Powder spraying method based on SMC material
By contacting the workpiece to be sprayed of the SMC material with the conductive and thermally conductive material and powdering it, the problems of insufficient strength and aesthetics of the SMC material in vehicle applications are solved, and higher adhesion and wear resistance are achieved.
Patent Information
- Application Number
- CN202410951471.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art is difficult to apply sheet molding (SMC) materials to vehicles because they are insufficient in strength and cannot meet aesthetic requirements.
By contacting the spray surface of the workpiece to be sprayed with the conductive and thermally conductive material, preheated and powdered, and baked and solidified at a preset temperature, the electrostatic adsorption and thermal insulation characteristics of the conductive and thermally conductive material are used to improve the attachment of the SMC material Focus and overall structural strength.
The strength and wear resistance of SMC materials are improved, making them suitable for vehicle manufacturing while meeting aesthetic requirements.
Smart Images

Figure CN118892979A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder spraying based on SMC materials, and in particular relates to a powder spraying method based on SMC materials. Background Art
[0002] At present, the bodies of most cars are made of metal materials. The advantages of using metal materials are, firstly, safety is guaranteed to a certain extent, and secondly, after painting the metal materials, the appearance is more beautiful.
[0003] With the development of society, lightweight and detachable designs have also emerged while ensuring vehicle safety. For example, the roofs of some cars can be detached, and the materials of the roofs also use lightweight non-metallic materials.
[0004] Sheet molding compound (SMC) is a sheet-like composite material composed of thickenable resin, chopped (and / or continuous) glass fiber reinforcement, fillers, additives, etc., and covered with a load-bearing film on the upper and lower surfaces. Commonly used is a molding compound made of unsaturated polyester resin as the resin matrix. Thickeners, inorganic fillers, initiators, additives and pigments are added to the unsaturated polyester resin to prepare a resin mixture, which is impregnated with chopped fibers or felt sheets, and PE films are covered on the upper and lower surfaces. After thickening, a thin sheet molding compound is obtained. It should be noted that there is currently no good way to apply SMC materials to vehicles. The reason is that although SMC materials are much lighter in weight than metal materials, the body strength of a vehicle made of pure SMC materials is insufficient, and at the same time, it cannot meet people's requirements for aesthetics. Summary of the invention
[0005] Based on this, an embodiment of the present invention provides a powder spraying method based on SMC material, which aims to improve the strength of SMC material for application in vehicles while meeting people's requirements for aesthetics.
[0006] The embodiment of the present invention provides a powder spraying method based on SMC material, comprising the following steps:
[0007] Prepare a workpiece to be sprayed, wherein the material of the workpiece to be sprayed is SMC material, and contact the spraying surface and / or the side away from the spraying surface on the workpiece to be sprayed with an electrically conductive and thermally conductive material;
[0008] Preheating the workpiece to be sprayed that is in contact with the conductive and thermally conductive material;
[0009] The spraying surface of the workpiece to be sprayed which is in contact with the conductive and thermally conductive material after the preheating treatment is subjected to powder spraying treatment, and is baked and cured at a preset temperature to complete the powder spraying process.
[0010] Furthermore, the electrically conductive and thermally conductive material is a metal material.
[0011] Furthermore, the metal material is one or an alloy of copper, aluminum, iron, silver and gold.
[0012] Furthermore, the electrically conductive and thermally conductive material is an electrically conductive liquid.
[0013] Furthermore, the electrically conductive and thermally conductive material is electrically conductive paint.
[0014] Furthermore, in the step of preheating the workpiece to be sprayed that is in contact with the conductive and thermally conductive material, the preheating temperature is 60° C. to 160° C., and the preheating time is 5 min to 15 min.
[0015] Furthermore, before the step of powder spraying the sprayed surface of the workpiece to be sprayed that is in contact with the conductive and thermally conductive material after the preheating treatment, the step includes:
[0016] Testing the surface temperature of the spraying surface of the workpiece to be sprayed which is in contact with the conductive and thermally conductive material after preheating treatment, and determining whether the difference between the maximum and minimum values of the surface temperature is less than a threshold value;
[0017] If the difference between the maximum and minimum surface temperatures is determined to be less than a threshold, powder spraying is performed.
[0018] Furthermore, the step of powder spraying the sprayed surface of the workpiece to be sprayed which is in contact with the conductive and thermally conductive material after the preheating treatment comprises:
[0019] Control the nozzle of the spray gun to maintain a preset distance from the spraying surface;
[0020] Control the spray gun to perform reciprocating operation to spray powder on the spraying surface layer by layer.
[0021] Furthermore, the preset distance is 15 cm to 30 cm.
[0022] Furthermore, in the step of controlling the spray gun to perform reciprocating operation and spraying powder on the spraying surface layer by layer, the angle between the spray gun and the spraying surface is controlled to be 85°~95°, the moving speed of the spray gun is 2m / min~4m / min, the powder spraying amount of the spray gun is 50g / min~250g / min, and the number of reciprocating times for each layer is 3~5 times.
[0023] Furthermore, in the step of baking and curing at a preset temperature, the preset temperature is 150° C. to 200° C., and the baking time is 10 min to 30 min.
[0024] Furthermore, in the step of subjecting the spraying surface of the workpiece to be sprayed that is in contact with the conductive and thermally conductive material after the preheating treatment to powder spraying, the material of the sprayed powder is polyurethane resin or polyester resin.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The method comprises the following steps: bringing a side of a workpiece to be sprayed of an SMC material away from a spraying surface into contact with an electrically conductive thermal conductive material; preheating the workpiece to be sprayed in contact with the electrically conductive thermal conductive material; spraying powder on the spraying surface of the workpiece to be sprayed in contact with the electrically conductive thermal conductive material after the preheating treatment, and baking and curing the workpiece at a preset temperature to complete the powder spraying process. Specifically, since the workpiece to be sprayed of the SMC material is in contact with the electrically conductive thermal conductive material, the stability of the overall surface temperature after the preheating treatment can be ensured. Meanwhile, in the subsequent powder spraying process, the electrostatic adsorption characteristics of the electrically conductive thermal conductive material are utilized, so that the powder can be better attached to the surface of the SMC material. Combined with the baking and curing process, the overall structure of the product finally prepared has high strength and good wear resistance, can be used in vehicles, and the product after powder spraying is more beautiful. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The present invention provides a flow chart of a powder spraying method based on SMC material.
[0028] The following specific implementation manner will be further described in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION
[0029] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0031] See also Figure 1 , is a flow chart of a powder spraying method based on SMC material provided by the present invention, wherein the preparation method specifically includes the following steps:
[0032] Step S01, preparing a workpiece to be sprayed, wherein the material of the workpiece to be sprayed is SMC material, and contacting the spraying surface and / or the side away from the spraying surface of the workpiece to be sprayed with an electrically conductive and thermally conductive material.
[0033] In this embodiment, the SMC material is first processed into a workpiece to be sprayed in a specific shape by common technical means, that is, the mixed SMC slurry is placed in a pre-designed mold for solidification. It can be understood that if a removable roof of a car needs to be prepared, then a workpiece to be sprayed in a specific shape is processed according to the customer's demand for the removable roof.
[0034] After obtaining the workpiece to be sprayed, it is generally necessary to pre-treat the surface of the workpiece to be sprayed. For example, an organic solvent can be manually wiped on the surface of the workpiece to be sprayed. The organic solvent is also alcohol. After pre-treatment, part of the spraying surface of the workpiece to be sprayed is masked. The masked area will not be attached to the powder. Generally, the masking area is the sealing area and the adhesive area. It should be noted that the masking area is determined according to the design. If the entire spraying surface needs to be powdered, no masking treatment is required. In this embodiment, the masking treatment can be handled by covering the masking area with tape and masking film.
[0035] In this embodiment, it can be positioned by tooling and then fixed by high-temperature tape. It can be understood that when the spraying surface of the workpiece to be sprayed contacts the conductive and thermally conductive material, a metal material that matches the shape of the spraying surface of the workpiece to be sprayed is prepared, or a conductive liquid or conductive paint is sprayed on the spraying surface of the workpiece to be sprayed. When the side of the workpiece to be sprayed away from the spraying surface contacts the conductive and thermally conductive material, a metal material that matches the shape of the side of the workpiece to be sprayed away from the spraying surface is prepared, or a conductive liquid or conductive paint is sprayed on the workpiece to be sprayed away from the spraying surface, so that the contact is closer. Among them, the conductive and thermally conductive material is a metal material, for example, an alloy composed of one or more of copper, aluminum, iron, silver, and gold. More specifically, in order to achieve a better powder spraying effect, the attachment area of the conductive and thermally conductive material to the side of the workpiece to be sprayed away from the spraying surface is at least 85%, and the thickness of the conductive and thermally conductive material is 0.1mm to 2mm.
[0036] In some other embodiments of the present invention, the conductive and thermally conductive material can also be a conductive liquid or a conductive paint, which is sprayed on the side of the workpiece to be sprayed away from the spraying surface by a spray gun. The area of the sprayed conductive liquid or conductive paint is at least 85% of the area of the workpiece to be sprayed away from the spraying surface, and the thickness after curing is 15μm to 20μm.
[0037] Step S02, preheating the workpiece to be sprayed that is in contact with the conductive and thermally conductive material.
[0038] Specifically, the conductive and thermally conductive material is contacted with the conductive and thermally conductive material at a preheating temperature of 60° C. to 160° C. for 5 min to 15 min to complete the preheating treatment.
[0039] Step S03, subjecting the preheated surface of the workpiece to be sprayed and in contact with the conductive and thermally conductive material to powder spraying, and baking and curing at a preset temperature to complete the powder spraying process.
[0040] In order to ensure the uniformity and stability of the powder spraying process, the surface temperature of the spraying surface of the workpiece to be sprayed in contact with the conductive and thermally conductive material after preheating is first tested, and it is determined whether the difference between the maximum and minimum surface temperatures is less than a threshold value;
[0041] If the difference between the maximum and minimum surface temperatures is determined to be less than a threshold, powder spraying is performed.
[0042] It should be noted that the surface temperature test may be performed at least at five points on the test surface, including the center point and points around the test surface. The difference between the maximum and minimum surface temperatures should be less than 12°C.
[0043] In this embodiment, the powder material used is polyurethane resin or polyester resin, which can be properly formulated according to customer needs, and different colors can be formulated to meet the needs of appearance, which is no different from the traditional spray painting effect.
[0044] Furthermore, during the powder spraying process, the nozzle of the spray gun is controlled to maintain a preset distance from the spraying surface, wherein the preset distance is 15 cm to 30 cm; the spray gun is controlled to perform a reciprocating operation to spray powder on the spraying surface layer by layer, wherein the angle between the spray gun and the spraying surface is controlled to be 85° to 95°. For example, when the angle between the spray gun and the spraying surface is 85°, it means that the muzzle of the spray gun is tilted upward, and the acute angle formed with the spraying surface is 85°; when the angle between the spray gun and the spraying surface is 95°, it means that the muzzle of the spray gun is tilted downward, and the obtuse angle formed with the spraying surface is 95°; when the angle between the spray gun and the spraying surface is 90°, it means that the muzzle of the spray gun is perpendicular to the spraying surface, the moving speed of the spray gun is 2 m / min to 4 m / min, the powder spraying amount of the spray gun is 50 g / min to 250 g / min, and the number of reciprocating times for each layer is 3 to 5 times.
[0045] Furthermore, in the step of baking and curing at a preset temperature, the preset temperature is 150° C. to 200° C., and the baking time is 10 min to 30 min.
[0046] In summary, an embodiment of the present invention provides a powder spraying method based on SMC material, which comprises the following steps: bringing a side of a workpiece to be sprayed of the SMC material away from the spraying surface into contact with a conductive and thermally conductive material; preheating the workpiece to be sprayed that is in contact with the conductive and thermally conductive material; powder spraying the spraying surface of the workpiece to be sprayed that is in contact with the conductive and thermally conductive material after the preheating treatment, and baking and curing at a preset temperature to complete the powder spraying process. Specifically, since the workpiece to be sprayed of the SMC material is in contact with the conductive and thermally conductive material, the thermal insulation properties of the conductive and thermally conductive material can be used to ensure the stability of the overall surface temperature after the preheating treatment. At the same time, in the subsequent powder spraying process, the electrostatic adsorption properties of the conductive and thermally conductive material are used to enable the powder to better adhere to the surface of the SMC material. Combined with the baking and curing process, the overall structure of the product finally prepared has high strength and good wear resistance, and the product after powder spraying is more beautiful.
[0047] In order to facilitate understanding of the present invention, several embodiments of the present invention are provided below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0048] Example 1
[0049] In Embodiment 1 of the present invention, a powder spraying method based on SMC material is provided. Specifically, a workpiece to be sprayed is prepared, the material of the workpiece to be sprayed is SMC material, and an adapted aluminum film is attached to the side of the workpiece to be sprayed away from the spraying surface, wherein the attachment area of the aluminum film to the side of the workpiece to be sprayed away from the spraying surface is 85%, and the thickness of the aluminum film is 0.1 mm;
[0050] Preheating the workpiece to be sprayed that is in contact with the conductive and thermally conductive material, wherein the preheating temperature is 160° C. and the preheating time is 10 minutes;
[0051] The surface temperature of the sprayed surface of the workpiece to be sprayed in contact with the conductive and thermally conductive material after preheating treatment was tested, and the difference between the maximum and minimum surface temperatures was 12°C;
[0052] The spray surface of the workpiece to be sprayed in contact with the conductive and thermally conductive material after preheating treatment is powder-sprayed, and then baked and cured at a preset temperature, wherein the spray gun is controlled to remain perpendicular to the spray surface, and the nozzle of the spray gun is kept at a preset distance of 30 cm from the spray surface; the spray gun is controlled to reciprocate and powder is sprayed on the spray surface layer by layer. Specifically, the angle between the spray gun and the spray surface is controlled to be 90°, that is, the muzzle of the spray gun is perpendicular to the spray surface, the moving speed of the spray gun is 3 m / min, the powder spraying amount of the spray gun is 200 g / min, and the number of reciprocating times for each layer is 4 times. In addition, in the step of baking and curing at a preset temperature, the preset temperature is 180°C and the baking time is 15 min.
[0053] Example 2
[0054] Embodiment 2 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 1 of the present invention is that the thickness of the aluminum plate is 0.3 mm, and the surface temperature of the spraying surface of the workpiece to be sprayed in contact with the conductive and thermally conductive material after preheating treatment is tested. The difference between the maximum and minimum surface temperatures is 10°C.
[0055] Example 3
[0056] Embodiment 3 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 1 of the present invention is that the thickness of the aluminum plate is 1 mm, and the surface temperature of the spraying surface of the workpiece to be sprayed in contact with the conductive and thermally conductive material after preheating treatment is tested. The difference between the maximum and minimum surface temperatures is 6°C.
[0057] Example 4
[0058] Embodiment 4 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 1 of the present invention is that the thickness of the aluminum plate is 2 mm, and the surface temperature of the spraying surface of the workpiece to be sprayed in contact with the conductive and thermally conductive material after preheating treatment is tested. The difference between the maximum and minimum surface temperatures is 6°C.
[0059] Example 5
[0060] Embodiment 5 of the present invention also provides a powder spraying method based on SMC material, which differs from Embodiment 4 of the present invention in that the preheating temperature is 60°C.
[0061] Example 6
[0062] Embodiment 6 of the present invention also provides a powder spraying method based on SMC material, which differs from Embodiment 4 of the present invention in that the preheating temperature is 100°C.
[0063] Example 7
[0064] Embodiment 7 of the present invention also provides a powder spraying method based on SMC material, which differs from Embodiment 4 of the present invention in that the preset distance is 15 cm.
[0065] Example 8
[0066] Embodiment 8 of the present invention also provides a powder spraying method based on SMC material, which differs from Embodiment 4 of the present invention in that the preset distance is 20 cm.
[0067] Example 9
[0068] Embodiment 9 of the present invention also provides a powder spraying method based on SMC material, which differs from Embodiment 4 of the present invention in that the preset distance is 25 cm.
[0069] Example 10
[0070] Embodiment 10 of the present invention also provides a powder spraying method based on SMC material, which differs from Embodiment 4 of the present invention in that the angle between the spray gun and the spraying surface is controlled to be 85°.
[0071] Embodiment 11
[0072] Embodiment 11 of the present invention also provides a powder spraying method based on SMC material, which differs from Embodiment 4 of the present invention in that the angle between the spray gun and the spraying surface is controlled to be 95°.
[0073] Example 12
[0074] Embodiment 12 of the present invention also provides a powder spraying method based on SMC material, which differs from embodiment 4 of the present invention in that the preset temperature is 150°C.
[0075] Embodiment 13
[0076] Embodiment 13 of the present invention also provides a powder spraying method based on SMC material, which differs from embodiment 4 of the present invention in that the preset temperature is 200°C.
[0077] Embodiment 14
[0078] Embodiment 14 of the present invention also provides a powder spraying method based on SMC material, which differs from embodiment 4 of the present invention in that the conductive and thermally conductive material is copper.
[0079] Embodiment 15
[0080] Embodiment 15 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 3 of the present invention is that the conductive and thermally conductive material is a conductive liquid, specifically a silicone conductive spray liquid. A W-71 standard spray gun is used to spray the conductive liquid onto the side of the workpiece to be sprayed away from the spraying surface. The spray gun caliber is 1 mm, the spraying pressure is 0.6 MPa, the spraying thickness is 20 μm, the spraying direction is horizontal, perpendicular to the spraying surface, and the spraying distance is 200 mm. After spraying, it is cured by vulcanization at 180°C for 25 minutes in a vertical oven.
[0081] Example 16
[0082] Embodiment 16 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 3 of the present invention is that the conductive and thermally conductive material is a conductive liquid, specifically a nanocarbon conductive liquid. A W-71 standard spray gun is used to spray the conductive liquid onto the side of the workpiece to be sprayed away from the spraying surface. The spray gun caliber is 1 mm, the spraying pressure is 0.6 MPa, the spraying thickness is 20 μm, the spraying direction is horizontal, perpendicular to the spraying surface, and the spraying distance is 200 mm. After spraying, it is cured by vulcanization at 180°C for 25 minutes in a vertical oven.
[0083] Embodiment 17
[0084] Embodiment 17 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 16 of the present invention is that a W-71 standard spray gun is used to spray the conductive liquid onto the spraying surface of the workpiece to be sprayed.
[0085] Embodiment 18
[0086] Embodiment 18 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 3 of the present invention is that the conductive and thermally conductive material is conductive paint, and a W-71 standard spray gun is used to spray the conductive paint onto the side of the workpiece to be sprayed away from the spraying surface. The spray gun caliber is 1 mm, the spraying pressure is 0.6 MPa, the spraying thickness is 20 μm, the spraying direction is horizontal, perpendicular to the spraying surface, and the spraying distance is 200 mm. After spraying, it is cured by vulcanization at 65°C for 30 minutes in a vertical oven.
[0087] Embodiment 19
[0088] Embodiment 19 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 18 of the present invention is that a W-71 standard spray gun is used to spray the conductive paint onto the spraying surface of the workpiece to be sprayed.
[0089] Embodiment 20
[0090] Embodiment 20 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 1 of the present invention is that an adaptive aluminum film is attached to the spraying surface of the workpiece to be sprayed, and then powder spraying treatment is performed on the spraying surface attached with the aluminum film.
[0091] Embodiment 21
[0092] Embodiment 21 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 4 of the present invention is that, on the basis of embodiment 4 of the present invention, an adaptive 0.1 mm aluminum film is attached to the spraying surface of the workpiece to be sprayed, that is, the spraying surface and the back of the spraying surface of the workpiece to be sprayed are in contact with aluminum material, and subsequently powder spraying treatment is performed on the spraying surface attached with the aluminum film.
[0093] Embodiment 22
[0094] Embodiment 22 of the present invention also provides a powder spraying method based on SMC material. The difference from embodiment 4 of the present invention is that, on the basis of embodiment 4 of the present invention, the spraying surface of the workpiece to be sprayed is sprayed with nano-carbon conductive liquid with a spraying thickness of 20 μm, and then powder spraying treatment is performed on the spraying surface with the nano-carbon conductive layer cured.
[0095] Comparative Example 1
[0096] Comparative Example 1 of the present invention also provides a powder spraying method based on SMC material, which is different from Implementation 4 of the present invention in that the angle between the spray gun and the spraying surface is 100°.
[0097] Comparative Example 2
[0098] Comparative Example 2 of the present invention also provides a powder spraying method based on SMC material, which is different from Implementation 4 of the present invention in that the angle between the spray gun and the spraying surface is 80°.
[0099] Comparative Example 3
[0100] Comparative Example 3 of the present invention also provides a powder spraying method based on SMC material, which is different from Implementation 4 of the present invention in that the preset distance is 35 cm.
[0101] Comparative Example 4
[0102] Comparative Example 4 of the present invention also provides a powder spraying method based on SMC material, which is different from Implementation 4 of the present invention in that the preset temperature is 140°C.
[0103] The coating adhesion test was conducted on the powder spray products in Examples 1 to 14 of the present invention and Comparative Examples 1 to 4, wherein the adhesion test was conducted by the cross-cut method. It should be noted that, Level 0: In the test, the coating film did not fall off from the substrate in the cross-cut area, indicating excellent adhesion; Level 1: Small pieces fell off at the intersection of the cross-cuts, but the falling area was less than 5%; Level 2: At the intersection of the cross-cuts, the coating film fell off in an area greater than 5%, but less than or equal to 15%; Level 3: The coating film fell off in an area greater than 15%, but less than or equal to 35%; Level 4: The coating film fell off in an area greater than 35%, but less than or equal to 65%; Level 5: The coating film fell off in an area greater than 65%, indicating very poor adhesion. The specific results are shown in the following table:
[0104]
[0105] It can be seen from the above table that the adhesion of the powder spraying product prepared in the embodiment of the present invention is at least level 2, which meets the vehicle use standard. It can be understood that the improvement in adhesion reflects the improvement in product strength to a certain extent. In addition, when the spray gun nozzle is tilted upward, the effect on adhesion is slightly worse; when the powder is sprayed beyond the preset distance, or the preset temperature is only 140°C, the adhesion is only level 3; there is no significant difference in the adhesion effect between the copper plate and the aluminum plate.
[0106] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0107] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the attached claims.
Claims
1. A powder spraying method based on SMC material, characterized in that: The following steps are involved: Prepare a workpiece to be sprayed, wherein the material of the workpiece to be sprayed is SMC material, and contact the spraying surface and / or the side away from the spraying surface on the workpiece to be sprayed with an electrically conductive and thermally conductive material; Preheating the workpiece to be sprayed that is in contact with the conductive and thermally conductive material; The spraying surface of the workpiece to be sprayed which is in contact with the conductive and thermally conductive material after the preheating treatment is subjected to powder spraying treatment, and is baked and cured at a preset temperature to complete the powder spraying process.
2. The powder spraying method based on SMC material according to claim 1, characterized in that: The electrically conductive and thermally conductive material is a metal material.
3. The powder spraying method based on SMC material according to claim 2, characterized in that: The metal material is one of copper, aluminum, iron, silver and gold or an alloy composed of several of them.
4. The powder spraying method based on SMC material according to claim 1, characterized in that: The electrically conductive and thermally conductive material is an electrically conductive liquid.
5. The powder spraying method based on SMC material according to claim 1, characterized in that: The electrically conductive and thermally conductive material is electrically conductive paint.
6. The powder spraying method based on SMC material according to claim 1, characterized in that: In the step of preheating the workpiece to be sprayed that is in contact with the conductive and thermally conductive material, the preheating temperature is 60° C. to 160° C. and the preheating time is 5 min to 15 min.
7. The powder spraying method based on SMC material according to claim 1, characterized in that: The step of powder spraying the sprayed surface of the workpiece to be sprayed which is in contact with the conductive and thermally conductive material after the preheating treatment comprises: Testing the surface temperature of the spraying surface of the workpiece to be sprayed which is in contact with the conductive and thermally conductive material after preheating treatment, and determining whether the difference between the maximum and minimum values of the surface temperature is less than a threshold value; If the difference between the maximum and minimum surface temperatures is determined to be less than a threshold, powder spraying is performed.
8. The powder spraying method based on SMC material according to claim 7, characterized in that: The step of powder spraying the sprayed surface of the workpiece to be sprayed which is in contact with the conductive and thermally conductive material after the preheating treatment comprises: Control the nozzle of the spray gun to maintain a preset distance from the spraying surface; Control the spray gun to perform reciprocating operation to spray powder on the spraying surface layer by layer.
9. The powder spraying method based on SMC material according to claim 8, characterized in that: The preset distance is 15 cm to 30 cm.
10. The powder spraying method based on SMC material according to claim 8, characterized in that: In the step of controlling the spray gun to reciprocate and spray powder on the spray surface layer by layer, the angle between the spray gun and the spray surface is controlled to be 85° to 95°, the moving speed of the spray gun is 2 m / min to 4 m / min, the powder spraying amount of the spray gun is 50 g / min to 250 g / min, and the number of reciprocating times for each layer is 3 to 5 times.
11. The powder spraying method based on SMC material according to claim 1, characterized in that: In the step of baking and curing at a preset temperature, the preset temperature is 150° C. to 200° C., and the baking time is 10 min to 30 min.
12. The powder spraying method based on SMC material according to claim 1, characterized in that: In the step of powder spraying the sprayed surface of the preheated workpiece in contact with the conductive and thermally conductive material, the material of the sprayed powder is polyurethane resin or polyester resin.