Method for producing coated electrode active material

By treating Ni-rich electrode active materials in lithium-ion batteries, using aqueous media and heat treatment technology to deposit different elements, the undesirable surface reaction problem in the battery is solved, and the electrochemical characteristics and cycling performance of the battery are significantly improved.

CN118891748APending Publication Date: 2024-11-01BASF SE
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380027946.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-15
Filing Date
2023-03-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing Ni-rich electrode active materials have undesired surface reactions in lithium-ion batteries, resulting in the decomposition of electrolytes or solvents, affecting battery performance, and the existing methods have failed to effectively improve the characteristics of the electrode active materials.

Method used

Using particulate electrode active material according to the general formula Li1+xTM1-xO2, water is treated by an aqueous medium and removed, followed by heat treatment and addition of Al or Sb compounds, different elements are deposited to improve surface characteristics, and finally heat treatment is carried out to form excellent electrochemical characteristic.

Benefits of technology

A Ni-rich electrode active material with excellent electrochemical characteristics is realized, especially during the cycle process, which reduces resistance growth and improves the safety and discharge performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005044328540000161
    Figure BDA0005044328540000161
  • Figure BDA0005044328540000162
    Figure BDA0005044328540000162
  • Figure BDA0005044328540000231
    Figure BDA0005044328540000231
Patent Text Reader

Abstract

Disclosed is a method for manufacturing a coated cathode active material, the method comprising the steps of: (a) providing a particulate electrode active material according to the general formula Li1 + xTM1-xO2, where TM is Ni, and optionally at least one of Co and Mn, and optionally at least one element selected from the group consisting of Al, Mg and Ba, a transition metal other than Ni, Co and Mn, and x is in the range of 0 to 0.2, wherein at least 50 mol-% of the transition metal of TM is Ni, (b) treating the particulate electrode active material with an aqueous medium containing a compound of Al or Sb, (c) at least partially removing the water from step (b), (d) optionally subjecting the mixture from step (c) to a heat treatment, (e) adding to the solid material obtained from step (d) (as applicable) or (c), respectively, at least one compound selected from the group consisting of compounds of Al or Sb or B, or at least one heteropolyacid or its corresponding ammonium salt or lithium salt or a salt of Al, Ga, In or Ba, thereby depositing on the surface of the particulate electrode active material at least one element selected from the group consisting of elements selected from the group consisting of elements selected from the group consisting of elements selected from the group consisting of elements selected from the group consisting of elements selected from the group consisting of elements selected from the group consisting of elements selected from the group consisting of elements selected from the group consisting of elements selected from the group consisting of elements selected from the group consisting of elements selected from the group consisting of elements selected from the group the elements deposited in step (e) are different from the elements deposited in step (b), and (f) subjecting the residue obtained from step (e) to a heat treatment.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for producing a coated cathode active material, the method comprising the following steps:

[0002] (a) providing a method according to the general formula Li 1+x TM 1-x O2 microparticle electrode active material, wherein TM is a combination according to general formula (I),

[0003] (Ni a Co b Mn c ) 1-d M d (I)

[0004] in

[0005] a is in the range of 0.86 to 0.94,

[0006] b is 0 or in the range of 0.01 to 0.1,

[0007] c is in the range of 0.01 to 0.1, and

[0008] d is in the range of 0 to 0.1,

[0009] M is at least one of Al, Mg, Nb, Ti, Mo, W and Zr, and

[0010] a+b+c=1,

[0011] and x is in the range of 0 to 0.05,

[0012] (b) treating the particulate electrode active material with an aqueous medium containing an Al or Sb compound,

[0013] (c) at least partially removing the water from step (b),

[0014] (d) optionally, subjecting the mixture from step (c) to a heat treatment,

[0015] (e) adding at least one compound selected from compounds of Al or Sb or B to the solid material obtained from step (d) (if applicable) or from step (c), respectively, thereby depositing at least one element selected from on the surface of the particulate electrode active material, wherein, respectively, the element deposited in step (e) is different from the element deposited in step (b), and

[0016] (f) subjecting the residue obtained from step (e) to a heat treatment.

[0017] Lithium-ion secondary batteries are modern devices for storing energy. Many applications have been and are being considered, from small devices such as mobile phones and laptops to automotive batteries and other batteries for electric vehicles. The various components of the battery, such as electrolytes, electrode materials, and separators, play a decisive role in the performance of the battery. Special attention has been paid to cathode materials. Several materials have been proposed, such as lithium iron phosphate, lithium cobalt oxide, and lithium nickel cobalt manganese oxide. Despite extensive research, the solutions found so far still leave room for improvement.

[0018] Currently, a certain interest may be observed in so-called Ni-rich electrode active materials, for example electrode active materials containing 75 mol-% or more Ni relative to the total TM content.

[0019] A problem with lithium-ion batteries, especially Ni-rich electrode active materials, is due to undesirable reactions on the surface of the electrode active material. Such reactions may be decomposition of the electrolyte or the solvent or both. Therefore, attempts have been made to protect the surface without hindering lithium exchange during charge and discharge. An example is an attempt to coat the electrode active material with, for example, aluminum oxide or calcium oxide, see, for example, US 8,993,051.

[0020] Other theories attribute the undesirable reaction to free LiOH or Li2CO3 on the surface. Attempts have been made to remove such free LiOH or Li2CO3 by washing the electrode active material with water, see, for example, JP 4,789,066 B, JP 5,139,024B, and US2015 / 0372300. However, in some cases it was observed that the properties of the resulting electrode active material were not improved.

[0021] One object of the present invention is to provide a method for producing a Ni-rich electrode active material having excellent electrochemical properties. Another object is to provide a Ni-rich electrode active material having excellent electrochemical properties, especially low resistance growth during cycling.

[0022] Accordingly, the method defined at the outset has been found, which is also referred to hereinafter as the "method of the invention". The method of the invention comprises the following steps:

[0023] (a) providing a method according to the general formula Li 1+x TM 1-x O2 microparticle electrode active material, wherein TM is a metal combination according to formula (I),

[0024] (Ni a Co b Mn c ) 1-d M d (I)

[0025] in

[0026] a is in the range of 0.86 to 0.94,

[0027] b is 0 or in the range of 0.01 to 0.1,

[0028] c is in the range of 0.01 to 0.1, and

[0029] d is in the range of 0 to 0.1,

[0030] M is at least one of Al, Mg, Nb, Ti, Mo, W and Zr, and

[0031] a+b+c=1,

[0032] and Mn, and x is in the range of 0 to 0.05,

[0033] (b) treating the particulate electrode active material with an aqueous medium containing an Al or Sb compound,

[0034] (c) at least partially removing the water from step (b),

[0035] (d) optionally, subjecting the mixture from step (c) to a heat treatment,

[0036] (e) adding at least one compound selected from compounds of Al or Sb or B to the solid material obtained from step (d) (if applicable) or from step (c), respectively, thereby depositing at least one element selected from on the surface of the particulate electrode active material, wherein, respectively, the element deposited in step (e) is different from the element deposited in step (b), and

[0037] (f) subjecting the residue obtained from step (e) to a heat treatment.

[0038] The method of the present invention comprises at least five steps: (a), (b), (c), (e) and (f), which are also referred to as step (a) and step (b) and step (c) and step (e) and step (e) respectively in the context of the present invention. Steps (a) to (g) are performed sequentially. Step (d) is optional.

[0039] In step (a), the method of the present invention comprises: 1+x TM 1-x Starting from an electrode active material of O2, wherein TM comprises Ni and optionally at least one transition metal selected from Co and Mn and optionally at least one element selected from Al, Mg and Ba, and wherein at least 50 mol-%, preferably at least 75 mol-% of TM is Ni, and x is in the range of 0 to 0.2. Said material is also referred to as starting material hereinafter.

[0040] In one embodiment of the invention, the starting material has an average particle size (D50) in the range of 3 to 20 μm, preferably 4 to 16 μm. The average particle size can be determined, for example, by light scattering or laser diffraction or electroacoustic spectroscopy. The particles are usually composed of agglomerates of primary particles, and the above particle sizes refer to the secondary particle diameters.

[0041] In one embodiment of the present invention, the starting material has a molecular weight of 0.1 to 2.0 μm. 2 The specific surface area (BET) in the range of 1000 Å / g is also referred to below as “BET surface”. The BET surface can be determined according to DIN ISO 9277:2010 by nitrogen adsorption after degassing the sample at 200° C. for 30 minutes or more and beyond this time.

[0042] In one embodiment of the present invention, the particulate material provided in step (a) has a moisture content in the range of 20 to 2,000 ppm, preferably 50 to 1,200 ppm, as determined by Karl-Fischer titration.

[0043] The variable TM corresponds to the general formula (I)

[0044] (Ni a Co b Mn c ) 1-d M 1 d (I)

[0045] where a+b+c=1 and

[0046] a is in the range of 0.6 to 0.99, preferably 0.75 to 0.95, more preferably 0.85 to 0.95,

[0047] b is 0 or in the range of 0.01 to 0.2, preferably 0.025 to 0.2, more preferably 0.025 to 0.1,

[0048] c is in the range of 0 to 0.2, preferably 0.025 to 0.2, more preferably 0.05 to 0.1,

[0049] d is in the range of 0 to 0.1, preferably 0 to 0.04,

[0050] M 1 It is at least one of Al, Mg, Ti, Nb, Mo, W and Zr, and preferably at least one of Al, Ti, Zr and W.

[0051] In one embodiment of the present invention, the variable c is 0, M 1 is Al, and d is in the range of 0.01 to 0.05.

[0052] In one embodiment of the present invention, TM corresponds to formula (I), and x is in the range of 0 to 0.2, preferably 0 to 0.1 and even more preferably 0.01 to 0.05.

[0053] In one embodiment of the present invention, TM is selected from Ni 0.6 Co 0.2 Mn 0.2 、Ni 0.7 Co 0.2 Mn 0.1 、Ni 0.8 Co 0.1 Mn 0.1 、Ni 0.83 Co 0.12 Mn 0.05 、Ni 0.89 Co 0.055 Al 0.055 、Ni 0.91 Co 0.045 Al 0.045 and Ni 0.85 Co 0.1 Mn 0.05 .

[0054] The electrode active material provided in step (a) is usually free of conductive carbon, which means that the conductive carbon content of the starting material is less than 1% by weight, preferably 0.001 to 1.0% by weight, relative to the starting material.

[0055] Some elements are ubiquitous. In the context of the present invention, trace amounts of ubiquitous metals such as sodium, calcium, iron or zinc as impurities will not be taken into account in the description of the present invention. Trace amounts in this context will mean amounts of 0.02 mol-% or less relative to the total metal content of the starting material.

[0056] In step (b), the electrode active material provided in step (a) is treated with an aqueous medium, preferably water. The aqueous medium may have a pH value in the range of 2 to 14, preferably at least 3.5, more preferably 5 to 7. The pH value is measured at the beginning of step (b). It is observed that during step (b), the pH value increases to at least 10, for example 11 to 13. In embodiments where the pH value is in the range of 10 to 11 at the beginning of step (b), the value increases to greater than 11 to a maximum of 13. In embodiments where the pH value is in the range of 3 to less than 10 at the beginning of step (b), the value increases to 11 to a maximum of 13 during step (b).

[0057] Preferably the aqueous medium used in step (b) is at least partially freed of water hardness, in particular calcium. Preferably desalinated water is used.

[0058] In one embodiment of the present invention, the aqueous medium may contain a compound selected from compounds of Al or Sb, which is dissolved or slurried.

[0059] In one embodiment of the present invention, the amount of the compound of Al or Sb is in the range of 0.05 to 1.5 mol-%, preferably 0.15 to 0.9 mol-%, relative to TM.

[0060] Examples of Al or Sb compounds used in step (b) are selected from water-soluble and water-insoluble compounds. Examples of water-soluble Al compounds are Al2(SO4)3, KAl(SO4)2 or Al(NO3)3. In this context, "water-soluble" means a solubility of at least 10 g Al or Sb compound / l water at 25°C, respectively.

[0061] In other embodiments, the inorganic Al compound is water-insoluble. In this context, "water-insoluble" means a solubility of less than 0.1 g Al compound / l water at 25°C. Examples are, for example, Al2O3, Al(OH)3, AlOOH, Al2O3·aqueous, preferably AlOOH and Al2O3.

[0062] Examples of water-insoluble Sb compounds are compounds of Sb(+III) and Sb(+V). Examples of Sb(+III) compounds are Sb(OH)3, Sb2O3·aqueous, Sb2(SO4)3, SbOOH, LiSbO2 and Sb2O3. Examples of Sb(+V) compounds are Sb2O5, LiSb3O8, LiSbO3, Li3SbO4, Li5SbO5, Li7SbO6, Sb2O4 (Sb(III)Sb(V)O4), and oxyhydroxides of Sb(+V), such as but not limited to SbO(OH)3, Sb2O4(OH)2, Sb2O3(OH)4, Sb3O6OH, Sb3O7OH. Preferred are Sb(OH)3, Sb2O3·aqueous and Sb2O3. Examples of water-soluble compounds are Sb2(SO4)3, SbONO3 and Sb(NO3)3.

[0063] The water-insoluble Al or Sb compound may be dispersed or slurried in water.

[0064] In the context of the present invention, AlOOH does not necessarily carry equimolar amounts of oxide ions and hydroxide ions and is sometimes also referred to as Al(O)(OH). This applies mutatis mutandis to SbOOH.

[0065] The Al or Sb compounds used in step (b), and in particular Al2O3 and Al(O)(OH), respectively, can be pure (≥99.9 mol % Al, relative to total metal including Si) or doped with oxides such as La2O3, Ce2O3, titanium dioxide or zirconium oxide in an amount of, for example, 0.1 to 5 mol %.

[0066] In step (b), more preferred compounds of Al and Sb are Al2(SO4)3 and Sb2O3.

[0067] In one embodiment of the present invention, the water-insoluble Al or Sb compound has an average particle diameter (D50) in the range of 10 nm to 10 μm, preferably 10 nm to 3 μm. The average diameter (D50) can be determined by imaging methods such as SEM.

[0068] In another embodiment, the aqueous medium does not contain any of the heteropolyacids or the corresponding lithium or ammonium salts, nor does it contain Al or Sb compounds that are neither dissolved nor slurried.

[0069] In one embodiment of the present invention, step (b) is carried out at a temperature ranging from 5°C to 85°C, preferably from 10°C to 60°C.

[0070] In one embodiment of the present invention, step (b) is carried out at normal pressure. However, it is preferred that step (b) is carried out at an elevated pressure (e.g., 10 mbar to 10 bar higher than normal pressure), or by using suction (e.g., 50 to 250 mbar lower than normal pressure, preferably 100 to 200 mbar lower than normal pressure).

[0071] Step (b) can be carried out, for example, in a container that can be easily drained, for example due to its location above the filtering device. The starting material can be loaded into such a container and the aqueous medium is subsequently introduced. In another embodiment, the aqueous medium is loaded into such a container and the starting material is subsequently introduced. In another embodiment, the starting material and the aqueous medium are introduced simultaneously.

[0072] In one embodiment of the present invention, in step (b), the amounts of water and the electrode active material have a weight ratio in the range of 1:5 to 5:1, preferably 2:1 to 1:2.

[0073] Step (b) can be supported by mixing operations (eg shaking) or in particular by stirring or shearing, see below.

[0074] In one embodiment of the invention, step (b) has a duration in the range of 1 minute to 90 minutes, preferably 1 minute to less than 60 minutes. In the embodiment where in step (b), water treatment and water removal overlap or are carried out simultaneously, a duration of 5 minutes or more is possible.

[0075] In one embodiment of the present invention, the treatment according to step (b) and the water removal according to step (c) are performed sequentially.

[0076] After or during the treatment with the aqueous medium according to step (b), the water can be removed by any type of filtration, for example on a belt filter or in a filter press.

[0077] In one embodiment of the invention, step (c) is started at the latest 5 minutes after starting step (b). Step (c) comprises partially removing water from the treated particulate material, for example by solid-liquid separation, for example by decantation or preferably by filtration. The "partial removal" may also be referred to as partially separating out.

[0078] In one embodiment of step (c), the slurry obtained in step (b) is discharged directly into a centrifuge (e.g., a decanting centrifuge or a filtering centrifuge) or onto a filtering device (e.g., a suction filter or a filter press or a belt filter), which is preferably located directly below the container in which step (b) is performed. Then, filtration is started.

[0079] In a particularly preferred embodiment of the invention, steps (b) and (c) are carried out in a filter press or in a filtration device with a stirrer, such as a pressure filter with a stirrer or a suction filter with a stirrer (German for example "stirred filter suction filter (Rührfilternutsche)"). The removal of the aqueous medium is started at most 5 minutes, preferably at most 3 minutes, or even immediately after the starting material and the aqueous medium are combined according to step (b) by starting the filtration. On a laboratory scale, steps (b) and (c) can be carried out on a Buchner funnel, and steps (b) and (c) can be supported by manual stirring.

[0080] In a preferred embodiment, step (b) is performed in a filtration device, such as an agitated filtration device that allows agitation of the slurry or filter cake in the filter.

[0081] In one embodiment of the present invention, the water removal according to step (c) has a duration ranging from 1 minute to 1 hour.

[0082] In one embodiment of the invention, the stirring in step (b) and step (c) (if applicable) is carried out at a speed ranging from 1 to 50 revolutions per minute ("rpm"), preferably from 5 to 20 rpm. In other embodiments, the speed is from 200 to 400 rpm.

[0083] In one embodiment of the present invention, the filter medium may be selected from the group consisting of ceramics, sintered glass, sintered metal, organic polymer membranes, nonwoven materials, and fabrics.

[0084] In one embodiment of the invention, steps (b) and (c) are carried out in an atmosphere with a reduced CO2 content, for example, a carbon dioxide content in the range of 0.01 to 500 ppm by weight, preferably 0.1 to 50 ppm by weight. The CO2 content can be determined by an optical method, for example using infrared light. Even more preferably, steps (b) and (c) are carried out in an atmosphere with a carbon dioxide content below the detection limit, for example using an optical method based on infrared light.

[0085] From step (c) a solid residue is obtained, preferably in the form of a wet filter cake.The moisture content of the solid residue and in particular the filter cake may be in the range of 3 to 20% by weight, preferably 4 to 9% by weight.

[0086] In an optional step (d), water or solvent is at least partially removed from the mixture obtained from step (d), for example by evaporation. In a preferred embodiment of step (d), water is at least partially evaporated at a temperature in the range of 40° C. to 250° C. Preferably, the water evaporation is carried out at 0.1 to 10 mbar (“in vacuum”).

[0087] In step (e), at least one compound selected from compounds of B or Al or Sb is added to the solid material obtained from step (d) (if applicable) or from step (c), respectively, thereby depositing at least one element selected from Al, Sb or B on the surface of the particulate electrode active material, wherein the element deposited in step (e) is different from the element deposited in step (b) or (d). This compound can be added as a slurry or solution or as a dry powder, preferably a dry powder.

[0088] Thus, if step (d) is performed, step (e) is performed on the solid material obtained from step (d). In embodiments where step (d) is not performed, step (e) is performed on the mixture obtained from step (c) (if applicable). In embodiments where step (d) is not performed, step (e) is performed on the solid material obtained from step (c).

[0089] Examples of the aluminum compound added in step (e) are selected from the same compounds as disclosed above and below with respect to step (c), preferably water-insoluble Al compounds and B compounds.

[0090] Examples of boron compounds are B2O3, boric acid (B(OH)3) and lithium borates, such as LiBO2. Boric acid is preferred.

[0091] In one embodiment of the present invention, the water-insoluble aluminum compound has an average particle size (D50) in the range of 200 nm to 5 μm, preferably 2 to 5 μm, the compound is dispersed in water and the D50 is measured by X-ray diffraction.

[0092] Examples of antimony compounds are compounds of Sb(+III) and Sb(+V). Examples of Sb(+III) compounds are Sb(OH)3, Sb2O3·aqueous, Sb2(SO4)3, SbOOH, LiSbO2 and Sb2O3. Examples of Sb(+V) compounds are Sb2O5, LiSb3O8, LiSbO3, Li3SbO4, Li5SbO5, Li7SbO6, Sb2O4 (Sb(III)Sb(V)O4), and oxyhydroxides of Sb(+V), such as but not limited to SbO(OH)3, Sb2O4(OH)2, Sb2O3(OH)4, Sb3O6OH, Sb3O7OH. Preferred are Sb(OH)3, Sb2O3·aqueous and Sb2O3.

[0093] In one embodiment of the present invention, the compound of B or Al or Sb is in the range of 0.05 to 1.5 mol-%, preferably 0.15 to 0.9 mol-% relative to TM.

[0094] When performing step (e), the compound or heteropolyacid of Sb or Al or B is selected in the following manner: by performing step (e), at least one element selected from Al, Sb and B is deposited on the surface of the particulate electrode active material, and wherein the element deposited in step (e) is different from the element deposited in steps (b) and (d).

[0095] In one embodiment of the present invention, the at least one compound of Al or B or Sb is added as a particulate solid, such as a dry powder. In particular, in the embodiment in which step (d) has been carried out, step (e) is carried out by adding the compound of Al or B or Sb as a dry powder. "Dry powder" means that the residual moisture content determined by Karl-Fischer titration is 0.1% by weight or less.

[0096] Step (e) can be supported by a mixing operation, such as shaking, or in particular by stirring or shearing or grinding, see below.

[0097] In one embodiment of the invention, step (e) has a duration in the range of 1 minute to 60 minutes, preferably 1 minute to less than 30 minutes. In the embodiment where in step (e), water treatment and water removal overlap or are carried out simultaneously, a duration of 5 minutes or more is possible.

[0098] In one embodiment of the present invention, step (e) is preferably at a temperature in the range of 10° C. to 80° C. Even more preferred is ambient temperature.

[0099] In one embodiment of the present invention, step (e) is carried out in an air atmosphere, or under an inert gas (such as nitrogen), preferably ambient air.

[0100] In one embodiment of the present invention, steps (c) to (f) are carried out in the same type of container, for example, in a filtration device with a stirrer, such as a pressure filter with a stirrer or a suction filter with a stirrer.

[0101] The method of the present invention comprises the following steps (gf:

[0102] (g) heat treating the material obtained from step (e).

[0103] The step (gf) is particularly preferred in embodiments wherein the one or more compounds of Al or B or Sb are added as an aqueous slurry or aqueous solution.

[0104] Step (gf) can be carried out in any type of oven, such as a roller hearth kiln, a push plate kiln, a rotary kiln, a pendulum kiln, or a muffle oven for laboratory scale experiments.

[0105] The temperature of the heat treatment according to step (gf) may be in the range of 150°C to 900°C, preferably 250°C to 700°C, and even more preferably 300°C to 650°C. The temperature refers to the maximum temperature of step (gf).

[0106] Without wishing to be bound by any theory, it is assumed that by the conduction of step (gf), the boron compound can react with the residual lithium compound to form a lithium-B compound, such as LiBO2. In addition, it is assumed that any aluminum compound is converted to Al2O3 and from Li 1+ x TM 1-x Lithium is extracted from O2 to produce Li 1+x1 TM 1-x1 For O2 and NiOOH, x1 is in the range of -0.02 to +0.03.

[0107] In one embodiment of the present invention, the temperature is increased and then reaches the desired temperature of 150° C. to 900° C., preferably 250° C. to 700° C. For example, the mixture of step (e) is first heated to a temperature of 350° C. to 550° C. and then kept constant for a period of 10 min to 4 hours, and then it is increased to 500° C. to 900° C., preferably 500° C. to 850° C.

[0108] In one embodiment of the present invention, the heating rate in step (gf) is in the range of 0.1 to 10°C / min.

[0109] In one embodiment of the present invention, step (gf) is carried out in a roller hearth kiln, a pusher kiln or a rotary kiln or a combination of at least two of the foregoing. The advantage of a rotary kiln is that the homogeneity of the material produced therein is very good. In roller hearth kilns and pusher kilns, different reaction conditions for the different steps can be easily set. In laboratory scale tests, box furnaces and tube furnaces as well as split tube furnaces are also feasible.

[0110] In one embodiment of the present invention, step (gf) is carried out in an oxygen-containing atmosphere, for example in a nitrogen-air mixture, in a noble gas-oxygen mixture, in air, in oxygen, in oxygen-enriched air, or in pure oxygen. In a preferred embodiment, the atmosphere in step (gf) is selected from air, oxygen, and oxygen-enriched air. Oxygen-enriched air can, for example, be a 50:50 mixture by volume of air and oxygen. Other options are a 1:2 mixture by volume of air and oxygen, a 1:3 mixture by volume of air and oxygen, a 2:1 mixture by volume of air and oxygen, and a 3:1 mixture by volume of air and oxygen. Pure oxygen is even more preferred.

[0111] In one embodiment of the invention, step (gf) has a duration in the range of 30 minutes to 5 hours. Preferably 60 minutes to 4 hours. In this context, the cooling time is neglected.

[0112] By carrying out the method of the invention, an electrode active material having excellent electrochemical characteristics is obtained. Without wishing to be bound by any theory, we assume that the decomposition products of the combination of compounds of B or Sb or Al (as the case may be) may lead to the removal of lithium compounds deposited at the surface of the electrode active material.

[0113] The cathode active material obtained by the method of the present invention has many advantages. The cathode made of such cathode active material exhibits reduced resistance growth during cycling.

[0114] A further aspect of the present invention relates to a coated cathode active material, also referred to hereinafter as the cathode active material of the present invention. The cathode active material of the present invention has a general formula Li 1+x1 TM 1-x1 O2 core, wherein TM is a metal combination according to formula (I), and x1 is in the range of -0.02 to 0.03, and the cathode active material has a shell comprising

[0115] - a lithium-boron oxide compound or B(OH)3, and

[0116] - Nickel oxyhydroxide, such as NiOOH, and

[0117] - Aluminium oxide compounds, such as Al2O3, or Sb compounds.

[0118] In one embodiment of the present invention, TM is a metal combination according to formula (I) wherein a+b+c=1, and

[0119] (Ni a Co b Mn c ) 1-d M 1 d (I)

[0120] a is in the range of 0.6 to 0.99, preferably 0.75 to 0.95, more preferably 0.85 to 0.95,

[0121] b is 0 or in the range of 0.01 to 0.2, preferably 0.025 to 0.2, more preferably 0.025 to 0.1,

[0122] c is in the range of 0 to 0.2, preferably 0.025 to 0.2, more preferably 0.05 to 0.1,

[0123] d is in the range of 0 to 0.1, preferably 0 to 0.04,

[0124] M 1 It is at least one of Al, Mg, Ti, Nb, Mo, W and Zr, and preferably at least one of Al, Ti, Zr and W.

[0125] In one embodiment of the present invention, the variable c is 0, M 1 is Al, and d is in the range of 0.01 to 0.05.

[0126] In one embodiment of the present invention, TM corresponds to formula (I), and x is in the range of 0 to 0.2, preferably 0 to 0.1 and even more preferably 0.01 to 0.05.

[0127] The cathode active material of the present invention further comprises a shell. The shell comprises

[0128] Lithium-boron oxide compounds or B(OH)3

[0129] and nickel oxyhydroxide, preferably NiOOH,

[0130] and an aluminum oxide compound or an Sb compound, preferably an aluminum oxide compound.

[0131] The nickel oxyhydroxide can be detected by X-ray diffraction.

[0132] In one embodiment of the present invention, the molar ratio of Al to B in the shell of the cathode active material of the present invention is in the range of 1:10 to 3:1, preferably 1:7 to 2:3.

[0133] In one embodiment of the present invention, the shell of the cathode active material of the present invention has a thickness in the range of 2 to 10 nm as determined by time-of-flight secondary ion mass spectrometry ("TOF-SIMS").

[0134] Another aspect of the invention is an electrode comprising at least one cathode active material according to the invention. They are particularly useful for lithium ion batteries. Lithium ion batteries comprising at least one electrode according to the invention exhibit very good discharge and cycling behavior, and they show good safety behavior.

[0135] In one embodiment of the present invention, the cathode of the present invention comprises

[0136] (A) at least one cathode active material of the present invention, as described above,

[0137] (B) carbon in a conductive state, and

[0138] (C) an adhesive,

[0139] (D) Current collector.

[0140] In a preferred embodiment of the present invention, the cathode of the present invention comprises

[0141] (A) 80 to 98% by weight of the cathode active material of the present invention,

[0142] (B) 1 to 17% by weight of carbon,

[0143] (C) 1 to 10% by weight of a binder,

[0144] Percentages are relative to the sum of (A), (B) and (C).

[0145] The cathode according to the invention contains conductive modified carbon, also referred to as carbon (B) for short. Carbon (B) can be selected from soot, activated carbon, carbon nanotubes, graphene and graphite. Carbon (B) can be added as is during the preparation of the electrode material according to the invention.

[0146] The electrodes according to the present invention may comprise additional components. They may include a current collector (D), such as but not limited to an aluminum foil. They further comprise a binder material (C), hereinafter also referred to as a binder (C). The current collector (D) is not further described herein.

[0147] Suitable binders (C) are preferably selected from organic (co)polymers. Suitable (co)polymers, i.e. homopolymers or copolymers, can be selected from (co)polymers obtainable, for example, by anionic, catalytic or free radical (co)polymerization, in particular from polyethylene, polyacrylonitrile, polybutadiene, polystyrene, and copolymers of at least two comonomers selected from ethylene, propylene, styrene, (meth)acrylonitrile and 1,3-butadiene. Polypropylene is also suitable. Polyisoprene and polyacrylates are also suitable. Polyacrylonitrile is particularly preferred.

[0148] In the context of the present invention, polyacrylonitrile is understood to mean not only polyacrylonitrile homopolymers but also copolymers of acrylonitrile with 1,3-butadiene or styrene. Polyacrylonitrile homopolymers are preferred.

[0149] In the context of the present invention, polyethylene is understood to mean not only homopolyethylene but also copolymers of ethylene, which copolymers contain at least 50 mol % of copolymerized ethylene and up to 50 mol % of at least one other comonomer, for example α-olefins such as propylene, butene (1-butene), 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-pentene, and also isobutylene, vinyl aromatics such as styrene, and also C1-C2 (meth)acrylic acid, vinyl acetate, vinyl propionate, C1-C2 (meth)acrylic acid ... 10 - Alkyl esters, especially methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, 2-ethylhexyl acrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, and also maleic acid, maleic anhydride and itaconic anhydride. The polyethylene may be HDPE or LDPE.

[0150] In the context of the present invention, polypropylene is understood to mean not only homopolypropylene, but also copolymers of propylene, the copolymers comprising at least 50 mol% of copolymerized propylene and up to 50 mol% of at least one other comonomer, for example ethylene and α-olefins such as butene, 1-hexene, 1-octene, 1-decene, 1-dodecene and 1-pentene. The polypropylene is preferably isotactic or substantially isotactic.

[0151] In the context of the present invention, polystyrene is understood to mean not only homopolymers of styrene but also C1-C12 copolymers with acrylonitrile, 1,3-butadiene, (meth)acrylic acid, (meth)acrylic acid, and the like. 10 - copolymers of alkyl esters, divinylbenzene, especially 1,3-divinylbenzene, 1,2-diphenylethylene and α-methylstyrene.

[0152] Another preferred binder (C) is polybutadiene.

[0153] Other suitable binders (C) are selected from polyethylene oxide (PEO), cellulose, carboxymethylcellulose, polyimide and polyvinyl alcohol.

[0154] In one embodiment of the present invention, the binder (C) is selected from a group consisting of binders having an average molecular weight M in the range of 50,000 to 1,000,000 g / mol, preferably to 500,000 g / mol. w Those (co)polymers.

[0155] The binder (C) may be a cross-linked or non-cross-linked (co)polymer.

[0156] In a particularly preferred embodiment of the present invention, binder (C) is selected from halogenated (co) polymers, especially fluorinated (co) polymers. Halogenated or fluorinated (co) polymers are understood to mean those (co) polymers comprising at least one (co) polymerized (co) monomer having at least one halogen atom or at least one fluorine atom per molecule, more preferably at least two halogen atoms or at least two fluorine atoms per molecule. Examples are polyvinyl chloride, polyvinylidene chloride, polytetrafluoroethylene, polyvinylidene fluoride (PVdF), tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), vinylidene fluoride-tetrafluoroethylene copolymer, perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer and ethylene-chlorofluoroethylene copolymer.

[0157] Suitable binders (C) are, in particular, polyvinyl alcohol and halogenated (co)polymers, for example polyvinyl chloride or polyvinylidene chloride, in particular fluorinated (co)polymers such as polyvinyl fluoride and in particular polyvinylidene fluoride and polytetrafluoroethylene.

[0158] The electrode of the present invention may contain 3 to 10% by weight of one or more binders (d), relative to the sum of component (a), component (b) and carbon (c).

[0159] Another aspect of the invention is a battery or electrochemical cell comprising

[0160] (1) at least one cathode comprising the cathode active material (A) of the present invention, carbon (B) and a binder (C),

[0161] (2) at least one anode, and

[0162] (3) At least one electrolyte.

[0163] Embodiments of the cathode (1) have been described in detail above.

[0164] The anode (2) may contain at least one anode active material, such as carbon (graphite), TiO2, lithium titanium oxide, silicon or tin. The anode (2) may additionally include a current collector, such as a metal foil such as copper foil.

[0165] The electrolyte (3) may contain at least one non-aqueous solvent, at least one electrolyte salt and optionally additives.

[0166] The nonaqueous solvent used for the electrolyte (3) may be liquid or solid at room temperature, and is preferably selected from polymers, cyclic or noncyclic ethers, cyclic and noncyclic acetals, and cyclic or noncyclic organic carbonates.

[0167] Examples of suitable polymers are in particular polyalkylene glycols, preferably polyC1-C4-alkylene glycols, and in particular polyethylene glycol. Here, the polyethylene glycol may contain up to 20 mol % of one or more C1-C4-alkylene glycols. The polyalkylene glycol is preferably a polyalkylene glycol with two methyl or ethyl end caps.

[0168] The molecular weight M of suitable polyalkylene glycols and in particular suitable polyethylene glycols is w It may be at least 400 g / mol.

[0169] The molecular weight M of suitable polyalkylene glycols and in particular suitable polyethylene glycols is w It may be up to 5,000,000 g / mol, preferably up to 2,000,000 g / mol.

[0170] Examples of suitable acyclic ethers are, for example, diisopropyl ether, di-n-butyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, of which 1,2-dimethoxyethane is preferred.

[0171] Examples of suitable cyclic ethers are tetrahydrofuran and 1,4-dioxane.

[0172] Examples of suitable acyclic acetals are, for example, dimethoxymethane, diethoxymethane, 1,1-dimethoxyethane and 1,1-diethoxyethane.

[0173] Examples of suitable cyclic acetals are 1,3-dioxane and in particular 1,3-dioxolane.

[0174] Examples of suitable acyclic organic carbonates are dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.

[0175] Examples of suitable cyclic organic carbonates are compounds of the general formula (II) and (III)

[0176]

[0177] Where R1 , R 2 and R 3 may be identical or different and are selected from hydrogen and C1-C4-alkyl, for example methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl, wherein R 2 and R 3 Preferably not all are tert-butyl.

[0178] In a particularly preferred embodiment, R 1 is methyl and R 2 and R 3 Each is hydrogen, or R 1 , R 2 and R 3 Each is hydrogen.

[0179] Another preferred cyclic organic carbonate is vinylene carbonate, formula (IV).

[0180]

[0181] The solvent or solvents are preferably used in anhydrous state, ie with a water content in the range from 1 ppm to 0.1% by weight, which can be determined, for example, by Karl-Fischer titration.

[0182] The electrolyte (3) further comprises at least one electrolyte salt. Suitable electrolyte salts are in particular lithium salts. Examples of suitable lithium salts are LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC(C n F 2n+1 SO2)3, lithium imide such as LiN(C n F 2n+1 SO2)2, wherein n is an integer in the range of 1 to 20, LiN(SO2F)2, Li2SiF6, LiSbF6, LiAlCl4 and compounds having the general formula (C n F 2n+1 SO2) t Salts of YLi, wherein m is defined as follows:

[0183] When Y is selected from oxygen and sulfur, t=1,

[0184] When Y is selected from nitrogen and phosphorus, t=2, and

[0185] When Y is selected from carbon and silicon, t=3.

[0186] Preferred electrolyte salts are selected from LiC(CF3SO2)3, LiN(CF3SO2)2, LiPF6, LiBF4, LiClO4, among which LiPF6 and LiN(CF3SO2)2 are particularly preferred.

[0187] In a preferred embodiment of the present invention, the electrolyte (3) contains at least one flame retardant. Available flame retardants can be selected from trialkyl phosphates (the alkyl groups are different or the same), triaryl phosphates, alkyl dialkyl phosphonates and halogenated trialkyl phosphates. Preferred are tri-C1-C4-alkyl phosphates (the C1-C4-alkyl groups are different or the same), tribenzyl phosphate, triphenyl phosphate, phosphonic acid C1-C4-alkyl di-C1-C4-alkyl esters and fluorinated tri-C1-C4-alkyl phosphates.

[0188] In a preferred embodiment, the electrolyte (3) comprises at least one flame retardant selected from trimethyl phosphate, CH3-P(O)(OCH3)2, triphenyl phosphate and tris-(2,2,2-trifluoro-ethyl)phosphate.

[0189] The electrolyte (3) may contain 1 to 10% by weight of a flame retardant based on the total amount of the electrolyte.

[0190] In an embodiment of the invention, the battery according to the invention comprises one or more separators (4) by means of which the electrodes are mechanically separated. Suitable separators (4) are polymer films, in particular porous polymer films, which are non-reactive to metallic lithium. Particularly suitable materials for the separators (4) are polyolefins, in particular film-forming porous polyethylene and film-forming porous polypropylene.

[0191] The membrane (4) made of polyolefin, in particular polyethylene or polypropylene, can have a porosity in the range of 35% to 45%. Suitable pore sizes are, for example, in the range of 30 to 500 nm.

[0192] In another embodiment of the present invention, the separator (4) may be selected from PET nonwovens filled with inorganic particles. Such separators may have a porosity in the range of 40% to 55%. Suitable pore sizes are, for example, in the range of 80 to 750 nm.

[0193] The battery according to the invention may further comprise a housing, which may have any shape, for example the shape of a cubic or cylindrical disk. In a variant, a metal foil configured as a pouch is used as housing.

[0194] The battery according to the invention provides very good discharge and cycling behavior, in particular at high temperatures (45° C. or higher, for example up to 60° C.), in particular with regard to capacity loss.

[0195] The battery according to the invention may comprise two or more electrochemical cells combined with one another, which may be connected in series or in parallel, for example. Preferably they are connected in series. In the battery according to the invention, at least one of the electrochemical cells comprises at least one electrode according to the invention. Preferably, in the electrochemical cells according to the invention, the majority of the electrochemical cells comprise an electrode according to the invention. Even more preferably, in the battery according to the invention, all electrochemical cells comprise an electrode according to the invention.

[0196] The invention further provides for the use of a battery according to the invention in an apparatus, in particular in a mobile device. Examples of mobile devices are vehicles, such as cars, bicycles, aircraft or water vehicles (such as ships or vessels). Other examples of mobile devices are those that are moved manually, such as computers, in particular laptops, telephones or electric hand tools, such as in the construction industry, in particular drills, battery-powered screwdrivers or battery-powered staplers.

[0197] The present invention is further illustrated by working examples.

[0198] General Description: N-Methyl-2-pyrrolidone: NMP.

[0199] Ultra-dry air: dehumidified air with a dew point below -30°C and a CO2 content of less than 50ppm

[0200] "In vacuum": 0.1 to 10 mbar

[0201] I. Synthesis of cathode active materials

[0202] I.1 Synthesis of Precursors

[0203] I.1.1 Synthesis of Precursor TM-O.1

[0204] A stirred tank reactor was filled with deionized water and 6 g of ammonia solution per kg of water. The solution was temperature adjusted to 55° C. and the pH was adjusted to 11.8 by adding aqueous sodium hydroxide solution.

[0205] The coprecipitation reaction was started by simultaneously feeding an aqueous solution of transition metal sulfate and an aqueous solution of sodium hydroxide through a coaxial nozzle at a flow rate ratio of 1.97 and a total flow rate resulting in an average residence time of 5 hours. The transition metal solution contained Ni, Co and Mn in a molar ratio of 91:4.5:4.5 and a total transition metal concentration of 1.65 mol / kg. The aqueous sodium hydroxide solution was a 25 wt.% sodium hydroxide solution and a 25 wt.% ammonia solution in a weight ratio of about 11. The pH was maintained at 11.8 by feeding the aqueous sodium hydroxide solution alone. From the start of all feeds, the suspension continued to overflow. The mixed transition metal (TM) oxyhydroxide precursor TM-OH.1 was obtained by filtering the resulting suspension, washing with sodium hydroxide and distilled water, and drying at 135°C. The dried precursor TM-OH.1 was further dehydrated at 475°C to produce TM-O.1.

[0206] I.1.2 Synthesis of precursor TM-OH.2

[0207] A stirred tank reactor was filled with deionized water and 20 g of ammonium sulfate per kg of water. The solution was warmed to 55°C and its pH was adjusted to 12 by adding aqueous sodium hydroxide solution.

[0208] The coprecipitation reaction was started by simultaneously feeding an aqueous solution of transition metal sulfate and an aqueous solution of sodium hydroxide at a flow rate ratio of 1.97 and a total flow rate resulting in an average residence time of 5 hours. The transition metal solution contained Ni, Co and Mn in a molar ratio of 88:7:5 and a total transition metal concentration of 1.65 mol / kg. The aqueous sodium hydroxide solution was a 25 wt.% sodium hydroxide solution and a 25 wt.% ammonia solution in a weight ratio of about 17:1. The pH value was maintained at 12 by feeding the aqueous sodium hydroxide solution alone. From the start of all feeds, a continuous overflow of the suspension was started. The mixed transition metal (TM) oxyhydroxide precursor TM-OH.2 was obtained by filtering the resulting suspension, washing with sodium hydroxide and distilled water, drying in air at 120°C and sieving.

[0209] I.2TM-O.1 and TM-OH.2 are converted into cathode active materials

[0210] I.2.1 Production of basic cathode active material B-CAM.1, step (a.1)

[0211] I.2.1.1 Synthesis of basic cathode active material B-CAM.1 from TM-O.1, step (a.1)

[0212] The precursor TM-0.1 in an amount of 2.5 kg was mixed with 1.48 kg of LiOH monohydrate, 35 g of Al2O3, 8 g of TiO2 and 13 g of ZrO2 in a grinder or high shear mixer for 15 minutes. The resulting mixture was loaded into a sagger and transferred to a muffle furnace. The temperature was raised to 765°C at a rate of 2C / min under flowing oxygen, and then kept constant at 765°C for 8 hours, and then allowed to cool naturally under flowing oxygen. The resulting powder was then deagglomerated in a grinder, further deagglomerated in an air classifying mill, and sieved through a 325 mesh screen. After deagglomeration, the resulting powder had an average particle size (D50) of 11 μm.

[0213] I.2.1.2 Synthesis of basic cathode active material B-CAM.4 from TM-O.1, step (a.2)

[0214] The precursor TM-0.1 in an amount of 2.5 kg is mixed with 1.48 kg of LiOH monohydrate, 21 g of Al2O3 and 13 g of ZrO2 in a grinder or high shear mixer for 15 minutes. The resulting mixture is loaded into a sagger and transferred to a muffle furnace. The temperature is raised to 765°C at a rate of 2C / min under flowing oxygen, and then kept constant at 765°C for 8 hours, and then allowed to cool naturally to ambient temperature under flowing oxygen. The resulting powder is then deagglomerated in a grinder and sieved through a 325 mesh screen. After deagglomeration, the powder has an average particle size (D50) of 11 μm.

[0215] I.2.1.3 Synthesis of basic cathode active material B-CAM.7 from TM-OH.2, step (a.3)

[0216] 2.7 kg of the dried precursor TM-OH.2 was mixed with 1.29 kg of LiOH monohydrate, 8 g of Al2O3, 4 g of TiO2 and 9 g of ZrO2 in a grinder or high shear mixer for 15 minutes. The resulting mixture was loaded into a sagger and transferred to a muffle furnace. The temperature was raised to 770°C at a rate of 1.2C / min under flowing oxygen, and then kept constant at 770°C for 10.5 hours, and then allowed to cool naturally under flowing oxygen. The resulting powder was then deagglomerated in a grinder and sieved through a 325 mesh screen. After deagglomeration, the resulting powder had an average particle size (D50) of 11 μm.

[0217] I.2.2 Preparation of cathode active material, steps (b) to (f)

[0218] I.2.2.1 Synthesis of C-CAM.2

[0219] Step (b.1): A beaker was charged with 67 ml of deionized water. B-CAM.1 in an amount of 100 g was added. The resulting slurry was stirred at ambient temperature over a period of 10 minutes, during which the slurry temperature was maintained at 25°C.

[0220] Step (c.1): Then, the water is removed by filtering through a filter press, leaving a wet cake.

[0221] Step (d.1): The obtained filter cake was dried in ultra-dry air at 120° C. for 10 hours.

[0222] Step (e.1): Then, 0.57 g (0.9 mol) of boric acid was added and mixed in a high-speed mixer at 25.000 rpm to obtain a mixture.

[0223] Step (f.1): The obtained mixture was heat treated at 300° C. for 2 hours in a muffle furnace in a forced oxygen flow. Then, the obtained powder was sieved with a 45 μm mesh to obtain a comparative cathode active material C-CAM.2.

[0224] I.2.2.2 Synthesis of CAM.3

[0225] Step (b.2): An amount of 100 g of B-CAM.1 was slurried in deionized water (the conductivity of the water was less than 5 μS / m) under constant stirring. An aqueous solution of Al2(SO4)3 was added at 0.3 mol-% relative to the TM in B-CAM.1. The total amount of deionized water used was 67 ml. The resulting slurry was stirred at ambient temperature over a period of 10 minutes.

[0226] Step (c.2): Then, water is removed by filtering through a filter press, leaving a wet cake.

[0227] Step (d.2): The obtained filter cake was dried in ultra-dry air at 120° C. for 10 hours.

[0228] Step (e.2): Then, 0.57 g (0.9 mol) of boric acid was added and mixed in a high-speed mixer at 25.000 rpm to obtain a mixture.

[0229] Step (f.2): The obtained mixture was heat treated in a muffle furnace at 300° C. for 2 hours in a forced oxygen flow. Then, the obtained powder was sieved with a 45 μm mesh to obtain the cathode active material CAM.3 of the present invention.

[0230] 1.2.2.3 Manufacturing of C-CAM.5

[0231] Step (b.3): A beaker was charged with 67 ml of deionized water. B-CAM.4 in an amount of 100 g was added. The resulting slurry was stirred at ambient temperature over a period of 10 minutes, during which the slurry temperature was maintained at 25°C.

[0232] Step (c.3): Then, water is removed by filtering through a filter press, leaving behind a wet cake.

[0233] Step (d.3): The filter cake was dried in UDA at 120°C for 10 hours.

[0234] Step (e.3): Then, 0.57 g (0.9 mol) of boric acid was added and mixed in a high-speed mixer at 25.000 rpm to obtain a mixture.

[0235] Step (f.3): The obtained mixture was heat treated in a muffle furnace at 300° C. for 2 hours in a forced oxygen flow. Then, the obtained powder was sieved with a 45 μm mesh to obtain a comparative cathode active material C-CAM.5.

[0236] I.2.2.4 Synthesis of CAM.6

[0237] Step (b.4): An amount of 100 g of B-CAM.4 was slurried in deionized water (the conductivity of the water was less than 5 μS / m) under constant stirring. An aqueous solution of Al2(SO4)3 was added at 0.3 mol-% relative to the TM in B-CAM.4. The total amount of deionized water used was 67 ml. The resulting slurry was stirred at ambient temperature over a period of 10 minutes.

[0238] Step (c.4): Then, water is removed by filtering through a filter press, leaving behind a wet cake.

[0239] Step (d.4): The obtained filter cake was dried in ultra-dry air at 120° C. for 10 hours.

[0240] Step (e.4): Then, 0.57 g (0.9 mol) of boric acid was added and mixed in a high-speed mixer at 25.000 rpm to obtain a mixture.

[0241] Step (f.4): The obtained mixture was heat treated in a muffle furnace at 300° C. for 2 hours in a forced oxygen flow. Then, the obtained powder was sieved with a 45 μm mesh to obtain the cathode active material CAM.6 of the present invention.

[0242] 1.2.2.5 Manufacturing of C-CAM.8

[0243] Step (b.5): A beaker was charged with 67 ml of deionized water. B-CAM.7 in an amount of 100 g was added. The resulting slurry was stirred at ambient temperature over a period of 10 minutes, during which the slurry temperature was maintained at 25°C.

[0244] Step (c.5): Then, water is removed by filtering through a filter press, leaving behind a wet cake.

[0245] Step (d.5): The obtained filter cake was dried in ultra dry air (air) at 120° C. for 10 hours.

[0246] Step (e.5): Then, 0.57 g (0.9 mol) of boric acid was added and mixed in a high-speed mixer at 25.000 rpm to obtain a mixture.

[0247] Step (f.5): The obtained mixture was heat treated in a muffle furnace at 300° C. for 2 hours in a forced oxygen flow. Then, the obtained powder was sieved with a 45 μm mesh to obtain a comparative cathode active material C-CAM.8.

[0248] I.2.2.6 Synthesis of CAM.9

[0249] Step (b.6): An amount of 100 g of B-CAM.7 was slurried in deionized water (the conductivity of the water was less than 5 μS / m) under constant stirring. An aqueous solution of Al2(SO4)3 was added at 0.3 mol-% relative to the TM in B-CAM.7. The total amount of deionized water used was 67 ml. The resulting slurry was stirred at ambient temperature over a period of 10 minutes.

[0250] Step (c.6): Then, water is removed by filtering through a filter press, leaving behind a wet cake.

[0251] Step (d.6): The obtained filter cake was dried in ultra-dry air at 120° C. for 10 hours.

[0252] Step (e.6): Then, 0.57 g (0.9 mol) of boric acid was added and mixed in a high-speed mixer at 25.000 rpm to obtain a mixture.

[0253] Step (f.6): The obtained mixture was heat treated in a muffle furnace at 300° C. for 2 hours in a forced oxygen flow. Then, the obtained powder was sieved with a 45 μm mesh to obtain the cathode active material CAM.9 of the present invention.

[0254] The results are summarized in Table 1.

[0255] Table 1: Fabrication details and composition of CAM

[0256]

[0257] The cathode active materials of the present invention each have a shell including an aluminum compound, a boron compound (191.8 eV) and NiOOH. NiOOH can be detected in the XP spectrum (855.8 eV).

[0258] II. Testing of cathode active materials

[0259] II.1 Electrode fabrication

[0260] II.1.1 Electrode fabrication, general procedure 1

[0261] Positive electrode: PVDF binder ( 5130) was dissolved in NMP (Merck) to produce an 8.0 wt.% solution. For the preparation of the electrodes, the binder solution (2.5 wt.%) and carbon black (Li400, 2.5 wt.-%) were suspended in NMP. After mixing using a planetary centrifugal mixer (ARE-250, Thinky Corp., Japan), any of the cathode active materials CAM.3 or CAM:.6 of the present invention, or the basic cathode active materials B-CAM.1 or B-CAM.4, or the comparative cathode active materials C-CAM.2 or C-CAM.5 (95 wt.%) were added and the suspension was mixed again to obtain a lumps-free slurry. The solid content of the slurry was adjusted to 65%. The slurry was coated on Al foil using a KTF-S roll-to-roll coater (Mathis AG). All electrodes were calendered before use. The thickness of the cathode material was 43 μm, corresponding to 15 mg / cm 2 Before cell assembly, all electrodes were dried at 120 °C for 7 h.

[0262] II.1.2 Electrode fabrication, general procedure 2

[0263] Positive electrode: PVDF binder ( 5130) was dissolved in NMP (Merck) to produce an 8.0 wt.% solution. For the preparation of the electrodes, the binder solution (4 wt.%) and carbon black (Li250, 3.5 wt.-%) were suspended in NMP. After mixing using a planetary centrifugal mixer (ARE-250, Nissinki, Japan), any of the CAM.9 of the present invention or the basic cathode active material B-CAM.7 or the comparative cathode active material C-CAM.8 (92.5 wt.%) was added and the suspension was mixed again to obtain a lump-free slurry. The solid content of the slurry was adjusted to 65%. The slurry was coated on Al foil using a KTF-S roll-to-roll coater (Mathis AG). All electrodes were calendered before use. The thickness of the cathode material was 48 μm, corresponding to 15 mg / cm 2 Before cell assembly, all electrodes were dried at 120 °C for 7 h.

[0264] II.2 Electrolyte preparation

[0265] The base electrolyte composition was prepared according to Table 2 below.

[0266] Table 2: Basic electrolyte composition

[0267] <![CDATA[LiPF6[%]]]> Ethylene carbonate [%] Ethyl methyl carbonate [%] Dimethyl carbonate [%] EL.1 11.8 44.1 - 44.1 EL.2 12.7 26.2 61.1 -

[0268] For solvents, % refers to % by volume

[0269] II.3 Fabrication of test cells

[0270] II.3.1 Fabrication of test cells based on B-CAM.1, C-CAM.2, CAM.3, B-CAM.4, C-CAM.5 or CAM.6

[0271] A coin-type half-cell (20 mm in diameter and 3.2 mm in thickness) comprising a cathode and lithium metal prepared as described under II.1 as a working electrode and a counter electrode, respectively, was assembled and packaged in an Ar-filled glove box. In addition, the cathode and anode and the separator were stacked in the order of cathode / / separator / / anode to produce a coin-type half-cell. Thereafter, 0.15 mL of EL.1 was introduced into the coin-type cell.

[0272] II.3.2 Fabrication of test cells based on B-CAM.7, C-CAM.8 or CAM.9

[0273] A coin-type half-cell (20 mm in diameter and 3.2 mm in thickness) comprising a cathode and lithium metal prepared as described under III.1.2 as a working electrode and a counter electrode, respectively, was assembled and packaged in an Ar-filled glove box. In addition, the cathode and anode and the separator were stacked in the order of cathode / / separator / / Li foil to produce a half coin cell. Thereafter, 0.15 mL of EL.2 described above (II.2) was introduced into the coin cell.

[0274] III. Coin-type half-cell performance evaluation

[0275] III.1.1 Cyclic tests with coin-type half-cells based on B-CAM.1, C-CAM.2, CAM.3, B-CAM.4, C-CAM.5 and CAM.6

[0276] The battery cell performance was evaluated using the produced button-type batteries. For the battery performance, the initial capacity and reaction resistance of the battery cell were measured. The initial performance and cycling were measured as follows: The button half-cell according to II.3.1 was tested at ambient temperature in the voltage range between 4.3V and 2.7V. For the initial cycle, the initial lithiation was carried out in CC-CV mode, i.e. a constant current (CC) of 0.5C was applied until 0.05C was reached. After a standing time of 10min, reduction lithiation was carried out at a constant current of 0.05C until 2.7V. The results are summarized in Table 3. For the cycle, the current density was 0.33C, and the charge and discharge were repeated 50 times.

[0277] III.1.2 Cyclic test with coin-type half-cells of B-CAM.7, C-CAM.8 or CAM.9

[0278] The battery cell performance was evaluated using the produced button-type batteries. For the battery performance, the initial capacity and reaction resistance of the battery cell were measured. The initial performance and cycling were measured as follows: The button half-cell according to II.3.1 was tested at ambient temperature in the voltage range between 4.35 V and 2.8 V. For the initial cycle, the initial lithiation was carried out in CC-CV mode, i.e. a constant current (CC) of 0.2 C was applied until 0.01 C was reached. After a standing time of 10 min, reduction lithiation was carried out at a constant current of 0.2 C until 2.8 V. The results are summarized in Table 3. For the cycle, the current density was 0.5 C, and the charge and 1.0 C discharge were repeated 50 times.

[0279] The battery cell reaction resistance growth is calculated by the following method:

[0280] After 25 cycles at 0.1C, the coin cell was recharged to 4.3V and the resistance was measured again by the electrochemical impedance spectroscopy (EIS) method. The ratio of the resistance value of the 26th cycle to the second cycle was defined as the resistance growth. The results are summarized in Table 3. [%] The relative resistance growth is based on the resistance growth of the battery cell based on C-CAM.8 as 100%.

[0281] Table 3: Initial charge and discharge capacity and initial reaction resistance, button cell

[0282]

Claims

1. A method for producing a coated cathode active material, the method The following steps are involved: (a) providing a method according to the general formula Li 1+x TM 1-x O 2 A microparticle electrode active material, wherein TM is a metal combination according to the general formula (I), (Ni a Co b Mr c ) 1-d M d (I) in a is in the range of 0.86 to 0.94, b is 0 or in the range of 0.01 to 0.1, c is in the range of 0.01 to 0.1, and d is in the range of 0 to 0.1, M is at least one of Al, Mg, Nb, Ti, Mo, W and Zr, and a+b+c=1, and x is in the range of 0 to 0.05, (b) treating the particulate electrode active material with an aqueous medium containing an Al or Sb compound, (c) at least partially removing the water from step (b), (d) optionally, subjecting the mixture from step (c) to a heat treatment, (e) adding at least one compound selected from compounds of Al or Sb or B to the solid material obtained from step (d) or from step (c), respectively, as applicable, thereby depositing at least one element selected from on the surface of the particulate electrode active material, wherein the element deposited in step (e) is different from the element deposited in step (b), respectively, and (f) subjecting the residue obtained from step (e) to a heat treatment.

2. The method according to claim 1, in, The compound of Al and Sb added in step (b) is selected from AlOOH, Al 2 O 3 、Al 2 (SO 4 ) 3 and Sb 2 O 3 .

3. The method according to claim 1 or 2, in, In step (b), add a mixture selected from AlOOH, Al 2 O 3 and Al 2 (SO 4 ) 3 Al compounds.

4. The method according to any one of the preceding claims, in, Step (f) comprises a calcination step at a maximum temperature in the range of 300°C to 700°C.

5. The method according to any one of the preceding claims, in, Step (f) comprises a drying step at a maximum temperature in the range of 40°C to 250°C.

6. A microparticle cathode active material having a general formula Li 1+x1 TM 1-x1 O 2 A core electrode active material, wherein TM is a metal combination according to the general formula (I) (Ni a Co b Mr c ) 1-d M d (I) in a is in the range of 0.86 to 0.94, b is 0 or in the range of 0.01 to 0.1, c is in the range of 0.01 to 0.1, and d is in the range of 0 to 0.1, M is at least one of Al, Mg, Nb, Ti, Mo, W and Zr, and a+b+c=1, and x1 is in the range of -0.02 to 0.03, and the cathode active material has a shell comprising: Lithium-boron oxide compounds or B(OH) 3 and nickel oxyhydroxide and an aluminum oxide compound or an Sb compound.

7. The cathode active material according to claim 6, in, The molar ratio of Al to B in the shell is in the range of 1:10 to 3:

1.

8. The cathode active material according to any one of claims 6 or 7, in, The shell has a thickness in the range of 2 to 10 nm as determined by time-of-flight secondary ion mass spectrometry.

9. A cathode comprising: (A) at least one cathode active material according to any one of claims 6 to 8, (B) carbon in a conductive state, and (C) Adhesive.

10. The cathode according to claim 9, comprising (A) 80 to 98% by weight of the cathode active material of the present invention, (B) 1 to 17% by weight of carbon, (C) 1 to 10% by weight of a binder, Percentages are relative to the sum of (A), (B) and (C).

11. A battery or electrochemical cell comprising (1) at least one cathode according to claim 9 or 10, (2) at least one anode, and (3) At least one electrolyte.

Citation Information

Patent Citations

  • Kankoseisoseibutsu

    JP1976039024A

  • Positive electrode active material for non-aqueous electrolyte secondary batteries and method for producing the same

    JP4789066B2

  • Nickel composite hydroxide particle and process for producing the same, positive electrode active material for non-aqueous electrolyte secondary battery and process for producing the same, and non-aqueous electrolyte secondary battery

    US20150372300A1

  • Method for covering particles, especially a battery electrode material particles, and particles obtained with such method and a battery comprising such particle

    US8993051B2