Composite modified cobalt-free lithium-rich manganese-based precursor, preparation method thereof and positive electrode material

By adopting a cobalt-free lithium-rich manganese-based precursor with a flower-like core-shell structure, the problems of slow Li+ diffusion speed and structural strain of cobalt-free lithium-rich manganese-based materials during charging and discharging are solved, and the electrochemical performance and reversible capacity are improved. effect.

CN118894558AActive Publication Date: 2024-11-05GUANGDONG BRUNP RECYCLING TECH CO LTD +1

Patent Information

Application Number
CN202411318304.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-05
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

The cobalt-free lithium-rich manganese-based material has slow diffusion speed and poor electrochemical performance during charging and discharging. Its capacity attenuation is fast under high current operating conditions, and the structural strain leads to rupture, which limits its application in the field of power batteries.

Method used

The composite modified cobalt-free lithium-rich manganese-based precursor adopts a flower-like core-shell structure, with the core of NiaMnb(OH)2 and the shell of NixMnyNbz(OH)2, and is prepared by coprecipitation reaction and batch coprecipitation reaction. Doping Nb elements is done to improve specific surface area and tap density.

Benefits of technology

Improve the electrochemical performance of cobalt-free lithium-rich manganese-based precursor, increase the Li+ storage site, buffer structural strain, improve the reversible capacity and electrochemical performance of the positive electrode material, reduce the content of Na and S impurities, and enhance the electrochemistry performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894558A_ABST
    Figure CN118894558A_ABST
Patent Text Reader

Abstract

The invention relates to a composite modified cobalt-free lithium-rich manganese-based precursor, a preparation method thereof and a positive electrode material. The cobalt-free lithium-rich manganese-based precursor is of a flower-shaped core-shell structure and is provided with an inner core and a shell layer; nb with the valence of + 5 is doped in the shell layer. The precursor is of a flower-shaped core-shell structure, more sites are provided for Li < + > storage in the subsequent sintering process, and the reversible capacity of the precursor can be improved; partial structural strain can be buffered, and the tap density is effectively improved; the doping of the Nb element reduces the primary particles disorderly inserted into the secondary particles, and meanwhile, the primary particle wafers are expanded in a flower shape, so that the specific surface area of the precursor is effectively increased, the reaction contact area between the positive electrode material and an electrolyte is increased, and the electrochemical performance is better; due to the relatively high specific surface area, Na and S elements in the precursor can be deviated as much as possible, so that the content of Na and S impurities in the precursor is reduced, and subsequent preparation of a positive electrode material is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries and relates to a core-shell structure precursor, in particular to a composite modified cobalt-free lithium-rich manganese-based precursor and a preparation method thereof and a positive electrode material. Background Art

[0002] Rechargeable lithium-ion batteries have excellent energy storage capacity and environmental protection characteristics. They have been widely used in portable devices, plug-in hybrid vehicles and electric vehicles. Most of these lithium-ion batteries use cobalt as a raw material. Cobalt resources are scarce and expensive, resulting in a high cost of cobalt-containing lithium-ion battery cathode materials. Cobalt-free lithium-rich manganese-based materials have extremely high discharge capacity, relatively low prices and low raw material toxicity, and are considered to be one of the ideal cathode materials in power lithium-ion batteries.

[0003] However, cobalt-free lithium-rich manganese-based materials have some inherent disadvantages: during the charge and discharge process, Li + The diffusion rate of cobalt-free lithium-rich manganese-based materials is slow, resulting in poor electrochemical performance; the capacity of cobalt-free lithium-rich manganese-based materials decays rapidly under high current working conditions, the layered structure collapses significantly, and the secondary particles are prone to rupture caused by structural strain. These shortcomings limit the practical application of cobalt-free lithium-rich manganese-based materials in the field of power batteries. In practical applications, cobalt-free lithium-rich manganese-based precursors are usually improved to optimize their performance. Therefore, selecting a suitable modification method to prepare cobalt-free lithium-rich manganese-based precursors can improve the structure and electrochemical properties of cobalt-free lithium-rich manganese-based precursors.

[0004] To this end, it is necessary to provide a composite modified cobalt-free lithium-rich manganese-based precursor with good particle uniformity, ordered layered structure, high specific surface area and tap density, and a preparation method and positive electrode material thereof. Summary of the invention

[0005] The object of the present invention is to provide a composite modified cobalt-free lithium-rich manganese-based precursor and a preparation method and a positive electrode material thereof. The composite modified cobalt-free lithium-rich manganese-based precursor has a flower-like core-shell structure, which improves the electrochemical properties of the composite modified cobalt-free lithium-rich manganese-based precursor, thereby improving the electrochemical properties of the positive electrode material prepared therefrom.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a composite modified cobalt-free lithium-rich manganese-based precursor, wherein the cobalt-free lithium-rich manganese-based precursor is a flower-like core-shell structure having a core and a shell;

[0008] The general formula of the core is Ni a Mn b (OH)2 , where a ranges from 0.2 to 0.4, b ranges from 0.6 to 0.8, and the sum of a and b is 1;

[0009] The general formula of the shell is Ni x Mn y Nb z (OH) 2 , where x ranges from 0.2 to 0.4, y ranges from 0.6 to 0.8, z ranges from 0.01 to 0.1, and the sum of x and y is 1;

[0010] In the general formula of the shell, the valence of Nb is +5.

[0011] The composite modified cobalt-free lithium-rich manganese-based precursor provided by the first aspect of the present invention is a flower-like core-shell structure, which is Li + It provides more sites for storage, which is beneficial to improve its reversible capacity; it can also buffer some structural strains and effectively improve the tap density; the doping of Nb element reduces the disordered insertion of primary particles in the secondary particles, and at the same time, the primary particle wafers unfold in a flower shape, which effectively increases the specific surface area of ​​the precursor, helps to increase the reaction contact area between the positive electrode material and the electrolyte, and has better electrochemical performance; the higher specific surface area allows the Na and S elements in the precursor to be deviated as much as possible, reducing the Na and S impurity content in the precursor, which is beneficial to the subsequent preparation of positive electrode materials.

[0012] In a second aspect, the present invention provides a method for preparing a composite modified cobalt-free lithium-rich manganese-based precursor, the preparation method comprising the following steps:

[0013] (1) mixing a first precipitant solution, a first complexing agent solution and a first metal salt solution in a base liquid to perform a coprecipitation reaction to obtain a seed crystal suspension;

[0014] (2) adjusting the pH value and ammonia concentration of the seed crystal suspension, and then mixing the second precipitant solution, the second complexing agent solution, the doping solution and the second metal salt solution in parallel to perform an intermittent coprecipitation reaction to obtain a modified cobalt-free lithium-rich manganese-based suspension;

[0015] The doping compound in the doping solution is Nb 2 O 5 and / or NaNb 2 O 4 ;

[0016] (3) The modified cobalt-free lithium-rich manganese-based suspension is washed and dried to obtain the composite modified cobalt-free lithium-rich manganese-based precursor;

[0017] The obtained cobalt-free lithium-rich manganese-based precursor is a flower-like core-shell structure with a core and a shell;

[0018] The general formula of the core is Ni a Mn b (OH) 2 , where a ranges from 0.2 to 0.4, b ranges from 0.6 to 0.8, and the sum of a and b is 1;

[0019] The general formula of the shell is Ni x Mn y Nb z (OH) 2 , where x ranges from 0.2 to 0.4, y ranges from 0.6 to 0.8, z ranges from 0.01 to 0.1, and the sum of x and y is 1;

[0020] In the general formula of the shell, the valence of Nb is +5.

[0021] The second aspect of the present invention provides a preparation method to prepare a cobalt-free lithium-rich manganese-based precursor having a flower-like core-shell structure, which is a Li + It provides more sites for storage, which is beneficial to improve its reversible capacity; it can also buffer some structural strains and effectively improve the tap density; the doping of Nb element reduces the disordered insertion of primary particles in the secondary particles, and at the same time, the primary particle wafers unfold in a flower shape, which effectively increases the specific surface area of ​​the precursor, helps to increase the reaction contact area between the positive electrode material and the electrolyte, and has better electrochemical performance; the higher specific surface area allows the Na and S elements in the precursor to be deviated as much as possible, reducing the Na and S impurity content in the precursor, which is beneficial to the subsequent preparation of positive electrode materials.

[0022] Preferably, the metal salt in the first metal salt solution in step (1) includes a first nickel salt and a first manganese salt;

[0023] In the first metal salt solution, the molar ratio of nickel to manganese is a:b.

[0024] Preferably, the metal salt in the second metal salt solution in step (2) comprises a second nickel salt and a second manganese salt;

[0025] In the second metal salt solution, the molar ratio of nickel to manganese is x:y.

[0026] Preferably, the temperature of the coprecipitation reaction in step (1) is 45°C to 55°C.

[0027] Preferably, the pH value of the coprecipitation reaction in step (1) is 10.8 to 11.1.

[0028] Preferably, the ammonia concentration of the coprecipitation reaction in step (1) is 0.8 g / L to 1.2 g / L.

[0029] Preferably, the end point of the coprecipitation reaction in step (1) is to make the seeds in the seed suspension satisfy: the particle size Dv50 is 2.8 μm to 3.2 μm, the specific surface area is 10 m 2 / g to 15m 2 / g, tap density is 0.8g / cm 2 Up to 1g / cm 2 .

[0030] Preferably, the temperature of the intermittent coprecipitation reaction in step (2) is 45°C to 55°C.

[0031] Preferably, the pH value of the intermittent coprecipitation in step (2) starts from the first pH value, decreases to the second pH value at a rate of 0.025 / h to 0.035 / h, and is maintained until the intermittent coprecipitation reaction is completed.

[0032] Preferably, the ammonia concentration of the intermittent co-precipitation in step (2) is 2.7 g / L to 3.3 g / L.

[0033] Preferably, the endpoint of the intermittent co-precipitation in step (2) is to make the material in the modified cobalt-free lithium-rich manganese-based suspension satisfy: the particle size Dv50 is 5.8 μm to 6.2 μm.

[0034] Preferably, the clearing rate of the intermittent co-precipitation reaction in step (2) is 7 L / h to 10 L / h.

[0035] Preferably, the washing in step (3) comprises alkaline washing and water washing performed sequentially.

[0036] Preferably, the concentration of the alkali solution used for the alkali washing is 0.01wt% to 0.015wt%.

[0037] Preferably, the alkali washing temperature is 75°C to 85°C.

[0038] Preferably, the water washing temperature is 75°C to 85°C.

[0039] Preferably, the coprecipitation reaction in step (1) is carried out under stirring.

[0040] Preferably, the intermittent coprecipitation reaction in step (2) is carried out under stirring conditions.

[0041] Preferably, the first precipitant solution is a sodium hydroxide solution.

[0042] Preferably, the second precipitant solution is a sodium hydroxide solution.

[0043] Preferably, the first complexing agent solution is aqueous ammonia.

[0044] Preferably, the second precipitant solution is aqueous ammonia.

[0045] In a third aspect, the present invention provides a positive electrode material, wherein the raw materials for preparing the positive electrode material include the composite modified cobalt-free lithium-rich manganese-based precursor described in the first aspect, or the composite modified cobalt-free lithium-rich manganese-based precursor obtained by the preparation method described in the second aspect.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] The composite modified cobalt-free lithium-rich manganese-based precursor provided by the present invention is a flower-shaped core-shell structure, which is Li + It provides more sites for storage, which is beneficial to improve its reversible capacity; it can also buffer some structural strains and effectively improve the tap density; the doping of Nb element reduces the disordered insertion of primary particles in the secondary particles, and at the same time, the primary particle wafers unfold in a flower shape, which effectively increases the specific surface area of ​​the precursor, helps to increase the reaction contact area between the positive electrode material and the electrolyte, and has better electrochemical performance; the higher specific surface area allows the Na and S elements in the precursor to be deviated as much as possible, reducing the Na and S impurity content in the precursor, which is beneficial to the subsequent preparation of positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is a scanning electron microscope (SEM) image of the cobalt-free lithium-rich manganese-based precursor obtained in Example 1;

[0049] Figure 2 This is a SEM image of the cobalt-free lithium-rich manganese-based precursor obtained in Example 1 after being treated with CP (Cross-section Polisher);

[0050] Figure 3 This is a SEM image of the cobalt-free lithium-rich manganese-based precursor obtained in Comparative Example 1;

[0051] Figure 4 X-ray diffraction (XRD) images of the cobalt-free lithium-rich manganese-based precursors obtained in Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0052] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0053] A certain embodiment of the present invention provides a composite modified cobalt-free lithium-rich manganese-based precursor, wherein the cobalt-free lithium-rich manganese-based precursor is a flower-shaped core-shell structure having a core and a shell;

[0054] The general formula of the core is Ni a Mn b (OH) 2 , where a ranges from 0.2 to 0.4, b ranges from 0.6 to 0.8, and the sum of a and b is 1;

[0055] The general formula of the shell is Ni x Mn y Nb z (OH) 2 , where x ranges from 0.2 to 0.4, y ranges from 0.6 to 0.8, z ranges from 0.01 to 0.1, and the sum of x and y is 1;

[0056] In the general formula of the shell, the valence of Nb is +5.

[0057] The composite modified cobalt-free lithium-rich manganese-based precursor provided by the present invention is a flower-shaped core-shell structure, which is Li + It provides more sites for storage, which is beneficial to improve its reversible capacity; it can also buffer some structural strains and effectively improve the tap density; the doping of Nb element reduces the disordered insertion of primary particles in the secondary particles, and at the same time, the primary particle wafers unfold in a flower shape, which effectively increases the specific surface area of ​​the precursor, helps to increase the reaction contact area between the positive electrode material and the electrolyte, and has better electrochemical performance; the higher specific surface area allows the Na and S elements in the precursor to be deviated as much as possible, reducing the Na and S impurity content in the precursor, which is beneficial to the subsequent preparation of positive electrode materials.

[0058] In the composite modified cobalt-free lithium-rich manganese-based precursor provided by the present invention, the general formula of the core is Ni a Mn b (OH) 2 , wherein the value range of a is 0.2 to 0.4, for example, it can be 0.2, 0.25, 0.3, 0.35 or 0.4, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are also applicable; the value range of b is 0.6 to 0.8, for example, it can be 0.6, 0.65, 0.7, 0.75 or 0.8, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are also applicable; and the sum of a and b is 1.

[0059] In some embodiments, the values ​​of a and b indicate the contents of Ni and Mn in the core. For example, the ratio of a to b indicates the molar ratio of Ni and Mn in the core.

[0060] In the composite modified cobalt-free lithium-rich manganese-based precursor provided by the present invention, the general formula of the shell is Ni x Mn yNb z (OH) 2 , wherein the value range of x is 0.2 to 0.4, for example, it can be 0.2, 0.25, 0.3, 0.35 or 0.4, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are equally applicable; the value range of y is 0.6 to 0.8, for example, it can be 0.6, 0.65, 0.7, 0.75 or 0.8, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are equally applicable; the value range of z is 0.01 to 0.1, for example, it can be 0.01, 0.03, 0.05, 0.08 or 0.1, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are equally applicable; and the sum of x and y is 1.

[0061] In some embodiments, the values ​​of x, y and z indicate the contents of Ni, Mn and Nb in the shell layer. For example, the ratio of x, y and z indicates the molar ratio of Ni, Mn and Nb in the shell layer.

[0062] In certain embodiments, the composite modified cobalt-free lithium-rich manganese-based precursor has a sulfur content of less than 1032 ppm and a sodium content of less than 80 ppm; wherein ppm (parts per million) is the mass content.

[0063] A certain embodiment of the present invention provides a method for preparing a composite modified cobalt-free lithium-rich manganese-based precursor, the preparation method comprising the following steps:

[0064] (1) mixing a first precipitant solution, a first complexing agent solution and a first metal salt solution in a base liquid to perform a coprecipitation reaction to obtain a seed crystal suspension;

[0065] (2) adjusting the pH value and ammonia concentration of the seed crystal suspension, and then mixing the second precipitant solution, the second complexing agent solution, the doping solution and the second metal salt solution in parallel to perform an intermittent coprecipitation reaction to obtain a modified cobalt-free lithium-rich manganese-based suspension;

[0066] The doping compound in the doping solution is Nb 2 O 5 and / or NaNb 2 O 4 ;

[0067] (3) The modified cobalt-free lithium-rich manganese-based suspension is washed and dried to obtain the composite modified cobalt-free lithium-rich manganese-based precursor;

[0068] The obtained cobalt-free lithium-rich manganese-based precursor is a flower-like core-shell structure with a core and a shell;

[0069] The general formula of the core is Ni a Mnb (OH) 2 , wherein the value range of a is 0.2 to 0.4, the value range of b is 0.6 to 0.8, and the sum of a and b is 1; wherein the value range of a is 0.2 to 0.4, for example, it can be 0.2, 0.25, 0.3, 0.35 or 0.4, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are also applicable; the value range of b is 0.6 to 0.8, for example, it can be 0.6, 0.65, 0.7, 0.75 or 0.8, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are also applicable; the ratio of a to b indicates the molar ratio of the Ni element to the Mn element in the kernel;

[0070] The general formula of the shell is Ni x Mn y Nb z (OH) 2 , wherein the value range of x is 0.2 to 0.4, the value range of y is 0.6 to 0.8, the value range of z is 0.01 to 0.1, and the sum of x and y is 1; wherein the value range of x is 0.2 to 0.4, for example, it can be 0.2, 0.25, 0.3, 0.35 or 0.4, but is not limited to the listed values, and the other values ​​not listed in the numerical range are also applicable; the value range of y is 0.6 to 0.8, for example, it can be 0. 6, 0.65, 0.7, 0.75 or 0.8, but not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; z ranges from 0.01 to 0.1, for example, it can be 0.01, 0.03, 0.05, 0.08 or 0.1, but not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; the ratio of x, y and z indicates the molar ratio of Ni element, Mn element and Nb element in the shell;

[0071] In the general formula of the shell, the valence of Nb is +5.

[0072] The cobalt-free lithium-rich manganese-based precursor prepared by the preparation method provided by the present invention has a flower-shaped core-shell structure, which is Li + It provides more sites for storage, which is beneficial to improve its reversible capacity; it can also buffer some structural strains and effectively improve the tap density; the doping of Nb element reduces the disordered insertion of primary particles in the secondary particles, and at the same time, the primary particle wafers unfold in a flower shape, which effectively increases the specific surface area of ​​the precursor, helps to increase the reaction contact area between the positive electrode material and the electrolyte, and has better electrochemical performance; the higher specific surface area allows the Na and S elements in the precursor to be deviated as much as possible, reducing the Na and S impurity content in the precursor, which is beneficial to the subsequent preparation of positive electrode materials.

[0073] The doping solution in the present invention uses Nb2 O 5 and / or NaNb 2 O 4 As a doping compound, it does not undergo redox reactions during the doping process, thereby stabilizing the crystal structure of the shell layer.

[0074] In certain embodiments, the preparation method provided by the present invention is carried out in a protective atmosphere, and the gas used in the protective atmosphere includes nitrogen and / or an inert gas.

[0075] In certain embodiments, the metal salt in the first metal salt solution in step (1) includes a first nickel salt and a first manganese salt;

[0076] In the first metal salt solution, the molar ratio of nickel to manganese is a:b.

[0077] Exemplarily, the first nickel salt includes any one of nickel sulfate, nickel chloride, nickel nitrate or nickel acetate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of nickel sulfate and nickel chloride, a combination of nickel chloride and nickel nitrate, a combination of nickel nitrate and nickel acetate, a combination of nickel sulfate, nickel chloride and nickel nitrate, a combination of nickel chloride, nickel nitrate and nickel acetate, or a combination of nickel sulfate, nickel chloride, nickel nitrate and nickel acetate.

[0078] Exemplarily, the first manganese salt includes any one of manganese sulfate, manganese chloride, manganese nitrate or manganese acetate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of manganese sulfate and manganese chloride, a combination of manganese chloride and manganese nitrate, a combination of manganese nitrate and manganese acetate, a combination of manganese sulfate, manganese chloride and manganese nitrate, a combination of manganese chloride, manganese nitrate and manganese acetate, or a combination of manganese sulfate, manganese chloride, manganese nitrate and manganese acetate.

[0079] In some embodiments, the temperature of the base liquid in step (1) is 45°C to 55°C, for example, 45°C, 48°C, 50°C, 52°C or 55°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0080] In some embodiments, the pH value of the base solution in step (1) is 10.8 to 11.1, for example, it can be 10.8, 10.9, 11 or 11.1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0081] In certain embodiments, the ammonia concentration of the base solution in step (1) is 0.8 g / L to 1.2 g / L, for example, 0.8 g / L, 0.9 g / L, 1 g / L, 1.1 g / L or 1.2 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0082] In certain embodiments, the temperature of the coprecipitation reaction in step (1) is 45°C to 55°C, for example, 45°C, 48°C, 50°C, 52°C or 55°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0083] In certain embodiments, the pH value of the coprecipitation reaction in step (1) is 10.8 to 11.1, for example, 10.8, 10.9, 11 or 11.1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0084] In certain embodiments, the ammonia concentration of the co-precipitation reaction in step (1) is 0.8 g / L to 1.2 g / L, for example, 0.8 g / L, 0.9 g / L, 1 g / L, 1.1 g / L or 1.2 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0085] In certain embodiments, the end point of the coprecipitation reaction in step (1) is to make the seeds in the seed suspension satisfy: a particle size Dv50 of 2.8 μm to 3.2 μm, a specific surface area of ​​10 m 2 / g to 15m 2 / g, tap density is 0.8g / cm 2 Up to 1g / cm 2 .

[0086] The present invention does not impose any specific restrictions on the flow rates of the first precipitant solution, the first complexing agent solution and the first metal salt solution in step (1), as long as the coprecipitation reaction in step (1) meets the pH value and ammonia concentration requirements.

[0087] In certain embodiments, the metal salt in the second metal salt solution in step (2) includes a second nickel salt and a second manganese salt;

[0088] In the second metal salt solution, the molar ratio of nickel to manganese is x:y.

[0089] Exemplarily, the second nickel salt includes any one of nickel sulfate, nickel chloride, nickel nitrate or nickel acetate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of nickel sulfate and nickel chloride, a combination of nickel chloride and nickel nitrate, a combination of nickel nitrate and nickel acetate, a combination of nickel sulfate, nickel chloride and nickel nitrate, a combination of nickel chloride, nickel nitrate and nickel acetate, or a combination of nickel sulfate, nickel chloride, nickel nitrate and nickel acetate.

[0090] Exemplarily, the second manganese salt includes any one of manganese sulfate, manganese chloride, manganese nitrate or manganese acetate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of manganese sulfate and manganese chloride, a combination of manganese chloride and manganese nitrate, a combination of manganese nitrate and manganese acetate, a combination of manganese sulfate, manganese chloride and manganese nitrate, a combination of manganese chloride, manganese nitrate and manganese acetate, or a combination of manganese sulfate, manganese chloride, manganese nitrate and manganese acetate.

[0091] In certain embodiments, adjusting the pH value and ammonia concentration of the seed crystal suspension in step (2) refers to adjusting the pH value to 10.5 to 10.7 and the ammonia concentration to 2.7 g / L to 3.3 g / L.

[0092] For example, when adjusting the pH value of the seed crystal suspension, sodium hydroxide solution is used for adjustment; when adjusting the ammonia concentration of the seed crystal suspension, aqueous ammonia is used for adjustment.

[0093] In certain embodiments, the temperature of the intermittent co-precipitation reaction in step (2) is 45°C to 55°C, for example, 45°C, 48°C, 50°C, 52°C or 55°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0094] In certain embodiments, the pH value of the intermittent co-precipitation in step (2) starts from the first pH value, decreases to the second pH value at a rate of 0.025 / h to 0.035 / h, and is maintained until the intermittent co-precipitation reaction is completed.

[0095] In certain embodiments, the first pH value is 10.5 to 10.7, for example, 10.5, 10.6 or 10.7, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0096] In certain embodiments, the second pH value is 9.8 to 10, for example, 9.8, 9.9 or 10, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0097] In the present invention, the rate of decreasing from the first pH value to the second pH value is 0.025 / h to 0.035 / h, for example, it can be 0.025 / h, 0.028 / h, 0.03 / h, 0.032 / h or 0.035 / h, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are also applicable.

[0098] In certain embodiments, the ammonia concentration of the intermittent co-precipitation in step (2) is 2.7 g / L to 3.3 g / L, for example, 2.7 g / L, 2.8 g / L, 3 g / L, 3.2 g / L or 3.3 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0099] In certain embodiments, the endpoint of the intermittent co-precipitation in step (2) is to make the material in the modified cobalt-free lithium-rich manganese-based suspension satisfy: the particle size Dv50 is 5.8 μm to 6.2 μm.

[0100] In certain embodiments, during the intermittent co-precipitation reaction, the reaction device is externally connected to a concentration device. When the feed rate of the second metal salt solution is 5 L / h, the clearance rate of the intermittent co-precipitation reaction is 7 L / h to 10 L / h, for example, it can be 7 L / h, 8 L / h, 9 L / h or 10 L / h, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are also applicable.

[0101] The present invention does not impose any specific restrictions on the flow rates of the second precipitant solution, the second complexing agent solution, the doping solution and the second metal salt solution in step (2), as long as the intermittent coprecipitation reaction in step (2) meets the requirements of pH value, ammonia concentration and the general requirements of the shell layer.

[0102] In certain embodiments, the washing in step (3) comprises alkaline washing and water washing performed sequentially.

[0103] In some embodiments, the concentration of the alkali solution used for alkali washing is 0.01wt% to 0.015wt%, for example, it can be 0.01wt%, 0.012wt%, 0.014wt% or 0.015wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0104] Exemplarily, the alkali solution is sodium hydroxide solution.

[0105] In some embodiments, the alkali washing temperature is 75°C to 85°C, for example, 75°C, 78°C, 80°C, 82°C or 85°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0106] In some embodiments, the water washing temperature is 75°C to 85°C, for example, 75°C, 78°C, 80°C, 82°C or 85°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0107] In certain embodiments, the coprecipitation reaction in step (1) is carried out under stirring conditions.

[0108] In certain embodiments, the intermittent co-precipitation reaction in step (2) is carried out under stirring conditions.

[0109] The coprecipitation reaction and the intermittent coprecipitation reaction of the present invention are respectively and independently carried out under stirring conditions, and the stirring speed is 300 rpm to 400 rpm, for example, it can be 300 rpm, 320 rpm, 350 rpm, 380 rpm or 400 rpm, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are also applicable.

[0110] In certain embodiments, the first precipitant solution is a sodium hydroxide solution.

[0111] In certain embodiments, the second precipitant solution is a sodium hydroxide solution.

[0112] In certain embodiments, the first complexing agent solution is aqueous ammonia.

[0113] In certain embodiments, the second precipitant solution is aqueous ammonia.

[0114] A certain embodiment of the present invention provides a positive electrode material, wherein the raw material for preparing the positive electrode material includes the composite modified cobalt-free lithium-rich manganese-based precursor described in any embodiment, or the composite modified cobalt-free lithium-rich manganese-based precursor obtained by the preparation method described in any embodiment.

[0115] In certain embodiments, the positive electrode material includes a sodium ion positive electrode material or a lithium ion positive electrode material.

[0116] Exemplarily, when the positive electrode material is a lithium ion positive electrode material, a lithium source is mixed with a composite modified cobalt-free lithium-rich manganese-based precursor, and sintered to obtain the positive electrode material.

[0117] The lithium source includes lithium hydroxide and / or lithium carbonate.

[0118] Example 1

[0119] This embodiment provides a composite modified cobalt-free lithium-rich manganese-based precursor, wherein the cobalt-free lithium-rich manganese-based precursor is a flower-shaped core-shell structure having a core and a shell;

[0120] The general formula of the core is Ni 0.25 Mn 0.75 (OH) 2 ;

[0121] The general formula of the shell is Ni 0.25 Mn 0.75 Nb 0.05 (OH) 2 , where the valence of Nb is +5;

[0122] The preparation method of the composite modified cobalt-free lithium-rich manganese-based precursor comprises the following steps:

[0123] (1) preparing a base liquid having a temperature of 50° C., an ammonia concentration of 1.2 g / L and a pH value of 10.98, and mixing a first precipitant solution, a first complexing agent solution and a first metal salt solution in parallel in the base liquid under a nitrogen atmosphere and stirring at a stirring rate of 311 rpm to perform a coprecipitation reaction to obtain a seed suspension;

[0124] The first precipitant solution is a sodium hydroxide solution with a concentration of 32 wt%; the first complexing agent solution is ammonia water with a concentration of 60 g / L; the first metal salt solution is a mixed solution of nickel sulfate and manganese sulfate, and the molar ratio of nickel to manganese is 0.25:0.75;

[0125] During the coprecipitation reaction, the pH value was 10.98, the ammonia concentration was maintained at 1.2 g / L, and the flow rate of the first metal salt solution was 5 L / h;

[0126] The seeds in the seed suspension satisfy the following requirements: particle size Dv50 is 3.18 μm, specific surface area is 113.2 m 2 / g, tap density is 0.82g / cm 2 ;

[0127] (2) using a sodium hydroxide solution with a concentration of 32 wt % and an ammonia solution with a concentration of 60 g / L to adjust the pH value of the seed suspension to 10.7 and the ammonia concentration to 3.3 g / L; then, in a nitrogen atmosphere, the second precipitant solution, the second complexing agent solution, the doping solution and the second metal salt solution were mixed in parallel at a stirring rate of 311 rpm to perform an intermittent coprecipitation reaction to obtain a modified cobalt-free lithium-rich manganese-based suspension;

[0128] The second precipitant solution is a sodium hydroxide solution with a concentration of 32wt%; the second complexing agent solution is an ammonia solution with a concentration of 60g / L, and the doping solution is Nb 2 O 5 The second metal salt solution is a mixed solution of nickel sulfate and manganese sulfate, the molar ratio of nickel to manganese being 0.25:0.75;

[0129] During the intermittent coprecipitation reaction, an external concentration device is connected, the flow rate of the second metal salt solution is 5 L / h, the clearing rate of the concentration device is 7.8 L / h, and the pH value decreases from 10.7 to 9.9 at a rate of 0.03 / h during the reaction and is maintained until the material particle size Dv50 is 6 μm;

[0130] (3) The modified cobalt-free lithium-rich manganese-based suspension was washed with alkali and water, centrifuged and dried, and then dried in an oven at 120° C. for 12 h to obtain Figure 1 and Figure 2 The XRD pattern of the composite modified cobalt-free lithium-rich manganese-based precursor is shown in Figure 4 shown; Figure 2 This is the SEM image after CP (Cross-section Polisher) treatment;

[0131] The alkali washing is carried out at a temperature of 80°C using a sodium hydroxide solution having a concentration of 0.012wt%;

[0132] The water washing temperature is 80°C.

[0133] Example 2

[0134] This embodiment provides a composite modified cobalt-free lithium-rich manganese-based precursor, wherein the cobalt-free lithium-rich manganese-based precursor is a flower-shaped core-shell structure having a core and a shell;

[0135] The general formula of the core is Ni 0.25 Mn 0.75 (OH) 2 ;

[0136] The general formula of the shell is Ni 0.25 Mn 0.75 Nb 0.05 (OH) 2 , where the valence of Nb is +5;

[0137] The preparation method of the composite modified cobalt-free lithium-rich manganese-based precursor comprises the following steps:

[0138] (1) preparing a base liquid having a temperature of 45° C., an ammonia concentration of 0.8 g / L and a pH value of 10.8, and mixing a first precipitant solution, a first complexing agent solution and a first metal salt solution in parallel in the base liquid under a nitrogen atmosphere and stirring at a stirring rate of 311 rpm to perform a coprecipitation reaction to obtain a seed suspension;

[0139] The first precipitant solution is a sodium hydroxide solution with a concentration of 32 wt%; the first complexing agent solution is ammonia water with a concentration of 60 g / L; the first metal salt solution is a mixed solution of nickel sulfate and manganese sulfate, and the molar ratio of nickel to manganese is 0.25:0.75;

[0140] During the coprecipitation reaction, the pH value was 10.8, the ammonia concentration was maintained at 0.8 g / L, and the flow rate of the first metal salt solution was 5 L / h;

[0141] The seeds in the seed suspension satisfy the following requirements: particle size Dv50 is 3.12 μm, specific surface area is 11.3 m 2 / g, tap density is 0.86g / cm 2 ;

[0142] (2) using a sodium hydroxide solution with a concentration of 32 wt % and an ammonia solution with a concentration of 60 g / L to adjust the pH value of the seed suspension to 10.5 and the ammonia concentration to 2.7 g / L; then, in a nitrogen atmosphere, the second precipitant solution, the second complexing agent solution, the doping solution and the second metal salt solution were mixed in parallel at a stirring rate of 311 rpm to perform an intermittent coprecipitation reaction to obtain a modified cobalt-free lithium-rich manganese-based suspension;

[0143] The second precipitant solution is a sodium hydroxide solution with a concentration of 32wt%; the second complexing agent solution is an ammonia solution with a concentration of 60g / L, and the doping solution is NaNb 2 O 4 The second metal salt solution is a mixed solution of nickel sulfate and manganese sulfate, the molar ratio of nickel to manganese being 0.25:0.75;

[0144] During the intermittent coprecipitation reaction, an external concentration device is connected, the flow rate of the second metal salt solution is 5 L / h, the clearing rate of the concentration device is 7 L / h, and the pH value decreases from 10.5 to 9.8 at a rate of 0.025 / h during the reaction and is maintained until the material particle size Dv50 is 5.8 μm;

[0145] (3) The modified cobalt-free lithium-rich manganese-based suspension is washed with alkali and water, centrifuged and then dried in an oven at 120° C. for 12 h to obtain the composite modified cobalt-free lithium-rich manganese-based precursor;

[0146] The alkali washing is carried out at a temperature of 75°C using a sodium hydroxide solution having a concentration of 0.01wt%;

[0147] The water washing temperature is 75°C.

[0148] Example 3

[0149] This embodiment provides a composite modified cobalt-free lithium-rich manganese-based precursor, wherein the cobalt-free lithium-rich manganese-based precursor is a flower-shaped core-shell structure having a core and a shell;

[0150] The general formula of the core is Ni 0.25 Mn 0.75 (OH) 2 ;

[0151] The general formula of the shell is Ni 0.25 Mn 0.75 Nb 0.05 (OH) 2 , where the valence of Nb is +5;

[0152] The preparation method of the composite modified cobalt-free lithium-rich manganese-based precursor comprises the following steps:

[0153] (1) preparing a base liquid having a temperature of 55° C., an ammonia concentration of 1 g / L and a pH value of 11.1, and mixing a first precipitant solution, a first complexing agent solution and a first metal salt solution in parallel in the base liquid under a nitrogen atmosphere and stirring at a stirring rate of 311 rpm to perform a coprecipitation reaction to obtain a seed suspension;

[0154] The first precipitant solution is a sodium hydroxide solution with a concentration of 32 wt%; the first complexing agent solution is ammonia water with a concentration of 60 g / L; the first metal salt solution is a mixed solution of nickel sulfate and manganese sulfate, and the molar ratio of nickel to manganese is 0.25:0.75;

[0155] During the coprecipitation reaction, the pH value is 11.1, the ammonia concentration is maintained at 1 g / L, and the flow rate of the first metal salt solution is 5 L / h;

[0156] The seeds in the seed suspension satisfy the following requirements: particle size Dv50 is 2.95 μm, specific surface area is 12.3 m 2 / g, tap density is 0.81g / cm 2 ;

[0157] (2) using a sodium hydroxide solution with a concentration of 32 wt % and an ammonia solution with a concentration of 60 g / L to adjust the pH value of the seed suspension to 10.7 and the ammonia concentration to 3 g / L; then, in a nitrogen atmosphere, the second precipitant solution, the second complexing agent solution, the doping solution and the second metal salt solution were mixed in parallel at a stirring rate of 311 rpm to perform an intermittent coprecipitation reaction to obtain a modified cobalt-free lithium-rich manganese-based suspension;

[0158] The second precipitant solution is a sodium hydroxide solution with a concentration of 32wt%; the second complexing agent solution is an ammonia solution with a concentration of 60g / L, and the doping solution is Nb 2 O 5 The second metal salt solution is a mixed solution of nickel sulfate and manganese sulfate, the molar ratio of nickel to manganese being 0.25:0.75;

[0159] During the intermittent coprecipitation reaction, an external concentration device is connected, the flow rate of the second metal salt solution is 5 L / h, the clearing rate of the concentration device is 10 L / h, and the pH value decreases from 10.7 to 10 at a rate of 0.035 / h during the reaction and is maintained until the material particle size Dv50 is 6.2 μm;

[0160] (3) The modified cobalt-free lithium-rich manganese-based suspension is washed with alkali and water, centrifuged and then dried in an oven at 120° C. for 12 h to obtain the composite modified cobalt-free lithium-rich manganese-based precursor;

[0161] The alkali washing is carried out at a temperature of 85°C using a sodium hydroxide solution having a concentration of 0.015wt%;

[0162] The water washing temperature is 85°C.

[0163] Example 4

[0164] This embodiment provides a composite modified cobalt-free lithium-rich manganese-based precursor. In addition to changing the flow rate of the doping solution during the intermittent coprecipitation reaction, the general formula of the shell is Ni 0.25 Mn 0.75 Nb 0.01 (OH) 2 Except for this, the rest are the same as in Example 1.

[0165] Example 5

[0166] This embodiment provides a composite modified cobalt-free lithium-rich manganese-based precursor. In addition to changing the flow rate of the doping solution during the intermittent coprecipitation reaction, the general formula of the shell is Ni 0.25 Mn 0.75 Nb 0.1 (OH) 2 Except for this, the rest are the same as in Example 1.

[0167] Example 6

[0168] This embodiment provides a composite modified cobalt-free lithium-rich manganese-based precursor, in addition to changing the nickel content and manganese content in the first metal salt solution and the second metal salt solution, so that the general formula of the core is Ni 0.2 Mn 0.8 (OH) 2 The general formula of the shell is Ni 0.2 Mn 0.8 Nb 0.05 (OH) 2 , the rest are the same as in Example 1.

[0169] Example 7

[0170] This embodiment provides a composite modified cobalt-free lithium-rich manganese-based precursor, in addition to changing the nickel content and manganese content in the first metal salt solution and the second metal salt solution, so that the general formula of the core is Ni 0.4 Mn 0.6 (OH) 2 The general formula of the shell is Ni 0.4 Mn 0.6 Nb 0.05 (OH) 2 , the rest are the same as in Example 1.

[0171] Comparative Example 1

[0172] This comparative example provides a cobalt-free lithium-rich manganese-based precursor, which is the same as Example 1 except that no doping solution is used.

[0173] The SEM image of the cobalt-free lithium-rich manganese-based precursor obtained in this comparative example is as follows Figure 3 As shown, the XRD pattern is Figure 4 shown.

[0174] Comparative Example 2

[0175] This comparative example provides a cobalt-free lithium-rich manganese-based precursor, except that a doping solution is used in the preparation of the core to make the core have the general formula of Ni 0.2 Mn 0.8 Nb 0.05 (OH) 2 The general formula of the shell is Ni 0.2 Mn 0.8 Nb 0.05 (OH) 2 , the rest are the same as in Example 1.

[0176] The cobalt-free lithium-rich manganese-based precursor provided in this comparative example is doped with Nb in the core. Although it can increase the tap density, the specific surface area decreases significantly and cannot meet the requirements of a cobalt-free lithium-rich manganese-based precursor having both high tap density and high specific surface area.

[0177] Comparative Example 3

[0178] This embodiment provides a composite modified cobalt-free lithium-rich manganese-based precursor. In addition to changing the flow rate of the doping solution during the intermittent coprecipitation reaction, the general formula of the shell is Ni 0.25 Mn 0.75 Nb 0.15 (OH) 2 Except for this, the rest are the same as in Example 1.

[0179] Performance Characterization

[0180] The specific surface area, Na content, S content, particle size distribution and tap density of the precursors obtained in the above examples and comparative examples were measured, and the results are shown in Table 1.

[0181] Table 1

[0182]

[0183]

[0184] In summary, the present invention provides a cobalt-free lithium-rich manganese-based precursor with a flower-like core-shell structure, which is Li +The core-shell structure provides more sites for storage, which is beneficial to improving its reversible capacity. Moreover, the core-shell structure can buffer part of the structural strain and effectively improve the tap density, so that the precursor can have both high specific surface area and tap density. The addition of Nb element in the shell can reduce the disordered insertion of primary particles in the secondary particles. At the same time, the primary particle crystals are unfolded in a flower-like manner, which effectively improves the specific surface area of ​​the precursor and helps to increase the reaction contact area between the positive electrode material and the electrode liquid, and has better electrochemical performance. At the same time, the external primary particles are in an orderly flower-like radial shape, so that impurities such as Na and S in the precursor are excluded as much as possible, reducing the content of Na and S impurities in the precursor. Moreover, the shell can act as a protective layer to reduce the erosion of the material in the subsequent sintering process, improve the good lithium ion transmission channel, enhance the electronic conductivity, and ensure the integrity of the structure during the charge and discharge process.

[0185] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A composite modified cobalt-free lithium-rich manganese-based precursor, characterized in that: The cobalt-free lithium-rich manganese-based precursor is a flower-shaped core-shell structure, having a core and a shell; The general formula of the core is Ni a Mn b (OH)2, wherein a ranges from 0.2 to 0.4, b ranges from 0.6 to 0.8, and the sum of a and b is 1; The general formula of the shell is Ni x Mn y Nb z (OH)2, wherein x ranges from 0.2 to 0.4, y ranges from 0.6 to 0.8, z ranges from 0.01 to 0.1, and the sum of x and y is 1; In the general formula of the shell, the valence of Nb is +5.

2. A method for preparing a composite modified cobalt-free lithium-rich manganese-based precursor, characterized in that: The preparation method comprises the following steps: (1) mixing a first precipitant solution, a first complexing agent solution and a first metal salt solution in a base liquid to perform a coprecipitation reaction to obtain a seed crystal suspension; (2) adjusting the pH value and ammonia concentration of the seed crystal suspension, and then mixing the second precipitant solution, the second complexing agent solution, the doping solution and the second metal salt solution in parallel to perform an intermittent coprecipitation reaction to obtain a modified cobalt-free lithium-rich manganese-based suspension; The doping compound in the doping solution is Nb2O5 and / or NaNb2O4; (3) The modified cobalt-free lithium-rich manganese-based suspension is washed and dried to obtain the composite modified cobalt-free lithium-rich manganese-based precursor; The obtained cobalt-free lithium-rich manganese-based precursor is a flower-like core-shell structure with a core and a shell; The general formula of the core is Ni a Mn b (OH)2, wherein the value of a ranges from 0.2 to 0.4, the value of b ranges from 0.6 to 0.8, and the sum of a and b is 1; The general formula of the shell is Ni x Mn y Nb z (OH)2, wherein x ranges from 0.2 to 0.4, y ranges from 0.6 to 0.8, z ranges from 0.01 to 0.1, and the sum of x and y is 1; In the general formula of the shell, the valence of Nb is +5.

3. The preparation method according to claim 2, characterized in that: Step (1) The metal salt in the first metal salt solution includes a first nickel salt and a first manganese salt; In the first metal salt solution, the molar ratio of nickel to manganese is a:b; Preferably, the metal salt in the second metal salt solution in step (2) comprises a second nickel salt and a second manganese salt; In the second metal salt solution, the molar ratio of nickel to manganese is x:y.

4. The preparation method according to claim 2 or 3, characterized in that: The temperature of the coprecipitation reaction in step (1) is 45° C. to 55° C.; Preferably, the pH value of the coprecipitation reaction in step (1) is 10.8 to 11.1; Preferably, the ammonia concentration of the coprecipitation reaction in step (1) is 0.8 g / L to 1.2 g / L; Preferably, the end point of the coprecipitation reaction in step (1) is to make the seeds in the seed suspension satisfy: the particle size Dv50 is 2.8 μm to 3.2 μm, the specific surface area is 10 m 2 / g to 15m 2 / g, tap density is 0.8g / cm 2 Up to 1g / cm 2 .

5. The preparation method according to any one of claims 2 to 4, characterized in that: The temperature of the intermittent coprecipitation reaction in step (2) is 45° C. to 55° C.; Preferably, the pH value of the intermittent coprecipitation in step (2) starts from the first pH value, decreases to the second pH value at a rate of 0.025 / h to 0.035 / h, and is maintained until the intermittent coprecipitation reaction ends; Preferably, the first pH value is 10.5 to 10.7, and the second pH value is 9.8 to 10; Preferably, the ammonia concentration of the intermittent coprecipitation in step (2) is 2.7 g / L to 3.3 g / L; Preferably, the endpoint of the intermittent co-precipitation in step (2) is to make the material in the modified cobalt-free lithium-rich manganese-based suspension satisfy: the particle size Dv50 is 5.8 μm to 6.2 μm.

6. The preparation method according to claim 5, characterized in that: The clearing rate of the intermittent co-precipitation reaction in step (2) is 7 L / h to 10 L / h.

7. The preparation method according to any one of claims 2 to 6, characterized in that: The washing in step (3) comprises alkali washing and water washing performed sequentially; Preferably, the concentration of the alkali solution used for the alkali washing is 0.01wt% to 0.015wt%; Preferably, the temperature of the alkali washing is 75°C to 85°C; Preferably, the water washing temperature is 75°C to 85°C.

8. The preparation method according to any one of claims 2 to 7, characterized in that: The coprecipitation reaction in step (1) is carried out under stirring; Preferably, the intermittent coprecipitation reaction in step (2) is carried out under stirring conditions.

9. The preparation method according to any one of claims 2 to 8, characterized in that: The first precipitant solution is a sodium hydroxide solution; Preferably, the second precipitant solution is a sodium hydroxide solution; Preferably, the first complexing agent solution is aqueous ammonia; Preferably, the second precipitant solution is aqueous ammonia.

10. A positive electrode material, characterized in that: The raw material for preparing the positive electrode material includes the composite modified cobalt-free lithium-rich manganese-based precursor according to claim 1, or the composite modified cobalt-free lithium-rich manganese-based precursor obtained by the preparation method according to any one of claims 2 to 9.

Citation Information

Patent Citations

  • Monocrystal positive electrode material precursor and preparation method and application thereof

    CN116730405A

  • Positive electrode material precursor with composite morphological structure, preparation method of positive electrode material precursor, lithium ion battery, positive electrode material and electric equipment

    CN117865234A

  • Surface-doped lithium-rich manganese-based precursor as well as preparation method and application thereof

    CN118579851A

Cited By

  • Lithium-rich manganese-based precursor material as well as preparation method and application thereof

    CN120887459A

  • Five-element doped lithium nickel manganese oxide positive electrode material as well as precursor and preparation method thereof