Optical laminate and display system
By using the adhesive layer controlled by the linear expansion coefficient and a specific polymer composition in the optical laminate, the problem of unstable optical properties of the optical laminate in harsh environments is solved, and the image under high temperature and high humidity conditions is achieved Show performance stability.
Patent Information
- Application Number
- CN202380027330.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-28
- Filing Date
- 2023-03-08
- Publication Date
- 2024-11-01
AI Technical Summary
The optical characteristics of the existing optical laminates are unstable in harsh environments, especially under high temperature and high humidity conditions, resulting in a degradation of the performance of the image display device.
An optical laminate is designed, including at least one adhesive layer, whose linear expansion coefficient meets the relationship of 0.8≤α1/α2≤1.2 when the temperature is increased to 20°C and the cooling is reduced by 30°C, ensuring the adhesive layer's The deformation rate changes small, thereby stabilizing the optical properties. The optical laminate includes a polarization member, a phase difference member and a protective member, and uses a (meth)acrylic polymer having a weight average molecular weight of more than 1.5 million as the adhesive composition.
It realizes optical properties stability in harsh environments, is suitable for applications such as virtual reality goggles, and ensures the performance consistency and durability of image display.
Smart Images

Figure CN118891565A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical layered body and a display system using the optical layered body. Background Art
[0002] Image display devices represented by liquid crystal display devices and electroluminescent (EL) display devices (e.g., organic EL display devices) are rapidly becoming popular. In image display devices, optical components such as polarization components and phase difference components are generally used to realize image display and improve image display performance (e.g., refer to Patent Document 1).
[0003] In recent years, new uses of image display devices have been developed. For example, goggles with displays (VR goggles) for realizing Virtual Reality (VR) have begun to be commercialized. Since the use of VR goggles in various scenarios has been studied, higher requirements are also put forward for stability in harsh environments such as high temperature and / or high humidity environments than for optical laminates used in previous image display devices.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-103286 Summary of the invention
[0007] Problems to be solved by the invention
[0008] A main object of the present invention is to provide an optical layered body having stable optical characteristics even in a harsh environment.
[0009] Solutions to the problem
[0010] [1] An optical laminate according to an embodiment of the present invention comprises at least one optical component and at least one adhesive layer, wherein, when the total number of the adhesive layers contained in the optical laminate is set to N, the adhesive layers greater than N / 2 are adhesive layers A whose linear expansion coefficient α1 when heated from 20°C to 30°C and linear expansion coefficient α2 when cooled from 30°C to 20°C satisfy the relationship of 0.8≤α1 / α2≤1.2.
[0011] [2] In the optical layered body described in [1] above, the pressure-sensitive adhesive layer A may have a thickness of 1 μm to 15 μm.
[0012] [3] The optical layered body described in [1] or [2] may have a thickness of 100 μm or more and 300 μm or less.
[0013] [4] The optical laminate described in any one of [1] to [3] above may have a first adhesive layer, a polarizing component, a second adhesive layer, a first phase difference component, a third adhesive layer, and a protective component in sequence, and at least two selected from the first adhesive layer, the second adhesive layer and the third adhesive layer are the adhesive layer A.
[0014] [5] In the optical layered body described in [4] above, the first phase difference member may include a λ / 4 member.
[0015] [6] In the optical layered body described in [4] or [5] above, the protective member may have a surface treatment layer.
[0016] [7] In the optical layered body according to any one of [1] to [6] above, the pressure-sensitive adhesive composition constituting the pressure-sensitive adhesive layer A may contain a (meth)acrylic polymer having a weight average molecular weight of 1,500,000 or more.
[0017] [8] A display system according to an embodiment of the present invention includes the optical layered body according to any one of [1] to [7].
[0018] [9] The display system described in [8] may include: a display element having a display surface that emits light displaying an image forward via a polarization component; a reflective polarization component arranged in front of the display element to reflect light emitted from the display element; a first lens portion arranged on an optical path between the display element and the reflective polarization component; a half-mirror arranged between the display element and the first lens portion to transmit light emitted from the display element and to reflect light reflected by the reflective polarization component toward the reflective polarization component; a first λ / 4 component arranged on an optical path between the display element and the half-mirror; and a second λ / 4 component arranged on an optical path between the half-mirror and the reflective polarization component, wherein the optical stack described in [5] is arranged on the display element side of the half-mirror so that the display element and the first λ / 4 plate are integrally provided.
[0019] Effects of the Invention
[0020] In the embodiment of the present invention, more than half of the adhesive layers included in the optical laminate are adhesive layers A whose linear expansion coefficient α1 when heated in the range of 20° C. to 30° C. and linear expansion coefficient α2 when cooled satisfy the relationship of 0.8≤α1 / α2≤1.2. Thus, an optical laminate having stable optical properties even in a harsh environment can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1AThis is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention.
[0022] Figure 1B This is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention.
[0023] Figure 2 This is a schematic diagram showing a schematic configuration of a display system according to one embodiment of the present invention.
[0024] Figure 3 It is a figure which shows the wet heat test result of the optical laminated body obtained in an Example and a comparative example.
[0025] Explanation of symbols
[0026] 2 Display system
[0027] 4 Lens section
[0028] 10 Polarization component
[0029] 12 Display components
[0030] 14 Reflective polarizing element
[0031] 16. First lens unit
[0032] 18 Half Mirror
[0033] 20 first phase difference member
[0034] 22. Second phase difference member
[0035] 24 Second lens unit
[0036] 100 Optical laminate DETAILED DESCRIPTION
[0037] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings, but the present invention is not limited to these embodiments. In addition, in order to explain more clearly, the drawings sometimes schematically show the width, thickness, shape, etc. of each part compared with the embodiments, but this is only an example and does not limit the interpretation of the present invention. In addition, in this specification, "to" indicating a numerical range includes the upper and lower limits thereof, and "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid".
[0038] (Definition of Terms and Symbols)
[0039] The definitions of terms and symbols in this specification are as follows.
[0040] (1) Refractive index (nx, ny, nz)
[0041] "nx" is the refractive index in the direction where the refractive index in the plane reaches the maximum (ie, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), and "nz" is the refractive index in the thickness direction.
[0042] (2) In-plane phase difference (Re)
[0043] "Re(λ)" is the in-plane phase difference measured at 23°C with light of wavelength λnm. For example, "Re(550)" is the in-plane phase difference measured at 23°C with light of wavelength 550nm. When the thickness of the layer (film) is d(nm), Re(λ) can be calculated by the formula: Re(λ) = (nx-ny)×d.
[0044] (3) Retardation in the thickness direction (Rth)
[0045] "Rth(λ)" is the phase difference in the thickness direction measured at 23°C with light of wavelength λnm. For example, "Rth(550)" is the phase difference in the thickness direction measured at 23°C with light of wavelength 550nm. When the thickness of the layer (film) is d(nm), Rth(λ) can be calculated by the formula: Rth(λ) = (nx-nz)×d.
[0046] (4) Nz coefficient
[0047] The Nz coefficient can be calculated by Nz=Rth / Re.
[0048] (5) Angle
[0049] In this specification, when an angle is mentioned, the angle includes both clockwise and counterclockwise relative to the reference direction. Therefore, for example, "45°" means 45° clockwise or counterclockwise. In addition, in this specification, "substantially parallel" includes the case within the range of 0°±10°, for example, 0°±5°, preferably 0°±3°, and more preferably 0°±1°, and "substantially orthogonal" includes the case within the range of 90°±10°, for example, 90°±5°, preferably 90°±3°, and more preferably 90°±1°.
[0050] A. Optical laminate
[0051] The optical laminate of the embodiment of the present invention includes at least one optical component and at least one adhesive layer. When the total number of adhesive layers contained in the above optical laminate is set to N, the adhesive layers above N / 2 are adhesive layers A whose linear expansion coefficient α1 when heated from 20°C to 30°C and linear expansion coefficient α2 when cooled from 30°C to 20°C satisfy the relationship of 0.8≤α1 / α2≤1.2. The adhesive layer having α1 / α2 less than 0.8 or exceeding 1.2 tends to have a large difference in deformation rate when heated and cooled. As a result of the increase in deformation due to repeated temperature changes, the optical properties of the optical laminate are sometimes changed. As a result, when it is used as a constituent member of goggles with a display, its display properties are sometimes affected. In contrast, by using an adhesive layer satisfying the relationship of 0.8≤α1 / α2≤1.2 in a given ratio or more, the change in the optical properties of the optical laminate caused by the deformation of the adhesive layer can be suppressed.
[0052] Examples of the optical member included in the optical layered body include an absorption-type polarization member, a reflection-type polarization member, and a phase difference member.
[0053] The total number N of the adhesive layers included in the optical laminate is 1 or more, preferably 2 or more, more preferably 3 or more, for example, 6 or less. In one embodiment, the total number N of the adhesive layers included in the optical laminate is 2 or more and 5 or less, preferably 3 or 4. The optical laminate has an adhesive layer, for example, in the outermost layer, so that it can be bonded to an adjacent member via the adhesive layer.
[0054] The ratio of the number of the pressure-sensitive adhesive layers A contained in the optical laminate to the total number of pressure-sensitive adhesive layers is 1 / 2 or more, preferably 2 / 3 or more, more preferably 3 / 4 or more, and may be 1.
[0055] It goes without saying that the number of adhesive layers A is an integer, so when the total number of adhesive layers N is an odd number, the number of adhesive layers A is an integer greater than or equal to N / 2 and less than or equal to N. Specifically, when N is 3, the number of adhesive layers A is an integer greater than or equal to 2 and less than or equal to 3, that is, 2 or 3, and when N is 4, the number of adhesive layers A is an integer greater than or equal to 2 and less than or equal to 4, that is, 2, 3 or 4. It should be noted that in this specification, all adhesive layers whose linear expansion coefficient α1 when heated from 20°C to 30°C and whose linear expansion coefficient α2 when cooled from 30°C to 20°C satisfy the relationship of 0.8≤α1 / α2≤1.2 are referred to as adhesive layers A. Thus, when the plurality of adhesive layers included in the optical laminate are adhesive layers A, as long as the plurality of adhesive layers satisfy the relationship of 0.8≤α1 / α2≤1.2, they do not need to be formed to the same thickness by adhesive compositions having the same composition, and may also be formed to the same or different thicknesses by adhesive compositions having different compositions.
[0056] The thickness of the optical laminate is, for example, 100 μm to 300 μm, preferably 110 μm to 250 μm, and more preferably 120 μm to 200 μm. In an optical laminate having a small overall thickness, the deformation of the adhesive layer has a large influence, so the effect of the present invention can be suitably obtained by using an adhesive layer having a small difference in deformation rate when heated and when cooled.
[0057] In one embodiment, the thickness of the adhesive layer A is, for example, 1 μm or more and 15 μm or less, preferably 2 μm or more and less than 10 μm, and more preferably 3 μm or more and 8 μm or less. By using an adhesive layer having a small difference in deformation rate when heated and cooled and a small thickness, an optical laminate having excellent stability such as optical properties can be suitably obtained.
[0058] Hereinafter, the optical layered body according to the embodiment of the present invention will be specifically described with reference to the drawings.
[0059] A-1. Implementation Method 1
[0060] Figure 1A This is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention. Figure 1A The optical laminate 100a shown has a first adhesive layer a1, a polarizing member 10, a second adhesive layer a2, a first phase difference member 20, a third adhesive layer a3, and a protective member 30 in sequence. Specifically, the polarizing member 10 and the first phase difference member 20 are bonded via the second adhesive layer a2, and the first phase difference member 20 and the protective member 30 are bonded via the third adhesive layer a3. The first adhesive layer a1 is an adhesive layer for bonding the optical laminate 100a itself to adjacent components (for example, other components constituting goggles with a display), and its surface can be protected by a release liner until it is used. In the optical laminate 100a, the total number of adhesive layers is 3, of which more than 2 are the above-mentioned adhesive layers A.
[0061] The thickness of the optical layered body 100 a is, for example, 100 μm or more and 300 μm or less, preferably 110 μm or more and 250 μm or less, and more preferably 120 μm or more and 200 μm or less.
[0062] <Adhesive layer>
[0063] The optical laminate 100 a has three pressure-sensitive adhesive layers in total (a first pressure-sensitive adhesive layer a1 , a second pressure-sensitive adhesive layer a2 , and a third pressure-sensitive adhesive layer a3 ), at least two of which are pressure-sensitive adhesive layers A, and preferably all of which are pressure-sensitive adhesive layers A.
[0064] When two of the three adhesive layers are adhesive layers A, the first adhesive layer a1 and the second adhesive layer a2 are preferably adhesive layers A. When the optical laminate is applied to VR goggles, the adhesive layer A having high shape stability against temperature changes is arranged near the display element and the first phase difference member 20, so that the effect of the present invention can be preferably obtained.
[0065] For the adhesive layer A, as described above, the linear expansion coefficient α1 when the temperature is increased from 20°C to 30°C and the linear expansion coefficient α2 when the temperature is decreased from 30°C to 20°C typically satisfy the relationship of 0.8≤α1 / α2≤1.2, preferably satisfying the relationship of 0.85≤α1 / α2≤1.15, and more preferably satisfying the relationship of 0.9≤α1 / α2≤1.1. By using such an adhesive layer A, an optical laminate having excellent stability of optical properties even in a harsh environment can be obtained. The α1 and α2 of the adhesive layer A are not limited as long as the effect of the present invention can be obtained, and can be any value. The α1 of the adhesive layer A can be, for example, 5.0×10 -4 / ℃ and above 7.0×10 -4 / °C or less. The α2 of the adhesive layer A may be, for example, 5.0×10 -4 / ℃ and above 7.0×10 -4 / °C or less, and for example, 6.0×10 -4 / ℃ and above 7.0×10 -4 / ℃ below.
[0066] The linear expansion coefficient β1 of the adhesive layer A when the temperature is increased from 60°C to 70°C and the linear expansion coefficient β2 when the temperature is decreased from 70°C to 60°C satisfy, for example, the relationship of 1.0≤β1 / β2≤1.5, preferably 1.05≤β1 / β2≤1.45, and more preferably 1.1≤β1 / β2≤1.4. By using such an adhesive layer, an optical laminate having excellent stability of optical properties even in a harsh environment can be obtained. The β1 and β2 of the adhesive layer A are not limited as long as the effect of the present invention can be obtained, and can be any value. The β1 of the adhesive layer A can be, for example, 8.0×10 -4 / ℃ and above 9.0×10 -4 / °C or less. The β2 of the adhesive layer A may be, for example, 6.0×10 -4 / ℃ and above 7.0×10 -4 / ℃ below.
[0067] The storage modulus of the adhesive layer A at 25°C is, for example, 5×10 4 Pa or more, preferably 10×10 4 Pa or more, more preferably 12×10 4 Pa or more, for example, 20×104 Pa or less, preferably 15×10 4 Pa or less. By using an adhesive layer having a small difference in deformation rate when heating and cooling and having such a storage modulus, an optical laminate having excellent stability of optical properties even in a harsh environment can be obtained. The storage modulus can be obtained, for example, by using a dynamic viscoelasticity measurement device ("Advanced Rheometric Expansion System (ARES)", manufactured by Rheometric Scientific) (e.g., parallel plates (8.0 mm φ), torsion mode, and measurement conditions of a frequency range of 1 Hz).
[0068] Adhesive layer A can be formed by any appropriate adhesive composition. As the adhesive composition forming adhesive layer A, there can be mentioned: acrylic adhesive composition, rubber adhesive composition, silicone adhesive composition, polyester adhesive composition, urethane adhesive composition, epoxy adhesive composition, and polyether adhesive composition. By adjusting the type, quantity, combination and ratio of the monomers of the base resin forming the adhesive composition, as well as the amount of the cross-linking agent, reaction temperature, reaction time, etc., it is possible to prepare an adhesive composition having the desired properties corresponding to the target. The base polymer of the adhesive composition can be used alone or in combination of two or more. The adhesive layer is preferably formed by an acrylic adhesive composition comprising a (meth) acrylic polymer as a base polymer.
[0069] In one embodiment, the monomer components constituting the above-mentioned (meth)acrylic polymer include as the main component a (meth)acrylic monomer represented by the general formula CH2=C(R1)COOR2 (wherein R1 is hydrogen or a methyl group, and R2 is an alkyl group having 2 to 14 carbon atoms, preferably 3 to 12 carbon atoms, and more preferably 4 to 9 carbon atoms).
[0070] Examples of the (meth)acrylic monomer represented by the general formula CH2=C(R1)COOR2 include ethyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate, isomyristyl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and phenoxyethyl (meth)acrylate. Among them, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc. can be preferably used. The (meth)acrylic monomer represented by the general formula CH2=C(R1)COOR2 may be used alone or in combination of two or more.
[0071] In the monomer components constituting the (meth)acrylic polymer, the content ratio of the (meth)acrylic monomer represented by the general formula CH2=C(R1)COOR2 is, for example, 50% to 98% by weight, preferably 60% to 90% by weight, and more preferably 70% to 80% by weight.
[0072] The monomer components constituting the (meth)acrylic polymer preferably further include a nitrogen-containing monomer. In the above-mentioned monomer components, the content ratio of the nitrogen-containing monomer is, for example, 0.1 wt % to 35 wt %, preferably 3 wt % to 30 wt %, and more preferably 5 wt % to 25 wt %. When the content ratio of the nitrogen-containing monomer is within the above range, an adhesive layer having excellent durability in a heated environment and / or a high-humidity environment can be obtained.
[0073] The nitrogen-containing monomer is a polymerizable monomer containing one or more nitrogen atoms in the monomer structure, and preferably includes an imide group-containing monomer, an amide group-containing monomer, etc. Among them, an amide group-containing monomer is more preferred. In the above-mentioned monomer components, the content ratio of the amide group-containing monomer is, for example, 3% to 15% by weight, preferably 5% to 10% by weight. The nitrogen-containing monomer can be used alone or in combination of two or more.
[0074] Examples of the imide group-containing monomer include N-cyclohexylmaleimide, N-phenylmaleimide, N-methylmaleimide, N-ethylmaleimide, N-propylmaleimide, N-isopropylmaleimide, N-butylmaleimide, and itaconimide.
[0075] Examples of the amide group-containing monomer include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-diethylmethacrylamide, N-isopropyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, dimethylaminoethyl(meth)acrylate, tert-butylaminoethyl(meth)acrylate, diacetone(meth)acrylamide, N-vinylacetamide, N,N'-methylenebis(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, and N-vinylcaprolactam.
[0076] Examples of other nitrogen-containing monomers include amino group-containing monomers, (meth)acrylonitrile, N-(meth)acryloylmorpholine, and N-vinyl-2-pyrrolidone.
[0077] The monomer component may contain other polymerizable monomers for adjusting the glass transition temperature and releasability of the (meth)acrylic polymer within a range not impairing the effects of the present invention.
[0078] As other polymerizable monomers, for example, carboxyl group-containing monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, vinyl ester monomers, aromatic vinyl monomers, etc. can be cited, which can help improve cohesion, heat resistance, etc. In addition, for example, anhydride group-containing monomers, hydroxyl group-containing monomers, epoxy group-containing monomers, vinyl ether monomers, etc. can be cited, which can help improve adhesion and have functional groups that act as crosslinking bases. In addition, for example, (meth) acrylic monomers having an alkyl group with 1 carbon atom or 15 or more carbon atoms can be used. These polymerizable monomers can be used alone or in combination of two or more.
[0079] Examples of the carboxyl group-containing monomer include acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, etc. Among them, acrylic acid and methacrylic acid are preferably used.
[0080] Examples of the sulfonic acid group-containing monomer include styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid.
[0081] As the phosphoric acid group-containing monomer, 2-hydroxyethyl acryloyl phosphate and the like can be mentioned.
[0082] Examples of the vinyl ester monomer include vinyl acetate, vinyl propionate, vinyl laurate, and vinyl pyrrolidone.
[0083] Examples of the aromatic vinyl monomer include styrene, chlorostyrene, chloromethylstyrene, and α-methylstyrene.
[0084] Examples of the acid anhydride group-containing monomer include maleic anhydride and itaconic anhydride.
[0085] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, (4-hydroxymethylcyclohexyl)methyl acrylate, N-hydroxymethyl (meth)acrylamide, N-hydroxy (meth)acrylamide, vinyl alcohol, allyl alcohol, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and diethylene glycol monovinyl ether.
[0086] Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate and allyl glycidyl ether.
[0087] Examples of the vinyl ether monomer include methyl vinyl ether, ethyl vinyl ether, and isobutyl vinyl ether.
[0088] Examples of the (meth)acrylic monomer having an alkyl group having 1 or 15 or more carbon atoms include methyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, and the like.
[0089] The content ratio of the other polymerizable monomer in the monomer components is, for example, 0.1 to 10% by weight, preferably 0.2 to 7% by weight, and more preferably 0.5 to 5% by weight.
[0090] In addition, as copolymerizable monomers other than the above, silane monomers containing silicon atoms can be cited. As silane monomers, 3-acryloxypropyl triethoxysilane, vinyl trimethoxysilane, vinyl triethoxysilane, 4-vinyl butyl trimethoxysilane, 4-vinyl butyl triethoxysilane, 8-vinyl octyl trimethoxysilane, 8-vinyl octyl triethoxysilane, 10-methacryloxy decyl trimethoxysilane, 10-acryloxy decyl trimethoxysilane, 10-methacryloxy decyl triethoxysilane, 10-acryloxy decyl triethoxysilane, etc. can be cited. The silane monomers can be used alone or in combination of two or more.
[0091] The amount of the silane monomer to be blended is preferably 0.1 to 3 parts by weight, more preferably 0.5 to 2 parts by weight, based on 100 parts by weight of the (meth)acrylic polymer. Copolymerization of the silane monomer is preferred for improving durability.
[0092] The weight average molecular weight of the (meth) acrylic polymer is, for example, 600,000 or more, preferably 1.5 million or more, more preferably 1.6 million or more, and further preferably 1.8 million or more. The weight average molecular weight of the (meth) acrylic polymer is, for example, 3 million or less, preferably 2.5 million or less. When the weight average molecular weight is within the above range, an adhesive layer that satisfies the above α1 / α2 relationship, and has excellent durability and operability can be obtained appropriately. It should be noted that the weight average molecular weight refers to a value measured by GPC (gel permeation chromatography) and calculated after polystyrene conversion.
[0093] In order to easily achieve a balance in adhesive performance, the glass transition temperature (Tg) of the (meth) acrylic polymer is, for example, -5°C or less, preferably -10°C or less. When the glass transition temperature is higher than -5°C, the polymer is difficult to flow, and the wetting of the adherend becomes insufficient, which may cause expansion between layers. It should be noted that the glass transition temperature (Tg) of the (meth) acrylic polymer can be adjusted to the above range by appropriately changing the monomer components and composition ratios used.
[0094] The production of (meth)acrylic polymers can be appropriately selected by known production methods such as solution polymerization, bulk polymerization, emulsion polymerization, and various free radical polymerizations. In solution polymerization, as polymerization solvents, for example, ethyl acetate, toluene, etc. can be used. As a specific solution polymerization example, in an inert gas stream such as nitrogen, for example, 0.01 to 0.2 parts by weight of azobisisobutyronitrile can be added as a polymerization initiator relative to 100 parts by weight of the total amount of monomers, and the polymerization can be carried out at about 50 to 70°C for about 8 to 30 hours. The obtained (meth)acrylic polymer can be any copolymer such as a random copolymer, a block copolymer, a graft copolymer, etc.
[0095] In the polymerization, any appropriate polymerization initiator, chain transfer agent, emulsifier, etc. may be appropriately selected and used as needed.
[0096] The acrylic pressure-sensitive adhesive composition contains a (meth)acrylic polymer as a base polymer, and preferably further contains a peroxide and an isocyanate crosslinking agent.
[0097] As the peroxide, any peroxide that can generate free radical active species by heating or light irradiation to promote crosslinking of the base polymer of the adhesive composition can be used appropriately, and in view of handleability and stability, it is preferred to use a peroxide having a 1-minute half-life temperature of 80° C. to 160° C., and more preferably a peroxide having a 1-minute half-life temperature of 90° C. to 140° C. If the 1-minute half-life temperature is too low, a reaction may occur during storage before coating and drying, and the viscosity may increase, making it impossible to coat. On the other hand, if the 1-minute half-life temperature is too high, a side reaction may occur due to the high temperature during the crosslinking reaction, and a large amount of unreacted peroxide may remain, causing crosslinking to proceed over time.
[0098] Examples of the peroxide include di(2-ethylhexyl) peroxydicarbonate (1-minute half-life temperature: 90.6° C.), di(4-tert-butylcyclohexyl) peroxydicarbonate (1-minute half-life temperature: 92.1° C.), di-sec-butyl peroxydicarbonate (1-minute half-life temperature: 92.4° C.), tert-butyl peroxyneodecanoate (1-minute half-life temperature: 103.5° C.), tert-hexyl peroxypivalate (1-minute half-life temperature: 109.1° C.), tert-butyl peroxypivalate (1-minute half-life temperature: 110.3° C.), dilauroyl peroxide (1-minute half-life temperature: 112.1° C.), and dilauroyl peroxide (1-minute half-life temperature: 113.3° C.). Half-life temperature: 116.4℃), dioctanoyl peroxide (1 minute half-life temperature: 117.4℃), 1,1,3,3-tetramethylbutyl peroxide 2-ethylhexanoate (1 minute half-life temperature: 124.3℃), di(4-methylbenzoyl) peroxide (1 minute half-life temperature: 128.2℃), dibenzoyl peroxide (1 minute half-life temperature: 130.0℃), tert-butyl peroxyisobutyrate (1 minute half-life temperature: 136.1℃), 1,1-di(tert-hexylperoxide)cyclohexane (1 minute half-life temperature: 149.2℃), etc. Among them, di(4-tert-butylcyclohexyl) peroxydicarbonate (1 minute half-life temperature: 92.1° C.), dilauroyl peroxide (1 minute half-life temperature: 116.4° C.), dibenzoyl peroxide (1 minute half-life temperature: 130.0° C.), etc. are preferably used because of their excellent crosslinking reaction efficiency. The peroxides may be used alone or in combination of two or more.
[0099] It should be noted that the half-life of peroxide is an index representing the decomposition rate of peroxide, refers to the time until the residual amount of peroxide reaches half. About the decomposition temperature for obtaining the half-life at any time, the half-life time at any temperature, in the manufacturer's catalogue etc., record is made, for example, is recorded in " the 9th edition (May, 2003) of Organic Peroxide Catalogue " etc. of NOF Corporation.
[0100] The amount of the peroxide is, for example, 0.02 to 2 parts by weight, preferably 0.04 to 1.5 parts by weight, and more preferably 0.05 to 1 part by weight, relative to 100 parts by weight of the (meth)acrylic polymer. When the amount of the peroxide is within the above range, an adhesive layer having excellent durability and adhesiveness can be obtained.
[0101] Examples of the isocyanate crosslinking agent include aromatic isocyanates such as tolylene diisocyanate and xylene diisocyanate, alicyclic isocyanates such as isophorone diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate. The isocyanate crosslinking agent may be used alone or in combination of two or more.
[0102] More specifically, the polyisocyanates include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate, alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate, aromatic diisocyanates such as 2,4-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate and polymethylene polyphenyl isocyanate, trimethylolpropane / toluene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name CORONATE L), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name CORONATE HL), isocyanurate of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name CORONATE Isocyanate adducts such as polyisocyanates (HX), polyether polyisocyanates, polyester polyisocyanates, and adducts thereof with various polyols, polyisocyanates multifunctionalized by isocyanurate bonds, biuret bonds, allophanate bonds, etc.
[0103] The amount of the isocyanate crosslinking agent is, for example, 0.02 to 2 parts by weight, preferably 0.04 to 1.5 parts by weight, and more preferably 0.05 to 1 part by weight, relative to 100 parts by weight of the (meth)acrylic polymer. When the amount of the isocyanate crosslinking agent is within the above range, an adhesive layer having excellent cohesive force and adhesiveness can be obtained.
[0104] The amount of the crosslinking agent (peroxide and isocyanate crosslinking agent) is adjusted so that the gel fraction of the adhesive layer after crosslinking reaches, for example, 45% to 95% by weight, preferably 50% to 90% by weight, and more preferably 55% to 85% by weight. The adhesive layer having a gel fraction within the above range has excellent durability and adhesion.
[0105] The gel fraction (weight %) of the adhesive layer can be a value calculated as (W2 / W1)×100 after immersing the dry weight W1 (g) of the adhesive layer in ethyl acetate at about 23°C for 7 days, removing the insoluble components of the adhesive layer from ethyl acetate, measuring the weight W2 (g) after drying.
[0106] The gel fraction can be adjusted to a desired range by adjusting the amount of peroxide and isocyanate crosslinking agent added, the crosslinking treatment temperature, the crosslinking treatment time, and the like.
[0107] The crosslinking treatment temperature and the crosslinking treatment time are preferably set so that the decomposed amount of the peroxide contained in the adhesive composition becomes 50 wt % or more, more preferably 60 wt % or more, and further preferably 70 wt % or more.
[0108] For example, when the crosslinking treatment temperature is a 1 minute half-life temperature, the decomposition amount of the peroxide is 50% by weight in 1 minute, and the decomposition amount of the peroxide is 75% by weight in 2 minutes, and a crosslinking treatment time of more than 1 minute is required. In addition, for example, when the half-life (half-life time) of the peroxide at the crosslinking treatment temperature is 30 seconds, a crosslinking treatment time of more than 30 seconds is required, and in addition, for example, when the half-life (half-life time) of the peroxide at the crosslinking treatment temperature is 5 minutes, a crosslinking treatment time of more than 5 minutes is required.
[0109] As such, the crosslinking treatment temperature and the crosslinking treatment time can be calculated by assuming that the peroxide is proportional to the half-life (half-life time) and by theoretical calculation, and the addition amount can be appropriately adjusted. On the other hand, the higher the temperature, the higher the possibility of side reactions, so the crosslinking treatment temperature is preferably below 170°C.
[0110] The cross-linking treatment time is generally about 0.2 to 20 minutes, preferably about 0.5 to 10 minutes.
[0111] The crosslinking treatment may be performed at the temperature of the drying step of the pressure-sensitive adhesive layer, or may be performed by separately providing a crosslinking treatment step after the drying step.
[0112] In order to improve the adhesive strength and durability, a silane coupling agent may be added to the adhesive composition. Examples of the silane coupling agent include epoxy-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, amino-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, and 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, (meth)acryl-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane, and isocyanate-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane. The silane coupling agent may be used alone or in combination of two or more.
[0113] The amount of the silane coupling agent to be added is, for example, 0.01 to 1 part by weight, preferably 0.02 to 0.6 part by weight, and more preferably 0.05 to 0.3 part by weight, based on 100 parts by weight of the (meth)acrylic polymer.
[0114] As required, the adhesive composition may further include any appropriate additives. Examples of additives include surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, softeners, antioxidants, anti-aging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, etc. A reducing agent may also be added within a controllable range.
[0115] By crosslinking the adhesive composition, the adhesive layer A can be suitably obtained. The difference in deformation rate between the temperature rise and the temperature drop of the adhesive layer A obtained by crosslinking the adhesive composition is small, and even in the case of a thin layer, the durability under high temperature and high humidity is excellent. The adhesive composition can be applied to a desired component (in Figure 1A In the structure, the surface of the polarizing member, the first phase difference member, or the protective member is cross-linked, or it can be applied to a support such as a release liner and cross-linked before being transferred to the desired member.
[0116] As described above, the thickness of the pressure-sensitive adhesive layer A is, for example, 1 μm or more and 15 μm or less, preferably 2 μm or more and less than 10 μm, and more preferably 3 μm or more and 8 μm or less.
[0117] The optical laminate may include an adhesive layer other than the above-mentioned adhesive layer A. Such an adhesive layer may also be formed by any appropriate adhesive composition. As the adhesive composition forming the adhesive layer other than the adhesive layer A, there may be mentioned: acrylic adhesive composition, rubber adhesive composition, silicone adhesive composition, polyester adhesive composition, urethane adhesive composition, epoxy adhesive composition, and polyether adhesive composition. Due to excellent transparency, heat resistance, etc., acrylic adhesive composition may be preferably used.
[0118] The storage modulus of the adhesive layer other than the adhesive layer A at 25° C. is, for example, 5×10 4 Pa or more, preferably 10×10 4 Pa or more, more preferably 14×10 4 Pa or more, for example, 20×10 4 Pa or less, preferably 15×10 4 Below Pa.
[0119] The thickness of the adhesive layer other than the adhesive layer A is, for example, 12 μm or more and 100 μm or less, or preferably 12 μm or more and 80 μm or less.
[0120] <Polarization member>
[0121] The polarizing element 10 is typically an absorbing polarizing element including a resin film containing a dichroic substance (sometimes referred to as an absorbing polarizing film), and may further include a protective layer on one or both sides thereof as required. The protective layer is typically bonded to the absorbing polarizing film via any appropriate adhesive layer. As an adhesive forming the adhesive layer, a UV curable adhesive can be typically cited.
[0122] The orthogonal transmittance (Tc) of the polarizing component (absorption type polarizing film) is preferably 0.5% or less, more preferably 0.1% or less, and further preferably 0.05% or less. The single transmittance (Ts) of the polarizing component (absorption type polarizing film) is, for example, 41.0% to 45.0%, and preferably 42.0% or more. The polarization degree (P) of the polarizing component (absorption type polarizing film) is, for example, 99.0% to 99.997%, and preferably 99.9% or more.
[0123] The above-mentioned orthogonal transmittance, single transmittance and polarization degree can be measured, for example, using an ultraviolet visible spectrophotometer. The polarization degree P can be measured using an ultraviolet visible spectrophotometer for single transmittance Ts, parallel transmittance Tp and orthogonal transmittance Tc, and the obtained Tp and Tc can be obtained by the following formula. It should be noted that Ts, Tp and Tc are Y values obtained by measuring the 2-degree field of view (C light source) of JIS Z8701 and correcting for visibility.
[0124] Polarization degree P (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100
[0125] The thickness of the absorption-type polarizing film is, for example, 1 μm to 20 μm, 2 μm to 15 μm, 12 μm or less, 10 μm or less, 8 μm or less, or 5 μm or less.
[0126] The absorption-type polarizing film may be produced by a single-layer resin film or by using a laminate of two or more layers.
[0127] In the case of a single-layer resin film, for example, a hydrophilic polymer film such as a polyvinyl alcohol (PVA) film, a partially formalized PVA film, or a partially saponified ethylene-vinyl acetate copolymer film can be subjected to dyeing treatment using a dichroic substance such as iodine or a dichroic dye, stretching treatment, etc., thereby obtaining an absorption-type polarizing film. Among them, an absorption-type polarizing film obtained by dyeing a PVA film with iodine and uniaxially stretching the film is preferred.
[0128] The dyeing using iodine can be performed by, for example, immersing the PVA film in an iodine aqueous solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching can be performed after the dyeing treatment or while dyeing. In addition, the dyeing can also be performed after the stretching. The PVA film can be subjected to swelling treatment, cross-linking treatment, cleaning treatment, drying treatment, etc. as needed.
[0129] As a laminate made using the above-mentioned two or more layers, there can be cited a laminate of a resin substrate and a PVA-type resin layer (PVA-type resin film) laminated on the resin substrate, or a laminate of a resin substrate and a PVA-type resin layer formed by coating on the resin substrate. The absorption-type polarizing film obtained by using a laminate of a resin substrate and a PVA-type resin layer formed by coating on the resin substrate can be made by the following method: for example, a PVA-type resin solution is applied to a resin substrate, dried to form a PVA-type resin layer on the resin substrate, and a laminate of a resin substrate and a PVA-type resin layer is obtained; the laminate is stretched and dyed to make the PVA-type resin layer into an absorption-type polarizing film. In this embodiment, it is preferred to form a polyvinyl alcohol-type resin layer containing a halide and a polyvinyl alcohol-type resin on one side of the resin substrate. Stretching typically includes immersing the laminate in a boric acid aqueous solution for stretching. In addition, stretching can further include stretching the laminate in a gas atmosphere at a high temperature (for example, above 95°C) before stretching in a boric acid aqueous solution as needed. In addition, in the present embodiment, it is preferred that the laminate is subjected to a drying shrinkage treatment in which the laminate shrinks by more than 2% in the width direction by heating while being conveyed in the length direction. Representatively, the manufacturing method of the present embodiment includes sequentially performing an auxiliary stretching treatment in a gas atmosphere, a dyeing treatment, a stretching treatment in an aqueous solution, and a drying shrinkage treatment on the laminate. By introducing auxiliary stretching, the crystallinity of the PVA can be improved even when the PVA is coated on the thermoplastic resin, and high optical properties can be achieved. In addition, by simultaneously improving the orientation of the PVA in advance, it is possible to prevent problems such as the reduction of the orientation and dissolution of the PVA when immersed in water in the subsequent dyeing process and the stretching process, and high optical properties can be achieved. In addition, when the PVA-type resin layer is immersed in a liquid, the orientation disorder of the polyvinyl alcohol molecules and the reduction of the orientation can be suppressed compared to the case where the PVA-type resin layer does not contain a halide. Thus, the optical properties of the absorption-type polarizing film obtained by the treatment process of immersing the laminate in a liquid such as a dyeing treatment and a stretching treatment in an aqueous solution can be improved. Further, the laminate is shrunk in the width direction by drying and shrinking treatment, thereby improving the optical properties. The obtained laminate of resin substrate / absorption type polarizing film can be used directly (that is, the resin substrate can be used as a protective layer of absorption type polarizing film), or the resin substrate can be peeled off from the laminate of resin substrate / absorption type polarizing film, and any appropriate protective layer corresponding to the purpose can be stacked on the peeling surface or on the side opposite to the peeling surface. The details of the manufacturing method of such an absorption type polarizing film are recorded in, for example, Japanese Patent Publication No. 2012-73580 and Japanese Patent No. 6470455. The records of these publications as a whole are cited in this specification as a reference.
[0130] The protective layer can be formed by any appropriate film that can be used as a protective layer of the absorption type polarizing film. As a specific example of the material that becomes the main component of the film, cycloolefins (COP) such as polynorbornenes, polyesters such as polyethylene terephthalate (PET), cellulose resins such as triacetyl cellulose (TAC), polycarbonate (PC), (meth) acrylic acid, polyvinyl alcohol, polyamide, polyimide, polyether sulfone, polysulfone, polystyrene, polyolefin, acetate and other transparent resins can be cited. In addition, thermosetting resins or ultraviolet curing resins such as (meth) acrylic acid, carbamate, (meth) acrylic acid carbamate, epoxy, silicone and the like can also be cited. In addition, glassy polymers such as siloxane polymers can also be cited. In addition, the polymer film described in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material of the film, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl and nitrile group in the side chain can be used, for example, a resin composition containing an alternating copolymer formed by isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer can be mentioned. The polymer film can be, for example, an extrusion molding of the above resin composition. The materials of the resin film can be used alone or in combination.
[0131] The thickness of the protective layer is typically 100 μm or less, for example, 5 μm to 80 μm, preferably 10 μm to 50 μm, and more preferably 15 μm to 35 μm.
[0132] <First phase difference member>
[0133] The first retardation member 20 includes a first λ / 4 member 20a. The first λ / 4 member 20a is arranged so that the angle between the absorption axis of the polarization member 10 (absorption type polarizing film) and the slow axis of the first λ / 4 member 20a is preferably 40° to 50°, more preferably 42° to 48°, for example, about 45°.
[0134] The in-plane phase difference Re(550) of the first λ / 4 component 20a is, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The first λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases in accordance with the wavelength of the measurement light. The Re(450) / Re(550) of the first λ / 4 component is, for example, not less than 0.75 and less than 1, or not less than 0.8 and not more than 0.95.
[0135] The refractive index characteristics of the first λ / 4 component preferably show a relationship of nx>ny≥nz. Here, "ny=nz" includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, within the range that does not impair the effect of the present invention, ny<nz may sometimes be satisfied. The Nz coefficient of the first λ / 4 component is preferably 0.9 to 3, more preferably 0.9 to 2.5, further preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.
[0136] The first λ / 4 member may be formed of any appropriate material that can satisfy the above-mentioned characteristics. The first λ / 4 member may be, for example, a stretched film of a resin film or an alignment fixing layer of a liquid crystal compound.
[0137] As the resin contained in the above-mentioned resin film, there can be mentioned: polycarbonate resin, polyester carbonate resin, polyester resin, polyvinyl acetal resin, polyarylate resin, cyclic olefin resin, cellulose resin, polyvinyl alcohol resin, polyamide resin, polyimide resin, polyether resin, polystyrene resin, acrylic resin, etc. These resins can be used alone or in combination. As a method of combination, for example, blending and copolymerization can be mentioned. In the case where the first λ / 4 component shows a reverse dispersion wavelength characteristic, a resin film containing a polycarbonate resin or a polyester carbonate resin (hereinafter, sometimes referred to as a polycarbonate resin) can be suitably used.
[0138] As the above-mentioned polycarbonate resin, any appropriate polycarbonate resin can be used. For example, the polycarbonate resin contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, and structural units derived from at least one dihydroxy compound selected from alicyclic diols, alicyclic dimethanols, di, tri or polyethylene glycols and alkylene glycols or spirodiols. Preferably, the polycarbonate resin contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, structural units derived from alicyclic dimethanols and / or structural units derived from di, tri or polyethylene glycols; more preferably, it contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, and structural units derived from di, tri or polyethylene glycols. The polycarbonate resin may also contain structural units derived from other dihydroxy compounds as needed. It should be noted that details of the polycarbonate resin that can be suitably used for the first λ / 4 component and the method for forming the first λ / 4 component are described in, for example, Japanese Patent Gazette No. 2014-10291, Japanese Patent Gazette No. 2014-26266, Japanese Patent Gazette No. 2015-212816, Japanese Patent Gazette No. 2015-212817, and Japanese Patent Gazette No. 2015-212818, and the records in these gazettes are cited as references in this specification.
[0139] The thickness of the first λ / 4 member formed of a stretched film of a resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 20 μm to 60 μm.
[0140] The orientation fixing layer of the above-mentioned liquid crystal compound is a layer in which the liquid crystal compound is oriented along a given direction within the layer and its orientation state is fixed. It should be noted that the "orientation fixing layer" is a concept that includes an orientation solidification layer obtained by solidifying a liquid crystal monomer as described later. In the 1st λ / 4 component, representatively, the rod-shaped liquid crystal compound is oriented in a state arranged along the slow axis direction of the 1st λ / 4 component (parallel orientation (homogeneous alignment)). As rod-shaped liquid crystal compounds, for example, liquid crystal polymers and liquid crystal monomers can be cited. The liquid crystal compound is preferably capable of polymerization. If the liquid crystal compound is capable of polymerization, the orientation state of the liquid crystal compound can be fixed by polymerizing after orienting the liquid crystal compound.
[0141] The orientation fixing layer (liquid crystal orientation fixing layer) of the above-mentioned liquid crystal compound can be formed by the following method: an orientation treatment is applied to the surface of a given substrate, a coating liquid containing a liquid crystal compound is applied to the surface, and the liquid crystal compound is oriented along the direction corresponding to the above-mentioned orientation treatment to fix the orientation state. As an orientation treatment, any appropriate orientation treatment can be adopted. Specifically, mechanical orientation treatment, physical orientation treatment, and chemical orientation treatment can be cited. As specific examples of mechanical orientation treatment, friction treatment and stretching treatment can be cited. As specific examples of physical orientation treatment, magnetic field orientation treatment and electric field orientation treatment can be cited. As specific examples of chemical orientation treatment, inclined evaporation method and optical orientation treatment can be cited. The processing conditions of various orientation treatments can adopt any appropriate conditions according to the purpose.
[0142] The liquid crystal compound can be aligned by treating it at a temperature corresponding to the type of the liquid crystal compound at which it exhibits a liquid crystal phase. By such a temperature treatment, the liquid crystal compound is in a liquid crystal state and is aligned in the alignment treatment direction of the substrate surface.
[0143] In one embodiment, the alignment state is fixed by cooling the aligned liquid crystal compound as described above. When the liquid crystal compound is polymerizable or crosslinkable, the alignment state can be fixed by subjecting the aligned liquid crystal compound to polymerization or crosslinking treatment as described above.
[0144] As the above-mentioned liquid crystal compound, any appropriate liquid crystal polymer and / or liquid crystal monomer can be used. Liquid crystal polymer and liquid crystal monomer can be used alone or in combination. Specific examples of liquid crystal compounds and methods for making liquid crystal orientation fixing layers are described in, for example, Japanese Patent Publication No. 2006-163343, Japanese Patent Publication No. 2006-178389, and International Publication No. 2018 / 123551. The records of these publications are cited as references in this specification.
[0145] The thickness of the first λ / 4 member composed of the liquid crystal alignment fixing layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and further preferably 1 μm to 4 μm.
[0146] <Protective components>
[0147] Typically, the protective member 30 includes a substrate. The substrate may be composed of any appropriate film. As the material that is the main component of the film constituting the substrate, for example, cellulose resins such as triacetyl cellulose (TAC), polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyether sulfones, polysulfones, polystyrenes, cycloolefins such as polynorbornene, polyolefins, (meth) acrylic acid, acetate resins, etc. can be cited. The thickness of the substrate is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and further preferably 15 μm to 35 μm.
[0148] The protective member preferably has a substrate and a surface treatment layer formed on the substrate. The surface treatment layer can be located on the outermost surface of the optical laminate 100a. The surface treatment layer can have any appropriate function. As the surface treatment layer, for example, a hard coating layer, an anti-reflection layer, an anti-adhesion layer, and an anti-glare layer can be cited. The protective member can also have more than two layers of surface treatment layers.
[0149] The anti-reflection layer is provided to prevent reflection of external light, etc. As the anti-reflection layer, for example, a fluororesin layer, a resin layer containing nanoparticles (representatively hollow nanoparticles, such as hollow nano silica particles), or an anti-reflection layer having a nanostructure (such as a moth-eye structure) can be cited. The thickness of the anti-reflection layer is preferably 0.05 μm to 1 μm. As a method for forming the above-mentioned resin layer, for example, a sol-gel method, a thermal curing method using isocyanate, an ionizing radiation curing method using a cross-linking monomer (such as a multifunctional acrylate) and a photopolymerization initiator (representatively a photocuring method) can be cited.
[0150] The hard coat layer preferably has sufficient surface hardness, excellent mechanical strength, and excellent light transmittance. The hard coat layer can be formed of any appropriate resin. Typically, the hard coat layer can be formed of an ultraviolet curable resin. Examples of ultraviolet curable resins include polyesters, acrylics, urethanes, amides, silicones, and epoxies. The thickness of the hard coat layer is, for example, 0.5 μm or more, preferably 1 μm or more, for example, 20 μm or less, preferably 15 μm or less.
[0151] A-2. Implementation Method 2
[0152] Figure 1B This is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention. Figure 1B The optical laminate 100b shown in the figure has a first adhesive layer a1, a polarizing member 10, a second adhesive layer a2, a first phase difference member 20 including a first λ / 4 member 20a, a third adhesive layer a3, and a protective member 30 in order, and the first phase difference member 20 is different from the optical laminate 100a in that it also includes a member (so-called positive C plate) 20b whose refractive index characteristic can show the relationship of nz>nx=ny in addition to the first λ / 4 member 20a. The angle formed by the absorption axis of the polarizing member 10 and the slow axis of the first λ / 4 member 20a is preferably 40° to 50°, more preferably 42° to 48°, for example, about 45°.
[0153] The first phase difference component 20 has a stacked structure of a 1st λ / 4 component 20a and a positive C plate 20b. Specifically, the 1st λ / 4 component 20a and the positive C plate 20b are stacked together via an adhesive layer b1. Preferably, as shown in the example in the figure, the 1st λ / 4 component 20a is located closer to the polarization component 10 side than the positive C plate 20b, but their configuration may also be the opposite. The adhesive layer b1 is representatively an adhesive layer or an adhesive layer. In the case where the adhesive layer b1 is an adhesive layer, the total number of adhesive layers in the optical laminate 100b is 3, of which more than two adhesive layers are adhesive layers A, and preferably all three are adhesive layers A. In the case where the adhesive layer b1 is an adhesive layer, the total number of adhesive layers in the optical laminate 100b is 4, in which case also more than two adhesive layers are the above-mentioned adhesive layers A, preferably more than three, and more preferably all four adhesive layers are adhesive layers A. The adhesive layer is formed of, for example, an ultraviolet curing adhesive, and has a thickness of, for example, 0.05 μm to 30 μm.
[0154] The thickness of the optical layered body 100 b is, for example, 100 μm or more and 300 μm or less, preferably 110 μm or more and 250 μm or less, and more preferably 120 μm or more and 200 μm or less.
[0155] The pressure-sensitive adhesive layer, the polarizing member, the first λ / 4 member, and the protective member are as described in the section A-1.
[0156] <Positive C plate>
[0157] The phase difference Rth(550) in the thickness direction of the positive C plate 20b is preferably -50nm to -300nm, more preferably -70nm to -250nm, further preferably -90nm to -200nm, and particularly preferably -100nm to -180nm. Here, "nx=ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The in-plane phase difference Re(550) of the positive C plate is, for example, less than 10nm.
[0158] The positive C plate can be formed of any appropriate material. The positive C plate is preferably composed of a film containing a liquid crystal material fixed in a homeotropic orientation. The liquid crystal material (liquid crystal compound) capable of homeotropic orientation can be a liquid crystal monomer or a liquid crystal polymer. As a specific example of such a liquid crystal compound and a method for forming a positive C plate, there can be cited the method for forming a liquid crystal compound and a phase difference layer described in
[0020] to
[0028] of Japanese Patent Gazette No. 2002-333642. In this case, the thickness of the positive C plate is preferably 0.5μm to 5μm.
[0159] B. Display System
[0160] Figure 2 Schematic diagram showing a simplified structure of an example of a display system (goggles with a display) including the optical laminate described in Item A. Figure 2 (a) schematically shows the configuration and shape of the main components of the display system 2. Figure 2 (b) Yes Figure 2 (a) is a schematic diagram for explaining the arrangement of the optical layered body in the case where the display system 2 shown is a liquid crystal display system.
[0161] like Figure 2As shown in (a), the display system 2 includes a display element 12, a reflective polarization member 14, a first lens unit 16, a half mirror 18, a first phase difference member 20, a second phase difference member 22, and a second lens unit 24. The reflective polarization member 14 is arranged on the display surface 12' side of the display element 12, that is, in front, and can reflect the light emitted from the display element 12. The first lens unit 16 is arranged on the optical path between the display element 12 and the reflective polarization member 14, and the half mirror 18 is arranged between the display element 12 and the first lens unit 16. The first phase difference member 20 is arranged on the optical path between the display element 12 and the half mirror 18, and the second phase difference member 22 is arranged on the optical path between the half mirror 18 and the reflective polarization member 14. Although not shown in the figure, the display system 2 may further include an absorptive polarization member between the reflective polarization member 14 and the second lens unit 24.
[0162] Components arranged in front of the half mirror (in the illustrated example, the half mirror 18 , the first lens unit 16 , the second phase difference element 22 , the reflective polarization element 14 , and the second lens unit 24 ) are sometimes collectively referred to as a lens unit (lens unit 4 ).
[0163] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12' for displaying an image. Light emitted from the display surface 12' passes through, for example, a polarizing member 10 that may be included in the display element 12, and then is emitted as first linearly polarized light.
[0164] The first phase difference component 20 includes a 1st λ / 4 component capable of converting the 1st linear polarized light incident on the first phase difference component 20 into the 1st circularly polarized light. In the case where the first phase difference component does not include a component other than the 1st λ / 4 component, the first phase difference component can be equivalent to the 1st λ / 4 component. It should be noted that in the example shown in the figure, for the sake of illustration, a space is sandwiched between the first phase difference component 20 and the display element 12, but as described later, by using an optical laminate including a polarization component and a first phase difference component (1st λ / 4 component) as described in item A in the display system of the embodiment of the present invention, the first phase difference component 20 and the display element 12 are integrally arranged.
[0165] The half mirror 18 transmits the light emitted from the display element 12 and reflects the light reflected by the reflective polarization member 14 toward the reflective polarization member 14. The half mirror 18 is integrally provided with the first lens portion 16.
[0166] The second phase difference member 22 includes a second λ / 4 member that allows the light reflected by the reflective polarization member 14 and the half mirror 18 to pass through the reflective polarization member 14. When the second phase difference member does not include a member other than the second λ / 4 member, the second phase difference member may be equivalent to the second λ / 4 member. The second phase difference member 22 may be integrally provided on the first lens portion 16.
[0167] The first circularly polarized light emitted from the first λ / 4 member included in the first phase difference member 20 passes through the half mirror 18 and the first lens unit 16, and is converted into the second linearly polarized light by the second λ / 4 member included in the second phase difference member 22. The second linearly polarized light emitted from the second λ / 4 member does not pass through the reflective polarization member 14, but is reflected toward the half mirror 18. At this time, the polarization direction of the second linearly polarized light incident on the reflective polarization member 14 is the same direction as the reflection axis of the reflective polarization member 14. Therefore, the second linearly polarized light incident on the reflective polarization member 14 is reflected by the reflective polarization member 14.
[0168] The second linear polarized light reflected by the reflective polarization member 14 is converted into the second circular polarized light by the second λ / 4 member included in the second phase difference member 22, and the second circular polarized light emitted from the second λ / 4 member passes through the first lens unit 16 and is reflected by the half mirror 18. The second circular polarized light reflected by the half mirror 18 passes through the first lens unit 16 and is converted into the third linear polarized light by the second λ / 4 member included in the second phase difference member 22. The third linear polarized light is transmitted through the reflective polarization member 14. At this time, the polarization direction of the third linear polarized light incident on the reflective polarization member 14 is the same direction as the transmission axis of the reflective polarization member 14. Therefore, the third linear polarized light incident on the reflective polarization member 14 is transmitted through the reflective polarization member 14.
[0169] As described above, the display system 2 may include an absorptive polarizing element (representatively an absorptive polarizing film) in front of the reflective polarizing element 14 (on the side close to the eyes). The reflection axis of the reflective polarizing element 14 and the absorption axis of the absorptive polarizing element may be arranged substantially parallel to each other, and the transmission axis of the reflective polarizing element and the transmission axis of the absorptive polarizing element may be arranged substantially parallel to each other. Thus, the third linear polarized light after passing through the reflective polarizing element 14 may directly pass through the absorptive polarizing element. The reflective polarizing element and the absorptive polarizing element may be laminated together, for example, via an adhesive layer.
[0170] The light transmitted through the reflective polarization element 14 passes through the second lens portion 24 and enters the eye 26 of the user.
[0171] For example, the absorption axis of the polarization component 10 included in the display element 12 and the reflection axis of the reflective polarization component 14 can be arranged approximately parallel to each other, or approximately orthogonal to each other. The angle formed by the absorption axis of the polarization component 10 included in the display element 12 and the slow axis of the 1st λ / 4 component included in the first phase difference component 20 is, for example, 40° to 50°, 42° to 48°, or approximately 45°. The angle formed by the absorption axis of the polarization component 10 included in the display element 12 and the slow axis of the 2nd λ / 4 component included in the second phase difference component 22 is, for example, 40° to 50°, 42° to 48°, or approximately 45°. The first phase difference component 20 including the polarization component 10 and the 1st λ / 4 component is as described in item A.
[0172] The in-plane phase difference Re(550) of the second λ / 4 component is, for example, 100nm to 190nm, 110nm to 180nm, 130nm to 160nm, or 135nm to 155nm. The second λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measurement light. The second λ / 4 component preferably satisfies the relationship Re(450)<Re(550)<Re(650). Re(450) / Re(550) of the second λ / 4 component is, for example, greater than 0.75 and less than 1, or greater than 0.8 and less than 0.95.
[0173] Figure 2 (b) shows the configuration of the optical stack when the display system 2 is a liquid crystal display system. As the optical stack 100, it is preferable to use Figure 1A or Figure 1BThe optical laminate 100a, 100b described in the figure. In the example shown in the figure, the display element 12 includes a backlight unit 12a, a backlight side polarization component 12b, a liquid crystal unit 12c, and a polarization component 10. Representatively, the backlight side polarization component 12b and the polarization component 10 are arranged in a manner so that the absorption axis directions are approximately orthogonal to each other, and together with the liquid crystal unit 12c, they constitute a liquid crystal panel. The optical laminate 100 is arranged on the display element 12 side of the half mirror 18, wherein the polarization component 10 is bonded to the liquid crystal unit 12c via an adhesive layer a1, and the first phase difference component 20 (the first λ / 4 component) is bonded to the polarization component 10 via an adhesive layer a2, as a result, the display element 12 and the first phase difference component 20 (the first λ / 4 component) are arranged as a whole. In addition, by configuring the protective member 30 having a surface treatment layer so that the surface treatment layer becomes the most surface, it is possible to obtain an excellent anti-reflection effect in a display system in which a space is formed between the half mirror 18 and the first phase difference member 20 (protective member 30). It should be noted that in the embodiment of the figure example, the optical laminate 100 is attached to the liquid crystal unit, but the optical laminate of the embodiment of the present invention can also constitute an organic EL display system together with the organic EL panel. In this case, a third phase difference member including a 3λ / 4 member can be configured between the optical laminate 100 and the organic EL panel. The third phase difference member may be included in the optical laminate of the embodiment of the present invention. For example, the optical laminate of the embodiment of the present invention may have a third phase difference member, a polarization member, a first phase difference member, and a protective member in sequence via an adhesive layer. Specifically, the optical laminate may have a structure of [adhesive layer / third phase difference member / adhesive layer / polarization member / adhesive layer / first phase difference member / adhesive layer / protective member], in which at least 4 adhesive layers may be included. When the total number of adhesive layers is 4, adhesive layer A can be used for 2 or more, preferably 3 or 4 of the adhesive layers. The in-plane phase difference Re (550) of the 3rd λ / 4 component is, for example, 100nm to 190nm, 110nm to 180nm, 130nm to 160nm, or 135nm to 155nm. As the 3rd λ / 4 component, the same description as the 1st λ / 4 component can be applied. The third phase difference component can be configured in such a way that the slow axis of the 3rd λ / 4 component forms an angle of, for example, 40° to 50°, 42° to 48°, or about 45° with the absorption axis of the polarization component 10.
[0174] Example
[0175] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. It should be noted that the thickness is a value measured by the following measurement method.
[0176] <Thickness>
[0177] The thickness of 10 μm or less was measured using a scanning electron microscope (manufactured by JEOL Ltd., product name “JSM-7100F”). The thickness exceeding 10 μm was measured using a digital micrometer (manufactured by Anritsu Co., Ltd., product name “KC-351C”).
[0178] <In-plane phase difference>
[0179] The in-plane phase difference at 23° C. was measured using “KOBRA-WPR” manufactured by Oji Scientific Instruments Co., Ltd.
[0180] <Linear expansion coefficient>
[0181] The adhesive layer (thickness 1 mm) was cut into approximately 5 mm squares and used as measurement samples. The measurement samples were set on a sample stand of a measurement device, and TMA measurement was performed under the following conditions.
[0182] ·Measurement device: "TMA / SS6000" manufactured by SII NanoTechnology
[0183] ·Measurement mode: Compression expansion method
[0184] ·Measurement load: 9.8mN
[0185] Probe diameter: 3.5mmφ (compression expansion method)
[0186] Temperature program: -60℃→210℃→-70℃→200℃
[0187] Heating / cooling speed: 10℃ / min
[0188] ·Measurement atmosphere: N2 (flow rate: 200ml / min)
[0189] <Determination of molecular weight>
[0190] The weight average molecular weight of the (meth)acrylic polymer was measured by GPC (gel permeation chromatography) and calculated in terms of polystyrene.
[0191] ·Analysis device: Made by Tosoh Corporation, HLC-8120GPC
[0192] Data processing device: GPC-8020 manufactured by Tosoh Corporation
[0193] ·Chromatographic column: Tosoh Corporation, G7000HXL-H+GMHXL+GMHXL
[0194] Column size: 7.8mmφ×30cm each (90cm in total)
[0195] Flow rate: 0.8ml / min
[0196] Injection sample concentration: about 0.1% by weight
[0197] Injection volume: 100μl
[0198] Column temperature: 40℃
[0199] ·Eluent: Tetrahydrofuran
[0200] Detector: Differential Refractometer (RI)
[0201] [Manufacturing Example 1A: Preparation of Adhesive Layer 1]
[0202] <Acrylic polymer 1>
[0203] In a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube, and a condenser, 92 parts by weight of butyl acrylate, 5 parts by weight of N-acryloylmorpholine (ACMO), 2.9 parts by weight of acrylic acid, 0.1 parts by weight of 2-hydroxyethyl acrylate, 0.1 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator, and 100 parts by weight of ethyl acetate were added, and nitrogen was introduced while slowly stirring to replace the atmosphere with nitrogen. Then, the liquid temperature in the flask was maintained at about 55° C. and a polymerization reaction was performed for 8 hours to prepare a solution of acrylic polymer 1. The weight average molecular weight of acrylic polymer 1 was 2,000,000.
[0204] <Binder solution 1>
[0205] With respect to 100 parts by weight of the solid content of the solution of acrylic polymer 1, 0.15 parts by weight of dibenzoyl peroxide (1 minute half-life: 130° C.) as a crosslinking agent and 0.6 parts by weight of a polyisocyanate crosslinking agent consisting of a trimethylolpropane adduct of toluene diisocyanate (Coronate L, manufactured by Nippon Polyurethane Industries, Ltd.) were mixed to prepare an acrylic adhesive solution 1.
[0206] <Adhesive layer 1>
[0207] The acrylic adhesive solution 1 was applied to one side of a silicone-treated polyethylene terephthalate (PET) film (Mitsubishi Chemical Polyester Film Co., Ltd., thickness: 38 μm) and dried / crosslinked at 150° C. for 3 minutes to form an adhesive layer 1 having a thickness of 5 μm after drying.
[0208] [Manufacturing Example 1B: Preparation of Adhesive Layer 2]
[0209] <Acrylic polymer 2>
[0210] A monomer mixture containing 94.9 parts by weight of butyl acrylate, 5 parts by weight of acrylic acid and 0.1 parts by weight of 2-hydroxyethyl acrylate was added to a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube and a condenser. Furthermore, 0.3 parts by weight of dibenzoyl peroxide as a polymerization initiator was added together with ethyl acetate to 100 parts by weight of the monomer mixture, and nitrogen was introduced while slowly stirring to replace the flask with nitrogen. The liquid temperature in the flask was maintained at 60° C. and a polymerization reaction was performed for 7 hours. Next, ethyl acetate was added to the obtained reaction solution to adjust the solid content concentration to 30% by weight to obtain a solution of acrylic polymer 2. The weight average molecular weight of acrylic polymer 2 was 2.2 million.
[0211] <Binder solution 2>
[0212] Acrylic adhesive solution 2 was prepared by mixing 0.6 parts by weight of a polyisocyanate crosslinking agent (trimethylolpropane / toluene diisocyanate adduct, Coronate L manufactured by Nippon Polyurethane Industries, Ltd.) and 0.075 parts by weight of a silane coupling agent (KBM403 manufactured by Shin-Etsu Chemical Co., Ltd.) with respect to 100 parts by weight of the solid content of the solution of acrylic polymer 2.
[0213] <Adhesive layer 2>
[0214] The acrylic adhesive solution 2 was applied to one side of a silicone-treated polyethylene terephthalate (PET) film (Mitsubishi Chemical Polyester Film Co., Ltd., thickness: 38 μm) and dried at a given temperature to form an adhesive layer 2 having a thickness of 12 μm, 15 μm, or 20 μm.
[0215] [Manufacturing Example 2: Preparation of Polarizing Film 1]
[0216] A 30 μm thick polyvinyl alcohol (PVA) resin film (manufactured by Kuraray Co., Ltd., product name "PE3000") was uniaxially stretched in the length direction to 5.9 times the length using a roller stretching machine, and then swollen, dyed, cross-linked, and cleaned, and finally dried to produce an absorption-type polarizing film with a thickness of 12 μm.
[0217] Specifically, the swelling treatment was carried out while being treated in pure water at 20°C and stretched to 2.2 times. Next, the dyeing treatment was carried out while being treated in a 30°C aqueous solution in which the weight ratio of iodine to potassium iodide was 1:7 after the iodine concentration was adjusted so that the monomer transmittance of the obtained absorption-type polarizing film reached 45.0%, and the film was stretched to 1.4 times. Furthermore, the cross-linking treatment adopted a two-stage cross-linking treatment, and the first stage of the cross-linking treatment was treated while being stretched to 1.2 times in an aqueous solution of boric acid and potassium iodide dissolved at 40°C. The boric acid content of the aqueous solution of the first stage of the cross-linking treatment was 5.0% by weight, and the potassium iodide content was 3.0% by weight. The second stage of the cross-linking treatment was treated while being stretched to 1.6 times in an aqueous solution of boric acid and potassium iodide dissolved at 65°C. The boric acid content of the aqueous solution of the second stage of the cross-linking treatment was 4.3% by weight, and the potassium iodide content was 5.0% by weight. In addition, the cleaning treatment was carried out in a potassium iodide aqueous solution at 20°C. The potassium iodide content of the aqueous solution in the washing treatment was adjusted to 2.6 wt %. Finally, the aqueous solution was dried at 70° C. for 5 minutes to obtain an absorption-type polarizing film.
[0218] A triacetyl cellulose (TAC) resin film (thickness: 22 μm) was laminated as a protective layer on both sides of the obtained absorption-type polarizing film via an ultraviolet curing adhesive. Specifically, the ultraviolet curing adhesive was applied so that the total thickness reached about 1 μm, and the film was laminated using a roller press. Then, UV light was irradiated from the TAC film side to cure the adhesive.
[0219] Thus, a polarizing film 1 (thickness 57 μm) having a structure of [TAC film (protective layer) / absorptive polarizing film / TAC film (protective layer)] was obtained.
[0220] [Manufacturing Example 3: Preparation of λ / 4 Member 1]
[0221] The polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and a reflux condenser controlled at 100° C. 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of isosorbide (ISB), 42.28 parts by mass (0.139 mol) of spiroglycol (SPG), 63.77 parts by mass (0.298 mol) of diphenyl carbonate (DPC), and 1.19×10-6 parts by mass of calcium acetate monohydrate as a catalyst were added. -2 Mass parts (6.78×10 -5mol). After the reactor was replaced with nitrogen under reduced pressure, it was heated by a heat medium and stirring was started when the internal temperature reached 100°C. The internal temperature reached 220°C 40 minutes after the start of the temperature rise, and the pressure was reduced while controlling to maintain the temperature, so that it reached 13.3kPa after 90 minutes after reaching 220°C. The phenol vapor produced as a by-product during the polymerization reaction was introduced into a 100°C reflux condenser, so that a certain amount of monomer components contained in the phenol vapor was returned to the reactor, and the uncondensed phenol vapor was introduced into a 45°C condenser for recovery. After nitrogen was introduced into the first reactor to temporarily restore it to atmospheric pressure, the reaction liquid after oligomerization in the first reactor was transferred to the second reactor. Next, the temperature rise and pressure reduction in the second reactor were started, so that it reached an internal temperature of 240°C and a pressure of 0.2kPa after 50 minutes. Then, the polymerization was carried out until the given stirring power was reached. When the predetermined power was reached, nitrogen gas was introduced into the reactor to restore the pressure, and the produced polyester carbonate resin was extruded into water, and the strands were cut to obtain pellets.
[0222] After the obtained polyester carbonate resin (pellets) was vacuum dried at 80°C for 5 hours, a long strip of resin film with a thickness of 135 μm was produced using a film-making device equipped with a single screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200 mm, setting temperature: 250°C), a chill roll (setting temperature: 120-130°C) and a winder. The obtained long strip of resin film was stretched in the width direction at a stretching temperature of 143°C and a stretching ratio of 2.8 times. Thus, a stretched film (λ / 4 component 1) with a thickness of 51 μm was obtained. The Re(590) of the λ / 4 component 1 is 143 nm, the Re(450) / Re(550) is 0.86, and the Nz coefficient is 1.12.
[0223] [Manufacturing Example 4: Preparation of Protective Member 1]
[0224] The hard coating layer forming material shown below was applied to the acrylic film having a lactone ring structure, and the coating layer was dried to form a hard coating layer with a thickness of 0.5 μm. Next, the antireflection layer forming material shown below was applied to the surface of the hard coating layer, heated at 80°C for 1 minute, and the heated coating layer was irradiated with a high pressure mercury lamp with a cumulative light intensity of 300 mJ / cm 2 The coating layer was cured by ultraviolet light to form an antireflection layer with a thickness of 0.1 μm. Thus, a protective member 1 (thickness 44 μm) having a structure of [acrylic film / hard coat layer / antireflection layer] was obtained.
[0225] (Hard coat layer forming material)
[0226] A material for forming a hard coat layer was prepared by adding 0.5 wt % of a leveling agent to an acrylic resin raw material (manufactured by Dainippon Ink Co., Ltd., trade name: GRANDIC PC1071), and further diluting with ethyl acetate so that the solid content concentration reaches 50 wt %. It should be noted that the leveling agent is a copolymer obtained by copolymerizing dimethylsiloxane:hydroxypropylsiloxane:6-isocyanatehexylisocyanuric acid:aliphatic polyester at a molar ratio of 6.3:1.0:2.2:1.0.
[0227] (Anti-reflection layer forming material)
[0228] 100 parts by weight of a multifunctional acrylate containing pentaerythritol triacrylate as the main component (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name "Viscoat #300", solid content 100% by weight), 100 parts by weight of hollow nano-silica particles (manufactured by JGC Catalysts & Chemicals Co., Ltd., trade name "THRULYA 5320", solid content 20% by weight, weight average particle size 75 nm), solid nano-silica particles (manufactured by Nissan Chemical Industries, Ltd., trade name "MEK-2140Z-AC", solid content 30% by weight, weight average particle size 10 nm), 12 parts by weight of a fluorine-containing additive (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KY-1203", solid content 20% by weight), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD 907", solid content 100% by weight) were mixed. To this mixture, a mixed solvent of tert-butyl alcohol, methyl isobutyl ketone, and propylene glycol monomethyl ether acetate in a weight ratio of 60:25:15 was added so that the total solid content became 4% by weight, and the mixture was stirred to prepare an antireflection layer forming material.
[0229] [Example 1]
[0230] On one side of the polarizing film 1, an adhesive layer 1 (5 μm thick) was attached together with a PET film, another adhesive layer 1 (5 μm thick) was transferred from the PET film to the other side of the polarizing film 1, and a λ / 4 member 1 was attached thereto. At this time, the arrangement was performed so that the absorption axis of the absorption-type polarizing film and the slow axis of the λ / 4 member 1 formed an angle of 45°.
[0231] Next, another adhesive layer 1 (5 μm thick) was transferred from the PET film to the surface of the λ / 4 member 1, and the protective member 1 was bonded thereto. At this time, the protective member 1 was bonded so that the acrylic film side surface was on the λ / 4 member 1 side (in other words, so that the surface treatment layer was on the uppermost surface).
[0232] Thus, an optical laminate having a structure of [release liner (PET film) / adhesive layer 1 / polarizing film 1 / adhesive layer 1 / λ / 4 member 1 / adhesive layer 1 / protective member 1] was obtained.
[0233] [Example 2, Comparative Examples 1-2]
[0234] An optical layered body was obtained in the same manner as in Example 1 except that at least one of the three pressure-sensitive adhesive layers 1 was replaced with a pressure-sensitive adhesive layer 2. The configuration of each optical layered body is shown in Table 1. Table 2 also shows the linear expansion coefficients of the pressure-sensitive adhesive layers 1 and 2 (average value for N=2).
[0235] <Wet heat test>
[0236] The release liner was peeled off from the optical laminate obtained in the embodiment and the comparative example, and the test sample was bonded to the glass plate via the exposed adhesive layer. The test sample was placed in a humid heat oven at 65°C and 90RH% for 240 hours. Before the test, the in-plane phase difference of the optical laminate that was placed for 120 hours or 240 hours was measured. The in-plane phase difference was measured by taking the test sample out of the oven and irradiating the measurement light from the glass plate side. The results are shown in Table 1 and Figure 3 It should be noted that in Table 1, the phase difference change represents the Re (590) of the optical laminate before the test. before Re(590) of the optical laminate after 240 hours of storage after Difference (Re(590) before -Re(590) after ).
[0237] [Table 1]
[0238]
[0239] [Table 2]
[0240]
[0241] As shown in Tables 1 and 2, the optical layered bodies of Examples in which two or more of the three pressure-sensitive adhesive layers satisfied the relationship of 0.8≤α1 / α2≤1.2 were excellent in the stability of optical properties under wet heat conditions.
[0242] The present invention is not limited to the above-described embodiments, and various modifications are possible. For example, the above-described embodiments may be replaced with substantially the same configuration, a configuration that exhibits the same effects, or a configuration that achieves the same purpose.
[0243] Industrial Applicability
[0244] The optical layered body according to the embodiment of the present invention can be used for the production of goggles with a display, such as VR goggles, for example.
Claims
1. An optical laminate comprising at least one optical member and at least one adhesive layer, When the total number of the adhesive layers included in the optical laminate is N, the adhesive layers greater than N / 2 are adhesive layers A whose linear expansion coefficient α1 when heated from 20°C to 30°C and linear expansion coefficient α2 when cooled from 30°C to 20°C satisfy the relationship 0.8≤α1 / α2≤1.
2.
2. The optical layered body according to claim 1, in, The thickness of the adhesive layer A is 1 μm or more and 15 μm or less. The optical layered body according to claim 1 , which has a thickness of 100 μm to 300 μm.
4. The optical layered body according to claim 1, in, The optical laminate includes a first adhesive layer, a polarizing member, a second adhesive layer, a first phase difference member, a third adhesive layer, and a protective member in this order. Two or more selected from the group consisting of the first adhesive layer, the second adhesive layer, and the third adhesive layer are the adhesive layer A.
5. The optical layered body according to claim 4, in, The first phase difference element includes a λ / 4 element.
6. The optical layered body according to claim 4, in, The protection member has a surface treatment layer.
7. The optical layered body according to claim 1, in, The pressure-sensitive adhesive composition constituting the pressure-sensitive adhesive layer A includes a (meth)acrylic polymer having a weight average molecular weight of 1.5 million or more. 8 . A display system comprising the optical layered body according to claim 1 .
9. The display system according to claim 8, comprising: A display element having a display surface for emitting light displaying an image forward via a polarizing member; a reflective polarizing member disposed in front of the display element to reflect light emitted from the display element; A first lens portion disposed on an optical path between the display element and the reflective polarization component; a half mirror disposed between the display element and the first lens portion, transmitting light emitted from the display element and reflecting light reflected from the reflective polarization member toward the reflective polarization member; a first λ / 4 member disposed on an optical path between the display element and the half mirror; as well as a second λ / 4 member disposed on an optical path between the half mirror and the reflective polarization member, The optical layered body according to claim 5 is disposed on the display element side of the half mirror, so that the display element and the first λ / 4 plate are provided integrally.