Top plate for haptic presentation device, method for manufacturing same, and haptic presentation device
By setting a specific concave and convex structure on the top plate of the tactile presentation device, the problem of insufficient frictional force change in the prior art is solved, and more sufficient tactile expressiveness and sliding sensory changes are achieved.
Patent Information
- Application Number
- CN202380027926.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-08
- Filing Date
- 2023-06-29
- Publication Date
- 2024-11-01
AI Technical Summary
The range of changes in friction in existing tactile presentation devices is insufficient, resulting in insufficient tactile expressiveness.
Design a top plate for a tactile presentation device, and a specific concave and convex structure is provided on the outer main surface of the main surface, including a first concave and convex with a large interval width and a second concave and convex with a small interval width, by adjusting the cutoff of the high-frequency filter and the low-pass filter. The value is used to control the surface roughness of the concave and convexity and increase the change amplitude of friction.
It effectively improves the tactile expressiveness of the tactile presentation device, increases the range of friction, enhances the change in the contact state between the fingertip and the outer main surface, and enhances the diversity of sliding sensation.
Smart Images

Figure CN118891604A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a top plate for a tactile presentation device, a tactile presentation device, and a method for manufacturing the top plate for the tactile presentation device. Background Art
[0002] In recent years, tactile presentation devices that provide information through tactile sensation have attracted much attention. For example, tactile presentation devices that can change the tactile sensation of a person when the person operates a touch panel have been studied.
[0003] For example, Patent Document 1 below discloses a tactile presentation device that changes the frictional force when a person touches the device. The tactile presentation device includes a top plate as a portion that comes into contact with a person. Ultrasonic waves are applied to the top plate to change the tactile sensation.
[0004] In addition, Patent Document 2 below discloses a top plate whose outer main surface located outside a tactile presentation device has an arithmetic mean roughness (Ra) of 2 nm or more and 100 nm or less. Patent Document 2 states that applying ultrasonic waves to such a top plate can improve the expressiveness of the tactile presentation device.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-181068
[0008] Patent Document 2: Japanese Patent Application Publication No. 2018-180621 Summary of the invention
[0009] Problems to be solved by the invention
[0010] However, the tactile presentation device described in Patent Document 1 has a problem that the change in friction force is small and the width of the tactile presentation is insufficient. In addition, the tactile presentation device described in Patent Document 2 also has a limited range of change in friction force, which makes it difficult to fully improve the tactile presentation.
[0011] The object of the present invention is to provide a top plate for a tactile presentation device, a tactile presentation device and a method for manufacturing the top plate for a tactile presentation device, which can fully increase the variation range of friction force and effectively improve the tactile expression.
[0012] Methods for solving problems
[0013] The top plate for a tactile presentation device of mode 1 of the present invention is a top plate for a tactile presentation device, characterized in that it has an outer main surface located outside the tactile presentation device, and is provided with concave-convex surfaces on at least a portion of the outer main surface, the concave-convex surfaces having: a first concave-convex surface, when the cutoff value of the high-frequency filter λc1 is set to a value 5 times the interval between the concave-convex surfaces of the measured cross-sectional curve, and the cutoff value of the low-pass filter λs1 is set to 26.6μm, the maximum height of the concave-convex surface is 0.5nm~2000nm, and the interval between the concave-convex surface is 50μm~2000μm; and a second concave-convex surface, when the cutoff value of the high-frequency filter λc2 is set to 14μm, and the cutoff value of the low-pass filter λs2 is set to 0.35μm, the three-dimensional arithmetic mean height Sa of the concave-convex surface is 0.5nm~100nm, and the maximum height Sz of the concave-convex surface is greater than 8nm.
[0014] The top plate for the tactile presentation device of method 2 can be in method 1, wherein the second concave-convex part is in the measuring area of 74×55μm, and when the cutoff value of the high-frequency filter λc2 is set to 14μm and the cutoff value of the low-pass filter λs2 is set to 0.35μm, the kurtosis Sku is greater than 3.2 and the skewness Ssk is less than -0.1.
[0015] The top plate for a tactile presentation device of mode 3 of the present invention is a top plate for a tactile presentation device, characterized in that it has an outer main surface located outside the tactile presentation device, and is provided with concave-convex portions on at least a portion of the outer main surface, the concave-convex portions having: a first concave-convex portion, wherein when the cutoff value of the high-frequency filter λc1 is set to 14μm and the cutoff value of the low-pass filter λs1 is set to 0.35μm, the maximum height of the concave-convex portion is 0.5nm~2000nm, and the interval between the concave-convex portions is 3μm to less than 50μm; and a second concave-convex portion, wherein in an area of a square with a side length of 5μm, when the cutoff value of the high-frequency filter λc2 is set to 2.5μm, the three-dimensional arithmetic mean height Sa of the concave-convex portion is 0.5nm~100nm, and the maximum height Sz of the concave-convex portion is greater than 8nm.
[0016] The top plate for the tactile presentation device of method 4 can be in method 3, wherein the second concave-convex is in a square area with a side length of 5 μm, and when the cutoff value of the high-frequency filter λc2 is set to 2.5 μm, the kurtosis Sku is greater than 3.2 and the skewness Ssk is less than -0.1.
[0017] The top plate for the tactile presentation device of aspect 5 may be made of glass in any of aspects 1 to 4.
[0018] The top plate for the tactile presentation device of aspect 6 may be transparent in any of aspects 1 to 5.
[0019] A tactile presentation device according to a seventh aspect of the present invention is characterized by comprising: a tactile presentation device top plate according to any one of aspects 1 to 6; and an actuator for applying ultrasonic waves to the tactile presentation device top plate.
[0020] The manufacturing method of the top plate for a tactile presentation device of mode 8 of the present invention is a manufacturing method of the top plate for a tactile presentation device of any one of modes 1 to 6, characterized in that it includes: a process of preparing an original panel having a main surface; and a process of performing a wet spray treatment on the main surface of the original panel.
[0021] Effects of the Invention
[0022] According to the present invention, it is possible to provide a top plate for a tactile presentation device, a tactile presentation device, and a method for manufacturing the top plate for a tactile presentation device that can sufficiently increase the variation range of frictional force and effectively improve the expressiveness of tactile sensation. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 1 is a schematic cross-sectional view showing a tactile sense presentation device according to an embodiment of the present invention.
[0024] Figure 2 It is a diagram for explaining a measured cross-sectional curve of the outer main surface of the top plate for a tactile presentation device.
[0025] Figure 3 This is a schematic cross-sectional view of a tactile sense presentation device showing a modified example of one embodiment of the present invention.
[0026] Figure 4 (a) and Figure 4 (b) is a schematic cross-sectional view for explaining an example of a method for manufacturing a top plate for a tactile presentation device. DETAILED DESCRIPTION
[0027] Hereinafter, preferred embodiments will be described. However, the following embodiments are merely illustrative, and the present invention is not limited to the following embodiments. In addition, in each of the drawings, components having substantially the same function are sometimes referred to with the same reference numerals.
[0028] [Top plate for tactile presentation device and tactile presentation device]
[0029] (First embodiment)
[0030] Figure 1 2 is a schematic cross-sectional view showing a tactile presentation device according to a first embodiment of the present invention. Figure 1As shown, the tactile presentation device 10 of this embodiment includes: a housing 2 having an opening 2a; a top plate 1 that seals the opening 2a; and an actuator 5 that is provided in contact with the top plate 1. The top plate 1 is a top plate for the tactile presentation device of the present invention. The actuator 5 is a piezoelectric element that applies ultrasonic waves to the top plate 1.
[0031] The tactile sense presentation device 10 further includes a display 3 provided in a housing 2 and a touch sensor 4 provided on the display 3. In the present embodiment, the top plate 1 is made of transparent glass, and the touch sensor 4 is a touch panel that transmits light.
[0032] The top plate 1 has an outer main surface 1a located outside (on the user side) of the tactile presentation device 10. The tactile presentation device 10 is a device that changes the tactile sensation of the outer main surface 1a. More specifically, the friction of the outer main surface 1a changes. For example, when a person slides a finger on the outer main surface 1a, if ultrasonic waves are applied to the portion by the actuator 5, the finger is lifted up by the vibrating outer main surface 1a. As a result, the friction between the finger and the outer main surface 1a becomes smaller.
[0033] The tactile presentation device 10 includes: a vibration control unit (not shown) that controls the position and amplitude of ultrasonic waves applied to the top plate 1 through the actuator 5; and an image control unit (not shown) that controls the image to be displayed on the display 3. The vibration control unit is connected to the actuator 5, the touch sensor 4 and the image control unit. When a person touches the top plate 1, the position touched by the person is detected by the touch sensor 4. The position data of the position touched by the person is input to the vibration control unit from the touch sensor 4. In addition, the position data of the image displayed on the display 3 and the like are also input to the vibration control unit from the image control unit. The vibration control unit controls the frequency and amplitude of ultrasonic waves applied to the top plate 1 through the actuator 5 based on the position data and the image displayed on the display 3.
[0034] By combining the part to which the ultrasonic wave is applied and the part to which the ultrasonic wave is not applied by the vibration control unit, or by controlling the frequency of the ultrasonic wave, the friction force of each part of the outer main surface 1a of the top plate 1 can be adjusted. By alternately arranging the part to which the ultrasonic wave is applied and the part to which the ultrasonic wave is not applied, it is also possible to express a sense of concavity and convexity. Alternatively, by alternately arranging the part with a large amplitude and the part with a small amplitude of the applied ultrasonic wave, it is also possible to express a sense of concavity and convexity. Thus, the tactile sense can be changed according to the part touched by the person or the image displayed on the display 3.
[0035] Here, the inventors have discovered that by forming a first concave-convex structure having a large interval width and a second concave-convex structure having a small interval width on at least a portion of the outer main surface 1a of the top plate 1, and by making the surface roughness of the first concave-convex structure and the second concave-convex structure within a specific range, the variation range of the friction force can be fully increased, and the tactile expressiveness can be effectively improved.
[0036] More specifically, in the first invention, it was found that at least a portion of the outer main surface 1a of the top plate 1 has a first concave-convex and a second concave-convex. When the cutoff value of the high-frequency filter λc1 is set to 5 times the value of the interval between the concave-convex of the measured cross-sectional curve and the cutoff value of the low-pass filter λs1 is set to 26.6μm, the maximum height of the concave-convex is 0.5nm~2000nm, and the interval between the concave-convex is 50μm~2000μm. When the cutoff value of the high-frequency filter λc2 is set to 14μm and the cutoff value of the low-pass filter λs2 is set to 0.35μm, the three-dimensional arithmetic mean height Sa of the concave-convex is 0.5nm~100nm, and the maximum height Sz of the concave-convex is greater than 8nm, thereby making it possible to fully increase the variation range of the friction force and effectively improve the tactile expressiveness.
[0037] In addition, it was found in the second invention that at least a portion of the outer main surface 1a of the top plate 1 has a structure of a first concave-convex structure and a second concave-convex structure. When the cutoff value of the high-frequency filter λc1 is set to 14μm and the cutoff value of the low-pass filter λs1 is set to 0.35μm, the maximum height of the first concave-convex structure is 0.5nm~2000nm, and the interval between the concave-convex structure is 3μm to less than 50μm. In the second concave-convex structure, in an area of a square with a side length of 5μm, when the cutoff value of the high-frequency filter λc2 is set to 2.5μm, the three-dimensional arithmetic mean height Sa of the concave-convex structure is 0.5nm~100nm, and the maximum height Sz of the concave-convex structure is greater than 8nm. As a result, the variation range of the friction force can be fully increased, and the tactile expressiveness can be effectively improved.
[0038] The first invention is adopted when the average value of the intervals between the first concavities and convexities of the measured cross-sectional curve is greater than 50 μm, and the second invention is adopted when the average value of the intervals between the first concavities and convexities of the measured cross-sectional curve is less than (less than) 50 μm. In addition, the first invention and the second invention are sometimes collectively referred to as the present invention hereinafter.
[0039] In this way, by controlling the surface roughness of the first concavoconvex and the second concavoconvex of the outer main surface 1a of the top plate 1 within a specific range, the contact area between the fingertip and the outer main surface 1a when ultrasonic waves are applied can be effectively reduced, and the change in the contact state between the fingertip and the outer main surface 1a can be increased. As a result, the change in the sliding feeling mode when ultrasonic waves are applied can be increased, and the expressiveness of touch can be effectively improved.
[0040] The maximum height of the first concavity and convexity can be measured, for example, using the maximum height roughness Rz1 of the roughness curve element. The interval between the first concavity and convexity can be measured, for example, using the average length RSm1 of the roughness curve element.
[0041] The above-mentioned "maximum height roughness Rz (Rz1)" is a parameter specified by JIS B0601: 2001. Specifically, Figure 2 As shown, the maximum height roughness Rz1 is the sum (sum of absolute values) of the height of the highest peak and the depth of the deepest valley in the measured cross-sectional curve of the outer main surface 1 a of the top plate 1 .
[0042] The above-mentioned “average length RSm (RSm1) of the roughness curve element” is a parameter specified in JIS B0601:2001, and is a parameter indicating the average distance between adjacent concave and convex portions in the measured cross-sectional curve of the outer main surface 1a of the top plate 1. Specifically, the average length RSm1 is Figure 2 The average of the period lengths Xs of the concavities and convexities of the specified reference length shown.
[0043] Among them, in the first invention, the maximum height and interval of the first concave-convex can be obtained by, for example, arbitrarily selecting 4 straight lines with a length of more than 5000 μm by removing singular points (high or low points) in the measurement area, and calculating the average value thereof as the measurement value.
[0044] In the second invention, the maximum height and interval of the first concavoconvexity can be determined by, for example, arbitrarily selecting four straight lines with a length of 74 μm by excluding singular points (high or low points) in the measurement area and calculating the average value thereof as the measurement value.
[0045] In the present invention, the above-mentioned "three-dimensional arithmetic mean height Sa" is a parameter specified by ISO 25178, and is a parameter obtained by extending a measured cross-sectional curve representing the cross-sectional shape of the concavities and convexities to a surface.
[0046] In each of the first invention and the second invention, the maximum height of the first concavoconvex is 0.5 nm or more, preferably 1 nm or more, more preferably 5 nm or more, further preferably 10 nm or more, further more preferably 20 nm or more, further more preferably 30 nm or more, further more preferably 40 nm or more, particularly preferably 50 nm or more, and is 2000 nm or less, preferably 1900 nm or less, more preferably 1800 nm or less, further preferably 1500 nm or less, further more preferably 1400 nm or less, further more preferably 1300 nm or less, further more preferably 1250 nm or less, further more preferably 1200 nm or less, further more preferably 1100 nm or less, further more preferably 1000 nm or less, further more preferably 800 nm or less, and particularly preferably 500 nm or less. When the maximum height of the first concavoconvex is above the above lower limit, the change in frictional force can be more fully increased, and the expressiveness of tactile sensation can be further effectively improved. When the maximum height of the first concavoconvexity is equal to or less than the above upper limit, the haze can be reduced, and the image viewed through the top plate 1 can be made less likely to bleed.
[0047] In the first invention, the interval between the first concavoconvex is preferably 100 μm or more, more preferably 200 μm or more, further preferably 400 μm or more, further more preferably 500 μm or more, further more preferably 700 μm or more, particularly preferably 1000 μm or more, preferably 1900 μm or less, more preferably 1800 μm or less, further preferably 1700 μm or less, further more preferably 1500 μm or less, further more preferably 1300 μm or less, and particularly preferably 1000 μm or less. In the second invention, the interval between the first concavoconvex is preferably 4 μm or more, more preferably 5 μm or more, further preferably 7 μm or more, preferably 48 μm or less, more preferably 45 μm or less, and further preferably 40 μm or less. When the interval between the first concavoconvex is above the lower limit and below the upper limit, the change in frictional force can be more fully increased, and the expressiveness of tactile sensation can be more effectively improved.
[0048] In each of the first invention and the second invention, the three-dimensional arithmetic mean height Sa of the second concavoconvex is preferably 1 nm or more, more preferably 1.5 nm or more, further preferably 2 nm or more, further preferably 5 nm or more, further more preferably 10 nm or more, preferably 90 nm or less, more preferably 75 nm or less, further preferably 70 nm or less, further preferably 60 nm or less, further more preferably 50 nm or less, further more preferably 40 nm or less, and particularly preferably 30 nm or less. When the three-dimensional arithmetic mean height Sa of the second concavoconvex is above the above lower limit, the change in friction force can be more fully increased, and the expressiveness of touch can be further effectively improved. When the three-dimensional arithmetic mean height Sa of the second concavoconvex is below the above upper limit, the haze can be reduced, and the image seen through the top plate 1 can be made more difficult to bleed.
[0049] In addition, in each of the first invention and the second invention, the maximum height Sz of the second concavoconvex is preferably 10 nm or more, more preferably 20 nm or more, further preferably 30 nm or more, further more preferably 50 nm or more, preferably 1500 nm or less, more preferably 1300 nm or less, further preferably 1000 nm or less, further more preferably 900 nm or less, further more preferably 700 nm or less, further more preferably 500 nm or less, further more preferably 300 nm or less, further more preferably 200 nm or less, further more preferably 170 nm or less, further more preferably 150 nm or less, further more preferably 130 nm or less, further more preferably 110 nm or less, and particularly preferably 100 nm or less. When the maximum height Sz of the second concavoconvex is above the lower limit, the change in frictional force can be more fully increased, and the expressiveness of tactile sense can be further effectively improved. When the maximum height Sz of the second concavoconvex is below the upper limit, the haze can be reduced, and the image seen through the top plate 1 can be made more difficult to bleed.
[0050] In each of the first invention and the second invention, the peak Sku1 of the first concavoconvex is preferably 2 or more, more preferably 2.1 or more, further preferably 2.2 or more, preferably 5.7 or less, more preferably 5.5 or less, further preferably 5 or less. When the peak Sku1 of the first concavoconvex is above the lower limit, the change in friction force can be more fully increased, and the tactile expression can be further effectively improved. When the peak Sku1 of the first concavoconvex is below the upper limit, the convex portion becomes an obtuse angle, and the durability of the top plate is further improved.
[0051] In addition, the skewness Ssk1 of the first concavoconvex is preferably greater than -0.7, more preferably greater than -0.5, further preferably greater than 0, preferably less than 0.6, more preferably less than 0.5, further preferably less than 0.4. When the skewness Ssk1 of the first concavoconvex is greater than the above lower limit and less than the above upper limit, the change in frictional force can be more fully increased, and the expressiveness of tactile sensation can be further effectively improved.
[0052] The kurtosis Sku1 and the skewness Ssk1 of the first concavity and convexity can be measured in accordance with ISO 25178. The kurtosis Sku1 and the skewness Ssk1 of the first concavity and convexity are also measured under the conditions of the first invention or the second invention.
[0053] In each of the first invention and the second invention, the kurtosis Sku2 of the second concavoconvex is preferably 3.2 or more, more preferably 3.3 or more, further preferably 3.4 or more, particularly preferably 3.5 or more, preferably 12 or less, more preferably 11 or less, and further preferably 8 or less. When the kurtosis Sku2 of the second concavoconvex is above the above lower limit, the change in frictional force can be more fully increased, and the expressiveness of tactile sense can be further effectively improved. When the kurtosis Sku2 of the second concavoconvex is below the above upper limit, the haze can be reduced, and the image seen through the top plate 1 can be made less likely to bleed.
[0054] In addition, the skewness Ssk1 of the second concavoconvex is preferably not less than -3, more preferably not less than -2.5, further preferably not less than -2, preferably not more than -0.1, more preferably not more than -0.11, further preferably not more than -0.12, and particularly preferably not more than -0.15. When the skewness Ssk1 of the second concavoconvex is not less than the above lower limit and not more than the above upper limit, the change in frictional force can be more fully increased, and the expressiveness of tactile sensation can be further effectively improved.
[0055] The kurtosis Sku2, skewness Ssk2, and maximum height Sz of the second concavity and convexity can be measured in accordance with ISO 25178. The kurtosis Sku2, skewness Ssk2, and maximum height Sz of the second concavity and convexity are also measured under the conditions of the first invention or the second invention.
[0056] In this embodiment, the haze of the top plate 1 is preferably 30% or less, more preferably 20% or less, further preferably 15% or less, further preferably 10% or less, and particularly preferably 5% or less. When the transparency of the top plate 1 is important, it may be 3% or less.
[0057] The thickness of the top plate 1 is preferably 0.1 mm to 2 mm, and more preferably 0.3 mm to 1.5 mm. If the thickness of the top plate 1 is too small, the mechanical strength is likely to decrease. On the other hand, if the thickness of the top plate 1 is too large, the vibration of the actuator 5 is difficult to transmit to the outer main surface 1a, and there is a tendency for the friction between the finger and the outer main surface 1a to increase.
[0058] In the present embodiment, the top plate 1 is transparent, but the top plate 1 may not be transparent. For example, an opaque portion with a pattern or the like (for example, a switch, a button, a painting or a photo of an animal, a musical instrument, etc.) may be added to the outer main surface 1a of the top plate 1. The area of the opaque portion of the top plate 1 may be more than 5% of the total area of the top plate 1, or more than 30%, or more than 50%, or more than 90%. In this case, the tactile presentation device 10 may not include the display 3. The touch sensor 4 is disposed on the surface of the top plate 1 on the opposite side to the outer main surface 1a, or a touch sensor using an infrared optical imaging method may be used. Transparency refers to a visible light transmittance of more than 70%.
[0059] In addition, in the present embodiment, the outer main surface 1a of the top plate 1 is provided with concavoconvexities as a whole, but according to the requirements, the concavoconvex portion can be provided on at least a part of the outer main surface 1a of the top plate 1, for example, it can be provided on a part (touch effective part, pattern part) where the expressiveness of tactile sensation is to be further improved. The area of the concavoconvex portion of the top plate 1 can be 5% or more of the overall area of the top plate 1, or 30% or more, or 50% or more, or 90% or more.
[0060] The top plate 1 of the tactile presentation device 10 is a substrate made of glass, but is not limited thereto and may be made of a material other than glass, such as resin or ceramic.
[0061] like Figure 1 As shown, the tactile presentation device 10 includes a plurality of actuators 5. More specifically, the tactile presentation device 10 includes an actuator 5 arranged to contact near one end of the top plate 1 and an actuator 5 arranged to contact near the other end. The plurality of actuators 5 are arranged between the top plate 1 and the housing 2. In addition, the configuration of the actuator 5 is not limited to the above, as long as it is arranged to be able to apply ultrasonic waves to the top plate 1. At least one actuator 5 is provided.
[0062] Figure 3 FIG. 1 is a schematic cross-sectional view of a tactile presentation device according to a modified example of an embodiment of the present invention. Figure 3 As shown in FIG. 1 , the top plate 21 has a substrate 26 as a main body and an outer layer film 27 provided on the substrate 26. In addition to the above points, the tactile presentation device 20 of this modified example has the same Figure 1The tactile presentation device 10 has the same structure.
[0063] The outer main surface 21a of the top plate 21 includes the surface of the outer layer film 27, and the outer layer film 27 has irregularities on its surface. The outer layer film 27 is, for example, an inorganic film. The inorganic film is not particularly limited, and for example, SiO 2 wait.
[0064] In the above inorganic film, SiO 2 In the case of a film, by spraying a SiO 2 The liquid containing the SiO 2 The liquid of the component is dried, thereby forming SiO 2 Coating film.
[0065] In this modification, Figure 1 The implementation method can also fully increase the variation range of the friction force and effectively improve the tactile expression.
[0066] [Method for manufacturing top plate for tactile presentation device]
[0067] Below, refer to Figure 4 (a) and (b) are described separately as a first method and a second method as specific examples of the method for manufacturing a top plate for a tactile presentation device of the present invention.
[0068] (Method 1)
[0069] like Figure 4 As shown in (a), an original panel 11 having a main surface 11a is prepared. Next, a wet blasting process (wet blasting / wet sandblasting process) is performed on the main surface 11a of the original panel 11. In the first method, the first concavo-convex and the second concavo-convex are formed simultaneously by the wet blasting process, thereby forming concavo-convex on the main surface 11a of the original panel 11.
[0070] The wet spraying treatment is carried out by uniformly stirring abrasive particles composed of solid particles such as aluminum oxide with liquids such as water to form a slurry and spraying it at high speed onto the original panel 11. The above-mentioned spraying can be carried out using a spray nozzle. The slurry is sprayed at high speed from the spray nozzle together with compressed air. In addition, by moving the spray gun including the spray nozzle relative to the original panel 11, various surface shapes can be formed. For example, by moving the spray gun in a grid shape at a certain speed at a predetermined scanning interval, the first concavoconvex and the second concavoconvex can be formed. In addition, by moving the spray gun including the spray nozzle relative to the original panel 11 like a stroke, a uniform surface shape can be formed on the entire surface.
[0071] In the wet spraying process, when the high-speed sprayed slurry collides with the original panel 11, the abrasive grains in the slurry grind the surface of the original panel 11, thereby forming unevenness on the main surface 11a of the original panel 11. Figure 4 (b) shows the top plate 1. In addition, the ejected abrasive grains and the fragments of the original plate 11 ground by the abrasive grains are washed away by the ejected liquid, so the number of particles remaining on the outer main surface 1a of the top plate 1 is reduced.
[0072] In the first method, the particle size of the abrasive can be set to, for example, 0.3 μm or more and 10 μm or less. The scanning interval of the spray gun can be set to, for example, 100 μm or more and 2000 μm or less. The number of scans of the spray gun can be set to, for example, 1 or more and 10 or less. The ejection pressure of the slurry can be, for example, 0.1 MPa or more and 0.4 MPa or less. The concentration of the slurry can be, for example, 1 wt% or more and 10 wt% or less. In addition, the moving speed of the spray gun can be, for example, 0.1 mm / s or more and 50 mm / s or less.
[0073] In addition, in the first method, the maximum height of the first concavoconvex can be increased by increasing the particle size of the abrasive in the wet blasting process, or changing the shape of the abrasive to a polygonal shape, increasing the number of scans of the spray gun, extending the scanning interval of the spray gun, increasing the spray pressure of the slurry, increasing the concentration of the slurry, slowing down the moving speed of the spray gun, or approaching the spray distance. In addition, the interval of the first concavoconvex can be increased by increasing the particle size of the abrasive in the wet blasting process, or changing the shape of the abrasive to a polygonal shape, increasing the number of scans of the spray gun, increasing the spray pressure of the slurry, increasing the concentration of the slurry, and slowing down the moving speed of the spray gun.
[0074] In addition, by increasing the particle size of abrasive grains in wet blasting, increasing the slurry spraying pressure, slowing down the movement speed of the spray gun, and increasing the number of spray gun scans, the three-dimensional arithmetic mean height Sa of the second concavoconvexity and the maximum height Sz of the concavoconvexity can be increased.
[0075] In the wet spraying process, when the slurry is sprayed onto the original panel 11, the liquid transports the abrasive grains to the original panel 11, so fine abrasive grains can be used compared with the dry sandblasting process. In addition, the impact when the abrasive grains collide with the original panel 11 becomes smaller, and precise processing can be performed. In addition, when using the dry sandblasting process, it is difficult to form a concave-convex of appropriate size even if small abrasive grains are used. In this way, by implementing the wet spraying process to the original panel 11, it is easy to form a concave-convex of appropriate size, and the rise of the haze can be suppressed.
[0076] (Method 2)
[0077] like Figure 4As shown in (a), an original panel 11 having a main surface 11a is prepared. Next, the main surface 11a of the original panel 11 is subjected to a first wet spraying process. In the second method, preliminary projections and depressions are formed on the main surface 11a of the original panel 11 by the first wet spraying process.
[0078] In the first wet blasting process, the particle size of the abrasive grains can be set to, for example, 0.3 μm or more and 10 μm or less. The scanning interval of the spray gun can be set to, for example, 500 μm or more and 2000 μm or less. The number of scans of the spray gun can be set to, for example, 1 or more and 10 or less. The ejection pressure of the slurry can be, for example, 0.1 MPa or more and 0.4 MPa or less. In addition, the moving speed of the spray gun can be set to, for example, 0.1 mm / s or more and 100 mm / s or less.
[0079] Next, the original panel 11 having the preliminary unevenness formed on the main surface 11a is subjected to an etching process. Thus, the first unevenness can be formed on the main surface 11a of the original panel 11. The etching process can be performed, for example, by immersing the original panel 11 in a solution containing hydrofluoric acid or hydrofluoric acid and other acids. As other acids, for example, sulfuric acid, nitric acid, hydrochloric acid, etc. can be used. Furthermore, a chelating agent such as citric acid can also be used.
[0080] The content of hydrofluoric acid in the etching solution can be set to, for example, 0.1 mass % to 50.0 mass %. The content of sulfuric acid in the etching solution can be set to, for example, 0 mass % to 60.0 mass %. In addition, the content of water in the etching solution can be set to, for example, 20.0 mass % to 99.9 mass %.
[0081] The liquid temperature of the etching solution can be set to, for example, 10° C. to 50° C. In addition, the immersion time in the etching solution can be set to, for example, 10 seconds to 60 minutes.
[0082] Alternatively, the etching process may be performed using hydrogen fluoride gas (HF).
[0083] Next, the main surface 11a of the original panel 11 having the first concavo-convex pattern formed thereon is subjected to a second wet spraying process. By the second wet spraying process, a second concavo-convex pattern is further formed on the main surface 11a of the original panel 11. Thus, a Figure 4 (b) The top plate 1 shown.
[0084] In the second wet blasting process, the particle size of the abrasive grains can be set to, for example, 0.3 μm or more and 10 μm or less. The scanning interval of the spray gun can be set to, for example, 100 μm or more and 2000 μm or less. The number of scans of the spray gun can be set to, for example, 1 or more and 10 or less. The ejection pressure of the slurry can be, for example, 0.1 MPa or more and 0.4 MPa or less. In addition, the moving speed of the spray gun can be set to, for example, 0.1 mm / s or more and 100 mm / s or less.
[0085] In the second method, the maximum height of the first concavity and the interval between the concavities can be increased by increasing the particle size of the abrasive in the first wet blasting process, increasing the slurry spraying pressure, reducing the movement speed of the spray gun, and increasing the number of scanning times of the spray gun.
[0086] In addition, by increasing the concentration of sulfuric acid in the etching process, the maximum height of the first concavities and convexities can be suppressed. On the other hand, by extending the immersion time in the etching solution, the maximum height of the first concavities and convexities and the interval between the first concavities and convexities can be increased.
[0087] In addition, by increasing the particle size of the abrasive in the second wet blasting process, increasing the slurry spraying pressure, slowing down the movement speed of the spray gun, and increasing the number of scanning times of the spray gun, the three-dimensional arithmetic mean height Sa of the second concavoconvexity and the maximum height Sz of the concavoconvexity can be increased.
[0088] Among them, in getting Figure 3 In the case of the top plate 21 of the outer layer film 27 shown, a coating agent containing, for example, a silica precursor is applied to the main surface of the original plate by spraying. Thus, a coating film is formed on the main surface. Next, the coating film is heated. The heating temperature is preferably in the range of 80°C to 250°C, more preferably in the range of 100°C to 230°C. Thus, the outer layer film 27 is formed.
[0089] Furthermore, an antireflection film for reducing reflectivity may be formed on at least one of the outer and inner sides of the top plate 1 , or an antifouling film for preventing fingerprints from adhering and imparting water repellency or oil repellency may be formed on the outer main surface 1 a of the top plate 1 .
[0090] As the antireflection film, for example, a low refractive index film having a lower refractive index than the top plate 1 or a dielectric multilayer film in which a relatively low refractive index film and a relatively high refractive index film are alternately stacked can be used. The antireflection film can be formed by sputtering or CVD.
[0091] When the outer main surface 1 a of the top plate 1 has an antireflection film, the irregularities of the outer main surface 1 a of the top plate 1 are formed so that the surface irregularities of the antireflection film have the first irregularities and the second irregularities described above.
[0092] The antifouling film preferably contains a fluorine-containing polymer containing silicon in the seed chain. As the fluorine-containing polymer, for example, a polymer having -Si-O-Si- units in the main chain and a fluorine-containing hydrophobic functional group in the side chain can be used. The fluorine-containing polymer can be synthesized, for example, by dehydration condensation of silanol.
[0093] When the outer main surface 1 a of the top plate 1 has an antireflection film and an antifouling film, the antireflection film is formed on the outer main surface 1 a of the top plate 1 , and the antifouling film is formed on the antireflection film.
[0094] When the outer main surface 1a of the top plate 1 has an anti-fouling film, or when the outer main surface 1a of the top plate 1 has an anti-reflection film and an anti-fouling film, the unevenness of the outer main surface 1a of the top plate 1 is formed in a manner such that the unevenness on the surface of the anti-fouling film has the above-mentioned first unevenness and second unevenness.
[0095] Hereinafter, the present invention will be described in more detail based on specific examples. The present invention is not limited to the following examples at all, and can be implemented by appropriately changing the scope of the present invention.
[0096] (Example 1)
[0097] The top plate was prepared by wet spraying the entire main surface of the original panel composed of aluminosilicate glass with a thickness of 1.1 mm, and the first concavo-convex and the second concavo-convex were formed at the same time. In addition, in the wet spraying, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #8000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.25 MPa while the spray gun was moved at a constant speed with a scanning interval of 500 μm relative to the processing table on which the original panel was placed. The moving speed of the spray gun was set to a condition where the maximum height of the first concavo-convex of the outer main surface of the top plate was 1.7 nm (the moving speed of the spray gun was 20 mm / s).
[0098] (Example 2)
[0099] A top plate was produced in the same manner as in Example 1 (spray gun moving speed 1 mm / s) except that the moving speed of the spray gun was set so that the maximum height of the first concavities and convexities on the outer main surface of the top plate was 21.6 nm.
[0100] (Example 3)
[0101] A top plate was produced in the same manner as in Example 1 (spray gun moving speed: 0.5 mm / s) except that the moving speed of the spray gun was set so that the maximum height of the first concavities and convexities on the outer main surface of the top plate was 45.1 nm.
[0102] (Example 4)
[0103] A top plate was manufactured in the same manner as in Example 1 (spray gun moving speed 30 mm / s), except that a slurry of 6 wt % abrasive composed of #4000 aluminum oxide and 94 wt % water was used as the slurry, the slurry spraying pressure was set to 0.32 MPa, and the moving speed of the spray gun was set to a condition where the maximum height of the first concave-convex on the outer main surface of the top plate was 20 nm.
[0104] (Example 5)
[0105] A top plate was manufactured in the same manner as in Example 1 (spray gun moving speed 15 mm / s), except that a slurry of 6 wt % abrasive consisting of #4000 aluminum oxide and 94 wt % water was used as the slurry, the slurry spraying pressure was set to 0.32 MPa, and the moving speed of the spray gun was set to a condition where the maximum height of the first concave-convex on the outer main surface of the top plate was 40 nm.
[0106] (Example 6)
[0107] A top plate was produced in the same manner as in Example 1 (spray gun moving speed 20 mm / s), except that the scanning interval of the spray gun was 750 μm and the moving speed of the spray gun was set so that the maximum height of the first concavities and convexities on the outer main surface of the top plate was 0.9 nm.
[0108] (Example 7)
[0109] A top plate was produced in the same manner as in Example 6 (spray gun moving speed 5 mm / s) except that the moving speed of the spray gun was set so that the maximum height of the first concavities and convexities on the outer main surface of the top plate was 6.9 nm.
[0110] (Example 8)
[0111] A top plate was produced in the same manner as in Example 6 (spray gun moving speed 1 mm / s) except that the moving speed of the spray gun was set so that the maximum height of the first concavities and convexities on the outer main surface of the top plate was 35.3 nm.
[0112] (Example 9)
[0113] A top plate was produced in the same manner as in Example 1 (spray gun moving speed 10 mm / s), except that the scanning interval of the spray gun was 1000 μm and the moving speed of the spray gun was set so that the maximum height of the first concavities and convexities on the outer main surface of the top plate was 9.1 nm.
[0114] (Example 10)
[0115] A top plate was produced in the same manner as in Example 9 (spray gun moving speed 2 mm / s) except that the moving speed of the spray gun was set so that the maximum height of the first concavities and convexities on the outer main surface of the top plate was 49.0 nm.
[0116] (Example 11)
[0117] A top plate was produced in the same manner as in Example 1 (spray gun moving speed 1 mm / s), except that the scanning interval of the spray gun was 1200 μm and the moving speed of the spray gun was set so that the maximum height of the first concavities and convexities on the outer main surface of the top plate was 101.0 nm.
[0118] (Example 12)
[0119] A top plate was produced in the same manner as in Example 1 (spray gun moving speed 1 mm / s), except that the scanning interval of the spray gun was set to 1500 μm and the moving speed of the spray gun was set to a condition that the maximum height of the first concavities and convexities on the outer main surface of the top plate was 149.0 nm.
[0120] (Example 13)
[0121] The first wet spraying treatment was performed on the entire main surface of the original panel composed of aluminosilicate glass with a thickness of 1.1 mm, thereby forming preliminary unevenness. In addition, in the first wet spraying treatment, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #4000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.15 MPa while the spray gun was moved at a constant speed of 10 mm / s relative to the processing table on which the original panel was placed.
[0122] Next, the original panel having the preliminary concavities and convexities formed on the main surface was immersed in an etching solution composed of 2 wt % hydrofluoric acid and 40 wt % sulfuric acid and left at a solution temperature of 25° C. for 20 minutes to perform etching treatment, thereby forming the first concavities and convexities from the preliminary concavities and convexities.
[0123] Next, the entire main surface of the original panel formed with the first concavoconvex is subjected to a second wet spraying treatment, thereby forming the second concavoconvex and manufacturing the top plate. In addition, in the second wet spraying treatment, a slurry prepared by uniformly stirring 3wt% of abrasive grains composed of aluminum oxide with a particle size of #4000 and 97wt% of water is used, and the slurry is sprayed at a spray pressure of 0.10MPa while the spray gun is moved at a constant speed relative to the processing table on which the original panel is placed. The moving speed of the spray gun is set to a condition where the maximum height of the second concavoconvex on the outer main surface of the top plate becomes 7.1nm (the moving speed of the spray gun is 10mm / s).
[0124] (Example 14)
[0125] The first wet spraying treatment was performed on the entire main surface of the original panel composed of aluminosilicate glass with a thickness of 1.1 mm, thereby forming preliminary unevenness. In addition, in the first wet spraying treatment, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #8000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.15 MPa while the spray gun was moved at a constant speed of 10 mm / s relative to the processing table on which the original panel was placed.
[0126] Next, the original panel having the preliminary concavities and convexities formed on the main surface was immersed in an etching solution composed of a mixed acid of 2 wt % hydrofluoric acid and 40 wt % sulfuric acid and left at a liquid temperature of 25° C. for 20 minutes to perform etching treatment, thereby forming the first concavities and convexities from the preliminary concavities and convexities.
[0127] Next, the entire main surface of the original panel formed with the first concavo-convex was subjected to a second wet spraying treatment, thereby forming the second concavo-convex and forming a top plate. In addition, in the second wet spraying treatment, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #4000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.12 MPa while the spray gun was moved at a constant speed relative to the processing table on which the original panel was placed. The moving speed of the spray gun was set to a condition where the maximum height of the second concavo-convex on the outer main surface of the top plate became 8.9 nm (the moving speed of the spray gun was 10 mm / s).
[0128] (Example 15)
[0129] The first wet spraying treatment was performed on the entire main surface of the original panel composed of aluminosilicate glass with a thickness of 1.1 mm, thereby forming preliminary unevenness. In addition, in the first wet spraying treatment, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #4000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.15 MPa while the spray gun was moved at a constant speed of 10 mm / s relative to the processing table on which the original panel was placed.
[0130] Next, the original panel having the preliminary concavities and convexities formed on the main surface was immersed in an etching solution composed of a mixed acid of 2 mass % hydrofluoric acid and 40 mass % sulfuric acid and left at a liquid temperature of 25° C. for 30 minutes to perform etching treatment, thereby forming the first concavities and convexities from the preliminary concavities and convexities.
[0131] Next, the entire main surface of the original panel formed with the first concavo-convex was subjected to a second wet spraying treatment, thereby forming the second concavo-convex and forming a top plate. In addition, in the second wet spraying treatment, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #4000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.15 MPa while the spray gun was moved at a constant speed relative to the processing table on which the original panel was placed. The moving speed of the spray gun was set to a condition that the maximum height of the second concavo-convex on the outer main surface of the top plate became 12.7 nm (the moving speed of the spray gun was 10 mm / s).
[0132] (Example 16)
[0133] The first wet spraying treatment was performed on the entire main surface of the original panel composed of aluminosilicate glass with a thickness of 1.1 mm, thereby forming preliminary unevenness. In addition, in the first wet spraying treatment, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #2000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.25 MPa while the spray gun was moved at a constant speed of 5 mm / s relative to the processing table on which the original panel was placed.
[0134] Next, the original panel having the preliminary concavities and convexities formed on the main surface was immersed in an etching solution composed of a mixed acid of 2 wt % hydrofluoric acid and 45 wt % sulfuric acid and left at a liquid temperature of 25° C. for 30 minutes to perform etching treatment, thereby forming the first concavities and convexities from the preliminary concavities and convexities.
[0135] Next, the entire main surface of the original panel formed with the first concavo-convex is subjected to a second wet spray treatment, thereby forming the second concavo-convex and forming a top plate. In addition, in the second wet spray treatment, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #4000 and 97 wt% of water is used, and the slurry is moved at a constant speed relative to the processing table on which the original panel is placed, while the slurry is sprayed at a spray pressure of 0.20 MPa. The moving speed of the spray gun is set to a condition where the maximum height of the second concavo-convex on the outer main surface of the top plate becomes 16.1 nm (the moving speed of the spray gun is 10 mm / s).
[0136] (Comparative Example 1)
[0137] The same original plate as in Example 1 was prepared and used as the top plate as it is. Thus, in Comparative Example 1, an untreated top plate was used.
[0138] (Comparative Example 2)
[0139] A silicon dioxide precursor composed of tetraethyl orthosilicate was prepared as a matrix precursor, and a mixture composed of an aqueous nitric acid solution, ethanol, isopropyl alcohol, and methyl ethyl ketone was prepared as a liquid medium. The matrix precursor and the liquid medium were stirred until uniform, thereby obtaining a coating agent.
[0140] Next, a coating agent was applied by spraying at a predetermined discharge amount and nozzle movement speed on the main surface of the original panel made of aluminosilicate glass with a thickness of 1.1 mm to form a coating film. Next, the coating film was heated at 150°C for 30 minutes. Thus, only SiO 2 The first concavo-convex structure formed by the outer layer film is used to make the top plate.
[0141] (Comparative Example 3)
[0142] The entire main surface of the original panel composed of aluminosilicate glass with a thickness of 1.1 mm was subjected to wet spraying treatment to form preliminary unevenness. In addition, in the wet spraying treatment, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #4000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.15 MPa while the spray gun was moved at a constant speed relative to the processing table on which the original panel was placed.
[0143] Next, the original panel with the preliminary projections and recesses formed on the main surface is immersed in an etching solution consisting of a mixed acid of 2% by mass hydrofluoric acid and 40% by mass sulfuric acid, and is left at a liquid temperature of 25°C for 20 minutes, thereby performing an etching treatment to form only the first projection and recess from the preliminary projections and recesses, thereby producing a top plate.
[0144] (Comparative Example 4)
[0145] The entire main surface of the original panel composed of aluminosilicate glass with a thickness of 1.1 mm was subjected to wet spraying treatment to form preliminary unevenness. In addition, in the wet spraying treatment, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #4000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.15 MPa while the spray gun was moved at a constant speed relative to the processing table on which the original panel was placed.
[0146] Next, the original panel with the preliminary depressions and projections formed on the main surface was immersed in an etching solution consisting of a mixed acid of 2 mass % hydrofluoric acid and 50 mass % sulfuric acid and left at a liquid temperature of 25°C for 20 minutes, thereby performing an etching treatment to form only the first depression and projection from the preliminary depressions and projections, thereby producing a top plate.
[0147] (Comparative Example 5)
[0148] The entire main surface of the original panel composed of aluminosilicate glass with a thickness of 1.1 mm was subjected to wet spraying treatment, thereby forming only the second concavoconvexity and producing a top plate. In addition, in the wet spraying treatment, a slurry prepared by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #4000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.10 MPa while the spray gun was moved at a constant speed relative to the processing table on which the original panel was placed. The moving speed of the spray gun was set to a condition where the maximum height of the second concavoconvexity on the outer main surface of the top plate became 6.9 nm (the moving speed of the spray gun was 10 mm / s).
[0149] (Comparative Example 6)
[0150] The entire main surface of the original panel composed of aluminosilicate glass with a thickness of 1.1 mm was subjected to wet spraying treatment, thereby forming only the second concavoconvexity and manufacturing the top plate. In addition, in the wet spraying treatment, a slurry adjusted by uniformly stirring 3 wt% of abrasive grains composed of aluminum oxide with a particle size of #4000 and 97 wt% of water was used, and the slurry was sprayed at a spray pressure of 0.20 MPa while the spray gun was moved at a constant speed relative to the processing table on which the original panel was placed. The moving speed of the spray gun was set to a condition where the maximum height of the second concavoconvexity on the outer main surface of the top plate became 15.4 nm (the moving speed of the spray gun was 10 mm / s).
[0151] <Evaluation>
[0152] [Measurement of surface roughness]
[0153] The surface roughness of the outer main surface of the top plates produced in Examples 1 to 16 and Comparative Examples 1 to 6 was measured.
[0154] The surface roughness was measured on the outer main surface having the first and second concavo-convex surfaces for Examples 1 to 16, on one outer main surface for Comparative Example 1, and on the SiO2-treated surface for Comparative Example 2. 2 The coating was performed on the outer main surface. For Comparative Examples 3 and 4, the coating was performed on the outer main surface having only the first concavity and convexity. For Comparative Examples 5 and 6, the coating was performed on the outer main surface having only the second concavity and convexity.
[0155] (1st concave and convex)
[0156] The parameters of the surface roughness of the first concavoconvex surface are the interval between the concavoconvex surfaces, the maximum height of the concavoconvex surfaces, the kurtosis Sku1 and the skewness Ssk1. Among them, the interval between the concavoconvex surfaces measures the average length RSm1 of the roughness curve element. In addition, the maximum height is the maximum height roughness Rz1. These parameters are measured using a white interference microscope (manufactured by Zygo, white interference microscope NewView7300) according to the following measurement conditions 1 and measurement conditions 2.
[0157] The measurement condition of the first concavity and convexity is 1;
[0158] In the measurement condition 1 of the first concavity and convexity, an objective lens of 2.5 times and a zoom lens of 0.5 times were used, and the camera pixel number was 640×480 points and the integration number was once for a measurement area of 5658 μm×4244 μm.
[0159] In addition, the cutoff value of the high-pass filter λc1 in the first concave-convex is set to a value 5 times the interval of the concave-convex of the measured cross-sectional curve, and the cutoff value of the low-pass filter λs1 is set to 26.6 μm, and the average length RSm1, maximum height roughness Rz1, kurtosis Sku1 and skewness Ssk1 of the roughness curve element in the first concave-convex are measured.
[0160] Among them, the parameters of the roughness curve elements in the first concavoconvex are measured by randomly selecting 4 straight lines with a length of 5658 μm in a manner that excludes singular points (high or low points) in the measurement area, and the average value is calculated as the measured value. In addition, in the case of a shape in which the first concavoconvex is regularly arranged, the parameters of the roughness curve elements are measured from a straight line connecting the convex parts of the arranged concavoconvex.
[0161] The measurement condition of the first concavity and convexity is 2;
[0162] In the measurement condition 2 of the first concavity and convexity, an objective lens of 50 times and a zoom lens of 2 times were used, and the measurement area was 74 μm×55 μm, the number of camera pixels was 640×480 points, and the number of integrations was 10 times.
[0163] In addition, the cutoff value of the high-frequency filter λc1 in the first concavoconvexity is set to 14μm, the cutoff value of the low-pass filter λs1 is set to 0.35μm, and the average length RSm1, maximum height roughness Rz1, kurtosis Sku1 and skewness Ssk1 of the roughness curve element in the first concavoconvexity are measured.
[0164] For each parameter of the roughness curve element in the first concavity and convexity, four straight lines with a measurement length of 74 μm were randomly selected to exclude singular points (high or low points) in the measurement area, and the average value was calculated as the measurement value.
[0165] In the first concavity and convexity, measurement condition 1 was used when the average value of the intervals between concavities and convexities in the measured cross-sectional curve was 50 μm or more, and measurement condition 2 was used when the average value of the intervals between concavities and convexities in the measured cross-sectional curve was less than 50 μm.
[0166] (Second concave and convex)
[0167] The parameters of the surface roughness of the second concavoconvex surface are the measured arithmetic mean height Sa, maximum height Sz, kurtosis Sku2 and skewness Ssk2. In addition, these parameters are measured under the following measurement condition 1 using the same white interference microscope as the first concavoconvex surface, and under the following measurement condition 2 using an atomic force microscope (AFM). Among them, regarding the atomic force microscope, the atomic force microscope "Dimension Icon (SPM unit) and Nano Scope V (Controller unit)" manufactured by Bruker was used, and the measurement was implemented based on ISO 25178.
[0168] The second concavity and convexity measurement condition 1;
[0169] In the measurement condition 1 of the second concavity and convexity, an objective lens of 50 times and a zoom lens of 2 times were used, and the measurement area was 74×55 μm, the number of camera pixels was 640×480 points, and the number of integrations was 10 times.
[0170] In addition, in the second concavoconvexity, the cutoff value of the high-frequency filter λc2 is set to 14μm, and the cutoff value of the low-pass filter λs2 is set to 0.35μm, and the arithmetic mean height Sa, maximum height Sz, kurtosis Sku2 and skewness Ssk2 in the second concavoconvexity are measured. In addition, each measurement value is obtained by averaging the results of measurement at any measurement location 4.
[0171] The second concavity and convexity measurement condition 2;
[0172] In the measurement condition 2 of the second concavoconvexity, the tapping mode is used, and the scanning rate is 1 Hz and the number of acquired data is 512×512 points for the measurement area of 5μm×5μm. Based on the acquired data obtained, the arithmetic mean height Sa, the maximum height Sz, the kurtosis Sku2 and the skewness Ssk2 in the second concavoconvexity are measured in the area of the square with a side length of 5μm. The analysis is performed by setting the cutoff value of the high-pass filter λc2 to 2.5μm. Each measurement value is obtained based on the result of measurement from any measurement site 1.
[0173] When the first concavity and convexity are measured using measurement condition 1, the second concavity and convexity are also measured using measurement condition 1. When the first concavity and convexity are measured using measurement condition 2, the second concavity and convexity are also measured using measurement condition 2.
[0174] (Sliding Functionality Evaluation)
[0175] The surface roughness of the outer main surface of the top plates produced in Examples 1 to 16 and Comparative Examples 1 to 6 was measured.
[0176] A 2 cm × 5 cm glass test piece simulating a top plate was attached to the top plate to which the actuator element was attached, thereby serving as an evaluation top plate. Next, a functional evaluation of sliding (sliding before ultrasonic application) was performed by sliding a finger on the outer main surface of the glass test piece. As the glass test piece, the top plates prepared in Examples 1 to 16 and Comparative Examples 1 to 6 were used.
[0177] Next, ultrasonic waves were applied to the top plate by an actuator. As a result, ultrasonic waves were applied to the glass test piece via the top plate, causing the top plate to vibrate at the natural vibration frequency of the ultrasonic wave band. In this state, the functional evaluation of sliding (sliding after ultrasonic wave application) was performed by sliding the index finger of the dominant hand on the outer main surface.
[0178] The evaluation of the sliding functionality was conducted according to the following four-level evaluation criteria.
[0179] <Evaluation Criteria>
[0180] Good sliding:◎
[0181] Sliding is relatively good: ○
[0182] Difference between any two slides: △
[0183] Sliding difference: ×
[0184] Next, the presence or absence of a difference in the degree of sliding felt by applying ultrasonic waves to each sample was evaluated with reference to the untreated comparative example 1. Regarding the evaluation, when the difference in sliding increased with the presence or absence of ultrasonic application, a 7-item reference consisting of "very good: 7", "thinking: 6", "though I think it is one way: 5", "I can't say either way: 4", "thinking which way: 3", "not thinking: 2", and "not thinking at all: 1" was set for evaluation. If the value is higher than 4, the difference in sliding felt is greater than that of the untreated comparative example 1, and if the value is less than 4, it means that the difference in sliding felt has not increased compared with the untreated comparative example 1.
[0185] The results are shown in Tables 1 and 2 below.
[0186] [Table 1]
[0187]
[0188] [Table 2]
[0189]
[0190] (Measurement results of surface roughness)
[0191] As shown in Table 1 and Table 2, regarding the top plates of Examples 1 to 16, the interval between the first concavities and convexities is within a range of 4.6 μm to 1500 μm, and the maximum height of the first concavities and convexities is within a range of 0.9 nm to 643.1 nm.
[0192] On the other hand, in the untreated top plate of Comparative Example 1, the interval between the first concavities and convexities was 0.9 μm, and the maximum height of the first concavities and convexities was 4.0 nm, which were all considerably smaller values than those of Examples 1 to 16.
[0193] In addition, for the case where the SiO 2 The top plate of the first concavities and convexities formed by the outer layer film was 6.5 μm apart, and the maximum height of the first concavities and convexities was 823.0 nm.
[0194] In addition, for the top plates provided with only the first concavities and convexities of Comparative Examples 3 and 4, the interval between the first concavities and convexities was within the range of 8.3 μm to 9.1 μm, and the maximum height of the first concavities and convexities was within the range of 149.4 nm to 286.3 nm.
[0195] In addition, in the top plates provided with only the second concavities and convexities of Comparative Examples 5 and 6, the interval between the first concavities and convexities was 2.2 μm to 2.6 μm, and the maximum height of the first concavities and convexities was within the range of 104.8 nm to 136.1 nm.
[0196] Moreover, as shown in Table 1 and Table 2, regarding the top plates of Examples 1 to 16, the three-dimensional arithmetic mean height Sa in the second concavities and convexities is a value within a range of 1.99 nm to 57.7 nm.
[0197] In contrast, the arithmetic mean height Sa of the untreated top plate of Comparative Example 1 is 0.15 nm, and the top plate of Comparative Example 2 made of SiO 2 The arithmetic mean height Sa of the top plate of the first concave-convex formed by the outer layer film is 0.57nm, the arithmetic mean height Sa of the top plate of the first concave-convex only given to Comparison Example 3 and Comparison Example 4 is 0.53nm, and the arithmetic mean height Sa of the top plate of the second concave-convex only given to Comparison Example 5 and Comparison Example 6 is in the range of 6.85nm to 15.40nm.
[0198] In addition, regarding Examples 1 to 16, the maximum height Sz in the second concavities and convexities is within the range of 67.4 nm to 1201.3 nm.
[0199] In contrast, the maximum height Sz of the untreated top plate of Comparative Example 1 is 1.4 nm, and the top plate of Comparative Example 2 made of SiO 2 The maximum height Sz of the top plate of the first concave-convex formed by the outer layer film is 7.1nm, the maximum height Sz of the top plate of the first concave-convex formed by comparison examples 3 and 4 is only within the range of 6.4nm to 7.2nm, and the maximum height Sz of the top plate of the second concave-convex formed by comparison examples 5 and 6 is only within the range of 135.0nm to 149.0nm.
[0200] In addition, regarding Examples 1 to 16, the kurtosis Sku2 in the second concavity and convexity is within the range of 3.37 to 10.50.
[0201] In contrast, the kurtosis Sku2 of the untreated top plate of Comparative Example 1 is 2.94, and the top plate of Comparative Example 2 made of SiO 2 The peak Sku2 of the top panel of the first concave-convex formed by the outer layer film is 3.02, the peak Sku2 of the top panel of the first concave-convex only given to comparison examples 3 and 4 is in the range of 3.06 to 3.17, and the peak Sku2 of the top panel of the second concave-convex only given to comparison examples 5 and 6 is in the range of 4.85 to 8.27.
[0202] In addition, regarding the top plates of Examples 1 to 16, the skewness Ssk2 in the second concavity and convexity is within the range of -1.810 to -0.125.
[0203] In contrast, the skewness Ssk2 of the untreated top plate of Comparative Example 1 is 0.040, and the top plate of Comparative Example 2 made of SiO 2The skewness Ssk2 of the top plate of the first concave-convex formed by the outer layer film is -0.040, the skewness Ssk2 of the top plate of the first concave-convex only given to Comparison Examples 3 and 4 is within the range of -0.079 to -0.030, and the skewness Ssk2 of the top plate of the second concave-convex only given to Comparison Examples 5 and 6 is within the range of -1.490 to -0.854.
[0204] (Sliding measurement results)
[0205] For the top plates of Examples 1 to 16, by forming appropriate first and second projections and depressions on the outer main surface of the tactile presentation device, the contact state between the fingertips and the outer main surface changes greatly (the effective contact area is reduced), which can increase the change in the sliding feeling when ultrasonic waves are applied, and can obtain good evaluation results.
[0206] On the other hand, in the untreated top plate of Comparative Example 1, since the smooth surface of the outer main surface monotonically contacts the finger, the amount of change in the sliding feeling when ultrasonic waves are applied is limited.
[0207] Regarding the SiO 2 The top plate of the first concavoconvexity formed by the outer layer film is large and the concavoconvexity formed on the outer main surface contacted by the finger is low in effect of reducing the contact area with the finger, so even if ultrasonic waves are applied, effective reduction of slippage cannot be achieved.
[0208] In the top plates of Comparative Examples 3 and 4 provided with only the first concavoconvexity, the concavoconvexity formed on the outer main surface contacted by the finger is large and the effect of reducing the contact area with the finger is low, so that the slip cannot be effectively reduced even if ultrasonic waves are applied.
[0209] For the top plates having only the second concavo-convex of Comparative Examples 5 and 6, the concavo-convex formed on the outer main surface contacted by the finger is small, and the effect of reducing the contact area with the finger is insufficient. Therefore, even if ultrasonic waves are applied, the amount of reduction in slippage is limited.
[0210] The top plate for a tactile presentation device of the present invention can be used for various tactile presentation devices, for example, mobile information terminals such as mobile phones, smart phones, PDAs, tablet computers, and game consoles, operation panels for educational digital terminals, televisions, PCs, digital signage, entertainment operation panels, vehicle-mounted operation panels, operation panels for household appliances such as microwave ovens, televisions, refrigerators, washing machines, lighting fixtures, and digital cameras, and operation panels for industrial equipment such as ATMs (automatic teller machines) and automatic ticket machines.
[0211] Description of Reference Numerals
[0212] 1…Top plate
[0213] 1a…Outer main surface
[0214] 2…Housing
[0215] 2a…Opening
[0216] 3…Display
[0217] 4…Touch sensor
[0218] 5…Actuator
[0219] 10…Haptic display devices
[0220] 11…Original panel
[0221] 11a…Main surface
[0222] 20…Haptic display device
[0223] 21…Top Plate
[0224] 21a…Outer main surface
[0225] 26...Substrate
[0226] 27…Outer membrane.
Claims
1. A top plate for a tactile presentation device, which is a top plate for a tactile presentation device, having an outer main surface located outside the tactile presentation device, At least a portion of the outer main surface is provided with projections and depressions, The concavoconvex has: The first concavity and convexity has a maximum height of 0.5 nm to 2000 nm and a concavity and convexity interval of 50 μm to 2000 μm when the cutoff value of the high-frequency filter λc1 is set to a value 5 times the interval between the concavities and convexities of the measurement cross-sectional curve and the cutoff value of the low-pass filter λs1 is set to 26.6 μm; and For the second concavity, when the cutoff value of the high-frequency filter λc2 is set to 14 μm and the cutoff value of the low-pass filter λs2 is set to 0.35 μm, the three-dimensional arithmetic mean height Sa of the concavity is 0.5 nm to 100 nm and the maximum height Sz of the concavity is not less than 8 nm.
2. The top plate for a tactile presentation device according to claim 1, wherein: The second concavity has a kurtosis Sku of 3.2 or more and a skewness Ssk of -0.1 or less in a measurement area of 74×55 μm when the cutoff value of the high-pass filter λc2 is set to 14 μm and the cutoff value of the low-pass filter λs2 is set to 0.35 μm.
3. A top plate for a tactile presentation device, which is a top plate for a tactile presentation device, having an outer main surface located outside the tactile presentation device, At least a portion of the outer main surface is provided with projections and depressions, The concavoconvex has: The first concavity and convexity has a maximum concavity and convexity height of 0.5 nm to 2000 nm and a concavity and convexity interval of 3 μm to less than 50 μm when the cutoff value of the high-frequency filter λc1 is set to 14 μm and the cutoff value of the low-pass filter λs1 is set to 0.35 μm; and The second concavity and convexity has a three-dimensional arithmetic mean height Sa of 0.5 nm to 100 nm and a maximum height Sz of 8 nm or more in a square region with a side length of 5 μm when the cutoff value of the high-frequency filter λc2 is set to 2.5 μm.
4. The top plate for a tactile presentation device according to claim 3, wherein: The second concavity and convexity has a kurtosis Sku of 3.2 or more and a skewness Ssk of -0.1 or less in a square region with a side length of 5 μm when the cutoff value of the high-frequency filter λc2 is set to 2.5 μm.
5. The top plate for a tactile presentation device according to any one of claims 1 to 4, wherein The top plate for the tactile presentation device is made of glass.
6. The top plate for a tactile presentation device according to any one of claims 1 to 4, wherein The top plate for the tactile presentation device is transparent.
7. A tactile presentation device, comprising: The top plate for a tactile presentation device according to any one of claims 1 to 4; and An actuator applies ultrasonic waves to the top plate of the tactile presentation device.
8. The method for manufacturing a top plate for a tactile presentation device according to any one of claims 1 to 4, comprising: A step of preparing an original panel having a main surface; and A step of performing a wet spraying process on the main surface of the original panel.
Citation Information
Patent Citations
Top panel for tactile sensation presentation device, tactile sensation presentation device, and method for producing top panel for tactile sensation presentation device
JP2018180621A