High-barrier green PET composite material for food packaging and preparation method of high-barrier green PET composite material
By modifying the hydroxyl groups in PET polyester molecules to form hydrogen bonds and organic heterocyclic structures, combined with ethylene glycol titanium catalyst, the problem of insufficient barrier properties and heat resistance of PET films is solved, and high barrier properties and environmentally friendly food packaging is achieved Materials, suitable for high-temperature food and environmental protection needs.
Patent Information
- Application Number
- CN202411206656.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-05
AI Technical Summary
PET films are not well blocked in food packaging, especially in areas where high barrier properties are required. If juice drinks and beer are not suitable, and their glass transition temperature is low, they cannot be used in food packaging with higher temperatures. The antimony trioxide catalyst used during processing is not environmentally friendly.
By modifying the hydroxyl groups in PET polyester molecules to form hydrogen bonds to enhance the intermolecular action force, combining organic heterocyclic structures to increase the thermal decomposition temperature, and using ethylene glycol titanium instead of antimony trioxide catalyst, high barrier properties and heat resistance are prepared Green PET composite material.
It significantly improves the barrier properties and heat resistance of PET materials, extends the shelf life of food, and uses environmentally friendly materials during the processing process, which is suitable for fast food boxes, self-heating food packaging and juice beverage bottles.
Smart Images

Figure BDA0005019211510000021 
Figure BDA0005019211510000031 
Figure BDA0005019211510000041
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of food packaging materials, and in particular, relates to a high-barrier green PET composite material for food packaging and a preparation method thereof. Background Art
[0002] PET is a thermoplastic polyester, which is mainly synthesized by direct esterification of terephthalic acid and ethylene glycol or transesterification of dimethyl terephthalate and ethylene glycol. The annual output of PET polyester in the world exceeds 79 million tons, and it is one of the five major engineering plastics. PET film is widely used in the field of food packaging because of its non-toxicity, high transparency, good stability within the temperature range, and acid and alkali corrosion resistance. However, PET film has poor barrier properties due to its large intermolecular gap. In the field of packaging, oxygen transmission rate (OTR) and water vapor transmission rate (WVTR) are used internationally to judge the barrier properties of polymer materials. Among them, PET material has the highest barrier performance. OTR is 49-90cm3·mm / (m2·day·MPa), and WVTR is 18-30g·mm / (m2·day·MPa). The disadvantage of poor barrier properties limits the large-scale application of PET materials in food packaging, especially in the field of fruit juice drinks and beer, which require higher barrier properties. PET materials are usually not used for their packaging. Moreover, the glass transition temperature of PET materials is relatively low, generally around 70°C, so it cannot be used to contain liquids or foods at higher temperatures. In addition, antimony trioxide is usually required as a catalyst during the processing of PET materials, so it is not environmentally friendly. Summary of the invention
[0003] The purpose of the present invention is to provide a high-barrier green PET composite material for food packaging and a preparation method thereof. The characteristics of a large number of hydroxyl groups in modified PET polyester molecules that can form hydrogen bonds to enhance the intermolecular forces are utilized to reduce the gap between molecules to enhance the barrier properties of the PET material. The hydroxyl groups also have good antioxidant effects, which can enhance the antioxidant properties of the PET composite material. The characteristics of a high thermal decomposition temperature of an organic heterocyclic structure in the modified PET polyester molecules can be utilized to enhance the heat resistance of the PET composite material. At the same time, ethylene glycol titanium is used as a catalyst instead of antimony trioxide during processing to achieve the purpose of green environmental protection.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A high-barrier green PET composite material for food packaging, comprising the following raw materials in parts by weight: 60-65 parts of modified PET polyester, 10-15 parts of polylactic acid, 0.4-1 parts of titanium dioxide, 0.1-0.3 parts of oleic acid amide, 0.9-2 parts of PET-g-MAH, and 0.5-1 parts of ethylene glycol titanium;
[0006] A method for preparing a high-barrier green PET composite material for food packaging comprises the following steps:
[0007] Step 1, weighing and screening each raw material according to the corresponding mass fraction;
[0008] Step 2, heat treating and drying the modified PET polyester;
[0009] Step 3, mixing the raw materials in a twin-screw extruder, heating and melting, and then extruding to obtain the green PET composite material;
[0010] Furthermore, the temperature condition of the heat treatment in step 2 is 140-160° C. and the time condition is 2-3 h;
[0011] Furthermore, the temperature settings of the twin-screw extruder in step 3 are 210-220° C. in zone 1, 195-205° C. in zone 2, 180-190° C. in zone 3, and 175-185° C. in zone 4;
[0012] Furthermore, the preparation method of the modified PET polyester comprises the following steps:
[0013] Step 1, add allyl alcohol, sodium hydroxide solution, benzene and trichlorophloroglucinol into a three-necked flask, install a condenser and a thermometer, turn on the magnetic stirrer, react at 90° C. for 2 hours, and after the reaction is completed, separate the organic layer with a separatory funnel, and then obtain intermediate 1 by rotary evaporation;
[0014] The reaction process is as follows:
[0015]
[0016] Step 2, dimethyl sulfoxide and sodium hydroxide solution are mixed in a three-necked flask, a condenser and a thermometer are installed, a magnetic stirrer is turned on, and then intermediate 1, phthalimide and cuprous iodide are added thereto, argon gas is continuously introduced thereto for protection, and the reaction is carried out at 90° C. for 18 hours. After the reaction is completed, the organic layer is separated by a separatory funnel, column chromatography is performed, and rotary evaporation is performed to obtain intermediate 2;
[0017] The reaction process is as follows:
[0018]
[0019] Step 3, PET polyester, benzoyl peroxide and o-xylene are mixed in a three-necked flask, a condenser and a thermometer are installed, a magnetic stirrer is turned on, and the mixture is preheated at 120° C. for 0.5 h, and then intermediate 2 and benzoyl peroxide are added thereto, and the mixture is reacted at 120° C. for 5 h. After the reaction is completed, the mixture is repeatedly rinsed with anhydrous ethanol, extracted with acetone for 24 h, and dried to obtain modified PET polyester;
[0020] The reaction process is as follows:
[0021]
[0022] Further, the sodium hydroxide solution in step 1 is a sodium hydroxide aqueous solution with a mass fraction of 45-50%, and its dosage is 55-65g, and the dosage ratio of allyl alcohol, benzene and trichlorophloroglucinol used in step 1 is 5-5.8g:150-170g:22.9g;
[0023] Furthermore, the sodium hydroxide solution in step 2 is a sodium hydroxide aqueous solution with a mass fraction of 17%, and its dosage is 110g, and the dosage ratio of dimethyl sulfoxide, intermediate 1, phthalimide and cuprous iodide used is 220g:15g:20-23g:9.5g;
[0024] Furthermore, for the PET polyester used in step 3, the dosage ratio of the benzoyl peroxide, o-xylene, intermediate 2 added for the first time and the benzoyl peroxide added for the second time is 35g:0.3g:250-270g:6-8g:0.4g.
[0025] Beneficial effects of the present invention:
[0026] 1) The present invention prepares a modified PET polyester, and utilizes the hydroxyl groups contained in its structure to form hydrogen bonds between molecules to enhance the interaction between molecules and reduce the gap between molecules, so as to achieve the purpose of improving the barrier properties of the PET composite material;
[0027] 2) The present invention uses allyl alcohol and trichlorophloroglucinol as raw materials, and obtains intermediate 1 by a nucleophilic substitution reaction between hydroxyl and halogen atoms in a strong alkaline environment, obtains intermediate 2 by a CN coupling reaction of halogen and imine between intermediate 1 and phthalimide under the catalysis of cuprous iodide, and then grafts intermediate 2 on PET polyester under the action of initiator benzoyl peroxide to obtain a modified PET material; there are three -OH in intermediate 2, which can not only form hydrogen bonds to increase the intermolecular force to achieve the purpose of reducing the gap between PET molecules, but also play an antioxidant role, the two organic heterocyclic rings connected by it have large cohesive energy and high thermal decomposition temperature, which can increase the system rigidity of the molecule, and grafting it on PET polyester can solve the problem of large intermolecular gap of PET polyester, improve the barrier property of PET polyester after molding, and enhance the heat resistance of PET polyester, so that the food packaging made of PET polyester can withstand higher temperatures, and has antioxidant properties, which can delay the deterioration of food;
[0028] 3) Compared with traditional PET materials, the PET composite material of the present invention not only has excellent heat resistance, but also has good barrier properties and antioxidant properties, can delay deterioration and provide a longer protection period. In addition, the PET composite material of the present invention does not use antimony trioxide during processing, is green and environmentally friendly, and can be widely used in fast food boxes, self-heating food packaging, juice beverage bottles and other fields. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] A modified PET polyester is prepared by the following steps:
[0032] Step 1, 5 g of allyl alcohol, 55 g of 45% sodium hydroxide solution, 150 g of benzene and 22.9 g of trichlorophloroglucinol were added into a container, stirred, and reacted at 90° C. for 2 h. After the reaction was completed, the organic layer was separated with a separatory funnel, and then subjected to rotary evaporation to obtain intermediate 1;
[0033] Step 2, 220g of dimethyl sulfoxide and 110g of 17% sodium hydroxide solution are mixed in a container, stirred evenly, and then 15g of intermediate 1, 20g of phthalimide, and 9.5g of cuprous iodide are added thereto, and argon is continuously introduced thereto for protection, and the reaction is carried out at 90°C for 18h. After the reaction is completed, the organic layer is separated by a separating funnel, and the mixture is subjected to column chromatography and rotary evaporation to obtain intermediate 2;
[0034] Step 3, 35g PET polyester, 0.3g benzoyl peroxide and 250g o-xylene are mixed in a container, preheated at 120°C for 0.5h, and then 6g intermediate 2 and 0.4g benzoyl peroxide are added thereto, and the mixture is reacted at 120°C for 5h. After the reaction is completed, the mixture is repeatedly rinsed with anhydrous ethanol and extracted with acetone for 24h, and then dried to obtain modified PET polyester.
[0035] Example 2
[0036] A modified PET polyester is prepared by the following steps:
[0037] Step 1, 5.4 g of allyl alcohol, 60 g of 47% sodium hydroxide solution, 160 g of benzene and 22.9 g of trichlorophloroglucinol were added into a container, stirred, and reacted at 90° C. for 2 h. After the reaction was completed, the organic layer was separated with a separatory funnel, and then subjected to rotary evaporation to obtain intermediate 1;
[0038] Step 2, 220g of dimethyl sulfoxide and 110g of 17% sodium hydroxide solution are mixed in a container and stirred evenly, and then 15g of intermediate 1, 21.5g of phthalimide and 9.5g of cuprous iodide are added thereto, and argon gas is continuously introduced thereto for protection, and the reaction is carried out at 90°C for 18h. After the reaction is completed, the organic layer is separated by a separating funnel, and the mixture is subjected to column chromatography and rotary evaporation to obtain intermediate 2;
[0039] Step 3, 35g PET polyester, 0.3g benzoyl peroxide and 260g o-xylene are mixed in a container, preheated at 120°C for 0.5h, then 7g intermediate 2 and 0.4g benzoyl peroxide are added thereto, and the mixture is reacted at 120°C for 5h. After the reaction is completed, the mixture is repeatedly rinsed with anhydrous ethanol and extracted with acetone for 24h, and then dried to obtain modified PET polyester.
[0040] Example 3
[0041] A modified PET polyester is prepared by the following steps:
[0042] Step 1, 5.8 g of allyl alcohol, 65 g of 50% sodium hydroxide solution, 170 g of benzene and 22.9 g of trichlorophloroglucinol were added into a container, stirred, and reacted at 90° C. for 2 h. After the reaction was completed, the organic layer was separated with a separatory funnel, and then subjected to rotary evaporation to obtain intermediate 1;
[0043] Step 2, 220g of dimethyl sulfoxide and 110g of 17% sodium hydroxide solution are mixed in a container, stirred evenly, and then 15g of intermediate 1, 23g of phthalimide and 9.5g of cuprous iodide are added thereto, argon is continuously introduced thereto for protection, and the reaction is carried out at 90°C for 18h. After the reaction is completed, the organic layer is separated by a separating funnel, and the mixture is subjected to column chromatography and rotary evaporation to obtain intermediate 2;
[0044] Step 3, 35g PET polyester, 0.3g benzoyl peroxide and 270g o-xylene are mixed in a container, preheated at 120°C for 0.5h, then 8g intermediate 2 and 0.4g benzoyl peroxide are added thereto, and the mixture is reacted at 120°C for 5h. After the reaction is completed, the mixture is repeatedly rinsed with anhydrous ethanol and extracted with acetone for 24h, and then dried to obtain modified PET polyester.
[0045] Comparative Example 1
[0046] This comparative example is a PET film sold by Dongguan Zhonglian Electronic Materials Co., Ltd.
[0047] After Example 1, Example 2, and Example 3 were processed into films, the oxygen transmission rate (OTR) and water vapor transmission rate (WVTR) were tested together with the PET film of Comparative Example 1 using an oxygen transmission rate meter and a water vapor transmission rate meter;
[0048] The test results are shown in Table 1:
[0049] Table 1
[0050]
[0051]
[0052] It can be seen from Table 1 that the oxygen transmission rate (OTR) and water vapor transmission rate (WVTR) of the films prepared in Examples 1-3 are much lower than that of Comparative Example 1, indicating that the films prepared in Examples 1-3 have good barrier properties and can effectively block external oxygen and water vapor. Therefore, the prepared food packaging can also have a longer shelf life.
[0053] Example 4
[0054] A high-barrier green PET composite material for food packaging, comprising the following raw materials in parts by weight: 60 parts of modified PET polyester, 10 parts of polylactic acid, 0.4 parts of titanium dioxide, 0.1 parts of oleamide, 0.9 parts of PET-g-MAH, and 0.5 parts of titanium glycolate;
[0055] A method for preparing a high-barrier green PET composite material for food packaging comprises the following steps:
[0056] Step 1, weighing and screening each raw material according to the corresponding mass fraction;
[0057] Step 2, heat treating the modified PET polyester at 140° C. for 2 h and drying;
[0058] Step 3, mixing the raw materials in a twin-screw extruder, heating and melting, and then extruding to obtain the green PET composite material, the temperature settings of the twin-screw extruder are 210° C. in zone 1, 195° C. in zone 2, 180° C. in zone 3, and 175° C. in zone 4.
[0059] Example 5
[0060] A high-barrier green PET composite material for food packaging, comprising the following raw materials in parts by weight: 65 parts of modified PET polyester, 15 parts of polylactic acid, 0.4 parts of titanium dioxide, 0.1 parts of oleamide, 0.9 parts of PET-g-MAH, and 0.5 parts of titanium glycolate;
[0061] A method for preparing a high-barrier green PET composite material for food packaging comprises the following steps:
[0062] Step 1, weighing and screening each raw material according to the corresponding mass fraction;
[0063] Step 2, heat treating the modified PET polyester at 150° C. for 2.5 h and drying;
[0064] Step 3, mixing the raw materials in a twin-screw extruder, heating and melting, and then extruding to obtain the green PET composite material, the temperature settings of the twin-screw extruder are 215° C. in zone 1, 200° C. in zone 2, 185° C. in zone 3, and 180° C. in zone 4.
[0065] Example 6
[0066] A high-barrier green PET composite material for food packaging, comprising the following raw materials in parts by weight: 60 parts of modified PET polyester, 10 parts of polylactic acid, 1 part of titanium dioxide, 0.3 parts of oleamide, 2 parts of PET-g-MAH, and 1 part of titanium glycolate;
[0067] A method for preparing a high-barrier green PET composite material for food packaging comprises the following steps:
[0068] Step 1, weighing and screening each raw material according to the corresponding mass fraction;
[0069] Step 2, heat treating the modified PET polyester at 140° C. for 2 h and drying;
[0070] Step 3, mixing the raw materials in a twin-screw extruder, heating and melting them, and then extruding them to obtain the green PET composite material. The temperature settings of the twin-screw extruder are 210-220° C. for zone 1, 195-205° C. for zone 2, 180-190° C. for zone 3, and 175-185° C. for zone 4.
[0071] Comparative Example 2
[0072] This comparative example is the PET raw material for food packaging sold by Suzhou Yesu International Trade Co., Ltd.
[0073] The PET composite materials obtained in Examples 4-6 and the PET raw material for food packaging in Comparative Example 2 were respectively subjected to heat resistance tests, use temperature tests and 4h oxidation weight gain tests;
[0074] Heat resistance test: The plastic cups made from Examples 4-6 and Comparative Example 2 were heated respectively to test their glass transition temperatures;
[0075] Antioxidation performance test: The PET materials of Examples 4-6 and Comparative Example 2 were placed in a box-type resistance furnace and subjected to an oxidation weight gain test at 50°C for 4 hours, and the oxidation weight gain was recorded;
[0076] The test results are shown in Table 2:
[0077] Table 2
[0078] project Glass transition temperature(℃) <![CDATA[Weight gain after 4h oxidation (mg / mm 2 )]]> Example 4 87 <![CDATA[0.19X10 -3 ]]> Example 5 89 <![CDATA[0.28X10 -3 ]]> Example 6 86 <![CDATA[0.23X10 -3 ]]> Comparative Example 2 73 <![CDATA[0.98X10 -1 ]]>
[0079] It can be seen from Table 2 that the glass transition temperature of the plastic cup made of the PET composite materials of Examples 4-6 is much higher than that of the plastic cup made of the PET raw material of Comparative Example 2, indicating that the PET composite materials of the present invention have good heat resistance and can withstand higher temperatures after being made into food packaging compared to general PET raw materials. The oxidation weight gain of the PET composite materials of Examples 4-6 after 4 hours is much smaller than that of the PET raw material of Comparative Example 2, indicating that the PET raw material of the present invention also has higher oxidation resistance than general PET raw materials. Therefore, after being made into food packaging, it can provide a longer shelf life and can be widely used in fast food boxes, self-heating food packaging, juice beverage bottles and other fields.
[0080] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A high barrier green PET composite material for food packaging, characterized in that: The raw materials include: modified PET polyester, polylactic acid, titanium dioxide, oleamide, PET-g-MAH and titanium glycol; Among them, the modified PET polyester is made by the following steps: Step 1, adding allyl alcohol, sodium hydroxide solution, benzene and trichlorophloroglucinol into a container, and reacting at 90° C. for 2 h to obtain intermediate 1; Step 2, dimethyl sulfoxide and sodium hydroxide solution are mixed in a container, intermediate 1, phthalimide and cuprous iodide are added thereto, inert gas is continuously introduced thereto for protection, and the mixture is reacted at 90° C. for 18 hours to obtain intermediate 2; Step 3, PET polyester, benzoyl peroxide and o-xylene are mixed in a container, preheated at 120° C. for 0.5 h, and then intermediate 2 and benzoyl peroxide are added thereto, and reacted at 120° C. for 5 h to obtain modified PET polyester.
2. The high barrier green PET composite material for food packaging according to claim 1, characterized in that: The sodium hydroxide solution in step 1 is a sodium hydroxide aqueous solution with a mass fraction of 45-50%, and its usage is 55-65g.
3. The high barrier green PET composite material for food packaging according to claim 1, characterized in that: The usage ratio of allyl alcohol, benzene and trichlorophloroglucinol used in step 1 is 5-5.8g:150-170g:22.9g.
4. The high barrier green PET composite material for food packaging according to claim 1, characterized in that: The sodium hydroxide solution in step 2 is a sodium hydroxide aqueous solution with a mass fraction of 17%, and its usage is 110g.
5. The high barrier green PET composite material for food packaging according to claim 1, characterized in that: The amount ratio of dimethyl sulfoxide, intermediate 1, phthalimide and cuprous iodide used is 220g:15g:20-23g:9.5g.
6. The high barrier green PET composite material for food packaging according to claim 1, characterized in that: The amount ratio of the PET polyester used in step 3, the benzoyl peroxide added for the first time, o-xylene, intermediate 2 and the benzoyl peroxide added for the second time is 35g:0.3g:250-270g:6-8g:0.4g.
7. The high barrier green PET composite material for food packaging according to claim 1, characterized in that: The mass proportions of each component are as follows: 60-65 parts of modified PET polyester, 10-15 parts of polylactic acid, 0.4-1 parts of titanium dioxide, 0.1-0.3 parts of oleic acid amide, 0.9-2 parts of PET-g-MAH, and 0.5-1 parts of titanium glycol.
8. A method for preparing a high barrier green PET composite material for food packaging, characterized in that: The following steps are involved: Step 1, weighing and screening each raw material according to the corresponding mass fraction; Step 2, heat treating and drying the modified PET polyester; Step 3, mixing the raw materials in a twin-screw extruder, heating and melting, and then extruding to obtain the green PET composite material.
9. The method for preparing a high barrier green PET composite material for food packaging according to claim 8, characterized in that: In step 2, the temperature condition for the heat treatment of PET polyester is 140-160° C. and the time condition is 2-3 hours.
10. The method for preparing a high barrier green PET composite material for food packaging according to claim 8, characterized in that: The temperature settings of the twin-screw extruder in step 3 are 210-220° C. in zone 1, 195-205° C. in zone 2, 180-190° C. in zone 3, and 175-185° C. in zone 4.