biscinnamaldehyde-1,6-hexanediamine, ethylenediamine carbamate, and hexamethylenediamine carbamate.

[0049] Examples of the thiourea-based vulcanizing agent include ethylenethiourea, 1,3-diethylthiourea, 1,3-dibutylthiourea, and trimethylthiourea.

[0050] Examples of the thiadiazole-based vulcanizing agent include 2,5-dimercapto-1,3,4-thiadiazole and 2-mercapto-1,3,4-thiadiazole-5-thiobenzoate.

[0051] Examples of the mercaptotriazine-based vulcanizing agent include 2,4,6-trimercapto-1,3,5-triazine, 2-methoxy-4,6-dimercaptotriazine, 2-hexylamino-4,6-dimercaptotriazine, 2-diethylamino-4,6-dimercaptotriazine, 2-cyclohexylamino-4,6-dimercaptotriazine, 2-dibutylamino-4,6-dimercaptotriazine, 2-anilino-4,6-dimercaptotriazine, and 2-phenylamino-4,6-dimercaptotriazine.

[0052] Examples of the pyrazine-based vulcanizing agent include 2,3-dimercaptopyrazine derivatives. Examples of 2,3-dimercaptopyrazine derivatives include pyrazine-2,3-dithiocarbonate, 5-methyl-2,3-dimercaptopyrazine, 5-ethylpyrazine-2,3-dithiocarbonate, 5,6-dimethyl-2,3-dimercaptopyrazine, and 5,6-dimethylpyrazine-2,3-dithiocarbonate.

[0053] Examples of the quinoxaline-based vulcanizing agent include 2,3-dimercaptoquinoxaline derivatives. Examples of 2,3-dimercaptoquinoxaline derivatives include quinoxaline-2,3-dithiocarbonate, 6-methylquinoxaline-2,3-dithiocarbonate, 6-ethyl-2,3-dimercaptoquinoxaline, 6-isopropylquinoxaline-2,3-dithiocarbonate, and 5,8-dimethylquinoxaline-2,3-dithiocarbonate.

[0054] Examples of the bisphenol-based vulcanizing agent include 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfone (bisphenol S), 1,1-bis(4-hydroxyphenyl)cyclohexane, 2-chloro-1,4-cyclohexylene-bis(4-hydroxybenzene), 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), bis(4-hydroxyphenyl)hexafluoroisopropane (bisphenol AF), and 2-fluoro-1,4-phenylene-bis(4-hydroxybenzene).

[0055] Examples of the sulfur-based vulcanizing agent include sulfur, morpholine disulfide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, N,N'-dimethyl-N,N'-diphenylthiuram disulfide, dipentamethylenethiuram tetrasulfide, dipentamethylenethiuram tetrasulfide, and dipentamethylenethiuram hexasulfide.

[0056] Examples of the peroxide-based vulcanizing agent include tert-butyl hydroperoxide, p-terpene hydroperoxide, diisopropylbenzene peroxide, tert-butyl peroxide, 1,3-bis(tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, benzoyl peroxide, and tert-butyl peroxybenzoate.

[0057] Examples of the resin-based vulcanizing agent include alkylphenol formaldehyde resins and the like.

[0058] Examples of the quinone dioxime-based vulcanizing agent include p-quinone dioxime and p,p′-dibenzoylquinone dioxime.

[0059] In the rubber layer (A) of the present invention, at least one vulcanizing agent selected from the group consisting of thiourea vulcanizing agents, quinoxaline vulcanizing agents, sulfur vulcanizing agents, peroxide vulcanizing agents, mercaptotriazine vulcanizing agents and bisphenol vulcanizing agents is preferred, at least one vulcanizing agent selected from the group consisting of thiourea vulcanizing agents, quinoxaline vulcanizing agents and bisphenol vulcanizing agents is more preferred, and quinoxaline vulcanizing agents are particularly preferred.

[0060] In the composition for vulcanization adhesive, the lower limit of the amount of the vulcanizing agent (a5) is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, further preferably 0.5 parts by mass or more, and particularly preferably 1 parts by mass or more, relative to 100 parts by mass of the epihalohydrin rubber (a1). As the upper limit, it is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and further preferably 3 parts by mass or less.

[0061] In the rubber layer (A) of the present invention, a known vulcanization accelerator, vulcanization accelerating auxiliary, or retarder may be used as it is in the present invention together with the vulcanizing agent (a5). Examples of the vulcanization accelerator used in combination with the vulcanizing agent (a5) include primary amines, secondary amines, tertiary amines, organic acid salts of the amines or adducts thereof, diazabicyclic vulcanization accelerators, guanidine vulcanization accelerators, thiuram vulcanization accelerators, dithiocarbamic acid vulcanization accelerators, aldehyde-amine vulcanization accelerators, aldehyde-amine vulcanization accelerators, thiurea vulcanization accelerators, thiazole vulcanization accelerators, sulfenamide vulcanization accelerators, xanthate vulcanization accelerators and the like, vulcanization retarders such as N-nitrosodiphenylamine, phthalic anhydride, and N-cyclohexylthiophthalimide, vulcanization accelerating aids such as zinc oxide, stearic acid, and zinc stearate, and various crosslinking aids such as quinonedioxime crosslinking aids, methacrylate crosslinking aids, allyl crosslinking aids, and maleimide crosslinking aids. In addition, as a retarder, N-cyclohexanethiophthalimide and the like can be cited. They can be used alone, or two or more can be used in combination. Among them, a diazabicyclic vulcanization accelerator is preferred. The diazabicyclic vulcanization accelerator can promote the hydrolysis of the vulcanizing agent and inhibit the gelation of the highly reactive (a2) trifunctional or higher and pentafunctional or lower acrylates that do not have a hydroxyl group, so by mixing with the above (a1) to (a5), better adhesion can be obtained.

[0062] Specific examples of the diazabicyclo vulcanization accelerator include 1,8-diazabicyclo(5.4.0)undec-7-ene (DBU), 1,5-diazabicyclo(4.3.0)non-5-ene, 1,4-diazabicyclo(2.2.2)octane, p-toluenesulfonate, phenolate, phenolic resin salt, phthalate, formates, octanoates, naphthoates, etc. Of these, 1,8-diazabicyclo(5.4.0)undec-7-ene and phenolic resin salts and naphthoates of 1,8-diazabicyclo(5.4.0)undec-7-ene are preferred from the viewpoint of normal physical properties and heat resistance, and 1,8-diazabicyclo(5.4.0)undec-7-ene and phenolic resin salts of 1,8-diazabicyclo(5.4.0)undec-7-ene are more preferred.

[0063] In the vulcanization adhesive composition, the amount of the diazabicyclic vulcanization accelerator blended is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the epihalohydrin rubber (a1).

[0064] In the vulcanization adhesive composition, the amount of the vulcanization accelerator, vulcanization accelerator aid, crosslinking aid, and vulcanization retarder is preferably 0 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the (a1) epihalohydrin rubber.

[0065] In addition, in the rubber layer (A) of the present invention, any rubber such as nitrile rubber (NBR), hydrogenated NBR (H-NBR), acrylic rubber (ACM), ethylene acrylic rubber (AEM), fluororubber (FKM), chloroprene rubber (CR), chlorosulfonated polyethylene (CSM), chlorinated polyethylene (CPE), ethylene propylene rubber (EPM, EPDM) may be contained. They may be used alone or in combination of two or more. When these rubbers are mixed, the mixing amount is preferably 1 to 50 parts by mass relative to 100 parts by mass of the epihalohydrin rubber (a1).

[0066] The rubber layer (A) of the present invention may also contain other resins other than epoxy resin. As resins, for example, polymethyl methacrylate (PMMA) resin, polystyrene (PS) resin, polyurethane (PUR) resin, polyvinyl chloride (PVC) resin, ethylene-vinyl acetate (EVA) resin, styrene-acrylonitrile (AS) resin, polyethylene (PE) resin, etc. can be listed. They can be used alone, and more than two kinds can also be used in combination. When these resins are mixed, the mixing amount is preferably 1 to 50 parts by mass relative to 100 parts by mass of (a1) epihalohydrin rubber.

[0067] In addition, in the rubber layer (A) of the present invention, according to the purpose or need, as long as the effect of the present invention is not damaged, the common additives compounded in the common rubber composition can be compounded, such as fillers, processing aids, plasticizers, acid absorbers, softeners, anti-aging agents, colorants, stabilizers, bonding aids, mold release agents, conductivity imparting agents, thermal conductivity imparting agents, surface non-adhesives, thickeners, flexibility imparting agents, heat resistance improvers, flame retardants, ultraviolet light absorbers, oil resistance enhancers, foaming agents, scorch retarder, lubricants and other various additives. In addition, one or more commonly used vulcanizing agents and vulcanization accelerators different from the above-mentioned can also be compounded. They can be used alone, and in addition, more than two can also be used in combination.

[0068] As fillers, metal sulfides such as molybdenum disulfide, iron sulfide, and copper sulfide can be listed; diatomaceous earth, lithopone (zinc sulfide / barium sulfide), graphite, carbon black, silicon dioxide, carbon fluoride, calcium fluoride, coke, quartz powder, talc, mica powder, wollastonite, carbon fiber, aramid fiber, various whiskers, glass fiber, organic reinforcing agent, organic filler, etc. These fillers can be used alone or in combination of two or more.

[0069] In the composition for vulcanization bonding, relative to 100 parts by mass of (a1) epihalohydrin rubber, the lower limit of the amount of filler is preferably more than 5 parts by mass, more preferably more than 10 parts by mass, and further preferably more than 20 parts by mass. As the upper limit, preferably less than 150 parts by mass, more preferably less than 100 parts by mass, and further preferably less than 75 parts by mass. If the filler is set outside these ranges, it is possible to cause adverse effects on compression set.

[0070] As processing aids, there can be listed higher fatty acids such as stearic acid, oleic acid, palmitic acid, and lauric acid; higher fatty acid salts such as sodium stearate and zinc stearate; higher fatty acid amides such as stearic acid amide and oleic acid amide; higher fatty acid esters such as ethyl oleate, higher fatty amines such as stearylamine and oleylamine; petroleum waxes such as carnauba wax and ceresin; polyethylene glycols such as ethylene glycol, glycerol, and diethylene glycol; aliphatic hydrocarbons such as vaseline and paraffin; silicone oils, silicone polymers, low molecular weight polyethylene, phthalate esters, phosphate esters, rosin, (halogenated) dialkylamines, (halogenated) dialkyl sulfones, surfactants, etc. These can be used alone or in combination of two or more.

[0071] In the vulcanized adhesive composition, the amount of the processing aid is preferably 1 to 10 parts by mass, more preferably 1.5 to 7.5 parts by mass, and even more preferably 2 to 5 parts by mass, based on 100 parts by mass of the epihalohydrin rubber (a1).

[0072] Examples of the plasticizer include phthalic acid derivatives such as dioctyl phthalate (bis(2-ethylhexyl)phthalate) and diallyl phthalate, adipic acid derivatives such as dibutyl diglycol monoadipate and di(butoxyethoxy)ethyl adipate, sebacic acid derivatives such as dioctyl sebacate, and trimellitic acid derivatives such as trioctyl trimellitate. These may be used alone or in combination of two or more.

[0073] In the vulcanization adhesive composition, the amount of the plasticizer blended is preferably 1 to 50 parts by mass, more preferably 1.5 to 30 parts by mass, and even more preferably 2 to 20 parts by mass, based on 100 parts by mass of the epihalohydrin rubber (a1).

[0074] As an antioxidant, in addition to (a4) nickel dibutyl dithiocarbamate, known antioxidants can also be used. As known antioxidants, amine antioxidants, phenolic antioxidants, benzimidazole antioxidants, dithiocarbamate antioxidants, thiourea antioxidants, organic thioacid antioxidants, and phosphite antioxidants can be exemplified, preferably dithiocarbamate antioxidants. They can be used alone, or two or more can be used in combination. In addition to (a4) nickel dibutyl dithiocarbamate, by also using (a4) nickel dibutyl dithiocarbamate other than nickel dibutyl dithiocarbamate, better heat resistance can be obtained, and the gelation of the acrylate with more than 3 functions and less than 5 functions that does not have a hydroxyl group (a2) with high reactivity can be suppressed, so by mixing with the above-mentioned (a1) to (a5), better adhesion can be obtained.

[0075] Specific examples of dithiocarbamate antioxidants include nickel diethyldithiocarbamate, nickel dimethyldithiocarbamate, nickel diisobutyldithiocarbamate, copper dimethyldithiocarbamate, copper diethyldithiocarbamate, copper dibutyldithiocarbamate, N-ethyl-N-phenyldithiocarbamate, copper N-pentamethylenedithiocarbamate, and copper dibenzyldithiocarbamate. Among them, copper dimethyldithiocarbamate is preferred.

[0076] In the vulcanization adhesive composition, the amount of the antioxidant (excluding the amount of the dithiocarbamate-based antioxidant other than the nickel dibutyl dithiocarbamate (preferably the nickel dibutyl dithiocarbamate (a4))) is preferably 0.01 to 3 parts by mass, more preferably 0.05 to 2 parts by mass, and even more preferably 0.075 to 1 part by mass, relative to 100 parts by mass of the epihalohydrin rubber (a1).

[0077] Examples of the acid absorbent include magnesium oxide, quicklime, zinc oxide, magnesium hydroxide, slaked lime, barium hydroxide, calcium carbonate, magnesium carbonate, barium carbonate, calcium silicate, calcium stearate, zinc stearate, tin stearate, calcium phosphite, calcium phthalate, tin oxide, basic tin phosphite and other metal compounds, synthetic hydrotalcites and the like. It should be noted that synthetic hydrotalcites are metal compounds having the general formula Mg x Al y (OH) 2x+3y-2 A compound represented by CO3·wH2O (wherein x represents a number from 1 to 10, y represents a number from 1 to 5, and w represents a real number), specifically, Mg 4.5 Al2(OH) 13 CO3·3.5H2O、Mg 4.5 Al2(OH) 13CO3、Mg4Al2(OH) 12 CO3·3.5H2O、Mg6Al2(OH) 16 CO3·4H2O、Mg5Al2(OH) 14 CO3·4H2O and Mg3Al2(OH) 10 CO3·1.7H2O, etc. These may be used alone or in combination of two or more.

[0078] In the vulcanization adhesive composition, the amount of the acid absorbent is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, and further preferably 1 to 10 parts by mass, relative to 100 parts by mass of the epihalohydrin rubber (a1). When the amount of the acid absorbent is too large, the hardness of the crosslinked rubber may become too high, and the Mooney viscosity of the vulcanization adhesive composition may increase, and there is a tendency for the compression set to decrease.

[0079] <Fluororubber layer (B)>

[0080] The fluororubber layer (B) used in the present invention is a layer formed of a fluororubber composition containing at least a peroxide-based vulcanizing agent in the fluororubber.

[0081] As the fluororubber used in the present invention, vinylidene fluoride-hexafluoropropylene binary copolymer, tetrafluoroethylene-hexafluoropropylene binary copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, vinylidene fluoride-perfluoroalkyl vinyl ether-tetrafluoroethylene terpolymer, tetrafluoroethylene-perfluoroethyl vinyl ether copolymer, tetrafluoroethylene-perfluoropropyl vinyl ether copolymer can be listed. They can be used alone, in addition, two or more kinds can also be used in combination. Among them, preferably containing vinylidene fluoride, vinylidene fluoride-hexafluoropropylene binary copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, vinylidene fluoride-perfluoroalkyl vinyl ether-tetrafluoroethylene terpolymer.

[0082] Examples of the peroxide-based vulcanizing agent include tert-butyl hydroperoxide, p-terpene hydroperoxide, diisopropylbenzene peroxide, tert-butyl peroxide, 1,3-bis(tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, benzoyl peroxide, tert-butyl peroxybenzoate, etc. These may be used alone or in combination of two or more.

[0083] In the fluororubber composition, the lower limit of the compounding amount of the peroxide-based vulcanizing agent is preferably 0.05 mass parts or more, more preferably 1.0 mass parts or more, relative to 100 mass parts of fluororubber. As the upper limit, it is preferably 10 mass parts or less, more preferably 5 mass parts or less. If it is lower than the lower limit, the crosslinking of the fluororubber cannot be fully carried out. In addition, if it exceeds the upper limit, it becomes over-crosslinked, and there is a tendency that the hardness of the crosslinked product becomes too high.

[0084] The fluororubber layer (B) used in the present invention may also use a co-crosslinking agent, for example, triallyl cyanurate, triallyl isocyanurate, 1,3,5-triacryloyl hexahydro-1,3,5-triazine (triacrylformal), triallyl trimellitate, N,N'-m-phenylene bismaleimide, dipropargyl terephthalate, diallyl phthalate, tetraallyl terephthalamide, triallyl phosphate, etc. These may be used alone or in combination of two or more. Among them, triallyl isocyanurate is preferably used.

[0085] In the fluororubber composition, the amount of the co-crosslinking agent is preferably not less than 0.1 parts by mass, more preferably not less than 0.5 parts by mass, and preferably not more than 10 parts by mass, more preferably not more than 5 parts by mass, per 100 parts by mass of the fluororubber.

[0086] According to the need, the usual additives mixed in the fluororubber composition may be mixed, for example, various additives such as fillers, processing aids, plasticizers, acid absorbers, softeners, anti-aging agents, colorants, stabilizers, adhesive aids, mold release agents, conductivity imparting agents, thermal conductivity imparting agents, surface non-adhesives, thickeners, flexibility imparting agents, heat resistance improvers, flame retardants, ultraviolet absorbers, oil resistance improvers, foaming agents, scorch retardants, lubricants, etc. These may be used alone or in combination of two or more.

[0087] As a method for compounding the vulcanized adhesive composition and the fluororubber composition, any means conventionally used in the field of polymer processing, for example, an open roll mill, a Banbury mixer, various kneading machines, etc., can be utilized.

[0088] The mixing step can be carried out according to the usual steps in the field of polymer processing. For example, the following steps can be used: first, only the polymer is kneaded, then the compounding agents other than the crosslinking agent and the crosslinking accelerator are added to prepare the A kneaded mixture, and then the crosslinking agent and the crosslinking accelerator are added to the B kneaded mixture.

[0089] <Method for preparing composition for vulcanized adhesive laminate>

[0090] As the manufacturing method of the composition for vulcanized adhesive laminated body in the present invention, for example, two rubber compositions (composition for vulcanized adhesive, fluororubber composition) are stacked by extrusion molding at the same time and extrusion molding successively. As the manufacturing method of the laminated body in the present invention, the composition for vulcanized adhesive laminated body is vulcanized, for example, there are the following methods, etc.: by extrusion molding at the same time and extrusion molding successively, two rubber compositions are stacked to obtain the composition for vulcanized adhesive laminated body, and then the composition for vulcanized adhesive laminated body is heated and vulcanized or heated and vulcanized, or a mold is used to heat and vulcanize the two rubber compositions while stacking. In addition, it is also possible to adopt a method in which the rubber composition of one is heated and flowed at a temperature that does not cause a vulcanization reaction, and then the two are stacked and fully heated and vulcanized. About the method for heating and vulcanizing the unvulcanized laminated body (composition for vulcanized adhesive laminated body) stacked by the above-mentioned extrusion molding, as a method for heating and vulcanizing, known methods such as steam tank, air bath, infrared, microwave, lead-clad vulcanization can be arbitrarily adopted. During vulcanization, the heating temperature is usually 100 to 200° C., and the heating time varies depending on the temperature, and is selected in the range of 0.5 to 300 minutes. As described above, the vulcanization adhesive composition and the vulcanization adhesive laminate composition of the present invention are suitable for steam vulcanization applications. In the case of steam vulcanization, the strong adhesion between the epihalohydrin rubber and the fluororubber is particularly significantly exerted. Therefore, the laminate of the present invention is preferably manufactured by steam vulcanizing the vulcanization adhesive composition and the vulcanization adhesive laminate composition of the present invention.

[0091] In view of excellent various physical properties, the laminate of the present invention preferably has a crosslinked product of a fluororubber composition as an inner layer and a crosslinked product of a vulcanized adhesive composition as an outer layer. In order to take advantage of the good adhesion of the vulcanized adhesive composition to the fluororubber composition, it is preferred that the crosslinked product of the fluororubber composition as the inner layer and the crosslinked product of the vulcanized adhesive composition as the outer layer are in contact at least partially.

[0092] The laminate of the present invention does not need to be incorporated into a particularly complicated process when the crosslinked product of the vulcanized adhesive composition and the crosslinked product of the fluororubber composition are stacked, and chemically firm bonding can be obtained when crosslinked, so even when exposed to severe conditions (such as being immersed in fuel oil), sufficient bonding strength is also provided. In addition, low-cost molding can be easily carried out, and formability is also good. In addition, since molding can be carried out by the common method such as extrusion molding, filmization can also be possible, and flexibility is also excellent. Therefore, the laminate of the present invention can be suitably used as a conduit or a hose formed by the laminate of the present invention.

[0093] When the laminate of the present invention is applied to a fuel oil hose, for example, a two-layer hose having a fluororubber (B) disposed in the inner layer of the hose and a rubber layer (A) disposed in the outer layer thereof, a three-layer hose having a braided reinforcement layer disposed in the outer layer thereof, or a four-layer hose having a rubber layer disposed in the outer layer thereof, etc. As the braided material used in the three-layer hose or the four-layer hose, a braided material of polyester fiber, polyamide fiber, glass fiber, vinylon fiber, cotton, etc. is generally used. In addition, as the material of the outermost layer used in the four-layer hose, in addition to the epihalohydrin rubber, a synthetic rubber having aging resistance, weather resistance, oil resistance, etc., such as ethylene acrylate rubber, chloroprene rubber, chlorinated polyethylene rubber, chlorosulfonated polyethylene, etc. is generally used.

[0094] The thus obtained composition for vulcanized adhesive laminates of the present invention has extremely excellent adhesion between the two vulcanized rubbers and a strong bonding surface. Therefore, it is very effective in applications where one surface is exposed to an environment requiring resistance to rancid gasoline, gasoline permeation, and alcohol-containing gasoline, and the other surface is exposed to an environment requiring resistance to aging, weathering, and gasoline, such as fuel hoses and feed hoses.

[0095] Example

[0096] Hereinafter, although Examples are given as representative examples, the present invention is not limited thereto.

[0097] The compounding agents used in Examples and Comparative Examples are shown below.

[0098] *1 "EPICHLOMER CG-105" made by Osaka Soda Co., Ltd.

[0099] *2 "EPICHLOMER C55" made by Osaka Soda Co., Ltd.

[0100] *3 "SEAST SO" manufactured by TOKAI CARBON CO., LTD.

[0101] *4 "ADK CIZER RS-107" manufactured by ADEKA Co., Ltd.

[0102] *5 "SPLENDER R-300" manufactured by Kao Corporation

[0103] *6 "STABIACE (registered trademark) HT-1" manufactured by Sakai Chemical Industry Co., Ltd.

[0104] *7 Kyowa Chemical Industry Co., Ltd. "Kyowamag #150"

[0105] *8 "P-152" made by Osaka Soda Co., Ltd.

[0106] *9 “Nocceler TTCu” manufactured by Ouchi Shinko Chemical Co., Ltd.

[0107] *10 "NOCRAC NBC" manufactured by Ouchi Shinko Chemical Co., Ltd.

[0108] *11 "LIGHTACRYLATE TMP-A" manufactured by Kyoeisha Chemical Co., Ltd.

[0109] *12MIWON's "M420"

[0110] *13 "DS CIZER MMK-08" made by Osaka Soda Co., Ltd.

[0111] *14 “LIGHT ESTER TMP” manufactured by Kyoeisha Chemical Co., Ltd.

[0112] *15 ARONIX M-402 manufactured by Toagosei Co., Ltd.

[0113] *16 "JER828" manufactured by Mitsubishi Chemical Corporation

[0114] *17 “RETARDER CTP” manufactured by Ouchi Shinko Chemical Co., Ltd.

[0115] *18 "DAISONET XL21-S" manufactured by Osaka Soda Co., Ltd.

[0116] *19 Daikin Industries, Ltd., “DAI EL G-8002”

[0117] *20Cancarb "Thermax N990"

[0118] *21 Triallyl isocyanurate manufactured by Tokyo Chemical Industry Co., Ltd.

[0119] *22 "PERHEXA 25B" manufactured by Nippon Oils and Fats Co., Ltd.

[0120] (Example 1)

[0121] The mixture was mixed as shown in Table 1, and 100 parts by mass of epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer, 50 parts by mass of carbon black N550, 10 parts by mass of adipic acid ether ester compound, 3 parts by mass of ester wax (fatty acid ester), 3 parts by mass of synthetic hydrotalcite, 3 parts by mass of magnesium oxide, 1 part by mass of DBU phenolic resin salt, 0.1 parts by mass of copper dimethyldithiocarbamate, 1 part by mass of nickel dibutyldithiocarbamate, and 5 parts by mass of trimethylolpropane triacrylate were added, and kneaded at 100° C. using a 1.67 L Banbury mixer to prepare a kneaded mixture A. Then, 1 part by mass of bisphenol A epoxy resin, 0.5 part by mass of N-cyclohexylthiophthalimide, and 1.7 parts by mass of quinoxaline vulcanizing agent were added to the kneaded mixture A, and kneaded with a kneading roller at room temperature to obtain a kneaded mixture B with a thickness of 2.0 to 2.5 mm, which was used as the rubber layer (A). In addition, as shown in Table 2, 100 parts by mass of fluororubber, 20 parts by mass of carbon black N990, and 3 parts by mass of triallyl isocyanurate were added, kneaded with a 1L kneader at 60°C, and then 2.5 parts by mass of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane was added, and kneaded with a kneading roller at room temperature to obtain a fluororubber layer (B) with a thickness of 2.0 to 2.5 mm. The rubber layer (A) and the fluororubber layer (B) are laminated together and vulcanized in a vulcanizer at 0.52 MPa (160°C) for 30 minutes (steam vulcanization molding method) to obtain a primary vulcanized laminate having a thickness of 4.0 to 5.0 mm. Then, vulcanization is performed at 160°C for 2 hours (steam vulcanization molding method) to obtain a secondary vulcanized laminate.

[0122] (Adhesion Evaluation (180° Peel Test))

[0123] The above secondary vulcanized laminate was cut into strips of 2.5×10 cm to prepare test pieces for the adhesion test. The test was performed using STROGRAPH E3 manufactured by Toyo Seiki Co., Ltd., and a 180° peel test was performed at 23°C at a tensile speed of 50 mm / min in accordance with JIS K6256-1. The peeling state at this time was visually observed, and the results are shown in Table 3. The evaluation criteria are as follows.

[0124] ○: Strong adhesion, rubber failure occurred between layers.

[0125] △: Although adhesion was achieved, the peel strength was weak, and rubber failure or peeling occurred locally at the interface.

[0126] ×: There is no adhesion at all, and separation occurs at the interface.

[0127] Furthermore, when performing the above peel test, the average value of the peel strength obtained from 0 to 100 mm was calculated. In the case where material damage occurred during the measurement, the measurement was stopped at this time, and the average value of the peel strength obtained until then was calculated. The test was performed 3 times respectively, and the median value of the peel strength obtained was used for evaluation, which was recorded in Table 3.

[0128] (Example 2)

[0129] The mixture was blended as shown in Table 1, and the trimethylolpropane triacrylate was changed to pentaerythritol tetraacrylate. The same procedure as in Example 1 was carried out to obtain a secondary vulcanized laminate, and the adhesiveness was evaluated as described above.

[0130] (Example 3)

[0131] The mixture was blended as shown in Table 1, and the epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer was changed to the epichlorohydrin-ethylene oxide copolymer. A secondary vulcanized laminate was obtained in the same manner as in Example 1, and the adhesion was evaluated as described above.

[0132] (Comparative Example 1)

[0133] The mixture was blended as shown in Table 1, and the bisphenol A type epoxy resin was not blended. The same procedure as in Example 1 was carried out to obtain a secondary vulcanized laminate, and the adhesiveness was evaluated as described above.

[0134] (Comparative Example 2)

[0135] The compounds were compounded as shown in Table 1, and nickel dibutyldithiocarbamate was not compounded. The same procedure as in Example 1 was carried out to obtain a secondary vulcanized laminate, and the adhesiveness was evaluated as described above.

[0136] (Comparative Example 3)

[0137] The mixture was blended as shown in Table 1, and a secondary vulcanized laminate was obtained in the same manner as in Example 1 except that a bisphenol A type epoxy resin and nickel dibutyl dithiocarbamate were not blended. The adhesiveness was evaluated as described above.

[0138] (Comparative Example 4)

[0139] The compounds were blended as shown in Table 1, and trimethylolpropane triacrylate was changed to trimethylolpropane trimethacrylate. A secondary vulcanized laminate was obtained in the same manner as in Example 1, and the adhesiveness was evaluated as described above.

[0140] (Comparative Example 5)

[0141] The mixture was blended as shown in Table 1, and the trimethylolpropane triacrylate was changed to dipentaerythritol hexaacrylate. The same procedure as in Example 1 was carried out to obtain a secondary vulcanized laminate, and the adhesiveness was evaluated as described above.

[0142] (Comparative Example 6)

[0143] The mixture was blended as shown in Table 1, and trimethylolpropane triacrylate was not blended. The same procedure as in Example 3 was carried out to obtain a secondary vulcanized laminate, and the adhesiveness was evaluated as described above.

[0144] (Comparative Example 7)

[0145] The mixture was blended as shown in Table 1, and the trimethylolpropane triacrylate was changed to pentaerythritol triacrylate. The same procedure as in Example 3 was carried out to obtain a secondary vulcanized laminate, and the adhesiveness was evaluated as described above.

[0146] (Comparative Example 8)

[0147] The mixture was blended as shown in Table 1, trimethylolpropane triacrylate was changed to pentaerythritol triacrylate, and nickel dibutyl dithiocarbamate and bisphenol A type epoxy resin were not blended. A secondary vulcanized laminate was obtained in the same manner as in Example 3, and the adhesion was evaluated as described above.

[0148] [Table 1]

[0149]

[0150] [Table 2]

[0151] Mass Fluororubber*19 100 Carbon black N990*20 20 Triallyl isocyanurate*21 3 2,5-Dimethyl-2,5-di(tert-butylperoxy)hexane*22 2.5

[0152] [Table 3]

[0153]

[0154] As shown in Table 3, the laminate using the composition for vulcanized adhesive laminates of the examples showed strong adhesion in the 180° peel test compared to the laminate using the composition for vulcanized adhesive laminates of the comparative examples. On the other hand, even for multifunctional acrylates, when the number of functional groups is too large, the result is that the adhesion is reduced.

[0155] Industrial Applicability

[0156] The laminate of the present invention has very good adhesion between the two vulcanized rubbers and has a strong adhesive surface. Therefore, it is very effective in applications where one surface is exposed to an environment requiring resistance to rancid gasoline, gasoline permeation, and alcohol-containing gasoline, and the other surface is exposed to an environment requiring resistance to aging, weathering, and gasoline, such as fuel hoses and feed hoses.

Claims

1. A vulcanization adhesive composition, It is characterized in that The composition comprises at least 2 to 7 parts by mass of (a2) a trifunctional or higher and pentafunctional or lower acrylate having no hydroxyl group, (a3) ​​0.5 to 3 parts by mass of an epoxy resin, (a4) 0.2 to 3 parts by mass of nickel dibutyl dithiocarbamate, and (a5) 0.1 to 10 parts by mass of a vulcanizing agent, relative to 100 parts by mass of the (a1) epihalohydrin rubber.

2. The vulcanization adhesive composition according to claim 1, in, The (a1) epihalohydrin rubber is at least one selected from the group consisting of an epihalohydrin-ethylene oxide copolymer, an epihalohydrin-propylene oxide copolymer, an epihalohydrin-allyl glycidyl ether copolymer, an epihalohydrin-ethylene oxide-allyl glycidyl ether terpolymer, an epihalohydrin-propylene oxide-allyl glycidyl ether terpolymer, and an epihalohydrin-ethylene oxide-propylene oxide-allyl glycidyl ether tetrapolymer.

3. The vulcanization adhesive composition according to claim 1, in, The (a2) trifunctional or higher and pentafunctional or lower acrylate having no hydroxyl group is at least one selected from the group consisting of trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and di(trimethylolpropane) tetraacrylate.

4. The vulcanization adhesive composition according to claim 1, in, The (a3) ​​epoxy resin is bisphenol A type epoxy resin.

5. The vulcanization adhesive composition according to claim 1, in, The (a5) vulcanizing agent is at least one vulcanizing agent selected from the group consisting of thiourea vulcanizing agents, quinoxaline vulcanizing agents, sulfur vulcanizing agents, peroxide vulcanizing agents, mercaptotriazine vulcanizing agents and bisphenol vulcanizing agents.

6. A composition for a vulcanizable adhesive laminate, comprising a laminate of a rubber layer (A) formed from the vulcanizable adhesive composition according to any one of claims 1 to 5 and a fluororubber layer (B) formed from a fluororubber composition containing at least a peroxide-based vulcanizing agent.

7. A laminate obtained by vulcanizing the composition for a vulcanizable adhesive laminate according to claim 6. 8 . A catheter or a hose, formed from the laminate according to claim 7 .