Method of forming capacitor electrodes
By adjusting the number of times the TiN and SiN films, and using compound raw materials of multiple Si atoms, the deposition rate and step coverage of capacitor electrodes are improved, and the problem of increasing electrode thickness in capacitors is solved, which leads to a decrease in dielectric layer space, and improves the problem of increasing electrode thickness in capacitors. dielectric constant.
Patent Information
- Application Number
- CN202380026963.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-01
AI Technical Summary
The low step coverage of the midsole electrode and top electrode of the existing capacitors leads to deterioration of capacitor characteristics, and increasing the electrode thickness takes a long time, resulting in a decrease in the dielectric layer space and a decrease in the dielectric constant.
By spraying titanium and silicon-containing raw materials with nitrogen reactants to form TiN and SiN films, the ratio of the number of times the formation of TiN film and SiN films is adjusted, and compound raw materials with multiple Si atoms are used to improve the deposition rate and step coverage of SiN films.
The deposition rate and step coverage of capacitor electrodes are improved, the electrode formation time is reduced, and the dielectric constant of the dielectric layer is enhanced.
Smart Images

Figure CN118891978A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for forming a capacitor electrode, and more particularly to a method for forming a capacitor electrode capable of improving a deposition rate. Background Art
[0002] A capacitor suitable for use in a semiconductor device includes a bottom electrode formed on a substrate, a dielectric layer formed on the bottom electrode, and a top electrode formed on the dielectric layer.
[0003] The substrate may have a groove, and the capacitor may be prepared by laminating a bottom electrode, a dielectric layer, and a top electrode on the substrate. Furthermore, each of the top electrode and the bottom electrode is formed by laminating a TiN film (titanium nitride film) and a SiN film (silicon nitride film).
[0004] On the other hand, the SiN film is formed using silane (SiH 4 ) as a raw material, and SiH 4 has a low deposition rate and a low deposition rate. Therefore, each of the bottom electrode and the top electrode has a low step coverage, which causes the characteristics of the capacitor to deteriorate.
[0005] The low step coverage can be improved by increasing the thickness of each of the bottom electrode and the top electrode. However, in this case, it takes a long time to form the bottom electrode and the top electrode each having a target thickness.
[0006] Furthermore, as the deposition time increases, the thickness of the bottom electrode also increases, and therefore, the space where the dielectric layer is formed inside the trench decreases. This may be a factor causing the dielectric constant of the dielectric layer to decrease.
[0007] (Related technical documents) (Patent document 1) Korean Patent Registration No. 10-1110077 Summary of the invention
[0008] Technical issues
[0009] The present disclosure provides a method of forming a capacitor electrode capable of improving a deposition rate.
[0010] Technical Solution
[0011] The present disclosure also provides a method of forming a capacitor electrode capable of improving step coverage.
[0012] According to an exemplary embodiment, a method for forming a capacitor electrode includes: forming a TiN film by spraying a titanium (Ti)-containing raw material and a nitrogen-containing reactant; and forming a SiN film by spraying a silicon (Si)-containing raw material and a nitrogen-containing reactant, and spraying at least one of the titanium (Ti)-containing raw material and the silicon (Si)-containing raw material multiple times.
[0013] The formation of the TiN film and the formation of the SiN film can be performed continuously.
[0014] The formation of the TiN film can be continuously performed more times than the formation of the SiN film.
[0015] The ratio (T1:T2) of the number of times T1 of forming the TiN thin film to the number of times T2 of forming the SiN thin film can be adjusted to 1:1 to 4:1.
[0016] The silicon (Si)-containing raw material may be a silicon (Si) gas containing hydrogen (H) or a silicon (Si) precursor containing chlorine (Cl) or a mixed gas of a silicon (Si) gas containing hydrogen (H) and a silicon (Si) precursor containing chlorine (Cl).
[0017] The silicon (Si) precursor containing chlorine (Cl) may be hexachlorodisilane (HCDS: Si2Cl6) or dichlorosilane (DCS: SiH2Cl2), and the silicon (Si) gas containing hydrogen (H) may be silane (SiH4).
[0018] The forming of the SiN film may include: forming a first SiN film by spraying a silicon (Si) gas containing hydrogen (H); and forming a second SiN film by spraying a silicon (Si) precursor containing chlorine (Cl).
[0019] The ratio of the number of times the formation of the second SiN thin film is performed to the number of times the formation of the first SiN thin film is performed may be adjusted to 1:3 to 3:1.
[0020] Injection of purge gas may be added between injections of different types of gas.
[0021] Beneficial Effects
[0022] According to an exemplary embodiment, when at least one of the top electrode and the bottom electrode of the capacitor is formed by laminating a TiN film and a SiN film, the SiN film is formed using a raw material having a plurality of Si atoms. Therefore, the deposition rate of the SiN film can be improved, and the step coverage of the film can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a conceptual diagram illustrating a capacitor where an electrode formed by a method of forming a capacitor electrode according to an exemplary embodiment is located.
[0024] Figure 2 is a conceptual diagram illustrating a bottom electrode formed on a substrate by a method according to an exemplary embodiment.
[0025] Figure 3 is a conceptual diagram illustrating a method of forming a bottom electrode according to an exemplary embodiment.
[0026] Figure 4 is a conceptual diagram illustrating a method of forming a bottom electrode according to a variation of the exemplary embodiment.
[0027] Figure 5 is a conceptual diagram illustrating a bottom electrode formed on a substrate by a method according to another exemplary embodiment.
[0028] Figure 6 is a conceptual diagram illustrating a method of forming a bottom electrode according to another exemplary embodiment.
[0029] Figure 7 is a conceptual diagram illustrating a method of forming a bottom electrode according to yet another exemplary embodiment.
[0030] Figure 8 is a conceptual diagram illustrating a method of forming a bottom electrode according to a variation of still another exemplary embodiment.
[0031] Fig. 9 is a drawing illustrating a bottom electrode formed on a substrate by a method according to an exemplary embodiment.
[0032] Fig.10 is a diagram illustrating a state in which a TiN thin film and a SiN thin film are laminated on a substrate having a groove by a method according to another exemplary embodiment. DETAILED DESCRIPTION
[0033] Hereinafter, exemplary embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. However, the present disclosure may be implemented in different forms and should not be construed as being limited to the embodiments described herein. On the contrary, these embodiments are provided to make the present disclosure thorough and complete and to fully convey the scope of the present disclosure to those of ordinary skill in the art. In the accompanying drawings, the dimensions of layers and regions may be exaggerated for clarity of description. Similar reference numerals throughout the text represent similar components.
[0034] Figure 1 is a conceptual diagram illustrating a capacitor in which an electrode is formed by a capacitor electrode forming method according to an exemplary embodiment.
[0035] refer to Figure 1 , the capacitor 100 may include a substrate 110 , a bottom electrode 120 formed on the substrate 110 , a dielectric layer 130 formed on the bottom electrode 120 , and a top electrode 140 formed on the dielectric layer 130 .
[0036] The substrate 110 may be a semiconductor substrate. More specifically, the substrate 110 may be a wafer (eg, one of a silicon (Si) wafer, a gallium arsenide (GaAs) wafer, and a silicon germanium (SiGe) wafer).
[0037] The dielectric layer 130 is formed on the substrate 110. Here, the dielectric layer 130 may be made of a dielectric material containing a metal oxide. More specifically, the dielectric layer 130 may be made of, for example, one of zirconium dioxide (ZrO2), aluminum oxide (Al2O3), titanium oxide (TiO2), tantalum dioxide (TaO2), and hafnium oxide (HfO2). Moreover, the dielectric layer 130 may be formed by an atomic layer deposition (ALD) method or a chemical vapor deposition (CVD) method.
[0038] Each of the bottom electrode 120 and the top electrode 140 is formed by laminating a TiN film and a SiN film, and the TiN film and the SiN film are formed by an ALD method. Here, the SiN film is formed using a raw material containing a compound having a plurality of Si atoms. As described above, the deposition rate of the SiN film can be improved, and the step coverage can be improved using a compound having a plurality of Si atoms or a raw material containing a compound having a plurality of Si atoms.
[0039] Below, we will refer to Figure 2 and Figure 3 A method of forming a bottom electrode on a substrate by a method according to an exemplary embodiment is described. Here, since the method of forming the bottom electrode is the same as the method of forming the top electrode, the method of forming the bottom electrode will be described and the method of forming the top electrode will be omitted.
[0040] Figure 2 is a drawing illustrating a bottom electrode formed on a substrate by a method according to an exemplary embodiment. Figure 3 is a conceptual diagram illustrating a method of forming a bottom electrode by a method according to an exemplary embodiment. Here, Figure 3 The term “on” in the description may represent that the gas is injected, and the term “off” may represent that the gas injection is stopped or terminated.
[0041] refer to Figure 2 , the bottom electrode 120 may include a TiN film 121 and a SiN film 122 deposited on the TiN film 121. Here, the TiN film 121 may be formed by an ALD method using a raw material containing titanium (Ti), and the SiN film 122 may be formed by an ALD method using a raw material containing a compound having a plurality of silicon (Si) atoms.
[0042] Each of the TiN film 121 and the SiN film 122 is provided in plural or has a multilayer structure. Here, the TiN film 121 may have a multilayer structure or be provided in plural between the substrate 110 and the SiN film 122 or between two SiN films 122. For example, Figure 2As shown, three layers of TiN film 121 may be formed between substrate 110 and SiN film 122 or between two layers of SiN film 122. Here, the multi-layer TiN film 121 is formed by repeating the ALD cycle multiple times. Although the multi-layer TiN film 121 is illustrated to distinguish the TiN films 121 deposited by each ALD cycle, these laminated TiN films may be integrated with each other.
[0043] The SiN film 122 may be formed on the two TiN films 121 and formed into a single layer or a multilayer structure. Also, the number of the laminated SiN films 122 may be smaller than the number of the laminated TiN films 121.
[0044] like Figure 3 As shown, the process of forming the bottom electrode 120 on the substrate 110 includes a process cycle C of forming a TiN film 121 and a SiN film 122 on the substrate 110. p Here, process cycle C p That is, the process of forming the bottom electrode 120 includes multiple process cycles C p (C p1 , C p2 ……C pn-1 , C pn ), and these process cycles C p (C p1 , C p2 ……C pn-1 , C pn ) each includes a first cycle C1 for depositing a TiN film 121 and a second cycle C2 for depositing a SiN film 122. In other words, these process cycles C p (C p1 , C p2 ……C pn-1 , C pn ) each includes a step of forming a TiN film 121 and a step of forming a SiN film 122. Moreover, the step of forming the TiN film 121 includes a first cycle C1, and the step of forming the SiN film 122 includes a second cycle C2.
[0045] In the following, for the convenience of description, these process cycles C are performed in sequence. p (C p1 , C p2 ……C pn-1 , C pn ) is called the first process cycle C p1 , Second process cycle C p2 、n-1th process cycle C pn-1 and the nth process cycle C pnHere, the letter "n" may represent the last round of the process cycle. Also, the last round n may be changed according to the target number of process cycles, and the target number of process cycles may be changed according to the target thickness of the bottom electrode 120 to be manufactured.
[0046] Process cycle C for forming the bottom electrode 120 of the capacitor p The invention comprises: a step of forming a TiN film by spraying a titanium (Ti)-containing raw material and a nitrogen (N)-containing reactant; and a step of forming a SiN film by spraying a silicon (Si)-containing raw material and a nitrogen (N)-containing reactant, and at least one of the titanium (Ti)-containing raw material and the silicon (Si)-containing raw material is sprayed multiple times.
[0047] Here, the multiple injections of at least one of the titanium (Ti)-containing raw material and the silicon (Si)-containing raw material are to continuously inject the titanium (Ti)-containing raw material in a pulsed form. Moreover, while the titanium (Ti)-containing raw material is continuously injected in a pulsed form, a purge gas or other types of gas may not be injected. Here, when the titanium (Ti)-containing raw material is injected and the purge gas is injected, continuously injecting the raw materials may, for example, represent injecting titanium (Ti) raw material-titanium (Ti) raw material-titanium (Ti) raw material...purge gas.
[0048] Moreover, the multiple injections of the silicon (Si)-containing raw material are to continuously inject the silicon (Si)-containing raw material in a pulsed form. Moreover, when the silicon (Si)-containing raw material is continuously injected in a pulsed form, a purge gas or other types of gas may not be injected during the continuous injection. Here, when the silicon (Si)-containing raw material is injected and the purge gas is injected, continuously injecting the raw material may represent injecting silicon (Si) raw material-silicon (Si) raw material-silicon (Si) raw material...purge gas.
[0049] Below, we will refer to Figure 3 Describe the process cycle C in detail p .
[0050] Here, the first process cycle C will be described. p1 As an example.
[0051] refer to Figure 3 , the first process cycle C p1 The method includes: a first cycle C1 for depositing a TiN film 121; and a second cycle C2 for depositing a SiN film 122. Here, the first cycle C1 is performed first before the second cycle C2.
[0052] The first cycle C1 may include: a step of spraying a first raw material containing Ti; a step of spraying a purge gas (first purge); a step of spraying a reactant; and a step of spraying a purge gas after stopping the spraying of the reactant (second purge). For example, a gas containing TiCl4 may be used as the first raw material containing Ti. Moreover, a gas containing N (such as NH3) may be used as a reactant. Moreover, argon (Ar) gas may be used as a purge gas. The TiN atomic layer (i.e., the TiN film 121) is deposited by the ALD method in the first cycle C1.
[0053] The first cycle C1 of depositing the TiN thin film 121 described above may be referred to as a “TiN deposition cycle”.
[0054] The second cycle C2 may include: a step of injecting a second raw material containing a compound having a plurality of Si atoms; a step of injecting a purge gas (first purge); a step of injecting a reactant; and a step of injecting a purge gas after stopping the injection of the reactant (second purge). Here, a precursor containing a compound having a plurality of Si atoms and Cl atoms may be used as the second raw material. Moreover, the second raw material may be in a liquid or gaseous state.
[0055] For example, a precursor containing a Si2Cl6 (HCDS) compound can be used as the second raw material. Here, the Si2Cl6 (HCDS) compound contained in the second raw material contains Si atoms and Cl atoms and has multiple Si atoms (i.e., two Si atoms). Alternatively, in addition to the above-mentioned precursor containing Si2Cl6 (HCDS), a raw material containing at least one of monochlorosilane (MCS: SiH3Cl), dichlorosilane (DCS: SiH2Cl2), trichlorosilane (TCS: SiHCl3) and hexachlorodisilane (HCDS: Si2Cl6) can also be used as the second raw material.
[0056] The same gas used in the first cycle C1 can be used as a reactant and a purge gas. That is, a nitrogen (N)-containing gas (such as a NH3-containing gas) can be used as a reactant, and an argon (Ar) gas can be used as a purge gas. The SiN atomic layer (i.e., the SiN film 122) is deposited by an atomic layer deposition (ALD) method through the second cycle C2.
[0057] The second cycle C2 of depositing the SiN film 122 may be referred to as a “SiN deposition cycle”.
[0058] In the above exemplary embodiment, a precursor containing a compound having a plurality of silicon (Si) atoms is used as a second raw material for depositing the SiN film 122, such as a precursor containing at least one of Si2Cl6 (HCDS), monochlorosilane (MCS: SiH3Cl), dichlorosilane (DCS: SiH2Cl2), trichlorosilane (TCS: SiHCl3), and hexachlorodisilane (HCDS: Si2Cl6). Therefore, the deposition rate of the SiN film 122 can be improved. That is, when the second raw material is used as in the exemplary embodiment, the deposition rate of the SiN film 122 can be improved compared to the related art using silane (SiH4) gas as a raw material.
[0059] This is because the second raw material used in the exemplary embodiment includes a Si compound having a plurality of Si atoms, but the raw material in the related art includes a gas including a SiH4 compound having one Si atom (Si single atom compound). That is, the compound having a plurality of Si atoms (i.e., Si2Cl6 (HCDS) compound) has a higher reactivity than the SiH4 compound which is a Si single atom compound.
[0060] Also, since the deposition rate of the SiN thin film 122 is improved as in the embodiment, the time to deposit the bottom electrode 120 having a target thickness may be reduced compared to the related art.
[0061] In an exemplary embodiment, when the first cycle C1 and the second cycle C2 are performed, the process cycle C p The number of times T1 of the first cycle C1 is performed is greater than the number of times T2 of the second cycle C2. That is, the number of times T1 of the first cycle C1 is performed is multiple times, and the number of times T2 of the second cycle C2 is less than the number of times T1 of the first cycle C1. Here, the number of times T2 of the second cycle C2 can be performed multiple times according to the number of times T1 of the first cycle C1. Moreover, when each of the first and second cycles C1 and C2 is performed multiple times, the first cycle C1 will be performed multiple times continuously, and then the second cycle C2 will be performed multiple times continuously.
[0062] Here, the ratio of the number of times T1 of the first cycle C1 to the number of times T2 of the second cycle C2 (T1:T2) is adjusted to 1:1 to 4:1 (T1:T2=1:1 to 4:1). Preferably, the ratio of the number of times T1 of the first cycle C1 to the number of times T2 of the second cycle C2 (T1:T2) is adjusted to 3:1 to 4:1 (T1:T2=3:1 to 4:1).
[0063] As described above, the first cycle C1 may be referred to as a "TiN deposition cycle", and the second cycle C2 may be referred to as a "SiN deposition cycle". Here, "the ratio of the number of times T1 of the first cycle C1 is performed to the number of times T2 of the second cycle C2 (T1:T2)" may be "the ratio of the number of times T1 of the TiN deposition cycle C1 is performed to the number of times T2 of the SiN deposition cycle C2 (T1:T2)".
[0064] Furthermore, the TiN deposition cycle may be referred to as a "step of forming a TiN film", and the SiN deposition cycle may be referred to as a "step of forming a SiN film". Therefore, the ratio (T1:T2) of the number of times T1 of the step of forming a TiN film to the number of times T2 of the step of forming a SiN film may be performed may be adjusted to 1:1 to 4:1, preferably 3:1 to 4:1.
[0065] Hereinafter, for convenience of description, “the ratio (T1:T2) of the number of times T1 of the first cycle C1 is performed to the number of times T2 of the second cycle C2 is performed” is referred to as “the ratio (T1:T2) of the number of times first and second cycles are performed”.
[0066] More specifically, reference will be made to Figure 3 The case where the ratio of the number of times the first and second cycles are performed (T1:T2) is 3:1 is described as an example. Figure 3 , these process cycles C p (C p1 , C p2 ……C pn-1 , C pn ) may include a first cycle C1 and a second cycle C2, and here, the ratio of the number of times the first cycle is performed to the number of times the second cycle is performed (T1:T2) may be 3:1.
[0067] More specifically, for example, these process cycles C p (C p1 , C p2 ……C pn-1 , C pn ) can be Figure 3 The figure shows three first cycles C1 and one second cycle C2. p1 In the case of , the first cycle C1 is performed three times in succession, for example. Figure 2 As shown, three layers of TiN film 121 are continuously deposited on substrate 110. When three first cycles C1 are completed, second cycle C2 is performed once. Therefore, a layer of SiN film 122 is deposited on TiN film 121. As described above, since first cycle C1 is continuously performed three times and then second cycle C2 is performed once, the ratio of the number of times the first cycle is performed to the second cycle (T1:T2) can be 3:1.
[0068] When the first process cycle C p1 At the end of the second cycle C2, the second process cycle C p2 Here, the second process cycle C p2 Can be used with the first process cycle C p1 The ratio of the first and second cycles (T1: T2) is the same. That is, when the second process cycle C p2 When the first cycle is performed, the ratio of the number of times the first cycle is performed to the number of times the second cycle is performed (T1:T2) is 3:1.
[0069] When the second process cycle C p2 When the second cycle C2 is finished, the next process cycle (C p3 ……C pn-1 , C pn ). Here, the process cycle will be as follows Figure 3 is performed until the target number n is reached.
[0070] Figure 4 is a conceptual diagram illustrating a method of forming a bottom electrode by a method according to a variation of the exemplary embodiment.
[0071] In the exemplary embodiment, the second raw material in the second cycle C2 is injected once. However, the exemplary embodiment is not limited thereto. For example, the second raw material may be injected as follows: Figure 4 In the variation example in the example, the second cycle C2 according to the variation example of the exemplary embodiment may be performed in the order of "first second raw material injection-second second raw material injection-purge gas injection-reactant injection-purge gas injection". Here, the second second raw material injection may be performed with a time difference after the first second raw material injection. In other words, the second raw material is injected in a pulsed form. Moreover, the sum of the injection amount of the first second raw material injection and the injection amount of the second second raw material injection may be adjusted to be the target injection amount of the second raw material to be injected in one second cycle C2.
[0072] In the above example, the second raw material is divided and injected twice. However, the second raw material may be divided more than twice, and "purge gas injection-reactant injection-purge gas injection" may be performed after the last second raw material injection.
[0073] Figure 5 is a drawing illustrating a bottom electrode formed on a substrate by a method according to another exemplary embodiment. Figure 6 is a conceptual diagram illustrating a method of forming a bottom electrode by a method according to another exemplary embodiment.
[0074] In an exemplary embodiment, a precursor including a compound having a plurality of Si atoms is used as a raw material (i.e., a precursor including a Si2Cl6 (HCDS) compound) in the deposition of the SiN film 122. That is, the SiN film 122 according to the exemplary embodiment is a film deposited using a second raw material including a compound having a plurality of Si atoms.
[0075] However, the exemplary embodiment is not limited thereto. For example, the SiN film 123 may be deposited using a raw material different from the second raw material (hereinafter, referred to as a third raw material). Here, the second cycle C2 of depositing the SiN film 122 using the second raw material and the cycle of depositing the SiN film 123 using the third raw material are performed as independent cycles. Therefore, the cycle of depositing the SiN film 123 using the third raw material is referred to as a third cycle C3.
[0076] refer to Figure 5 The bottom electrode 120 may include a TiN film 121 and SiN films 122 and 123 deposited on the TiN film 121 .
[0077] Here, one of the SiN films 122 and 123 is the film 123 formed by the third cycle C3, and the rest is the film 122 formed by the second cycle C2. Here, the third raw material used in the third cycle C3 may include a Si single-atom compound. More specifically, the third raw material may be a gas containing silicon (Si) and hydrogen (H) (e.g., silane (SiH4) gas). Therefore, one of the SiN films 122 and 123 is the film 123 formed using the third raw material (i.e., a gas containing a SiH4 compound or made of a SiH4 compound that is a Si single-atom compound), and the rest is the film 122 formed using the second raw material containing a gas containing a compound having a plurality of Si atoms (e.g., a precursor containing a Si2Cl6 (HCDS) compound).
[0078] Also, in the bottom electrode 120 , the number of laminated SiN films 122 , 123 formed through the second and third cycles C2 , C3 may be less than the number of laminated TiN films 121 .
[0079] refer to Figure 6 , according to another exemplary embodiment of the process cycle C p (C p1 , C p2 ……C pn-1 , C pn ) includes a first cycle C1 for depositing a TiN film 121 and a second and third cycle C2 and C3 for depositing SiN films 122 and 123.
[0080] Here, since the first and second cycles C1, C2 are the same as those in the exemplary embodiment, description thereof will be omitted.
[0081] The third cycle C3 may include: a step of injecting a third raw material (ie, a gas containing a Si monatomic compound); a step of injecting a purge gas (first purge); a step of injecting a reactant; and a step of injecting a purge gas after stopping the injection of the reactant (second purge).
[0082] Here, as described above, a gas containing Si and H (i.e., silane (SiH4) gas) may be used as the third raw material. Moreover, the reactant and the purge gas may be the same as the reactant and the purge gas used in the first and second cycles C1 and C2. That is, a gas containing N (e.g., NH3) may be used as a reactant, and argon (Ar) gas may be used as a purge gas. The SiN atomic layer (i.e., the SiN film 123) is deposited by the ALD method in the third cycle C3.
[0083] When the process cycle C including the first to third cycles C1 to C3 p (C p1 , C p2 ……C pn-1 , C pn ), the first cycle C1 is first performed to deposit the TiN film 121, and then the second and third cycles C2 and C3 are performed to deposit the SiN films 122 and 123. Here, when the SiN films 122 and 123 are deposited, the third cycle C3 is first performed, and then the second cycle C2 is performed. In other words, the SiN film 123 is deposited using the third raw material including silane (SiH4), and then the SiN film 122 is deposited using the second raw material including a compound having a plurality of Si atoms. That is, in yet another exemplary embodiment, the process cycle C p The process is carried out in the order of “first cycle C1 - third cycle C3 - second cycle C2”.
[0084] Furthermore, when the second and third cycles C2 and C3 are performed, the ratio (T2:T3) of the number of times the second cycle C2 is performed to the number of times the third cycle C3 is performed is adjusted to 1:3 to 3:1 (T2:T3=1:3 to 3:1).
[0085] Here, since the second cycle C2 is performed after the third cycle C3 is performed, the third cycle C3 can be referred to as a step of forming a first SiN film, and the second cycle C2 can be referred to as a step of forming a second SiN film. Therefore, when the SiN film is formed, the ratio of the number of times T2 of the step of forming the second SiN film to the number of times T3 of the step of forming the first SiN film (T2:T3) can be adjusted to 1:3 to 3:1.
[0086] Furthermore, when the first to third cycles C1 to C3 are performed, the number of times T1 of the first cycle C1 is performed is greater than the number T 2+3 (ie, the sum of the number of times T2 of the second cycle C2 and the number of times T3 of the third cycle C3) 2+3 ) is adjusted to 1:1 to 4:1, preferably 3:1 to 4:1.
[0087] Hereinafter, for convenience of description, “the ratio of the number of times T2 of the second cycle C2 to the number of times T3 of the third cycle C3 (T2:T3)” is referred to as “the ratio of the number of times of the second and third cycles (T2:T3)”.
[0088] Moreover, "the number of times T1 of the first cycle is equal to the number of times T 2+3 (ie, the sum of the number of times the second cycle is performed T2 and the number of times the third cycle is performed T3) ratio (T1:T 2+3 )” is referred to as “the number of TiN deposition cycles T1 and the number of SiN deposition cycles C2 and C3 T 2+3 The ratio (T1:T 2+3 )”.
[0089] More specifically, the number of TiN deposition cycles T1 and the number of SiN deposition cycles C2 and C3 are T 2+3 The ratio (T1:T 2+3 ) is a case reference of 3:1 Figure 6 It is described as an example. Moreover, a case where the ratio of the number of times the second and third cycles C2 and C3 are performed (T2: T3) is 1:1 is described as an example. Therefore, the ratio of the number of times T1 of the first cycle C1, the number of times T2 of the second cycle C2, and the number of times T3 of the third cycle C3 (T1: T2: T3) is 6:1:1.
[0090] These process cycles C p (C p1 , C p2 ……C pn-1 , C pn ) can be Figure 6 The figure shows six first cycles C1, one second cycle C2 and one third cycle C3. p1 In the case of , the first cycle C1 is performed six times in succession, for example. Figure 5As shown, six layers of TiN film 121 are continuously deposited on substrate 110. When the six first cycles C1 are completed, the third cycle C3 is performed once. That is, ALD using the third raw material including silane (SiH4) is performed once. Therefore, a layer of SiN film 123 is deposited on TiN film 121.
[0091] When the third cycle C3 is finished, the second cycle C2 is performed once. That is, ALD using a second raw material including a precursor including a compound having a plurality of Si atoms (e.g., a precursor including a Si2Cl6 (HCDS) compound) is performed once. Therefore, the SiN film 122 using the second raw material including the Si2Cl6 (HCDS) precursor is deposited on the SiN film 123 deposited using the third raw material including silane (SiH4).
[0092] When six first cycles C1, one third cycle C3 and one second cycle C2 are performed in sequence, the next process cycle (C p2 ……C pn-1 , C pn ) will be carried out in the same way. Here, when each process cycle (C p2 ……C pn-1 , C pn ), the ratio of the number of times T1, T2, and T3 of the first to third cycles C1 to C3 is the same. Therefore, the ratio of the number of times T1 of the first cycle C1, the number of times T2 of the second cycle C2, and the number of times T3 of the third cycle C3 (T1:T2:T3) is adjusted to 6:1:1. That is, in each process cycle C p (C p1 , C p2 ……C pn-1 , C pn ), the number of TiN deposition cycles T1 is greater than the number of SiN deposition cycles C2 and C3. 2+3 The ratio (T1:T 2+3 ) is adjusted to 3:1. Moreover, in each process cycle, the ratio of the number of times the second cycle C2 and the third cycle C3 are performed (T2:T3) is adjusted to 1:1.
[0093] As described above, the first cycle C1 is a cycle for depositing the TiN film 121, and the second and third cycles C2 and C3 are cycles for depositing the SiN films 122 and 123. In another exemplary embodiment, the process cycle C p The first cycle C1, the third cycle C3, and the second cycle C2 are performed in this order. Therefore, the first cycle C1 can be referred to as a "TiN deposition cycle", the third cycle C3 can be referred to as a "first SiN deposition cycle", and the second cycle C2 can be referred to as a "second SiN deposition cycle".
[0094] Figure 7 is a conceptual diagram illustrating a method of forming a bottom electrode according to yet another exemplary embodiment.
[0095] These process cycles C p (C p1 , C p2 ……C pn-1 , C pn ) is performed in the same manner as in the exemplary embodiment and another exemplary embodiment. However, the exemplary embodiment is not limited thereto. For example, these process cycles C p (C p1 , C p2 ……C pn-1 , C pn ) can be performed in different ways.
[0096] That is, when the SiN film is deposited, the method for forming the bottom electrode according to yet another exemplary embodiment includes a first type TY1 process cycle using SiH4 gas as the third raw material and a second type TY2 process cycle using a raw material (i.e., the second raw material) containing a compound precursor having a plurality of Si atoms. Moreover, the first type TY1 process cycle and the second type TY2 process cycle are alternately performed multiple times.
[0097] First, each of a process cycle of the first type TY1 and a process cycle of the second type TY2 will be described.
[0098] The process cycle of the first type TY1 includes a first cycle C1 and a third cycle C3. That is, the process cycle of the first type TY1 includes a first cycle C1 for depositing a TiN film and a third cycle C3 for depositing a SiN film using a third raw material including SiH4. Here, the ratio of the number of times T1 of the first cycle C1 is performed to the number of times T3 of the third cycle C3 (T1:T3) is adjusted to 1:1 to 4:1, preferably 3:1 to 4:1. That is, the ratio of the number of times the first and third cycles are performed (T1:T3) can be 1:1 to 4:1, preferably 1:1 to 4:1.
[0099] The process cycle of the second type TY2 includes a first cycle C1 and a second cycle C2. That is, the process cycle of the second type TY2 includes a first cycle C1 for depositing a TiN film and a second cycle C2 for depositing a SiN film using a second raw material containing a compound precursor having a plurality of Si atoms. Here, the ratio of the number of times the first cycle is performed to the second cycle (T1:T2) may be 1:1 to 4:1, preferably 3:1 to 4:1.
[0100] The process cycle of the first type TY1 and the process cycle of the second type TY2 are performed alternately for many times.p1 is the process cycle of the first type TY1. Figure 7 As shown, the first process cycle C p1 Can be used as the first type TY1, the second process cycle C p2 Can be used as the second type TY2, the third process cycle C p3 Can be used as the first type TY1, the fourth process cycle C p4 Can be used as the second type TY2, the n-1th process cycle C pn-1 It can be carried out as the first type TY1 and the nth process cycle C pn It can be performed as the second type TY2.
[0101] Figure 8 is a conceptual diagram illustrating a method of forming a bottom electrode by a method according to a variation of still another exemplary embodiment.
[0102] In yet another exemplary embodiment described above, the second cycle C2 of injecting the second raw material and the third cycle C3 of injecting the third raw material are performed in different process cycles.
[0103] However, the exemplary embodiment is not limited thereto. For example, the second raw material and the third raw material may be as follows: Figure 8 That is, the second cycle C2 according to the variation of yet another exemplary embodiment can be as follows: Figure 8 The second and third raw materials are sprayed in the order of “injection of the second and third raw materials-injection of the purge gas-injection of the reactant-injection of the purge gas” as shown. Here, the second raw material and the third raw material may be stored independently and sprayed toward the substrate 110 at the same time. However, the exemplary embodiment is not limited thereto. For example, the second raw material and the third raw material may be mixed and stored, and the mixed gas may be sprayed toward the substrate 110.
[0104] Furthermore, when the SiN film is deposited in the exemplary embodiment to the further exemplary embodiment and the variation, only the second raw material including the compound precursor having a plurality of Si atoms is used alone, or the second raw material and the third raw material including silane (SiH4) are used together. However, the exemplary embodiment is not limited thereto. For example, the SiN film may be deposited using the third raw material including silane (SiH4) instead of the second raw material.
[0105] In this case, process cycle C p The process cycle includes a first cycle C1 for depositing a TiN film 121 and a third cycle C3 for depositing a SiN film using a third raw material including silane (SiH4). Here, the process cycle may not include the second cycle C2.
[0106] Here, the injection of the third raw material in the third cycle C3 may be divided into multiple times (e.g., twice). That is, the third cycle C3 may be performed in the order of "first injection of the third raw material - second injection of the third raw material - injection of the purge gas - injection of the reactant - injection of the purge gas". Here, the second injection of the third raw material may be performed after the first injection of the third raw material with a time difference. In other words, the third raw material is injected in a pulsed form. Moreover, the sum of the injection amount of the first injection of the third raw material and the injection amount of the second injection of the third raw material may be adjusted to be the target injection amount of the third raw material to be injected in the third cycle C3.
[0107] Fig. 9 is a drawing illustrating a bottom electrode formed on a substrate by a method according to an exemplary embodiment.
[0108] In the above description, the bottom electrode 120 of the capacitor is formed on the flat substrate 110. However, the exemplary embodiment is not limited thereto. Fig. 9 As shown, a capacitor may be manufactured by forming a bottom electrode 120 on a substrate 110 having a groove 111 by a method according to an exemplary embodiment.
[0109] When the bottom electrode 120 is formed on the substrate 110 having the groove 111, the step coverage is improved by using the method according to the exemplary embodiment compared to the case of the related art. That is, in the bottom electrode 120 formed on the substrate 110 having the groove 111, the thickness of the bottom electrode deposited on the inner side surface surrounding the groove 111, the thickness of the bottom electrode deposited on the bottom surface, and the thickness of the bottom electrode deposited on the top surface are uniform compared to the related art.
[0110] In other words, the step coverage (percentage, %) can be calculated as the deposition thickness TH formed on the bottom surface in the trench 111. b Than the deposition thickness TH formed on the top surface of the substrate 110 t That is, the step coverage (%) is the thickness TH of the bottom electrode 120 deposited on the bottom surface of the separation trench 111. b divided by the thickness TH of the bottom electrode 120 deposited on the top surface of the substrate 110 corresponding to the outside of the groove 111 t The obtained ratio (refer to equation 1).
[0111] [Equation 1]
[0112] Step coverage (%) = TH b / TH t ×100%
[0113] Compared with the related art, the step coverage rate is improved in the case of using the method according to the exemplary embodiment. That is, when the bottom electrode 120 is prepared by laminating a TiN film and a SiN film on the substrate 110 having the groove 111, the step coverage rate is improved in the case of using a gas containing a compound having a plurality of Si atoms (e.g., a gas containing a Si2Cl6 (HCDS) compound) as a raw material to deposit the SiN film as the exemplary embodiment, compared with the case of using a silane (SiH4) gas as a raw material as the related art. This is because the reactivity of the gas containing a compound having a plurality of Si atoms such as the Si2Cl6 (HCDS) gas is higher than the reactivity of the silane (SiH4) gas, and therefore, the deposition rate of the SiN film 122 is improved.
[0114] Fig.10 is a diagram illustrating a state in which a TiN thin film and a SiN thin film are laminated on a substrate having a groove by a method according to another exemplary embodiment.
[0115] here, Fig.10 (a) reveals the state of the first cycle C1 and the third cycle C3 of the first process cycle, and Fig.10 (b) reveals the state in which the second cycle C2 is performed after the first and third cycles C1 and C3 are completed.
[0116] When the bottom electrode 120 is formed on the substrate 110 having the groove 111 to prepare the capacitor 100 , the step coverage may be more effectively improved when the bottom electrode 120 is formed according to another exemplary embodiment from one of exemplary embodiments to yet another exemplary embodiment.
[0117] This will refer to Figure 6 and Fig.10 First, the first process cycle C p1 The bottom electrode 120 is formed on the substrate 110 having the groove 111. For example, the first process cycle C p1 like Figure 6 This is repeated six times in a row. Fig.10 As shown in FIG. 1 (a), six layers of TiN thin films 121 are continuously deposited on the substrate 110 .
[0118] When the six first cycles C1 are completed, the third cycle C3 is performed once. That is, ALD using the third raw material containing silane (SiH4) is performed once. Therefore, a layer of SiN film 123 (hereinafter referred to as the first SiN film 123) is deposited on the TiN film 121. Here, Fig.10 As shown in (a), the thickness TH of the first SiN film 123 formed on the inner side and bottom surface of the TiN film 121 surrounding the groove 111 iss-sin1 , TH b-sin1 will be smaller than the thickness TH of the first SiN film 123 deposited on the top surface of the TiN film 121 outside the trench 111 t-sin1 This may be due to the low deposition rate of SiH4.
[0119] When the third cycle C3 is finished, the second cycle C2 is performed once. That is, the ALD using the second raw material containing the gas containing the compound precursor having a plurality of Si atoms (e.g., the Si2Cl6 (HCDS) compound precursor) is performed once. Therefore, the SiN film (the second SiN film 122) using the second raw material containing the Si2Cl6 (HCDS) precursor is deposited on the first SiN film 123 deposited using the third raw material made of the SiH4 compound (i.e., the Si single atom compound) or the third raw material containing the SiH4 compound. Here, as Fig.10 As shown in (b), in the second SiN film 122, the thickness TH of the second SiN film 122 formed on the bottom surface and the inner side surface surrounding the groove 111 is s-sin2 , TH b-sin2 is greater than the thickness TH formed in the region corresponding to the top surface of the substrate 110 t-sin2 This may be due to the low deposition rate of SiH4.
[0120] This is because the first SiN film 123 formed using the raw material of SiH4 prevents the second SiN film 122 from being deposited on the surface of the first SiN film 123. Here, the second SiN film 122 is formed using a second raw material containing a gas containing a compound precursor having a plurality of Si atoms (e.g., a Si2Cl6 (HCDS) precursor). Moreover, the first SiN film 123 is formed on the top surface of the substrate 110 with a relatively thick thickness and on the inner side and bottom surfaces in the trench 111 with a relatively thin thickness. As the thickness increases, the tendency to prevent or hinder the deposition of the second SiN film 122 may increase. Moreover, compared with the SiH4 compound gas having one Si atom, the second raw material containing the compound precursor having a plurality of Si atoms in the trench 111 may descend to a deep depth faster and more easily.
[0121] Therefore, when the second SiN film 122 is formed on the first SiN film 123, the second SiN film 122 can be formed with a relatively small thickness TH t-sin2 The first SiN film 123 is deposited on the top surface of the first SiN film 123 , and the second SiN film 122 may be deposited on the inner side surface and the bottom surface of the first SiN film 123 with a relatively large thickness in the trench 111 .
[0122] When the first process cycle C1, the third cycle C3, and the second cycle C2 are performed in the order of p1 At the end, if Fig.10 As shown in (b), the thickness of the thin film formed on the top surface of the substrate 110 is less than or equal to the thickness of the thin film formed on the inner side surface and the bottom surface of the substrate 110 in the groove 111.
[0123] Therefore, when the bottom electrode 120 is formed by repeating the process cycles a plurality of times, the bottom electrode 120 having excellent step coverage may be prepared.
[0124] Table 1 discloses the results of forming the bottom electrode 120 on the substrate 110 having the trench 111 and calculating the step coverage according to the exemplary embodiment and the comparative example.
[0125] 〔Table 1〕
[0126] category Comparative Example Exemplary Embodiments Step coverage (%) 75.4% 77.2%
[0127] For the experiment, two substrates 110 each having a groove 111 were prepared, a bottom electrode 120 was formed on a substrate 110 by a method according to a comparative example, and a bottom electrode 120 was formed on another substrate 110 by a method according to an exemplary embodiment.
[0128] All bottom electrodes 120 according to the comparative example and the exemplary embodiment are formed on the substrate 110 by depositing the TiN film 121 and the SiN film 122 by the ALD method. Moreover, the ratio of the number of times the first and second cycles are performed (T1: T2) according to the comparative example and the exemplary embodiment is 3: 1. In addition, the first raw material, the purge gas and the reactant used for the deposition of the first cycle C1 or the TiN film 121 are also used in the comparative example and the exemplary embodiment. That is, in the comparative example and the exemplary embodiment, TiCl4 gas is used as the first raw material, NH3 gas is used as the reactant, and argon (Ar) gas is used as the purge gas.
[0129] Here, the second raw material used for deposition of the second cycle C2 or SiN film 122 is used differently in the comparative example and the exemplary example. That is, the comparative example uses silane (SiH4) gas as the second raw material, and the exemplary example uses a gas containing a Si2Cl6 (HCDS) precursor as the second raw material.
[0130] In addition, NH 3 gas is also used as a reactant used for deposition of the SiN film 122 or the second cycle C2, and argon (Ar) gas is also used as a purge gas in the comparative example and the exemplary embodiment.
[0131] Furthermore, in the comparative example and the exemplary embodiment, the number of times T1 of the first cycle C1 and the number of times T2 of the second cycle C2 are performed are the same, and the ratio of the number of times the first cycle is performed to the number of times the second cycle is performed is equal to 3:1.
[0132] The bottom electrode was formed by the above method, and the step coverage was calculated by the method as in Equation 1.
[0133] Referring to Table 1, the step coverage of the bottom electrode formed by the method according to the exemplary embodiment is greater than the step coverage of the bottom electrode formed by the method according to the comparative example. This is because although the SiN film 122 is deposited using silane (SiH4) gas as a raw material according to the comparative example, the deposition rate of the SiN film 122 using a gas containing a Si2Cl6 (HCDS) compound as a raw material according to the exemplary embodiment is still greater than the deposition rate of the comparative example.
[0134] It is described above that the bottom electrode 120 of the capacitor is formed by the method according to the exemplary embodiment. However, the top electrode 140 may be formed by the method according to the exemplary embodiment, or the bottom electrode 120 and the top electrode 140 may be formed by the method according to the exemplary embodiment.
[0135] As described above, in an exemplary embodiment, when at least one of the top electrode 140 and the bottom electrode 120 of the capacitor 100 is formed by laminating the TiN film 121 and the SiN film 122, the SiN film 122 is deposited using a raw material including a compound precursor having a plurality of Si atoms. Therefore, the deposition rate of the SiN film 122 can be improved, and the step coverage of the film can be improved.
[0136] Industrial Applicability
[0137] According to an exemplary embodiment, when at least one of the top electrode and the bottom electrode of the capacitor is formed by laminating a TiN film and a SiN film, the SiN film is formed using a raw material having a plurality of Si atoms. Therefore, the deposition rate of the SiN film can be improved, and the step coverage of the film can be improved.
Claims
1. A method for forming a capacitor electrode, the method comprising: forming a titanium nitride (TiN) film by spraying a titanium (Ti)-containing raw material and a nitrogen-containing reactant; as well as A silicon nitride (SiN) film is formed by spraying a silicon (Si)-containing raw material and a nitrogen-containing reactant. Wherein, at least one of the titanium (Ti)-containing raw material and the silicon (Si)-containing raw material is sprayed multiple times.
2. The method for forming a capacitor electrode according to claim 1, wherein: The forming of the TiN film and the forming of the SiN film are performed continuously.
3. The method for forming a capacitor electrode according to claim 2, wherein: The formation of the TiN film is continuously performed more times than the formation of the SiN film.
4. The method for forming a capacitor electrode according to claim 2, wherein: The ratio (T1:T2) of the number of times (T1) of forming the TiN film to the number of times (T2) of forming the SiN film is adjusted to be 1:1 to 4:
1.
5. The method for forming a capacitor electrode according to claim 1, wherein: The silicon (Si)-containing raw material is a hydrogen (H)-containing silicon (Si) gas or a chlorine (Cl)-containing silicon (Si) precursor, or A mixed gas containing the hydrogen (H) silicon (Si) gas and the chlorine (C1) silicon (Si) precursor.
6. The method for forming a capacitor electrode according to claim 5, wherein: The chlorine-containing (C1) silicon (Si) precursor is hexachlorodisilane (HCDS: Si2C16) or dichlorosilane (DCS: SiH2Cl2), and The hydrogen (H) silicon (Si) gas is silane (SiHH4).
7. The method for forming a capacitor electrode according to claim 5, wherein: Forming the SiN film comprises: forming a first SiN film by spraying the hydrogen (H)-containing silicon (Si) gas; and A first SiN film is formed by spraying the chlorine (Cl)-containing silicon (Si) precursor.
8. The method for forming a capacitor electrode according to claim 7, wherein: The ratio of the number of times the second SiN film is formed to the number of times the first SiN film is formed is adjusted to be 1:3 to 3:
1.
9. The method for forming a capacitor electrode according to any one of claims 1 to 8, wherein: Add injection of purge gas between injections of different types of gas.
Citation Information
Patent Citations
Semiconductor device and method of manufacturing the same
KR101110077B1