Manufacturing and recycling method of YSZ water-based casting sheet for nitrogen-oxygen sensor

By using negative pressure vacuum defoaming and recycling slurry in the water system casting process, the problems of slurry dispersion and waste recycling are solved, the quality and sintering density of casting sheets are improved, and the reuse and production of resources are realized. Reduced costs.

CN118894723APending Publication Date: 2024-11-05ZHENJIANG XINYUAN CHENGDA SENSOR TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410929156.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing water system casting process has problems such as difficulty in dispersing slurry, defoaming and waste recycling, resulting in waste of resources and high production costs.

Method used

The YSZ water-based casting sheet was prepared by negative pressure vacuum defoaming, and the waste casting sheet was used to recover the slurry, and the production process of the casting sheet was optimized and the sintering density was improved.

Benefits of technology

It effectively solves the difficulty of slurry dispersion and defoaming, improves the quality and sintering density of cast sheets, and realizes the recycling and reuse of cast sheets, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894723A_ABST
    Figure CN118894723A_ABST
Patent Text Reader

Abstract

The invention provides a manufacturing and recycling method of a YSZ water system casting sheet for a nitrogen-oxygen sensor, and belongs to the technical field of nitrogen-oxygen sensors. Manufacturing slurry is subjected to casting treatment after being subjected to vacuum defoaming under the negative pressure of 0.3-0.8 Mpa; the height of a casting knife for casting treatment is 180-310mu m, the casting speed is 0.5-1m / min, the thickness of a casting sheet is 100-160mu m at the temperature of three areas, and sintering is performed for 2h at the temperature of 1450 DEG C to obtain a first-time casting sheet finished product and a waste casting sheet; the recycled slurry is subjected to vacuum defoaming under the negative pressure of 0.3-0.8 Mpa and then subjected to tape casting treatment; the height of a tape-casting knife for tape-casting treatment is 180-310 microns, the tape-casting speed is 0.5-1 m / min, the thickness of a tape-casting sheet is 100-160 microns at the temperature of three areas, sintering is conducted for 2 h at the temperature of 1450 DEG C, and a second-time tape-casting sheet finished product is obtained.The method has the advantages that few bubbles are generated in slurry manufacturing, the quality of the tape-casting sheet is improved, the problem of slurry dispersion of a water system tape-casting process is effectively solved, and the production cost is lowered. And meanwhile, the production process of the water-based slurry is optimized, the defoaming difficulty is reduced, and the quality of the cast sheet and the density of the sintered cast sheet are effectively improved. And meanwhile, recycling and reusing of the cast sheet are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nitrogen oxygen sensors, and in particular to a method for manufacturing and recovering a YSZ water-based cast sheet for a nitrogen oxygen sensor. Background Art

[0002] With the rapid development of the economy, the number of cars in my country is increasing, and the problem of air pollution caused by automobile exhaust is becoming more and more serious. Among them, nitrogen oxides in exhaust gas can cause acid rain and photochemical pollution, causing great harm to the environment and people's physical and mental health. As the world's second largest economy, it is our unshirkable responsibility to reduce exhaust emissions and harmful substances in exhaust gas. As the core component of the automobile exhaust emission SCR system, the nitrogen oxide sensor can detect the concentration of nitrogen oxides in the exhaust gas in real time, and feed it back to the SCR system to determine the amount of fuel injection and the amount of urea for treating nitrogen oxides, so that the exhaust emissions meet the standards.

[0003] At present, the chip-type nitrogen and oxygen sensors for automobiles are all made of yttria-stabilized zirconia (YSZ) substrates with printed multiple functional layers. Among them, YSZ substrates are mostly prepared by tape casting. As an important molding method, tape casting has been widely used in the preparation of ceramic substrates and multilayer structural materials, but the quality of molding largely affects the material structure and determines the performance, application and price of the product. The tape casting process can be divided into water-based tape casting and non-aqueous tape casting according to the solvent used in the slurry. Among them, non-aqueous tape casting mostly uses organic solvents such as toluene, xylene, trichloroethylene, ethanol, butanone, etc., polyvinyl butyral ester (PVB), ethyl cellulose, etc. as binders, butyl benzyl phthalate, polyethylene glycol, etc. as plasticizers. The surface of the diaphragm is smooth and uniform, the drying speed is fast, the diaphragm quality is high, and the application in multilayer ceramic composite devices has been very mature. However, its solvents are mostly hazardous chemicals, flammable and explosive, and are more demanding on the storage and use environment. There are greater safety hazards in the production process and the production cost is high. The viscosity of water-based cast slurry is difficult to control, and it is difficult to disperse. The slurry has a large surface tension and many bubbles, making it difficult to degas. It is difficult to recycle the waste film in the production process, resulting in a waste of resources. Water-based cast slurry often uses distilled water instead of organic solvents. The water-based slurry cast forming process has the advantages of being cheap and non-toxic, and no environmental protection measures are required in the production process. Therefore, the research on safe, clean, and low-cost water-based cast forming technology has become an irreversible trend. Summary of the invention

[0004] The present invention aims to solve the above technical problems and provide a method for preparing YSZ water-based tape casting slurry for nitrogen oxygen sensor. The method effectively solves the slurry dispersion problem of the water-based tape casting process, optimizes the production process of the water-based slurry, reduces the difficulty of degassing, and effectively improves the quality of the tape casting sheet and the density after sintering. At the same time, a new method is provided to realize the recycling and reuse of the tape casting sheet.

[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:

[0006] A method for making and recycling a YSZ water-based cast sheet for a nitrogen and oxygen sensor, comprising making slurry and recycling slurry;

[0007] The method for making and recycling the cast sheet comprises the following steps:

[0008] S1, prepare slurry and perform casting treatment after vacuum degassing under negative pressure of 0.3-0.8Mpa;

[0009] S2, the height of the casting blade in the casting process is 180-310 μm, the casting speed is 0.5-1 m / min, the casting sheet thickness is 100-160 μm, and the casting sheet is sintered at 1450 ° C for 2 hours to obtain the first cast sheet finished product and the waste cast sheet;

[0010] S3, the recovered slurry is subjected to vacuum degassing under a negative pressure of 0.3-0.8Mpa and then subjected to tape casting treatment;

[0011] S4, the height of the casting blade of the casting treatment is 180-310μm, the casting speed is 0.5-1m / min, the casting sheet thickness is 100-160um, and it is sintered at 1450℃ for 2h to obtain the second casting sheet finished product;

[0012] The slurry is composed of distilled water, YSZ powder, binder, dispersant, plasticizer and defoamer;

[0013] The recovered slurry consists of distilled water, ammonia water and waste cast sheets.

[0014] Preferably, the slurry is composed of 20-50 parts of distilled water, 50-80 parts of YSZ powder, 5-10 parts of binder, 0.5-5 parts of dispersant, 2-5 parts of plasticizer and 0.05-0.1 parts of defoamer.

[0015] Preferably, the binder is polyacrylic acid resin, the dispersant is polyacrylic acid or a copolymer of polyacrylic acid, the plasticizer is polyethylene glycol or dibutyl phthalate, and the defoamer is n-butanol.

[0016] Preferably, the recovered slurry consists of 18-50 parts of distilled water, 0.5-5 parts of aqueous ammonia and 50-80 parts of waste cast film.

[0017] Preferably, the temperatures of the three zones in steps S2 and S4 are respectively 40-60°C for zone one, 70-90°C for zone two, and 95-110°C for zone three.

[0018] Preferably, the solid content of the prepared slurry is greater than 73%, and the viscosity is less than 1200 mPa·s, and the solid content of the recovered slurry is greater than 70%, and the viscosity is less than 1500 mPa·s.

[0019] Preferably, the method for making the slurry is to place distilled water and a dispersant in a sand mill and grind for 15 minutes, place the YSZ powder in the grinder, continue grinding for 1 hour, then transfer to a stirring tank, add a binder and a plasticizer, stir at 80r / min for 4 hours, add a defoamer, stir at 50r / min for 2 hours, and obtain the slurry.

[0020] Preferably, the method for preparing the recycled slurry is to weigh distilled water and ammonia water, place them in a ball mill, adjust the pH value to 9-10, take the waste cast sheet, place it in the ball mill, and ball mill for 12 hours to obtain a recycled slurry with a suitable viscosity.

[0021] Preferably, the particle size of the YSZ powder is 0.5-1 micron.

[0022] After adopting the above structure, the present invention has the following advantages:

[0023] The invention produces fewer bubbles in the slurry, improves the quality of the cast sheet, effectively solves the slurry dispersion problem in the water-based casting process, optimizes the production process of the water-based slurry, reduces the difficulty of degassing, effectively improves the quality of the cast sheet and the density after sintering, and realizes the recycling and reuse of the cast sheet.

[0024] The above summary is for illustrative purposes only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments and features described above, further aspects, embodiments and features of the present invention will be readily apparent by reference to the accompanying drawings and the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or technical descriptions will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 Schematic diagram of SEM of the water-based cast sheet after sintering of the present invention;

[0027] Figure 2 It is a schematic diagram of SEM of the recycled cast sheet after sintering of the present invention. DETAILED DESCRIPTION

[0028] Specific embodiments of the present invention will now be mentioned in detail. Although the present invention is described in conjunction with these specific embodiments, it should be appreciated that it is not intended to limit the present invention to these specific embodiments. On the contrary, these embodiments are intended to cover substitutions, changes or equivalent embodiments that may be included in the spirit and scope of the invention defined by the claims. In the following description, a large number of specific details are set forth in order to provide a comprehensive understanding of the present invention. The present invention can be implemented without some or all of these specific details. In other cases, in order not to make the present invention unnecessarily obscure, well-known process operations are not described in detail.

[0029] When used in conjunction with "including," "methods comprising," or similar language in this specification and the appended claims, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

[0030] The present invention is further described in detail below in conjunction with the full text.

[0031] Combined with Figure 1-Figure 2 , a method for making and recycling a YSZ water-based cast sheet for a nitrogen and oxygen sensor, comprising making a slurry and recycling the slurry;

[0032] The method for making and recycling the cast sheet comprises the following steps:

[0033] S1, prepare slurry and perform casting treatment after vacuum degassing under negative pressure of 0.3-0.8Mpa;

[0034] S2, the height of the casting blade in the casting process is 180-310 μm, the casting speed is 0.5-1 m / min, the casting sheet thickness is 100-160 μm, and the casting sheet is sintered at 1450 ° C for 2 hours to obtain the first cast sheet finished product and the waste cast sheet;

[0035] S3, the recovered slurry is subjected to vacuum degassing under a negative pressure of 0.3-0.8Mpa and then subjected to tape casting treatment;

[0036] S4, the height of the casting blade of the casting treatment is 180-310μm, the casting speed is 0.5-1m / min, the casting sheet thickness is 100-160um, and it is sintered at 1450℃ for 2h to obtain the second casting sheet finished product;

[0037] The invention improves the dispersion efficiency and dispersion effect of nano powder in water, improves the sintering density of the YSZ substrate of the cast sheet, and realizes the recycling and reuse of the waste cast sheet.

[0038] The slurry is composed of distilled water, YSZ powder, binder, dispersant, plasticizer and defoamer;

[0039] The recovered slurry consists of distilled water, ammonia water and waste cast sheets.

[0040] The slurry is composed of 20-50 parts of distilled water, 50-80 parts of YSZ powder, 5-10 parts of binder, 0.5-5 parts of dispersant, 2-5 parts of plasticizer and 0.05-0.1 parts of defoamer.

[0041] The binder is polyacrylic acid resin, the dispersant is polyacrylic acid or a copolymer of polyacrylic acid, the plasticizer is polyethylene glycol or dibutyl phthalate, and the defoamer is n-butanol.

[0042] The recovered slurry is composed of 18-50 parts of distilled water, 0.5-5 parts of ammonia water and 50-80 parts of waste cast sheets.

[0043] The temperatures of the three zones in the steps S2 and S4 are respectively 40-60°C for zone one, 70-90°C for zone two, and 95-110°C for zone three.

[0044] The solid content of the prepared slurry is greater than 73%, and the viscosity is less than 1200 mPa·s; the solid content of the recovered slurry is greater than 70%, and the viscosity is less than 1500 mPa·s.

[0045] The method for preparing the slurry is as follows: placing distilled water and a dispersant in a sand mill and grinding for 15 minutes, placing YSZ powder in the grinder, continuing to grind for 1 hour, and then transferring to a stirring tank, adding a binder and a plasticizer, stirring at 80 r / min for 4 hours, adding a defoamer, stirring at 50 r / min for 2 hours, and discharging the material to obtain the slurry.

[0046] The preparation method of the recycling slurry is as follows: weighing distilled water and ammonia water and placing them in a ball mill, adjusting the pH value to 9-10, taking the waste cast film, placing it in the ball mill, and ball milling for 12 hours to obtain a recycling slurry with a suitable viscosity. The recycling slurry and the preparation method of the slurry effectively reduce the bubbles generated by the ball milling process and reduce the difficulty of degassing.

[0047] The particle size of the YSZ powder is 0.5-1 micron. YSZ is yttria-stabilized zirconia, which is a ceramic material.

[0048] Embodiment 1:

[0049] Preparation of slurry: 22 parts of distilled water and 0.8 parts of polyacrylic acid copolymer are placed in a sand mill and ground for 15 minutes; 68 parts of YSZ powder with a particle size of 0.5 microns are placed in a grinder and continue to grind for 1 hour; the dispersed slurry is transferred to a stirring tank, 6 parts of polyacrylic acid resin and 3 parts of polyethylene glycol are added, stirred at 80r / min for 4 hours, and then 0.2 parts of n-butanol are added at 50r / min and stirred for 2 hours to obtain the slurry;

[0050] According to the above process, the slurry prepared has a solid content of 74%, a viscosity of 620 mPa·s, a casting blade height of 200 μm, a casting speed of 1 m / min, and three-zone temperature, in order, the temperature of the first zone is 40°C, the temperature of the second zone is 70°C, and the temperature of the third zone is 95°C. The prepared casting sheet has a thickness of 100 μm. After sintering at 1450°C for 2 hours, the density is 99.923%;

[0051] Cast sheet recovery: Use 2 parts of ammonia water, adjust the pH value of 20 parts of distilled water to 9.2, add 80 parts of cast sheet prepared by the above process, use a horizontal ball mill at 40r / min for 24 hours and then discharge. The prepared recycled slurry has a solid content of 73% and a viscosity of 750mPa·s. The casting blade height of the casting treatment is 200μm, the casting speed is 1m / min, and the temperature of the three zones is 40℃ in the first zone, 70℃ in the second zone, and 95℃ in the third zone. The thickness of the cast sheet is 100um. After sintering at 1450℃ for 2h, a cast sheet with a density of 99.992% is obtained;

[0052] Embodiment 2:

[0053] To prepare the slurry, 20 parts of distilled water and 0.8 parts of a copolymer of polyacrylic acid are placed in a sand mill and ground for 15 minutes; 68.5 parts of YSZ powder with a particle size of 1 micron are placed in a grinder and continued to grind for 1 hour; the dispersed slurry is transferred to a stirring tank, 7 parts of polyacrylic acid resin and 3.5 parts of polyethylene glycol are added, stirred at 80 r / min for 4 hours, and then 0.2 parts of n-butanol are added at 50 r / min and stirred for 2 hours to obtain the slurry;

[0054] According to the above process, the solid content of the slurry prepared was 75%, the viscosity was 1100mPa·s, the casting blade height was 300μm, the casting speed was 0.5m / min, and the three-zone temperature was 60℃ for zone 1, 90℃ for zone 2, and 110℃ for zone 3. The prepared casting sheet had a thickness of 160um, and after sintering at 1450℃ for 2h, the casting sheet was obtained with a density of 99.995%.

[0055] Cast sheet recovery: Use 2 parts of ammonia water, adjust the pH of 20 parts of distilled water to 9.5, add 80 parts of cast sheet prepared by the above process, use horizontal ball mill 40r / min ball mill for 24h and then discharge. The prepared slurry has a solid content of 76%, a viscosity of 1345mPa·s, a casting knife height of 300μm, a casting speed of 0.5m / min, and three zone temperatures, in turn, the temperature of zone 1 is 60℃, the temperature of zone 2 is 90℃, and the temperature of zone 3 is 110℃. The prepared cast sheet has a thickness of 160um. After sintering at 1450℃ for 2h, a cast sheet with a density of 99.939% is obtained.

[0056] Embodiment three:

[0057] To prepare the slurry, 50 parts of distilled water and 2 parts of polyacrylic acid were placed in a sand mill and ground for 15 minutes; 55 parts of YSZ powder with a particle size of 0.8 microns were placed in a grinder and continued to grind for 1 hour; the dispersed slurry was transferred to a stirring tank, 8 parts of polyacrylic acid resin and 2 parts of polyethylene glycol were added and stirred at 80 r / min for 4 hours, and then 0.2 parts of n-butanol were added at 50 r / min and stirred for 2 hours to obtain the slurry;

[0058] According to the above process, the solid content of the slurry prepared was 77%, the viscosity was 1120mPa·s, the casting blade height was 280μm, the casting speed was 0.8m / min, and the three-zone temperature was 55℃, 85℃, and 105℃, respectively. The prepared casting sheet had a thickness of 160um, and after sintering at 1450℃ for 2h, the casting sheet was obtained with a density of 99.995%.

[0059] Cast sheet recovery: Use 2 parts of ammonia water, adjust the pH of 25 parts of distilled water to 9.5, add 80 parts of cast sheet prepared by the above process, use horizontal ball mill 40r / min ball mill for 24h and then discharge. The prepared slurry has a solid content of 78%, a viscosity of 1315mPa·s, a casting blade height of 289μm, a casting speed of 0.5m / min, and three zone temperatures, in turn, the temperature of zone 1 is 45℃, the temperature of zone 2 is 75℃, and the temperature of zone 3 is 95℃. The prepared cast sheet has a thickness of 160um. After sintering at 1450℃ for 2h, a cast sheet with a density of 99.961% is obtained.

[0060] Embodiment 4:

[0061] Preparation of slurry: 45 parts of distilled water and 2 parts of polyacrylic acid are placed in a sand mill and ground for 15 minutes; 80 parts of YSZ powder with a particle size of 0.8 microns are placed in a grinder and continued to grind for 1 hour; the dispersed slurry is transferred to a stirring tank, 8 parts of polyacrylic acid resin and 4 parts of dibutyl phthalate are added, stirred at 80r / min for 4 hours, and then 0.2 parts of n-butanol are added at 50r / min and stirred for 2 hours to obtain the slurry;

[0062] According to the above process, the solid content of the slurry prepared was 79%, the viscosity was 1020mPa·s, the casting blade height was 280μm, the casting speed was 1m / min, and the three-zone temperature was 58℃, 89℃, and 102℃. The prepared casting sheet had a thickness of 160um, and after sintering at 1450℃ for 2h, the casting sheet was obtained with a density of 99.995%.

[0063] Cast sheet recovery: Use 2 parts of ammonia water, adjust the pH of 45 parts of distilled water to 9.5, add 78 parts of cast sheet prepared by the above process, use horizontal ball mill 40r / min ball mill for 24h and then discharge. The prepared slurry has a solid content of 79%, a viscosity of 1215mPa·s, a casting knife height of 280μm, a casting speed of 0.8m / min, and three zone temperatures, in turn, the temperature of zone 1 is 55℃, the temperature of zone 2 is 85℃, and the temperature of zone 3 is 99℃. The prepared cast sheet has a thickness of 160um. After sintering at 1450℃ for 2h, a cast sheet with a density of 99.981% is obtained.

[0064] The present invention and its embodiments are described above, and such description is not restrictive. What is shown in the full text is only one of the embodiments of the present invention, and the actual structure is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design a structure and embodiment similar to the technical solution without creativity, which should belong to the protection scope of the present invention.

Claims

1. A method for making and recycling YSZ water-based cast sheet for nitrogen and oxygen sensors. It is characterized in that Including making pulp and recycling pulp; The method for making and recycling the cast sheet comprises the following steps: S1, prepare slurry and perform casting treatment after vacuum degassing under negative pressure of 0.3-0.8Mpa; S2, the height of the casting blade in the casting process is 180-310 μm, the casting speed is 0.5-1 m / min, the casting sheet thickness is 100-160 μm, and the casting sheet is sintered at 1450 ° C for 2 hours to obtain the first cast sheet finished product and the waste cast sheet; S3, the recovered slurry is subjected to vacuum degassing under a negative pressure of 0.3-0.8Mpa and then subjected to tape casting treatment; S4, the height of the casting blade of the casting treatment is 180-310μm, the casting speed is 0.5-1m / min, the casting sheet thickness is 100-160um, and it is sintered at 1450℃ for 2h to obtain the second casting sheet finished product; The slurry is composed of distilled water, YSZ powder, binder, dispersant, plasticizer and defoamer; The recovered slurry consists of distilled water, ammonia water and waste cast sheets.

2. A method for making and recycling a YSZ aqueous cast sheet for a nitrogen oxygen sensor according to claim 1, Features: The slurry is composed of 20-50 parts of distilled water, 50-80 parts of YSZ powder, 5-10 parts of binder, 0.5-5 parts of dispersant, 2-5 parts of plasticizer and 0.05-0.1 parts of defoamer.

3. A method for preparing and recycling a YSZ aqueous cast sheet for a nitrogen oxygen sensor according to claim 1 or 2, Features: The binder is polyacrylic acid resin, the dispersant is polyacrylic acid or a copolymer of polyacrylic acid, the plasticizer is polyethylene glycol or dibutyl phthalate, and the defoamer is n-butanol.

4. A method for making and recycling a YSZ water-based cast sheet for a nitrogen oxygen sensor according to claim 1, Features: The recovered slurry is composed of 18-50 parts of distilled water, 0.5-5 parts of ammonia water and 50-80 parts of waste cast sheets.

5. A method for making and recycling a YSZ water-based cast sheet for a nitrogen oxygen sensor according to claim 1, Features: The temperatures of the three zones in the steps S2 and S4 are respectively 40-60°C for zone one, 70-90°C for zone two, and 95-110°C for zone three.

6. A method for making and recycling a YSZ water-based cast sheet for a nitrogen oxygen sensor according to claim 1, Features: The solid content of the prepared slurry is greater than 73%, and the viscosity is less than 1200 mPa·s; the solid content of the recovered slurry is greater than 70%, and the viscosity is less than 1500 mPa·s.

7. A method for making and recycling a YSZ water-based cast sheet for a nitrogen oxygen sensor according to claim 1, Features: The method for preparing the slurry is as follows: placing distilled water and a dispersant in a sand mill and grinding for 15 minutes, placing YSZ powder in the grinder, continuing to grind for 1 hour, and then transferring to a stirring tank, adding a binder and a plasticizer, stirring at 80 r / min for 4 hours, adding a defoamer, stirring at 50 r / min for 2 hours, and discharging the material to obtain the slurry.

8. A method for making and recycling a YSZ water-based cast sheet for a nitrogen oxygen sensor according to claim 1, Features: The preparation method of the recycling slurry is as follows: weighing distilled water and ammonia water, placing them in a ball mill, adjusting the pH value to 9-10, taking the waste cast sheet, placing it in the ball mill, and ball milling for 12 hours to obtain the recycling slurry.

9. A method for making and recycling a YSZ water-based cast sheet for a nitrogen oxygen sensor according to claim 1, Features: The particle size of the YSZ powder is 0.5-1 micron.

Citation Information

Patent Citations

  • Method for preparing ceramic sheet with composite caking agent series water-based cast

    CN101269977A

  • Zirconia ceramic blank return material processing method

    CN106187172A

  • Preparation method of water-based cast film tape for nitrogen-oxygen sensor

    CN115838284A

  • Preparation method of solid electrolyte cast film

    CN117417187A