Catalyst for preparing cyclopropyl ketone, preparation method of catalyst and preparation method of cyclopropyl ketone
Through the catalyst supported by noble metals with acidic support, combined with catalytic hydrogen transfer and rearrangement reaction, the problems of reduced catalyst activity and high temperature inactivation in the existing cyclopropyl ketone preparation are solved, and high yield and high purity cyclopropyl ketone preparation are achieved , simplifies the process and enhances safety and separation.
Patent Information
- Application Number
- CN202410921894.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-10
AI Technical Summary
In the existing industrial preparation methods of cyclopropylone, the catalyst is easily toxic by impurities, resulting in reduced catalytic activity, prolonged process cycle, low yield, and deactivated catalysts under high temperature conditions, increasing side reactions, difficult to separate impurities, affecting product purity.
The catalyst supported by precious metals on acid support was prepared by equal volume impregnation-reduction method. The noble metals accounted for 4% of the mass of the acid support, and palladium and titanium dioxide were mainly composed of to avoid the use of high-pressure hydrogen. Catalytic hydrogen transfer and rearrangement reactions were used. The hydrogen-supply solvent is formic acid, the reaction temperature is 40℃-120℃, and the reaction time is 1h-7h.
It improves catalytic activity and the yield of cyclopropylone, shortens the process cycle, enhances process safety, reduces three waste emissions, simplifies the process process, improves the purity and selectivity of the product, and is suitable for large-scale generation.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic synthesis, and in particular relates to a catalyst for preparing cyclopropyl ketone and a preparation method thereof, and a preparation method of cyclopropyl ketone. Background Art
[0002] Cyclopropyl ketone is an important organic synthetic raw material. It plays a role in introducing cyclopropyl structure in the preparation of many compounds, and this type of structure can improve the lipid solubility and metabolic rate of the product. For example, Bayer AG of Germany has developed a triazolethione green fungicide, prothioconazole, which is used to prevent and control wheat diseases and can be degraded in the natural environment without residue. Merck of the United States has developed efavirenz as a non-nucleoside reverse transcriptase inhibitor, which is used in combination with other drugs to treat HIV-1 infected patients. In addition, cyclopropyl ketone has a strained ring structure and can be used to prepare a series of synthetic fuels to improve their key properties such as energy density and specific impulse, thereby improving their carrying capacity. Therefore, the research on the industrial preparation method of cyclopropyl ketone is of great significance.
[0003] At present, one method for the industrial preparation of cyclopropyl ketone is to use 2-methylfuran as a raw material and obtain it through three steps of catalytic hydrogenation, chlorination and cyclization reaction. The Pd / C catalyst used in the catalytic hydrogenation step is easily poisoned by trace impurities in the raw materials, resulting in reduced catalytic activity of the catalyst, which in turn leads to an extension of the process cycle and a low yield of cyclopropyl ketone; and a large amount of acid and alkali will be consumed in the chlorination and cyclization steps, resulting in saline wastewater and tar waste liquid with no practical use, resulting in a low yield of cyclopropyl ketone.
[0004] Another method for the industrial preparation of cyclopropyl ketone is to use alkali metal iodides such as sodium iodide and potassium iodide to catalyze the cracking of 2-acetyl-γ-butyrolactone, and the product cyclopropyl ketone can be generated in one step. This method only generates CO2 as a byproduct, does not emit other toxic and harmful wastes, and is environmentally friendly. However, this process requires high temperature conditions above 150°C, which makes the iodide catalyst easily deactivated under this condition, and the catalytic activity is greatly reduced. Although the addition of high boiling point polar solvents such as N-methylpyrrolidone, dimethylpropylene urea or hexamethylphosphoric triamide can effectively inhibit the deactivation of the iodide catalyst, the side reactions will be accelerated at this time, thereby introducing new impurities that are difficult to separate and reducing the purity of the product.
[0005] Chinese invention patent CN106554263 A discloses a novel method for preparing cyclopropyl ketone. Cyclopropyl ketone can be prepared at a relatively low temperature with a relatively considerable yield by only two steps of catalytic hydrogenation and acid-catalyzed rearrangement, while avoiding the generation of tar byproducts and the discharge of a large amount of three wastes. However, this method still requires two steps of reaction and different types of catalysts, which prolongs the post-reaction treatment process and increases the difficulty of separating the reaction mixture.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a catalyst for preparing cyclopropyl ketone and a preparation method thereof and a preparation method of cyclopropyl ketone. On the one hand, the catalyst can improve the catalytic activity, thereby improving the yield of cyclopropyl ketone; on the other hand, the preparation method of the catalyst is simple, can be prepared in batches for industrial amplification, and has good recycling reusability; on the other hand, the preparation method of cyclopropyl ketone can avoid the use of high-pressure hydrogen, improve process safety, shorten the process cycle, and has the characteristics of easy product separation, less three wastes, and simple process, providing a feasible solution for large-scale production.
[0008]
[0009] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:
[0010] The present invention provides a catalyst for preparing cyclopropyl ketone, comprising an acidic carrier and a noble metal loaded on the surface of the acidic carrier;
[0011] In the catalyst, the content of the noble metal is 0.1-5 parts by weight relative to 100 parts by weight of the acidic carrier.
[0012] Further, in the catalyst, the content of the noble metal is 2-4 parts by weight, equivalent to 100 parts by weight of the acidic carrier;
[0013] Preferably, in the catalyst, the content of the noble metal is 4 parts by weight, equivalent to 100 parts by weight of the acidic carrier.
[0014] It can be summarized that the mass percentage of precious metal in the acid carrier is 0.1%-5%;
[0015] Within the above defined range, the reaction yield increases with the increase of the noble metal loading.
[0016] As the most preferred solution, the mass percentage of the noble metal in the acidic carrier is 4%;
[0017] When the precious metal loading reaches 4%, further increasing the precious metal loading will shield the acid sites of the acidic carrier, hinder the rearrangement reaction, and reduce the reaction yield. Therefore, under the premise of ensuring a high yield of the product, the mass percentage of the precious metal in the carrier is selected to be 4%.
[0018] Further, the acidic carrier is selected from one or more combinations of alumina, titanium dioxide, zirconium dioxide, hafnium dioxide, vanadium pentoxide, niobium pentoxide or tantalum pentoxide;
[0019] The precious metal is selected from one or more combinations of palladium, platinum, ruthenium and rhodium;
[0020] Preferably, the acidic carrier is titanium dioxide and the noble metal is palladium.
[0021] When the precious metal is palladium, the hydrogen production efficiency is the highest, which can accelerate the generation of cyclopropyl ketone.
[0022] Furthermore, the acidic carrier titanium dioxide is titanium dioxide P25, wherein titanium dioxide P25 is purchased from Evonik-Degussa. Titanium dioxide P25 as a carrier has a large specific surface area (about 50m 2 / g), thereby increasing the loading amount of the precious metal and making it evenly dispersed, thereby significantly improving the catalytic performance, making the catalyst highly stable and not easy to deactivate, and the carrier has strong acidity, which can effectively promote the occurrence of the rearrangement reaction.
[0023] Further, 0.1-5 parts by weight of noble metal chloride powder is dissolved in water to prepare an aqueous solution of noble metal chloride;
[0024] Mixing 100 parts by weight of an acidic carrier powder with an aqueous solution of a noble metal chloride, and sequentially drying and cooling the mixture to obtain a dry catalyst precursor;
[0025] The catalyst precursor is subjected to calcination, reduction and cooling treatments in sequence to obtain catalyst powder.
[0026] The preparation method of the above-mentioned catalyst is an equal volume impregnation-reduction method. The prepared catalyst is a powder. The noble metal chloride can be one or more combinations of palladium chloride, platinum tetrachloride, ruthenium trichloride and rhodium trichloride. During the preparation process, an acidic carrier powder is added to an aqueous solution of the noble metal chloride under stirring, or the aqueous solution of the noble metal chloride is added to the acidic carrier powder under stirring.
[0027] The added noble metal chloride accounts for 0.1%-5% of the carrier by weight, which is equivalent to 0.1-5 parts by weight of the noble metal in 100 parts by weight of the acidic carrier.
[0028] The present invention also provides a method for preparing cyclopropyl ketone using the catalyst of the above technical solution.
[0029] 2-Methylfuran and a hydrogen-donating solvent undergo catalytic hydrogen transfer, catalytic hydrogenation and rearrangement reactions under the action of a catalyst to obtain cyclopropyl ketone.
[0030] In the above scheme, the noble metal is loaded on the acidic carrier in the form of a single substance. The noble metal plays the role of catalyzing the decomposition of the hydrogen supply solvent to produce hydrogen and catalyzing the hydrogenation of 2-methylfuran. The noble metal first catalyzes the decomposition of the hydrogen supply solvent to promote the generation of hydrogen, and then catalyzes the hydrogenation of 2-methylfuran adsorbed on the surface to generate 2-methyl-4,5-dihydrofuran. The acidic carrier provides acidic conditions for the rearrangement reaction of 2-methyl-4,5-dihydrofuran, which can effectively promote the occurrence of the rearrangement reaction and effectively promote the generation of cyclopropyl ketone from 2-methylfuran.
[0031] Furthermore, the hydrogen-donating solvent undergoes a catalytic hydrogen transfer reaction under the action of the noble metal in the catalyst to generate hydrogen and carbon dioxide;
[0032] 2-Methylfuran undergoes catalytic hydrogenation reaction under the action of the noble metal in the catalyst to produce 2-methyl-4,5-dihydrofuran;
[0033] 2-Methyl-4,5-dihydrofuran undergoes a rearrangement reaction under the acidic conditions provided by the acidic carrier in the catalyst to produce cyclopropyl ketone.
[0034] Further, 2-methylfuran, a hydrogen-donating solvent and a catalyst powder are mixed;
[0035] The mixture is heated to a reaction temperature for reaction, and the reaction temperature is maintained until the reaction is completed;
[0036] The product obtained after the reaction is treated to obtain cyclopropyl ketone.
[0037] Furthermore, the hydrogen-donating solvent is selected from one or more combinations of formic acid, ammonium formate, hydrazine formate, hydrazine acetate, hydrazine hydrochloride, and hydrazine sulfate.
[0038] In the above scheme, under the catalysis of precious metals, the negative hydrogen in the hydrogen supply solvent molecules is transferred to the catalyst surface and combined with protons to generate hydrogen in situ, so the above hydrogen supply solvent can be used as a hydrogen storage material. Compared with high-pressure hydrogen, the above hydrogen supply solvent has better stability, narrower explosion limit, and is liquid or solid at room temperature, which is convenient for feeding operation and enhances process safety.
[0039] Formic acid has the lowest price, and its decomposition hydrogen production byproduct is only CO2, which is easy to remove and does not interfere with the reaction. Therefore, formic acid is the preferred hydrogen supply solvent.
[0040] Further, the reaction temperature is 40°C-120°C;
[0041] The molar ratio of the hydrogen-donating solvent to 2-methylfuran is 1.0:1-1.4:1;
[0042] The mass of the acidic catalyst is 1%-10% of the mass of 2-methylfuran;
[0043] Preferably, the reaction temperature is 50-100°C;
[0044] The molar ratio of the hydrogen-donating solvent to 2-methylfuran is 1.1:1-1.3:1;
[0045] The mass of the acidic catalyst is 5%-8% of the mass of 2-methylfuran;
[0046] Further preferably, the reaction temperature is 60°C;
[0047] The molar ratio of hydrogen-donating solvent to 2-methylfuran is 1.1:1;
[0048] The mass of the acidic catalyst was 6% of the mass of 2-methylfuran.
[0049] In the above scheme, it is necessary to ensure that the hydrogen donor reagent is in excess of cyclopropyl ketone and can provide sufficient hydrogen. However, excessive use of the hydrogen donor reagent will promote the intermediate in the reaction process to continue hydrogenation to generate 2-methyltetrahydrofuran, thereby reducing the reaction selectivity. Therefore, the molar ratio of the hydrogen donor solvent to 2-methylfuran is 1.0:1-1.4:1; in order to further increase the yield of cyclopropyl ketone, the preferred molar ratio of the hydrogen donor solvent to 2-methylfuran is 1.1:1.
[0050] At the above-defined temperature, 2-methylfuran can be smoothly converted into cyclopropyl ketone. However, if the reaction temperature is too high, side reactions will occur, reducing the reaction selectivity; if the reaction temperature is too low, the reaction will be too slow, reducing production efficiency.
[0051] When the mass of the catalyst and the mass of cyclopropyl ketone are within the above-defined range, the catalyst has a good catalytic effect, is convenient for post-processing, and has high production efficiency; however, when the amount of catalyst is large, the product selectivity decreases; when the amount of catalyst is small, the reaction time is prolonged and the production efficiency is reduced.
[0052] Further, the reaction time for preparing cyclopropyl ketone is 1h-7h;
[0053] Preferably, the reaction time is 4h-5h,
[0054] More preferably, the reaction time is 5 h.
[0055] In the above scheme, the reaction time can be understood as the time for the reactant to contact the catalyst. Under the above-defined reaction time range, 2-methylfuran can be fully contacted with the catalyst, the catalytic reaction proceeds normally, and no overreaction occurs, thereby ensuring the utilization rate of the raw materials and the yield of the product and improving the selectivity of the product. If the reaction time is too short, the raw materials cannot be converted in time and the yield is too low; if the reaction time is too long, by-products are easily generated, which reduces the selectivity of the product.
[0056] Furthermore, the reaction pressure for preparing cyclopropyl ketone is 0.1MPa-2MPa, preferably 0.1MPa-1MPa. Since 2-methylfuran has a low boiling point, the system pressure increases after the reaction temperature is increased, and there are certain pressure resistance requirements for the inner wall material of the reactor. Therefore, the reaction pressure is limited to the range of 0.1MPa-2MPa; if the pressure is too high, the pressure resistance requirement becomes more stringent, causing safety hazards.
[0057] Furthermore, the purity of 2-methylfuran is not less than 98.5%, and the purity of the hydrogen donor reagent is not less than 99%.
[0058] In the above scheme, the purity of the raw material 2-methylfuran is relatively high, which is conducive to the smooth progress of the reaction; if the purity is too low, the palladium in the catalyst will be poisoned, resulting in the cessation of the reaction;
[0059] Both 2-methylfuran and the hydrogen-donating agent are industrial raw materials and can be purchased conveniently.
[0060] Specifically, a catalyst, a hydrogen-donating solvent and 2-methylfuran are loaded into a reactor, the reactor is purged with argon, the temperature is adjusted to the reaction temperature, the reactor is kept at a constant temperature, and the temperature is maintained until the reaction is completed, and the product obtained after the reaction is completed is treated to obtain cyclopropyl ketone. During the process, 2-methylfuran and the hydrogen-donating reagent are fully contacted with the catalyst by stirring to generate cyclopropyl ketone.
[0061] Further, the products obtained after the reaction are filtered in sequence to obtain product filtrate and catalyst filter cake;
[0062] Recycling the catalyst filter cake;
[0063] The product filtrate is distilled, and the fractions at normal pressure and set temperature are collected, and the collected fractions are cyclopropyl ketone.
[0064] In the above scheme, the step of treating the product obtained after the reaction includes filtering and distilling, specifically: using a hydrophobic polytetrafluoroethylene filter membrane, wherein the pore size of the filter membrane is selected to be 450nm, filtering the product obtained after the reaction, recovering the catalyst for the next reaction, and distilling the obtained filtrate using a vertical barbed distillation column to collect the 114°C±1°C fraction under normal pressure, which is cyclopropyl ketone.
[0065] The yield of the product cyclopropyl ketone prepared according to the method of the invention is as high as 98%, and the purity is as high as 99.8%.
[0066] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0067] 1. The catalyst of the present invention can improve the catalytic activity, thereby improving the yield of cyclopropyl ketone;
[0068] 2. The catalyst of the present invention has a simple preparation method, can be prepared in batches for industrial scale-up, and has good recycling reusability.
[0069] 3. The preparation method of cyclopropyl ketone of the present invention can avoid the use of high-pressure hydrogen, is low in price, and improves process safety; and
[0070] The preparation method of cyclopropyl ketone adopts a one-pot process, which can shorten the process cycle on the basis of improving the yield of the product, has the characteristics of less product separation, less three wastes and simple process, is conducive to process amplification, and lays a foundation for subsequent large-scale production of products.
[0071] The specific embodiments of the present invention are described in further detail below. DETAILED DESCRIPTION
[0072] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is clearly and completely described below in conjunction with some embodiments. It can be understood by those skilled in the art that the following implementation is only used to explain the technical principle of the present invention and is not intended to limit the scope of protection of the present invention. For example, although the present application describes the steps of the method of the present invention in a specific order, these orders are not restrictive. Without departing from the basic principles of the present invention, those skilled in the art can perform the steps in different orders.
[0073] The calculation method of the productive rate of the cyclopropyl ketone mentioned in the following embodiment is:
[0074] Yield of cyclopropyl ketone = (amount of substance of cyclopropyl ketone / amount of substance of 2-methylfuran) * 100%;
[0075] The calculation method of the purity of the cyclopropyl ketone mentioned in the following examples is:
[0076] Taking o-dichlorobenzene as the calibration substance, the same mass of o-dichlorobenzene was added to the same mass of the standard cyclopropyl ketone sample and the reaction solution to be tested, and the peak area was determined by gas chromatography.
[0077] Wherein, S1 = standard cyclopropyl ketone peak area / o-dichlorobenzene peak area;
[0078] S2 = cyclopropyl ketone peak area of the reaction solution to be tested / o-dichlorobenzene peak area;
[0079] Cyclopropyl ketone purity = (S2 / S1) * 100%.
[0080] Example 1
[0081] A catalyst for preparing cyclopropyl ketone, comprising an acidic carrier and a noble metal loaded on the surface of the acidic carrier;
[0082] In the catalyst, the content of the noble metal was 0.1 parts by weight relative to 100 parts by weight of the acidic support.
[0083] Example 2
[0084] A catalyst for preparing cyclopropyl ketone, comprising an acidic carrier and a noble metal loaded on the surface of the acidic carrier;
[0085] In the catalyst, the content of the noble metal was 5 parts by weight relative to 100 parts by weight of the acidic support.
[0086] Example 3
[0087] A catalyst for preparing cyclopropyl ketone, comprising an acidic carrier and a noble metal loaded on the surface of the acidic carrier;
[0088] In the catalyst, the content of the noble metal was 4 parts by weight relative to 100 parts by weight of the acidic support.
[0089] Example 4
[0090] A method for preparing the catalyst as described in any one of Examples 1-3 is as follows:
[0091] Impregnation: 668 mg of palladium chloride was dissolved in 25 mL of deionized water to obtain an aqueous solution of palladium chloride; the aqueous solution of palladium chloride was added to a beaker containing 100 g of titanium dioxide carrier powder and mixed, and the mixture was ultrasonicated for 20 minutes to make the palladium chloride evenly distributed on the surface of the titanium dioxide carrier. After that, the mixture was first dried at 120° C. for 1 hour, and then cooled to room temperature to obtain a dry catalyst precursor.
[0092] Calcination and reduction: The dried catalyst precursor was taken out of the beaker and transferred to a tubular furnace. The temperature inside the tubular furnace was raised to 300°C at a rate of 20°C / min in an argon atmosphere, and a 10% hydrogen / argon mixture was continuously introduced into the tubular furnace at a rate of 10 mL / min until no hydrogen chloride gas was generated. By monitoring the pH of the tubular furnace exhaust gas from acidic to neutral, it was considered that no hydrogen chloride gas was generated. Thereafter, the inside of the tubular furnace was continued to be cooled to room temperature in an argon atmosphere, and the product was taken out and weighed in total of 104 g, which was the palladium@titanium dioxide catalyst powder.
[0093] Example 5
[0094] A method for preparing cyclopropyl ketone using the catalyst described in any one of Examples 1 to 3, comprising:
[0095] 1250 g of 2-methylfuran, 772 g of formic acid, and 75 g of palladium@titanium dioxide catalyst powder were added to a 5 L reactor and mixed, and the interior of the reactor was replaced with argon three times;
[0096] The mixture was heated to a reaction temperature of 60°C for reaction, and the reaction was vigorously stirred for 5 hours, wherein the reaction temperature was maintained until the reaction was completed;
[0097] The product obtained after the reaction is cooled to room temperature and filtered through a hydrophobic polytetrafluoroethylene filter membrane with a pore size of 450 nm; the product filtrate obtained by filtration is transferred into a 5L round-bottom flask and heated and distilled through a vertical thorn distillation column with an inner diameter of 32 mm and an effective length of 300 mm. The fraction at 114°C±1°C under normal pressure is collected, which is the product cyclopropyl ketone.
[0098] Comparative Example 1
[0099] On the basis of Example 5, the palladium@titanium dioxide catalyst powder was replaced with an equal molar amount of palladium powder and titanium dioxide powder, and other preparation conditions remained unchanged.
[0100] Comparative Example 2
[0101] On the basis of Example 5, formic acid was replaced with 0.5 MPa hydrogen, and other preparation conditions remained unchanged.
[0102] Comparative Example 3
[0103] On the basis of Example 5, the palladium@titanium dioxide catalyst powder was replaced with equal moles of palladium acetate and methanesulfonic acid to make it a homogeneous reaction system, and other preparation conditions remained unchanged.
[0104] Example 5, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested for the yield of cyclopropyl ketone, and the test results are shown in Table 1:
[0105] Table 1
[0106]
[0107] As shown in Table 1, in Comparative Example 1, unloaded palladium was physically mixed with a titanium dioxide carrier, and the palladium particles agglomerated during the reaction, affecting its catalytic hydrogenation activity, resulting in a significant decrease in the yield of cyclopropyl ketone;
[0108] In Comparative Example 2, hydrogen was used as the hydrogen source. Although the yield of cyclopropyl ketone was close to that of Example 1, the reaction pressure was high and there were potential safety hazards in the reaction system.
[0109] In Comparative Example 3, a homogeneous catalyst was used instead of a heterogeneous catalyst. Although the yield of cyclopropyl ketone was as high as 91%, the catalyst could hardly be recovered after the reaction, which increased the cost and was not suitable for industrial production.
[0110] Embodiment 7-9
[0111] In the preparation process described in Example 5, in order to investigate the influence of the type of precious metal on the reaction effect, only the precious metal component was changed, and other conditions were the same, and Examples 7 to 9 were obtained, as shown in Table 2:
[0112] Table 2
[0113]
[0114] From the data in Table 2, it can be seen that when the active components are palladium, platinum, ruthenium, and ruthenium, they can all catalyze 2-methylfuran to prepare cyclopropyl ketone, with a yield of more than 64% and a product purity of more than 91%. This is because the above-mentioned noble metals can catalyze the decomposition of formic acid to produce hydrogen and the hydrogenation of 2-methylfuran, and palladium has the best catalytic effect, so the yield of cyclopropyl ketone is the highest.
[0115] Examples 10-14
[0116] The preparation process was the same as that described in Example 5. To investigate the effect of the hydrogen donor on the reaction effect, only the hydrogen donor was changed, and other conditions were the same, to obtain Examples 10 to 14, as shown in Table 3:
[0117] Table 3
[0118]
[0119]
[0120] It can be seen from the data in Table 3 that the above hydrogen donors can catalyze 2-methylfuran to prepare cyclopropyl ketone, with a yield of more than 42% and a product purity of more than 71%. This is because hydrazine can also provide negative hydrogen, but its activity is weaker than that of formic acid, while hydrazine formate is too active to generate an over-hydrogenation product 2-methyltetrahydrofuran. Formic acid has reasonable activity, so the yield and purity of cyclopropyl ketone are the highest.
[0121] Experimental Examples 15-20
[0122] The preparation process described in Example 5 was carried out to investigate the influence of the mass percentage of the noble metal in the acidic carrier on the reaction effect. Only the mass percentage of the noble metal in the acidic carrier was changed, and other conditions were the same to obtain Examples 15 to 20, as shown in Table 4:
[0123] Table 4
[0124]
[0125] It can be seen from the data in Table 4 that when the mass percentage of palladium in the acidic carrier is 0.1-4%, the yield of preparing cyclopropyl ketone is greatly improved; however, if the palladium loading is further increased, the acid sites of the carrier are shielded, resulting in a decrease in the yield of cyclopropyl ketone; on the premise of ensuring that the product has a high yield and selectivity and not increasing the cost, an excessively high loading amount is not used, but a mass percentage of the precious metal palladium in the carrier is 4%.
[0126] Examples 21-24
[0127] The preparation process was as described in Example 5. In order to investigate the effect of reaction temperature on the reaction effect, only the reaction temperature was changed, and other conditions were the same to obtain Examples 21 to 24, as shown in Table 5:
[0128] Table 5
[0129]
[0130] It can be seen from the data in Table 5 that when the reaction temperature is 60°C, the yield of cyclopropyl ketone is as high as 98% and the purity is as high as 99.8%. However, catalytic hydrogenation is an exothermic reaction. If the reaction temperature continues to rise, it will be unfavorable for the catalytic hydrogenation reaction of 2-methylfuran, thereby reducing the yield and purity of cyclopropyl ketone. If the reaction temperature is too low, the reaction will be too slow.
[0131] Examples 25-33
[0132] The preparation process was the same as that described in Example 5, except that the mass of the catalyst was changed to a percentage of the mass of 2-methylfuran, and other conditions were the same, to obtain Examples 25 to 33, as shown in Table 6:
[0133] Table 6
[0134]
[0135]
[0136] It can be seen from the data in Table 6 that when the mass of the catalyst is 1%-6% of the mass of 2-methylfuran, as the mass of the catalyst increases, the yield of the product gradually increases. However, when the mass of the catalyst accounts for more than 6% of the mass of cyclopropyl ketone, the increase in the mass of the catalyst has no effect on the improvement of the yield of cyclopropyl ketone. Therefore, under the premise of ensuring that the target product can be obtained, it is preferred that the mass of the catalyst accounts for 6% of the mass of 2-methylfuran.
[0137] Examples 34-38
[0138] In order to investigate the effect of the amount of hydrogen donor reagent on the reaction effect, the molar ratio of the hydrogen donor reagent to 2-methylfuran was changed, and other conditions remained unchanged to obtain Examples 34 to 38, as shown in Table 7:
[0139] Table 7
[0140]
[0141] It can be seen from the data in Table 7 that increasing the amount of formic acid is beneficial to improving the yield of cyclopropyl ketone. However, when the molar ratio of formic acid to 2-methylfuran reaches 1.1:1, continuing to increase the amount of formic acid will cause excessive hydrogenation of 2-methylfuran to generate 2-methyltetrahydrofuran, which reduces the yield and purity of cyclopropyl ketone. Therefore, the preferred molar ratio of formic acid to 2-methylfuran is 1.1:1.
[0142] Examples 39-42
[0143] The preparation process is the same as that described in Example 5. In order to investigate the effect of the catalyst carrier on the reaction effect, only the catalyst carrier is changed, and other conditions are the same, and Examples 39 to 42 are obtained, as shown in Table 8:
[0144] Table 8
[0145]
[0146] It can be seen from the data in Table 8 that when the precious metal is palladium and the catalyst carrier is titanium dioxide, zirconium dioxide, vanadium pentoxide, or niobium pentoxide, the yield of cyclopropyl ketone is above 20% and the product purity is above 70%; when the catalyst carrier is titanium dioxide, zirconium dioxide, and hafnium dioxide, the product purity of cyclopropyl ketone is above 95%, and especially when the catalyst carrier is titanium dioxide, the yield of cyclopropyl ketone is as high as 98% and the product purity is as high as 99.8%. This is because titanium dioxide as a carrier has a large specific surface area, thereby increasing the loading amount of palladium and making it uniformly dispersed, thereby significantly improving the catalytic performance and making the catalyst highly stable. In addition, the titanium dioxide carrier has strong acidity, which can effectively promote the occurrence of rearrangement reaction, thereby improving the yield and purity of cyclopropyl ketone.
[0147] The above description is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modifications to equivalent embodiments of equivalent changes by using the technical content suggested above without departing from the scope of the technical solution of the present invention. The implementation scheme in the above embodiment can also be further combined or replaced. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the solution of the present invention.
Claims
1. A catalyst for preparing cyclopropyl ketone, characterized in that It includes an acidic carrier and a noble metal loaded on the surface of the acidic carrier; In the catalyst, the content of the noble metal is 0.1-5 parts by weight relative to 100 parts by weight of the acidic carrier.
2. The catalyst according to claim 1, characterized in that In the catalyst, the content of the noble metal is 2-4 parts by weight, equivalent to 100 parts by weight of the acidic carrier; Preferably, in the catalyst, the content of the noble metal is 4 parts by weight, equivalent to 100 parts by weight of the acidic carrier.
3. The catalyst according to claim 1 or 2, characterized in that The acidic carrier is selected from one or more combinations of alumina, titanium dioxide, zirconium dioxide, hafnium dioxide, vanadium pentoxide, niobium pentoxide and tantalum pentoxide; The precious metal is selected from one or more combinations of palladium, platinum, ruthenium and rhodium; Preferably, the acidic carrier is titanium dioxide and the noble metal is palladium.
4. A method for preparing a catalyst as claimed in any one of claims 1 to 3, characterized in that: include: Dissolving 0.1-5 parts by weight of noble metal chloride powder in water to prepare a noble metal chloride aqueous solution; Mixing 100 parts by weight of an acidic carrier powder with an aqueous solution of a noble metal chloride, and sequentially drying and cooling the mixture to obtain a dry catalyst precursor; The catalyst precursor is subjected to calcination, reduction and cooling treatments in sequence to obtain catalyst powder.
5. A method for preparing cyclopropyl ketone using the catalyst according to any one of claims 1 to 3, characterized in that: include: 2-Methylfuran and a hydrogen-donating solvent undergo catalytic hydrogen transfer, catalytic hydrogenation and rearrangement reactions under the action of a catalyst to obtain cyclopropyl ketone.
6. The preparation method according to claim 5, characterized in that: include: The hydrogen-donating solvent undergoes a catalytic hydrogen transfer reaction under the action of the noble metal in the catalyst to generate hydrogen and carbon dioxide; 2-Methylfuran undergoes catalytic hydrogenation reaction under the action of the noble metal in the catalyst to produce 2-methyl-4,5-dihydrofuran; 2-Methyl-4,5-dihydrofuran undergoes a rearrangement reaction under the acidic conditions provided by the acidic carrier in the catalyst to produce cyclopropyl ketone.
7. The preparation method according to claim 5 or 6, characterized in that: include: Mixing 2-methylfuran, a hydrogen-donating solvent and a catalyst powder; The mixture is heated to a reaction temperature for reaction, and the reaction temperature is maintained until the reaction is completed; The product obtained after the reaction is treated to obtain cyclopropyl ketone.
8. The preparation method according to claim 7, characterized in that: The hydrogen-donating solvent is selected from one or more combinations of formic acid, ammonium formate, hydrazine formate, hydrazine acetate, hydrazine hydrochloride, and hydrazine sulfate; Preferably, the hydrogen donating solvent is formic acid.
9. The preparation method according to claim 7, characterized in that: The reaction temperature is 40°C-120°C; The molar ratio of the hydrogen-donating solvent to 2-methylfuran is 1.0:1-1.4:1; The mass of the acidic catalyst is 1%-10% of the mass of 2-methylfuran; Preferably, the reaction temperature is 50-100°C; The molar ratio of the hydrogen-donating solvent to 2-methylfuran is 1.1:1-1.3:1; The mass of the acidic catalyst is 5%-8% of the mass of 2-methylfuran; Further preferably, the reaction temperature is 60°C; The molar ratio of hydrogen-donating solvent to 2-methylfuran is 1.1:1; The mass of the acidic catalyst was 6% of the mass of 2-methylfuran.
10. The preparation method according to claim 7, characterized in that: include: The products obtained after the reaction are filtered in sequence to obtain product filtrate and catalyst filter cake; Recycling the catalyst filter cake; The product filtrate is distilled, and the fractions at normal pressure and set temperature are collected, and the collected fractions are cyclopropyl ketone.
Citation Information
Patent Citations
Process for producing 3-methyltetrahydrofuran, and process for producing an intermediate thereof
CA2308555A1
Preparing method of cyclopropyl methyl ketone
CN106554263A
Preparation method of methyl furan homolog by catalytic conversion of furfuraldehyde homolog
CN106986846A
Titanium dioxide material and preparation method thereof as well as supported palladium catalyst
CN108906134A
Method for preparing 2, 5-dicyanotetrahydrofuran through selective hydrogenation of 2, 5-dicyanofuran
CN112079798A