LCP resin composition for circuit board, LCP film for circuit board, and method for producing same
By pressurized heating treatment of liquid crystal polyester and oxazoline group-containing LCP resin composition, the problem of large linear expansion coefficient of liquid crystal polymer resin in circuit substrate insulating materials is solved, dimensional stability and adhesion are improved, and the dimensional stability and adhesion are achieved. Efficient preparation of circuit substrate material.
Patent Information
- Application Number
- CN202410945430.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-29
- Filing Date
- 2020-11-20
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When used as an insulating material for circuit substrates such as flexible printed wiring boards, it is difficult to maintain mechanical characteristics, electrical characteristics and heat resistance. At the same time, the linear expansion coefficient is large, which affects dimensional stability. and closeness.
By using an LCP resin composition composed of liquid crystal polyester and an oxazoline group-containing polymer, melt extrusion and pressurized heating treatment, the linear expansion coefficient is reduced, and dimensional stability and adhesion are improved.
On the basis of maintaining excellent mechanical characteristics, electrical characteristics and heat resistance, the linear expansion coefficient is significantly reduced, the dimensional stability of the LCP film for circuit substrates and its adhesion to metal foil are improved, and productivity and economy are improved.
Smart Images

Figure CN118895039A_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese invention patent application No. 202080075177.1 (PCT application number is PCT / JP2020 / 043340), whose application date is November 20, 2020 and whose invention name is "LCP resin composition for circuit substrate, LCP film for circuit substrate and its manufacturing method". Technical Field
[0002] The present invention relates to an LCP resin composition for a circuit board, an LCP film for a circuit board, a method for producing the same, and the like. Background Art
[0003] Liquid crystal polymer (LCP) is a polymer that exhibits liquid crystal properties in a molten state or a solution state. In particular, thermotropic liquid crystal polymers that exhibit liquid crystal properties in a molten state have excellent properties such as high gas barrier properties, high film strength, high heat resistance, high insulation, and low water absorption, and therefore, their practical use is rapidly progressing in gas barrier film material applications, electronic material applications, and electrical insulation material applications.
[0004] As a resin composition using a liquid crystal polymer, for example, Patent Document 1 discloses a liquid crystal polyester resin composition, which is formed by (A) a liquid crystal polyester and (B) an oxazolyl-containing polymer, and the ratio of component (A) to component (B) is as follows: component (A) is 99.9 to 0.1% by weight, and component (B) is 0.1 to 99.9% by weight.
[0005] In addition, as a resin composition using a liquid crystal polymer, for example, Patent Document 2 discloses a polymer alloy characterized in that it is formed by 97.1 to 99.0 weight % of a thermoplastic polymer capable of forming an optically anisotropic molten phase and 1.0 to 2.9 weight % of an amorphous polymer (based on the total amount of the polymer).
[0006] On the other hand, for example, Patent Document 3 discloses a liquid crystal polymer blended film, characterized in that it is a film formed by a blend of a liquid crystal polymer and at least one thermoplastic resin selected from polyethersulfone, polyetherimide, polyamideimide, polyetheretherketone, polyarylate and polyphenylene sulfide, the proportion of the thermoplastic resin in the blend is 25 to 55% by weight, the linear expansion coefficient of the film in the MD and TD directions is 5 to 25 ppm / K, and the linear expansion coefficient of the film in the thickness direction exceeds 270 ppm / K.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 09-286903
[0010] Patent Document 2: Japanese Patent Application Publication No. 2000-290512
[0011] Patent Document 3: Japanese Patent Application Publication No. 2004-175995 Summary of the invention
[0012] Problems to be solved by the invention
[0013] LCP resin compositions using liquid crystal polymers, especially liquid crystal polyesters, have excellent high-frequency characteristics and low dielectric properties. Therefore, they have attracted attention in recent years as insulating materials for circuit substrates such as flexible printed wiring boards (FPCs), flexible printed wiring board laminates, and fiber-reinforced flexible laminates in the fifth-generation mobile communication systems (5G) and millimeter-wave radars to be developed in the future.
[0014] However, in Patent Document 1, the gas barrier properties and mechanical strength of the LCP resin composition are focused on, and only the application to gas barrier molded products, containers, tubes, sheets, fibers, coating materials, electronic material packaging films, etc. is studied, and there is no study on the applicability as an insulating material for flexible printed wiring boards (FPCs), etc.
[0015] In addition, although Patent Document 2 mentions the usefulness of LCP resin compositions as electrical insulating materials and circuit board materials, in reality, only proposals for improving the mechanical strength (end tear strength, i.e., strength against defects and breakages occurring at the ends of the film, etc.) of the LCP film are made.
[0016] On the other hand, in Patent Document 3, a liquid crystal polymer blended film having no anisotropy in the linear expansion coefficient in the plane direction (TD direction and MD direction) and a small linear expansion coefficient in the thickness direction is obtained by melt-extruding a resin composition of a liquid crystal polymer and a specific thermoplastic resin from a T-die to obtain an LCP blended film and then biaxially stretching the film. However, since the obtained liquid crystal polymer blended film contains a large amount of thermoplastic resins such as polyarylate, it becomes a film with reduced heat resistance, dielectric properties, tensile strength, etc., and has poor practicality.
[0017] The present invention is made in view of the above-mentioned problems. The purpose of the present invention is to provide an LCP film for circuit substrates, an LCP resin composition for circuit substrates, etc., which can realize a circuit substrate with a small linear expansion coefficient and excellent dimensional stability without excessively damaging the excellent basic properties of liquid crystal polyester such as mechanical properties, electrical properties, and heat resistance.
[0018] In addition, another object of the present invention is to provide an LCP film for circuit boards and a method for producing the same which does not excessively impair the excellent basic properties of liquid crystal polyester such as mechanical properties, electrical properties, and heat resistance, and which has a small linear expansion coefficient and excellent dimensional stability.
[0019] Means for solving problems
[0020] The inventors of the present application have conducted intensive research to solve the above-mentioned problems, and have found that by using a specified LCP resin composition and by pressurizing and heating the LCP film obtained by melt-extruding the specified LCP resin composition, the linear expansion coefficient can be made small, thereby improving the dimensional stability and the adhesion with the metal foil. The inventors have found that this can solve the above-mentioned problems, thereby completing the present invention.
[0021] That is, the present invention provides various specific aspects shown below.
[0022] (1) A method for producing an LCP film for a circuit substrate, characterized in that it comprises at least the following steps: a composition preparation step of preparing an LCP resin composition containing at least 100 parts by weight of a liquid crystal polyester and 1 to 20 parts by weight of an oxazoline-containing polymer; a film forming step of melt-extruded the LCP resin composition to form an LCP film having a linear expansion coefficient (α2) of 50 ppm / K or more in the TD direction; and a pressurizing and heating step of pressurizing and heating the LCP film to obtain an LCP film for a circuit substrate having a linear expansion coefficient (α2) of 16.8±12 ppm / K in the TD direction.
[0023] (2) The method for producing an LCP film for a circuit board according to (1), wherein the LCP resin composition further contains 1 to 20 parts by mass of a polyarylate.
[0024] (3) The method for producing an LCP film for a circuit board according to (1) or (2), wherein the tensile elastic modulus Y of the LCP film in the MD direction is MD Tensile elastic modulus Y in TD direction TD The ratio (Y MD / Y TD ) is 2 or more and 10 or less, in the aforementioned pressurizing and heating step, the aforementioned LCP film is pressurized and heated to obtain a tensile elastic modulus Y in the MD direction MD Tensile elastic modulus Y in TD direction TD The ratio (Y MD / Y TD ) is not less than 0.8 and not more than 2.0.
[0025] (4) A method for manufacturing an LCP film for a circuit substrate as described in any one of (1) to (3), wherein, in the aforementioned pressurization and heating step, the aforementioned LCP film is subjected to a pressurization and heating treatment to obtain an LCP film for a circuit substrate having a linear expansion coefficient in the TD direction of not less than 5.0 ppm / K and not more than 16.0 ppm / K.
[0026] (5) The method for producing an LCP film for a circuit board according to any one of (1) to (4), wherein the LCP film has a thickness of 10 μm to 500 μm.
[0027] (6) The method for producing an LCP film for a circuit board according to any one of (1) to (5), wherein the LCP film for a circuit board has a relative dielectric constant ε r The dielectric properties (36 GHz) are 3.0 to 3.9 and the dielectric loss tangent tanδ is 0.0005 to 0.003.
[0028] (7) An LCP resin composition for a circuit board, comprising at least 100 parts by mass of a liquid crystal polyester and 1 to 20 parts by mass of an oxazoline group-containing polymer.
[0029] (8) The LCP resin composition for circuit boards according to (7), wherein the LCP resin composition further contains 1 to 20 parts by mass of polyarylate.
[0030] (9) An LCP film for a circuit board, comprising at least 100 parts by weight of a liquid crystal polyester and 1 to 20 parts by weight of an oxazoline group-containing polymer, wherein the linear expansion coefficient (α2) in the TD direction of the LCP film for a circuit board is 16.8±12 ppm / K.
[0031] (10) The LCP film for a circuit board according to (9), further comprising 1 to 20 parts by mass of polyarylate.
[0032] (11) The LCP film for circuit board according to (9) or (10), wherein the tensile elastic modulus Y in the MD direction is MD Tensile elastic modulus Y in TD direction TD The ratio (Y MD / Y TD ) is greater than 0.8 and less than 2.0.
[0033] (12) The LCP film for a circuit board according to any one of (9) to (11), wherein the linear expansion coefficient of the LCP film in the TD direction is 5.0 ppm / K or more and 16.0 ppm / K or less.
[0034] (13) The LCP film for a circuit board according to any one of (9) to (12), which has a relative dielectric constant ε r The dielectric properties (36 GHz) are 3.0 to 3.9 and the dielectric loss tangent tanδ is 0.0005 to 0.003.
[0035] (14) The LCP film for a circuit board according to any one of (9) to (13), which has a thickness of 10 μm to 500 μm.
[0036] Effects of the Invention
[0037] According to the present invention, it is possible to provide an LCP film for circuit substrates and a method for manufacturing the same, which reduces the linear expansion coefficient and improves the dimensional stability without excessively damaging the excellent basic properties of liquid crystal polyester such as mechanical properties, electrical properties, high-frequency properties, and heat resistance. In addition, according to a preferred embodiment of the present invention, it is possible to easily and reproducibly provide an LCP film for circuit substrates that not only has excellent basic properties such as mechanical properties, electrical properties, high-frequency properties, and heat resistance, but also has small anisotropy in the film surface direction and can improve the adhesion with metal foil, thereby improving productivity and economy. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] [ Figure 1 ] is a flow chart showing a method for manufacturing an LCP film 11 for a circuit substrate according to one embodiment.
[0039] [ Figure 2 ] is a schematic diagram showing an LCP film 11 for a circuit substrate according to one embodiment.
[0040] [ Figure 3 ] is a schematic diagram showing a laminated plate 31 covered with a metal foil according to one embodiment. DETAILED DESCRIPTION
[0041] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. It should be noted that, unless otherwise specified, positional relationships such as up, down, left, and right are based on the positional relationships shown in the accompanying drawings. In addition, the dimensional ratios of the accompanying drawings are not limited to the ratios shown in the drawings. Among them, the following embodiments are examples for illustrating the present invention, and the present invention is not limited to these. That is, the present invention can be implemented with arbitrary changes within the scope of the subject matter. It should be noted that in this specification, the expression of a numerical range such as "1 to 100" includes both its lower limit "1" and upper limit "100". In addition, the expression of other numerical ranges is the same.
[0042] (LCP film)
[0043] Figure 1 2 is a flowchart showing a method for manufacturing the LCP film 11 for a circuit board according to the present embodiment. Figure 2 It is a schematic diagram showing the outline of the LCP film 11 for circuit boards of this embodiment.
[0044] The manufacturing method of this embodiment comprises at least the following steps: a composition preparation step (S1), preparing a specified LCP resin composition; a film forming step (S2), melt-extruding the LCP resin composition to form a specified LCP film; and a pressurizing and heating step (S3), performing a pressurizing and heating treatment on the LCP film to obtain a specified LCP film 11 for a circuit substrate.
[0045] <Composition preparation step (S1)>
[0046] In the composition preparation step (S1), an LCP resin composition containing at least 100 parts by mass of a liquid crystal polyester as a liquid crystal polymer and 1 to 20 parts by mass of an oxazoline group-containing polymer is prepared.
[0047] As liquid crystal polyesters, liquid crystal polyesters known in the industry can be used, and their types are not particularly limited. It is preferred to use liquid crystal polyesters that show thermotropic liquid crystal properties and have a melting point of 250°C or more, preferably a melting point of 280°C to 380°C. As such liquid crystal polyesters, aromatic polyesters synthesized from monomers such as aromatic diols, aromatic carboxylic acids, and hydroxycarboxylic acids that show liquid crystal properties when melted are known. As representative examples thereof, polycondensates of ethylene terephthalate and p-hydroxybenzoic acid, polycondensates of phenol and phthalic acid and p-hydroxybenzoic acid, polycondensates of 2,6-hydroxynaphthoic acid and p-hydroxybenzoic acid, etc. can be cited, but are not particularly limited thereto. It should be noted that the liquid crystal polyesters can be used alone, or two or more can be used in any combination and ratio.
[0048] Among the liquid crystal polyesters, from the viewpoint of excellent basic properties such as mechanical properties, electrical properties, and heat resistance, an aromatic polyester-based liquid crystal polymer having 6-hydroxy-2-naphthoic acid and its derivatives (hereinafter sometimes referred to as "monomer component A") as a basic structure and having at least one or more selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate and their derivatives (hereinafter sometimes referred to as "monomer component B") as a monomer component is preferred.
[0049] For the aromatic polyester liquid crystal polymer containing the above-mentioned monomer component A and monomer component B, the linear chains of the molecules are regularly arranged in the molten state to form an anisotropic melt phase, typically showing thermotropic liquid crystal properties, and having excellent basic properties in terms of mechanical properties, electrical properties, high-frequency properties, heat resistance, hygroscopicity, etc. It should be noted that the properties of the anisotropic melt phase of the above-mentioned aromatic polyester liquid crystal polymer can be confirmed by known methods such as polarization inspection using orthogonal polarizers. More specifically, the confirmation of the anisotropic melt phase can be implemented in the following manner: using a Leitz polarizing microscope, in a nitrogen atmosphere, the sample placed on the Leitz hot stage is observed at a magnification of 40 times.
[0050] The above-mentioned aromatic polyester-based liquid crystal polymer can have any structure as long as it has monomer component A and monomer component B as essential units. For example, it can have more than two monomer components A, or more than three monomer components A. In addition, the above-mentioned aromatic polyester-based liquid crystal polymer can also contain other monomer components other than monomer components A and monomer component B. That is, the aromatic polyester-based liquid crystal polymer can be a condensation product of more than two monomer components formed only by monomer components A and monomer component B, or a condensation product of more than three monomer components formed by monomer components A, monomer component B and other monomer components. As other monomer components (hereinafter, sometimes referred to as "monomer component C"), monomer components other than the above-mentioned monomer components A and monomer component B can be cited, specifically aromatic or aliphatic dihydroxy compounds and their derivatives; aromatic or aliphatic dicarboxylic acids and their derivatives; aromatic hydroxycarboxylic acids and their derivatives; aromatic diamines, aromatic hydroxyamines or aromatic aminocarboxylic acids and their derivatives; etc., but are not particularly limited to these.
[0051] It should be noted that, in the present specification, the term "derivative" refers to a group in which a halogen atom (e.g., fluorine atom, chlorine atom, bromine atom, iodine atom), an alkyl group having 1 to 5 carbon atoms (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, etc.), an aryl group such as phenyl, a hydroxyl group, an alkoxy group having 1 to 5 carbon atoms (e.g., methoxy, ethoxy, etc.), a carbonyl group, -O-, -S-, -CH 2 - or the like (hereinafter, sometimes referred to as "monomer component having a substituent"). Here, the "derivative" may also be an ester-forming monomer such as an acylate, an ester derivative, or an acyl halide of the monomer components A and B which may have the above-mentioned modifying groups.
[0052] More preferred aromatic polyester liquid crystal polymers include: binary polycondensates of p-hydroxybenzoic acid and its derivatives and 6-hydroxy-2-naphthoic acid and its derivatives; ternary or higher polycondensates of p-hydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, and monomer component C; polycondensates of p-hydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, and a monomer component C selected from terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-diphenol, 4-hydroxy-2-naphthoic acid ... A ternary or higher polycondensate formed from one or more of the group consisting of hydroxydiphenol, ethylene terephthalate and their derivatives; a quaternary or higher polycondensate formed from one or more of p-hydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxydiphenol, ethylene terephthalate and their derivatives and one or more monomer components C. These can be obtained as substances having a lower melting point than, for example, a homopolymer of p-hydroxybenzoic acid, and therefore, an LCP film using these becomes a film having excellent molding processability during thermal compression bonding to an adherend.
[0053] From the viewpoint of lowering the melting point of the aromatic polyester-based liquid crystal polymer, improving the molding processability when the LCP film is thermally pressed to the adherend, or obtaining high peel strength when the LCP film is thermally pressed to the metal foil, the molar ratio of the content of the monomer component A relative to the aromatic polyester-based liquid crystal polymer is preferably 10 mol% to 70 mol%, more preferably 10 mol% to 50 mol%, further preferably 10 mol% to 40 mol%, more preferably 15 mol% to 30 mol%. Similarly, the molar ratio of the content of the monomer component B relative to the aromatic polyester-based liquid crystal polymer is preferably 30 mol% to 90 mol%, more preferably 50 mol% to 90 mol%, further preferably 60 mol% to 90 mol%, more preferably 70 mol% to 85 mol%.
[0054] The content of the monomer component C in the aromatic polyester-based liquid crystal polymer is preferably 10% by mass or less, more preferably 8% by mass or less, further preferably 5% by mass or less, and preferably 3% by mass or less in terms of molar ratio.
[0055] It should be noted that the synthesis method of the liquid crystal polyester can be applied by known methods, and is not particularly limited. Known polycondensation methods, such as melt polymerization, melt acidolysis, slurry polymerization, etc., which form ester bonds generated by the above-mentioned monomer components, can be applied. When these polymerization methods are applied, they can be acylated or acetylated according to conventional methods.
[0056] The polymer containing oxazoline groups is a polymer having at least 2 or more oxazoline groups in the molecule. By containing the polymer containing oxazoline groups, the anisotropy of the film in-plane direction of the LCP film produced in the film forming process (S2) can be effectively reduced by crosslinking with the liquid crystal polyester or compatibilization promotion with the liquid crystal polyester in the pressurized heating process (S3). The polymer containing oxazoline groups can be appropriately selected from known polymers and used, and its type is not particularly limited. For example, the polymerization of monomers containing oxazoline compounds with polymerizable groups such as 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline and 2-isopropenyl-2-oxazoline, the copolymerization of unsaturated monomers containing oxazoline groups and vinyl monomers (such as styrene and / or acrylonitrile), the graft copolymerization of unsaturated monomers containing oxazoline groups and thermoplastic resins (such as polystyrene, styrene-acrylonitrile copolymers) other than liquid crystal polyester and liquid crystal polyester resin composition, etc. can be obtained. In addition, oxazoline-based polymers have been used in various purposes such as properties-correcting agent, crosslinking agent of thermoplastic resins, can suitably select and use from these known polymers.As the commercially available product of the polymer containing oxazoline-based, for example Epocros (registered trademark), Epocros (registered trademark) RPS series, Epocros (registered trademark) RAS series etc. of Nippon Catalyst Co., Ltd. system are commercially available.It should be noted that the polymer containing oxazoline-based can use 1 kind separately respectively, or uses more than 2 kinds with arbitrary combination and ratio.
[0057] The total content ratio of the above-mentioned oxazoline-containing polymer can be appropriately set according to the desired performance, without particular limitation, and is preferably 1 to 20 parts by mass, more preferably 1 to 15 parts by mass, and further preferably 1.5 to 10 parts by mass, relative to the total amount of 100 parts by mass of the LCP resin composition, according to the solid content conversion. By making the content ratio of the oxazoline-containing polymer within the above-mentioned preferred range, there is a tendency to effectively play the effect of reducing the anisotropy of the film surface direction of the LCP film. If the content ratio of the oxazoline-containing polymer exceeds the above-mentioned preferred range, the content ratio of the liquid crystal polyester is relatively reduced, and there is a tendency to reduce the basic performances such as mechanical properties, electrical properties, high-frequency properties, and heat resistance. Therefore, the balance between the effect of reducing anisotropy brought about by the present invention and the reduction of the basic performance of the liquid crystal polyester can be considered, and the content ratio of the oxazoline-containing polymer is adjusted.
[0058] In addition, the LCP resin composition of the present embodiment preferably contains polyarylate in addition to the above-mentioned liquid crystal polyester and the polymer containing oxazoline group. By containing polyarylate as a non-crystalline polymer, it can be effectively reduced by promoting compatibilization with liquid crystal polyester in the pressurized heating process (S3). As polyarylate, it can be appropriately selected from known polyarylates and used, and its type is not particularly limited. For example, it is preferably an amorphous polyester carbonate composed of aromatic dicarboxylic acid units such as isophthalic acid, terephthalic acid or their mixtures, and diphenol units such as bisphenol. In addition, as a commercial product of polyarylate, for example, U-POLYMER (registered trademark) made by Unitika Co., Ltd., Durer (registered trademark) made by Celanese Co., Ltd. in the United States, etc. are known. It should be noted that polyarylate can be used alone or in any combination and ratio.
[0059] The total content ratio of the above-mentioned polyarylate can be appropriately set according to the desired performance, without particular limitation, and is preferably 1 to 20 parts by mass, more preferably 1 to 15 parts by mass, and further preferably 1.5 to 10 parts by mass, relative to the total amount of 100 parts by mass of the LCP resin composition, in terms of solid content conversion. By making the content ratio of the polyarylate within the above-mentioned preferred range, there is a tendency to effectively exert the effect of reducing the anisotropy of the film surface direction of the LCP film. If the content ratio of the polyarylate exceeds the above-mentioned preferred range, the content ratio of the liquid crystal polyester and the oxazoline-containing polymer is relatively reduced, and there is a tendency that the basic properties such as mechanical properties, electrical properties, high-frequency properties, and heat resistance are reduced, or the effect of reducing anisotropy brought about by the present invention is reduced. Therefore, the balance between the effect of reducing anisotropy brought about by the present invention and the reduction of the basic properties of the liquid crystal polyester can be considered, and the content ratio of the polyarylate is adjusted.
[0060] It should be noted that, in addition to the above-mentioned components, the LCP resin composition of the present embodiment may also include additives known in the industry, such as higher fatty acids with carbon atoms of 10 to 25, higher fatty acid esters, higher fatty acid amides, higher fatty acid metal salts, polysiloxanes, fluororesins and other release modifiers within the scope of not excessively damaging the effect of the present invention; colorants such as dyes, pigments, and carbon black; organic fillers; inorganic fillers; antioxidants; heat stabilizers; light stabilizers; ultraviolet absorbers; flame retardants; lubricants; antistatic agents; surfactants; rust inhibitors; foaming agents; defoamers; fluorescent agents, etc. These additives can be included in the molten resin composition during the film formation of the LCP film. These additives can be used alone or in combination of two or more. The content of the additive is not particularly limited, but from the viewpoints of molding processability, thermal stability, etc., it is preferably 0.01 to 10% by mass, more preferably 0.1 to 7% by mass, and further preferably 0.5 to 5% by mass relative to the total amount of the LCP film.
[0061] The preparation of the LCP resin composition of the present embodiment can be carried out according to conventional methods without special limitations. The above-mentioned components can be manufactured and processed by known methods such as kneading, melt mixing, granulation, extrusion molding, pressurization or injection molding. It should be noted that when melt kneading is performed, kneading devices such as commonly used single-screw or twin-screw extruders, various kneading machines, etc. can be used. When supplying each component to these melt kneading devices, liquid crystal polyesters, polymer materials, etc. can be dry mixed in advance using mixing devices such as rollers and Henschel mixers. During melt kneading, the barrel setting temperature of the kneading device can be appropriately set, without special limitations, and is usually preferably in the range of 360°C above the melting point of the liquid crystal polyester, and more preferably above the melting point of the liquid crystal polyester + 10°C and below 360°C.
[0062] <Film forming step (S2)>
[0063] In the film forming process (S2), the above-mentioned LCP resin composition is formed into a film by a known melt extrusion film-making method such as a T-die method to form an LCP film having a linear expansion coefficient (α2) of 50 ppm / K or more in the TD direction. It should be noted that in this specification, the linear expansion coefficient refers to the following value: in order to check the value after the thermal history is eliminated, the LCP film or the circuit substrate LCP film 11 is heated at a heating rate of 5°C / min (first heating (1st heating)), cooled to the measurement environment temperature (23°C) (first cooling (1st cooling)), and then heated for the second time (second heating (2nd heating)) at a heating rate of 5°C / min. In addition, with respect to the others, the measurement conditions described in the embodiments described later are followed.
[0064] Specifically, for example, the above-mentioned LCP resin composition can be melt-kneaded by an extruder, and the molten resin can be extruded through a nozzle (such as a T-die) to obtain an LCP film. At this time, it is also possible to dry-mix the components in advance without going through the process of melt-kneading, knead them during the operation of melt extrusion, and directly obtain the LCP film while preparing the LCP resin composition. The setting conditions of the extruder during such film-making can be appropriately set according to the type and composition of the LCP resin composition used, the desired performance of the target LCP film, etc., and are not particularly limited. Usually, the setting temperature of the barrel of the extruder is preferably 230 to 360°C, and more preferably 280 to 350°C. In addition, for example, the slit gap of the T-die can also be appropriately set according to the type and composition of the LCP resin composition used, the desired performance of the target LCP film, etc., and is not particularly limited. It is usually preferably 0.1 to 1.5 mm, and more preferably 0.1 to 0.5 mm.
[0065] The thickness of the obtained LCP film can be appropriately set according to the required performance, and is not particularly limited. Considering the operability and productivity during T-die melt extrusion molding, it is preferably from 10 μm to 500 μm, more preferably from 20 μm to 300 μm, and further preferably from 30 μm to 250 μm.
[0066] The melting point (melting temperature) of the LCP film is not particularly limited, but from the viewpoints of the heat resistance and processability of the film, the melting point (melting temperature) is preferably 200-400°C, especially from the viewpoint of improving the thermal compression bonding to the metal foil, preferably 250-360°C, more preferably 260-355°C, further preferably 270-350°C, and particularly preferably 275-345°C. It should be noted that in this specification, the melting point of the LCP film refers to: in order to check the value of the thermal history eliminated, the LCP film for compression bonding is heated at a heating rate of 20°C / min (first heating), cooled at a cooling rate of 50°C / min (first cooling), and then heated for the second time (second heating) at a heating rate of 20°C / min. The melting peak temperature in the differential scanning calorimetry (DSC). In addition, with respect to the others, the measurement conditions described in the embodiments described later are followed.
[0067] When the LCP resin composition is melt-extruded and the LCP film is subjected to T-die melt extrusion molding, typically, an LCP film having a linear expansion coefficient (CTE, α2) of -40 to 40 ppm / K in the MD direction (Machine Direction; longitudinal direction) and a linear expansion coefficient (CTE, α2) of 50 to 120 ppm / K in the TD direction (Transverse Direction; transverse direction) is easily obtained. In addition, when the LCP resin composition is melt-extruded and the LCP film is subjected to T-die melt extrusion molding, typically, a tensile elastic modulus Y in the MD direction is easily obtained. MD Tensile elastic modulus Y in TD direction TD The ratio (Y MD / Y TD ) is 2 or more and 10 or less. Such physical properties can be obtained because the main chain of the liquid crystal polyester tends to be easily oriented along the MD direction during T-die melt extrusion molding, and an anisotropic melt phase of the liquid crystal polyester exists during T-die melt extrusion molding.
[0068] As described above, in the film forming step (S2), it is easy to form an LCP film with a high degree of orientation (large anisotropy). In the present invention, even such an LCP film with a high degree of orientation can be greatly reduced in orientation (anisotropy) by using the LCP resin composition of the above composition for a pressurized heating step (S3). Therefore, the LCP film with a high degree of orientation that was previously considered to lack industrial applicability can be used as a semi-finished product (intermediate product), which is one of its characteristics. Therefore, when an LCP film with an extremely high degree of orientation (extremely high anisotropy) is used, there is a tendency for the effect of the present invention to be more obvious. It should be noted that the linear expansion coefficient (CTE, α2) of the LCP film in the MD direction is not particularly limited, but is preferably -40 to 0 ppm / K, and more preferably -30 to 0 ppm / K. In addition, the linear expansion coefficient (CTE, α2) of the LCP film in the TD direction is not particularly limited, but is preferably 50 to 120 ppm / K, and more preferably 50 to 100 ppm / K. In addition, the tensile modulus Y of the MD direction of the obtained LCP film MD Tensile elastic modulus Y in TD direction TD The ratio (Y MD / Y TD ) is not particularly limited, but is preferably 2-9, more preferably 3-8.
[0069] <Pressure and heating step (S3)>
[0070] In the pressurizing and heating step (S3), the LCP film with a high orientation degree (large anisotropy) is pressurized and heated to reduce its orientation degree (anisotropy) to obtain a circuit board LCP film 11 having a linear expansion coefficient (CTE, α2) in the TD direction of 16.8±12 ppm / K. The pressurizing and heating can relax the orientation of the polymer chain of the liquid crystal polyester, improve the dimensional stability of the film in advance, and thus achieve excellent adhesion to the metal foil.
[0071] The heating and pressurizing treatment can be carried out using methods known in the industry, such as contact heat treatment, non-contact heat treatment, etc., and its type is not particularly limited. For example, known equipment such as non-contact heater, baking oven, blowing device, hot roller, cooling roller, hot press, double belt hot press can be used for heat setting. At this time, as required, a peeling film and a porous film known in the industry can be configured on the surface of the LCP film and heat treated. In addition, from the viewpoint of controlling orientation, it is preferred to use the following hot pressing forming method: a peeling film and a porous film are configured on the surface and back of the LCP film, and hot pressing is performed while being clamped between the endless belts of the double belt press, and thereafter the peeling film and the porous film are removed. The hot pressing forming method can be implemented with reference to, for example, Japanese Patent Laid-Open No. 2010-221694. As the processing temperature when the LCP film using the above-mentioned LCP resin composition is subjected to heat press molding between the endless belt pairs of the double belt press machine, in order to control the crystallization state of the LCP film, it is preferably carried out at a temperature higher than the melting point of the liquid crystal polyester and below the temperature of 70°C higher than the melting point, more preferably at a temperature higher than 5°C higher than the melting point and below the temperature of 60°C higher than the melting point, and further preferably at a temperature higher than 10°C higher than the melting point and below the temperature of 50°C higher than the melting point. The heat pressing conditions at this time can be appropriately set according to the desired performance, and are not particularly limited, but are preferably carried out under the conditions of a surface pressure of 0.5 to 10 MPa and a heating and pressing time of 250 to 430°C, more preferably under the conditions of a surface pressure of 0.6 to 8 MPa and a heating and pressing time of 260 to 400°C, and further preferably under the conditions of a surface pressure of 0.7 to 6 MPa and a heating and pressing time of 270 to 370°C. On the other hand, when a non-contact heater or an oven is used, it is preferably carried out under the conditions of, for example, 200 to 320° C. and 1 to 20 hours.
[0072] (LCP film for circuit board)
[0073] The thickness of the LCP film 11 for circuit substrate obtained after the pressurization and heating step (S3) can be appropriately set according to the required performance, and is not particularly limited. Considering the operability and productivity during the pressurization and heating treatment, it is preferably 10 μm to 500 μm, more preferably 20 μm to 300 μm, and further preferably 30 μm to 250 μm.
[0074] The coefficient of linear expansion (CTE, α2) in the TD direction of the LCP film 11 for circuit substrates is not particularly limited, but from the viewpoint of improving the adhesion with the metal foil, it is preferably 16.8±12ppm / K, more preferably 16.8±10ppm / K, and further preferably 16.8±8ppm / K. The present invention has a significant effect from the viewpoint that the coefficient of linear expansion (CTE, α2) in the TD direction can be greatly reduced even though a highly anisotropic LCP film with a coefficient of linear expansion (CTE, α2) of 50ppm / K or more in the TD direction is initially used as the processed object. It should be noted that, from the viewpoint of improving the adhesion with the electrolytic copper foil, in one embodiment of the LCP film 11 for circuit substrates, the coefficient of linear expansion (CTE, α2) in the TD direction is preferably 5.0ppm / K to 16.0ppm / K, more preferably 6.0ppm / K to 16.0ppm / K, and further preferably 7.0ppm / K to 16.0ppm / K.
[0075] The linear expansion coefficient (CTE, α2) in the MD direction of the LCP film 11 for circuit boards is not particularly limited, but from the viewpoint of improving the adhesion with the metal foil, it is preferably 0 to 40 ppm / K, more preferably 0 to 30 ppm / K, and further preferably 0 to 20 ppm / K. It should be noted that the linear expansion coefficient (CTE, α2) in the film thickness direction is not particularly limited, but is preferably 150 ppm / K or less.
[0076] On the other hand, from the viewpoint of reducing the anisotropy in the film plane, the tensile elastic modulus Y in the MD direction of the LCP film 11 for circuit boards is MD Tensile elastic modulus Y in TD direction TD The ratio (Y MD / Y TD ) is preferably 0.8 to 2.0, more preferably 0.9 to 1.5, and even more preferably 0.95 to 1.2.
[0077] It should be noted that the dielectric properties of the LCP film 11 for circuit boards can be appropriately set according to the desired performance and are not particularly limited. From the viewpoint of obtaining higher dielectric properties, the relative dielectric constant ε rIt is preferably 3.0 to 3.9, and more preferably 3.0 to 3.6. In addition, the dielectric loss tangent tanδ (36 GHz) is preferably 0.0005 to 0.0030, and more preferably 0.0005 to 0.0025.
[0078] The melting point (melting temperature) of the LCP film 11 for circuit substrate is not particularly limited, but from the viewpoints of heat resistance and processability of the film, the melting point (melting temperature) is preferably 200 to 400° C., and especially from the viewpoint of improving the thermal compression bonding to the metal foil, preferably 250 to 360° C., more preferably 260 to 355° C., further preferably 270 to 350° C., and particularly preferably 275 to 345° C. It should be noted that in this specification, the melting point of the LCP film 11 for circuit substrate refers to a value measured under the same measurement conditions as the melting point of the above-mentioned LCP film.
[0079] (Laminated board covered with metal foil)
[0080] Figure 3 The following is a schematic diagram showing an example of a laminated plate 31 covered with metal foil according to the present embodiment. The laminated plate body 31 (metal foil laminated LCP film) covered with metal foil according to the present embodiment comprises: the above-mentioned LCP film 11 for circuit substrate; and one or more metal foils 21, which are arranged on at least one surface of the LCP film 11 for circuit substrate. Here, in the present specification, the so-called "arranged on one (another) side of ~" not only includes a method in which the metal foil 21 is arranged only on one surface 11a of the LCP film 11 for circuit substrate, but also includes any method in which the metal foil 21 is arranged on the other surface 11b of the LCP film 11 for circuit substrate, and the metal foil 21 is arranged on both surfaces 11a, 11b of the LCP film 11 for circuit substrate.
[0081] The material of the metal foil 21 is not particularly limited, and gold, silver, copper, copper alloy, nickel, nickel alloy, aluminum, aluminum alloy, iron, iron alloy, etc. can be cited. Among them, copper foil, aluminum foil, stainless steel foil, and alloy foil of copper and aluminum are preferred, and copper foil is more preferred. As the copper foil, any copper foil manufactured by rolling method or electrolysis method can be used, but electrolytic copper foil and rolled copper foil with large surface roughness are preferred. The thickness of the metal foil 21 can be appropriately set according to the desired performance and is not particularly limited. It is usually preferably 1.5 to 1000 μm, more preferably 2 to 500 μm, further preferably 5 to 150 μm, and particularly preferably 7 to 100 μm. It should be noted that as long as the effect of the present invention is not impaired, the metal foil 21 can be subjected to surface treatments such as chemical surface treatments such as acid cleaning.
[0082] The method of providing the metal foil 21 on the surface 11a, 11b of the LCP film 11 for circuit substrates can be implemented according to a conventional method, and is not particularly limited. It can be any method of laminating the metal foil 21 on the LCP film 11 for circuit substrates to make the two layers adhere or press-bond, a physical method (dry method) such as sputtering and evaporation, a chemical method (wet method) such as electroless plating, electroplating after electroless plating, a method of applying a metal paste, etc.
[0083] As a preferred lamination method, the following method can be cited: the LCP film 11 for circuit substrate is laminated with the metal foil 21 to form a laminated body in which the metal foil 21 is placed on the LCP film 11 for circuit substrate, and the laminated body is hot-pressed while being clamped between a pair of endless belts of a double-belt press. As described above, the LCP film 11 for circuit substrate used in this embodiment significantly reduces the linear expansion coefficient (CTE, α2) in the TD direction without excessively damaging the excellent basic properties of the liquid crystal polyester, and in a preferred embodiment, sufficiently reduces the tensile elastic modulus Y in the MD direction. MD Tensile elastic modulus Y in TD direction TD The anisotropy of the metal foil 21 can provide a higher peel strength than before. Therefore, the process margin during the manufacture of the circuit board and the metal foil-covered laminate 31 can be improved, and the productivity and economic efficiency can be improved.
[0084] The temperature during the hot pressing of the metal foil 21 can be appropriately set according to the required performance, and is not particularly limited, but is preferably a temperature 50°C lower than the melting point of the liquid crystal polyester and below the melting point, more preferably a temperature 40°C lower than the melting point of the liquid crystal polyester and below the melting point, further preferably a temperature 30°C lower than the melting point of the liquid crystal polyester and below the melting point, and particularly preferably a temperature 20°C lower than the melting point of the liquid crystal polyester and below the melting point. It should be noted that the temperature during the hot pressing of the metal foil 21 is a value measured at the surface temperature of the LCP film of the aforementioned laminate. In addition, the pressing conditions at this time can be appropriately set according to the desired performance, and are not particularly limited. For example, when using a double belt press, it is preferably carried out under the conditions of a surface pressure of 0.5 to 10 MPa and a heating time of 200 to 360°C.
[0085] The metal foil-covered laminate 31 of the present embodiment only needs to have a double-layer structure of the LCP film 11 for circuit substrate and the metal foil 21, and may also have a further laminated structure. For example, it can be made into a two-layer structure of metal foil 21 / LCP film 11 for circuit substrate; a three-layer structure such as metal foil 21 / LCP film 11 for circuit substrate / metal foil 21, LCP film 11 for circuit substrate / metal foil 21 / LCP film 11 for circuit substrate; a five-layer structure such as metal foil 21 / LCP film 11 for circuit substrate / metal foil 21 / LCP film 11 for circuit substrate / metal foil 21; and other multi-layer structures having at least the above-mentioned double-layer structure. In addition, multiple (for example, 2 to 50) metal foil-covered laminates 31 may be laminated and thermally pressed.
[0086] In the metal foil covered laminate 31 of the present embodiment, the peel strength between the LCP film 11 for the circuit substrate and the metal foil 21 is not particularly limited, but from the viewpoint of having a higher peel strength, it is preferably 1.0 (N / mm) or more, more preferably 1.1 (N / mm) or more, and further preferably 1.2 (N / mm) or more. As described above, in the metal foil covered laminate 31 of the present embodiment, a higher peel strength than that of the prior art can be achieved, and therefore, the peeling of the LCP film 11 for the circuit substrate and the metal foil 21 can be suppressed in, for example, the heating process of substrate manufacturing. In addition, when obtaining a peel strength equivalent to that of the prior art, a moderate manufacturing condition can be applied, and therefore, the degradation of the basic performance of the liquid crystal polyester can be suppressed while maintaining the same degree of peel strength as before.
[0087] For the laminated plate 31 covered with metal foil of the present embodiment, at least a portion of the metal foil 21 can be pattern-etched, etc., so as to be used as a raw material for electronic circuit substrates, multilayer substrates, etc., and can also be used for high heat dissipation substrates, antenna substrates, optoelectronic hybrid substrates, IC packaging, etc. In addition, the laminated plate 31 covered with metal foil of the present embodiment has excellent high-frequency characteristics and low dielectric properties, the LCP film 11 for the circuit substrate and the metal foil 21 have excellent adhesion, and can have good dimensional stability, so it becomes a particularly useful raw material as an insulating material for flexible printed wiring boards (FPCs) and the like in fifth-generation mobile communication systems (5G), millimeter-wave radars, etc.
[0088] Example
[0089] Embodiment and comparative example are enumerated below, feature of the present invention is described in more detail, but the present invention is not subject to any limitation thereof. That is, the material, usage amount, ratio, processing content, processing step etc. shown in the following examples can be appropriately changed, as long as do not depart from the gist of the present invention. In addition, the value of various manufacturing conditions, evaluation result in the following examples has the meaning of preferred upper limit or preferred lower limit in the embodiment of the present invention, and preferred numerical range can also be the scope specified by the combination of the aforementioned upper limit or lower limit, the value of the following examples or the values of the examples each other.
[0090] (Example 1)
[0091] Synthesis of LCP
[0092] Into a reaction tank equipped with a stirrer and a vacuum distillation device, p-hydroxybenzoic acid (74 mol%), 6-hydroxy-2-naphthoic acid (26 mol%), and acetic anhydride in an amount of 1.025 times the molar amount of the total monomer amount were added, and the reaction tank was heated to 150°C under a nitrogen atmosphere, and maintained for 30 minutes. The temperature was then rapidly raised to 190°C while distilling off the acetic acid generated as a by-product, and maintained for 1 hour to obtain an acetylated reaction product. The obtained acetylated reaction product was heated to 320°C over 3.5 hours, and then reduced to 2.7 kPa over about 30 minutes, melt polycondensed, and then gradually reduced to normal pressure to obtain a polymer solid. The obtained polymer solid was crushed and granulated using a twin-screw extruder at 300°C to obtain LCP pellets of an aromatic polyester liquid crystal polymer (molar ratio of 74:26) formed of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid.
[0093] Preparation of LCP resin composition
[0094] The obtained LCP pellets and an oxazoline-containing polymer (polystyrene containing 5% by mass of an oxazoline component, trade name: Epocros RPS-1005, manufactured by Nippon Shokubai Co., Ltd.) were supplied in the proportions shown in Table 1, and mixed, reacted, and granulated at 300°C using a twin-screw extruder to obtain LCP resin composition pellets.
[0095] Manufacturing of LCP membrane
[0096] The obtained LCP resin composition pellets were used to form a film by a T-die casting method at 300° C., thereby obtaining an LCP melt-extruded film having a melting temperature of 280° C. and a thickness of 50 μm.
[0097] Production of LCP film after pressure and heat treatment
[0098] The obtained LCP melt-extruded film was subjected to contact heat treatment at 320° C. for 30 seconds using a double belt heat press to obtain a pressurized and heat-treated LCP film having a melt temperature of 280° C. and a thickness of 50 μm.
[0099] (Example 2)
[0100] Preparation of LCP resin composition
[0101] The LCP pellets obtained in Example 1, the oxazoline-containing polymer (polystyrene containing 5% by mass of oxazoline component, trade name: Epocros RPS-1005, manufactured by Nippon Shokubai Co., Ltd.) and polyarylate (trade name: U-POLYMER POWDER CK, manufactured by Unitika Co., Ltd.) (PAR) were supplied in the proportions described in Table 1, and mixed, reacted and granulated at 300°C using a twin-screw extruder to obtain LCP resin composition pellets.
[0102] Manufacturing of LCP membrane
[0103] The obtained LCP resin composition pellets were used to form a film by a T-die casting method at 300° C., thereby obtaining an LCP melt-extruded film having a melting temperature of 280° C. and a thickness of 50 μm.
[0104] Production of LCP film after pressure and heat treatment
[0105] The obtained LCP melt-extruded film was subjected to contact heat treatment at 320° C. for 30 seconds using a double belt heat press to obtain a pressurized and heat-treated LCP film having a melt temperature of 280° C. and a thickness of 50 μm.
[0106] (Comparative Example 1)
[0107] An LCP resin composition was prepared in the same manner as in Example 1 except that the oxazoline-containing polymer was omitted, thereby obtaining an LCP film having a melting point of 280°C and a thickness of 50 μm, and an LCP film having been subjected to a pressurized heat treatment and having a melting point of 280°C and a thickness of 50 μm.
[0108] <Performance Evaluation>
[0109] The performance evaluation was performed on the LCP films obtained in Examples 1 and 2 and Comparative Example 1 and the LCP films subjected to the pressure and heat treatment. The measurement conditions were as follows.
[0110] [Linear expansion coefficient]
[0111] Measuring equipment: TMA 4000SE (manufactured by NETZSCH)
[0112] Measurement method: tensile mode
[0113] Measurement conditions: Sample size 20mm×4mm×thickness 50μm
[0114] Temperature range: room temperature ~ 200℃ (2nd RUN)
[0115] Heating rate: 5℃ / min
[0116] Atmosphere nitrogen (flow rate 50ml / min)
[0117] Test load 5gf
[0118] ※In order to check the value after eliminating the thermal history, the value of 2ndRUN [tensile elastic modulus] is used.
[0119] Measuring equipment: Strograph VE1D (manufactured by Toyo Seiki Seisaku-sho, Ltd.)
[0120] Determination method: tensile test
[0121] Measurement environment: temperature 23℃ relative humidity 50%
[0122] Measurement conditions: Sample size dumbbell-shaped, thickness 50 μm
[0123] Test speed: 50 mm / min
[0124] Marking distance 25mm
[0125] [Relative dielectric constant ε r , dielectric loss tangent tanδ (36GHz) electrical characteristics]
[0126] Measurement method: Cylindrical cavity resonator method
[0127] Measurement environment: temperature 23℃ relative humidity 50%
[0128] Measurement conditions: Sample size: 15 mm × 15 mm × thickness: 200 μm
[0129] Cavity: 36GHz
[0130] [Heat resistance]
[0131] Measuring equipment: DSC8500 (manufactured by PerkinElmer)
[0132] Measurement method: Differential scanning calorimetry (DSC)
[0133] Measurement conditions: Temperature range 30~400℃
[0134] First heating 20℃ / min
[0135] First cooling 50℃ / min
[0136] Second heating 20℃ / min
[0137] ※In order to check the values after eliminating the thermal history, the measurement results are shown in Table 1 using the values of 2nd RUN.
[0138] [Table 1]
[0139]
[0140] (Examples 3 to 5)
[0141] Except for changing the mixing ratio of the oxazoline-containing polymer and the polyarylate as described in Table 2, the same operation as in Example 1 was carried out to prepare an LCP resin composition, thereby obtaining an LCP film having a melting temperature of 280°C and a thickness of 50 μm, and an LCP film having been subjected to a pressurized heat treatment and having a melting temperature of 280°C and a thickness of 50 μm.
[0142] <Performance Evaluation>
[0143] The performance of the LCP films obtained in Examples 1 to 5 and Comparative Example 1 and the LCP film subjected to the pressure and heat treatment was evaluated.
[0144] Table 2 shows the measurement results.
[0145] [Table 2]
[0146]
[0147] Industrial Applicability
[0148] The LCP film for circuit substrate of the present invention can be widely and effectively used in applications such as electronic circuit substrates, multi-layer substrates, high heat dissipation substrates, flexible printed wiring boards, antenna substrates, optoelectronic hybrid substrates, IC packaging, etc., and is particularly excellent in high-frequency characteristics and low dielectric properties. Therefore, it can be particularly widely and effectively used as an insulating material for flexible printed wiring boards (FPCs) in fifth-generation mobile communication systems (5G), millimeter-wave radars, etc.
[0149] Description of Reference Numerals
[0150] 11···LCP film for circuit board
[0151] 11a···Surface
[0152] 11b···Surface
[0153] 21···Metal foil
[0154] 31···Laminated board covered with metal foil
Claims
1. An LCP resin composition for a circuit board, comprising at least 100 parts by mass of a liquid crystal polyester, 1 to 20 parts by mass of a polyarylate, and 1 to 20 parts by mass of an oxazoline group-containing polymer.
2. An LCP film for a circuit substrate, comprising at least 100 parts by mass of a liquid crystal polyester, 1 to 20 parts by mass of a polyarylate, and 1 to 20 parts by mass of an oxazoline group-containing polymer, The linear expansion coefficient (α2) of the LCP film for circuit board in the TD direction is 16.8±12 ppm / K.
3. The LCP film for circuit substrate according to claim 2, wherein: Tensile elastic modulus Y in MD direction MD Tensile elastic modulus Y in TD direction TD The ratio (Y MD / Y TD ) is greater than 0.8 and less than 2.
0. 4 . The LCP film for circuit board according to claim 2 , wherein the linear expansion coefficient of the LCP film in the TD direction is 5.0 ppm / K or more and 16.0 ppm / K or less.
5. The LCP film for circuit substrate according to claim 2 or 3, having a relative dielectric constant ε measured at 36 GHz. r The dielectric properties are 3.0 to 3.9 and the dielectric loss tangent tanδ measured at 36 GHz is 0.0005 to 0.
003. 6 . The LCP film for a circuit board according to claim 2 , which has a thickness of 10 μm to 500 μm.