High-elasticity PPS applied to sealing ring and preparation method of high-elasticity PPS

By rationally formulating and preparing high-elastic polyphenylene sulfide (PPS) materials, the shortcomings of traditional rubber sealing rings in high temperature and chemical corrosion resistance are solved, and high elasticity and heat resistance are achieved. They are suitable for automotive sealing rings and improved Life and performance of seal rings.

CN118895047APending Publication Date: 2024-11-05PENGYUN ENG PLASTICS GUANGZHOU
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411138301.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Traditional rubber seals have insufficient performance in high temperature and chemical corrosion resistance, resulting in a short service life, especially in automotive engines and cylinder applications.

Method used

Highly elastic polyphenylene sulfide (PPS) materials are used to form highly elastic PPS by reasonably preparing components such as PPS resin, compatibility agent, toughener, antioxidant, lubricant and coupling agent, and extrude through twin screws. The equipment is prepared to ensure high elasticity and heat resistance of the material.

Benefits of technology

It has achieved the preparation of high elastic PPS, with excellent heat resistance and chemical corrosion resistance, and the flame retardant grade is V0, which significantly improves the service life and performance of the sealing ring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005000017050000081
    Figure BDA0005000017050000081
Patent Text Reader

Abstract

The invention discloses high-elasticity PPS (polyphenylene sulfide) applied to a sealing ring and a preparation method of the high-elasticity PPS, and the high-elasticity PPS is prepared from the following components in percentage by weight: 74 to 94 weight percent of PPS resin, 1 to 5 weight percent of compatilizer, 5 to 20 weight percent of flexibilizer, 0.1 to 0.4 weight percent of antioxidant, 0.1 to 0.3 weight percent of lubricant and 0.1 to 0.3 weight percent of coupling agent. The PPS resin is modified and optimized through compounding of all component materials, the prepared high-elasticity PPS has high elasticity, meanwhile, excellent heat resistance and chemical corrosion resistance are kept, the flame retardant rating is V0 grade, the high-elasticity PPS is applied to preparation of the sealing ring, and the sealing ring has the good sealing performance. The problem that a traditional rubber sealing ring is insufficient in temperature resistance and corrosion resistance is well solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a high-elastic PPS used in a sealing ring and a preparation method thereof. Background Art

[0002] For seals used in extruders, there are requirements for high temperature resistance and corrosion resistance; in the automotive field, seals used in engines and oil cylinders need to be oil-resistant, acid-resistant, and able to operate at high temperatures because they come into contact with engine oil. However, traditional rubber seals are not high enough in terms of temperature resistance and corrosion resistance, resulting in a short service life, and there is still room for improvement.

[0003] Polyphenylenesulfide (PPS) is resistant to high temperatures and can work stably at 260℃~270℃ for a long time. It is also resistant to chemical corrosion and is superior to traditional rubber seals. At the same time, PPS resin has high strength and high rigidity, and its rigidity decreases very little under high temperature conditions, and it has excellent fatigue resistance and creep resistance.

[0004] Therefore, there is an urgent need for a highly elastic PPS material that can be used in sealing rings to solve the problem of insufficient temperature and corrosion resistance of traditional rubber sealing rings. Summary of the invention

[0005] The purpose of the present invention is to provide a high-elastic PPS for sealing rings and a preparation method thereof, which has high elasticity while maintaining excellent heat resistance and chemical corrosion resistance, and has a flame retardant grade of V0, thus effectively solving the problem of insufficient temperature and corrosion resistance of traditional rubber sealing rings.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] In the first aspect, the present invention provides a high-elastic PPS for use in a sealing ring. Calculated by weight percentage, the high-elastic PPS is composed of the following components: 74wt% to 94wt% of PPS resin, 1wt% to 5wt% of a compatibilizer, 5wt% to 20wt% of a toughening agent, 0.1wt% to 0.4wt% of an antioxidant, 0.1wt% to 0.3wt% of a lubricant, and 0.1wt% to 0.3wt% of a coupling agent.

[0008] Furthermore, the PPS resin is a linear PPS resin.

[0009] Furthermore, the compatibilizer is POE grafted maleic anhydride.

[0010] Furthermore, the toughening agent is ethylene-acrylic acid-methacrylate glycidyl ester or polyethylene terephthalate.

[0011] Furthermore, the antioxidant is antioxidant 1010.

[0012] Furthermore, the lubricant is ethylene bis stearamide or pentaerythritol stearate.

[0013] Furthermore, the coupling agent is silane coupling agent KH560.

[0014] Preferably, calculated by weight percentage, the high elastic PPS is composed of 79.4 wt % of PPS resin, 5 wt % of compatibilizer, 15 wt % of toughening agent, 0.2 wt % of antioxidant, 0.3 wt % of lubricant and 0.1 wt % of coupling agent.

[0015] Alternatively, calculated by weight percentage, the high elastic PPS is composed of 89.4 wt % of PPS resin, 5 wt % of compatibilizer, 5 wt % of toughening agent, 0.2 wt % of antioxidant, 0.3 wt % of lubricant and 0.1 wt % of coupling agent.

[0016] Alternatively, calculated by weight percentage, the high elastic PPS is composed of 83.4 wt % of PPS resin, 1 wt % of a compatibilizer, 15 wt % of a toughening agent, 0.2 wt % of an antioxidant, 0.3 wt % of a lubricant and 0.1 wt % of a coupling agent.

[0017] In a second aspect, the present invention also provides a method for preparing the above-mentioned high elastic PPS for use in a sealing ring, comprising the following steps:

[0018] Step 1: Mix the PPS resin and the coupling agent and stir for 10 to 60 minutes;

[0019] Step 2: Add the compatibilizer, toughening agent, antioxidant and lubricant to step 1 and stir for 10 to 60 minutes to obtain a mixture;

[0020] Step 3: Finally, the mixture obtained in step 2 is sent to a twin-screw extruder for extrusion and granulation to obtain high-elastic PPS.

[0021] Further, in step three, the temperature of the twin-screw extruder is set to: sections 1 to 3 are set to 280°C to 300°C, sections 4 to 6 are set to 280°C to 290°C, sections 7 to 9 are set to 270°C to 280°C, and sections 10 to 12 are set to 290°C to 310°C.

[0022] Preferably, in step three, the temperature of the twin-screw extruder is set to: the temperature of section 1 is set to 280°C, the temperature of section 2 is set to 290°C, the temperature of section 3 is set to 295°C, the temperature of sections 4 to 6 is set to 280°C, the temperature of section 7 is set to 270°C, the temperature of section 8 is set to 270°C, the temperature of section 9 is set to 275°C, the temperature of section 10 is set to 285°C, the temperature of section 11 is set to 295°C, and the temperature of section 12 is set to 305°C.

[0023] Compared with the prior art, the present invention provides a high-elastic PPS for use in a sealing ring and a preparation method thereof, which has the following beneficial effects:

[0024] The present invention greatly improves toughness and strength by adding a toughening agent; adds an antioxidant to improve aging resistance; adds a compatibilizer to improve the compatibility of PPS resin and the toughening agent; adds a coupling agent to improve the affinity and compatibility between materials; and adds a lubricant to improve lubricity for easy processing.

[0025] The present invention modifies and optimizes the PPS resin by compounding various component materials. The prepared high-elasticity PPS has high elasticity while maintaining excellent heat resistance and chemical corrosion resistance, and the flame retardant grade is V0. The high-elasticity PPS is used in preparing sealing rings, which well solves the problem of insufficient temperature resistance and corrosion resistance of traditional rubber sealing rings. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In the embodiments and comparative examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0028] The invention provides a high-elastic PPS used for a sealing ring. Calculated by weight percentage, the high-elastic PPS consists of the following components: 74wt%-94wt% of PPS resin, 1wt%-5wt% of a compatibilizer, 5wt%-20wt% of a toughening agent, 0.1wt%-0.4wt% of an antioxidant, 0.1wt%-0.3wt% of a lubricant and 0.1wt%-0.3wt% of a coupling agent.

[0029] As an example, the PPS resin may be a linear PPS resin, with a typical grade being CXP-300.

[0030] As an example, the compatibilizer may be POE grafted maleic anhydride (ie, POE-g-MAH), and the typical brand is AD-92.

[0031] As an example, the toughening agent can be ethylene-acrylic acid-methacrylate glycidyl ester (ie, E-MA-GMA) or polyethylene terephthalate (ie, PTE). The typical grade of E-MA-GMA is Lotader AX8900, produced by Atofina, France, with m(E) / m(MA) / m(GMA) of 64:24:8 and a melt flow rate of 610rain. The typical grade of PTE is 8900, produced by DuPont, USA.

[0032] As an example, the antioxidant may be antioxidant 1010 .

[0033] As an example, the lubricant can be ethylene bis stearamide (ie, EBS) or pentaerythritol stearate (ie, PETS). A typical brand of EBS is KAOWAX EB-FF from Kao Corporation of Japan.

[0034] As an example, the coupling agent may be silane coupling agent KH560 (i.e., γ-glycidyloxypropyltrimethoxysilane). Typical brands of silane coupling agent KH560 are A-187 of Union Carbide Corporation of the United States, KBM-403 of Shin-Etsu Chemical Co., Ltd. of Japan, and Z-6040 of Dow Corning Corporation of the United States.

[0035] The preparation method of the high-elastic PPS comprises the following steps:

[0036] Step 1: Mix the PPS resin and the coupling agent and stir for 10 to 60 minutes;

[0037] Step 2: Add the compatibilizer, toughening agent, antioxidant and lubricant to step 1 and stir for 10 to 60 minutes to obtain a mixture;

[0038] Step 3: Finally, the mixture obtained in step 2 is sent to a twin-screw extruder for extrusion and granulation to obtain high-elastic PPS.

[0039] In step three, the temperature of the twin-screw extruder is set to: 280°C to 300°C for sections 1 to 3, 280°C to 290°C for sections 4 to 6, 270°C to 280°C for sections 7 to 9, and 290°C to 310°C for sections 10 to 12.

[0040] The present invention is further described in detail below through detailed examples.

[0041] Example 1

[0042] This embodiment provides a high-elastic PPS for use in a sealing ring. Calculated by weight percentage, the high-elastic PPS is composed of the following components: 79.4wt% of PPS resin, 5wt% of compatibilizer, 15wt% of toughening agent, 0.2wt% of antioxidant, 0.3wt% of lubricant and 0.1wt% of coupling agent.

[0043] Among them, PPS resin uses linear PPS resin, and the typical brand is CXP-300; the compatibilizer uses POE grafted maleic anhydride (i.e. POE-g-MAH), and the typical brand is AD-92; the toughening agent uses ethylene-acrylic acid-methacrylate glycidyl ester (i.e. E-MA-GMA), and the typical brand is Lotader AX8900, which is produced by France's Atofina Company, with m(E) / m(MA) / m(GMA) of 64:24:8 and a melt flow rate of 610rain; the antioxidant can use antioxidant 1010; the lubricant can use ethylene bisstearamide (i.e. EBS), and the typical brand is KAOWAX EB-FF of Kao Corporation of Japan; the coupling agent can use silane coupling agent KH560 (i.e. γ-glycidyl ether oxypropyl trimethoxy silane), and the typical brand is A-187 of Union Carbide Corporation of the United States.

[0044] The preparation method of the high-elastic PPS comprises the following steps:

[0045] Step 1: Mix the PPS resin and coupling agent and stir for 20 minutes;

[0046] Step 2: Add the compatibilizer, toughening agent, antioxidant and lubricant to step 1 and stir for 40 minutes to obtain a mixture;

[0047] Step 3: Finally, the mixture obtained in step 2 is sent to a twin-screw extruder for extrusion and granulation to obtain high elastic PPS. Specifically, the temperature of the twin-screw extruder is set as follows: the temperature of section 1 is set to 280°C, the temperature of section 2 is set to 290°C, the temperature of section 3 is set to 295°C, the temperature of sections 4 to 6 is set to 280°C, the temperature of section 7 is set to 270°C, the temperature of section 8 is set to 270°C, the temperature of section 9 is set to 275°C, the temperature of section 10 is set to 285°C, the temperature of section 11 is set to 295°C, and the temperature of section 12 is set to 305°C.

[0048] Example 2

[0049] This embodiment provides a high-elastic PPS for use in a sealing ring. Calculated by weight percentage, the high-elastic PPS is composed of the following components: 89.4wt% of PPS resin, 5wt% of compatibilizer, 5wt% of toughening agent, 0.2wt% of antioxidant, 0.3wt% of lubricant and 0.1wt% of coupling agent.

[0050] The specific selection of each component and the preparation method of high elastic PPS are the same as those in Example 1.

[0051] Example 3

[0052] This embodiment provides a high-elastic PPS for use in a sealing ring. Calculated by weight percentage, the high-elastic PPS is composed of the following components: 83.4wt% of PPS resin, 1wt% of a compatibilizer, 15wt% of a toughening agent, 0.2wt% of an antioxidant, 0.3wt% of a lubricant, and 0.1wt% of a coupling agent.

[0053] The specific selection of each component and the preparation method of high elastic PPS are the same as those in Example 1.

[0054] Comparative Example 1

[0055] This comparative example provides a high elastic PPS for sealing rings, and its formula components and the dosage ratio of each component are the same as those in Example 1. The difference is that the preparation method of the high elastic PPS is different. Specifically, the temperature of the twin-screw extruder is set as follows: the temperature of section 1 is set to 270°C, the temperature of section 2 is set to 280°C, the temperature of section 3 is set to 285°C, the temperature of sections 4 to 6 is set to 270°C, the temperature of section 7 is set to 260°C, the temperature of section 8 is set to 260°C, the temperature of section 9 is set to 265°C, the temperature of section 10 is set to 275°C, the temperature of section 11 is set to 285°C, and the temperature of section 12 is set to 295°C.

[0056] Comparative Example 2

[0057] This comparative example provides a high-elastic PPS for use in a sealing ring. Calculated by weight percentage, the high-elastic PPS consists of the following components: 94.4wt% of PPS resin, 5wt% of compatibilizer, 0.2wt% of antioxidant, 0.3wt% of lubricant and 0.1wt% of coupling agent.

[0058] The specific selection of each component and the preparation method of high elastic PPS are the same as those in Example 1.

[0059] The high elastic PPS prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were tested and inspected, and corresponding data such as elongation at break, unnotched impact strength, Rockwell hardness, and heat deformation temperature were obtained. The specific test results are shown in Table 1 below.

[0060]

[0061] It can be seen from the results in Table 1 that as the amount of toughening agent added increases, the elongation at break of the prepared material also increases accordingly, indicating that the material has higher elasticity; at the same time, by comparing the results of Example 1 with Example 3, it can be seen that by increasing the proportion of the compatibilizer, the compatibility of the toughening agent and the PPS resin can be effectively promoted, thereby improving the performance of the high-elastic PPS; by comparing the results of Example 1 with Comparative Example 1, it can be seen that by adopting appropriate preparation process parameters, it is possible to facilitate the processing of modified PPS resin, thereby promoting the improvement of the performance of the high-elastic PPS.

[0062] It can be seen from the above comparative analysis that the high elasticity PPS prepared in Example 1 has the best comprehensive performance; it has high elasticity while maintaining excellent heat resistance and chemical corrosion resistance, and its flame retardant grade is V0. By applying the high elasticity PPS to the preparation of sealing rings, the problem of insufficient temperature resistance and corrosion resistance of traditional rubber sealing rings can be well solved.

[0063] The above embodiments are merely illustrative of the concept and technical solution of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person with ordinary knowledge in the technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.

[0064] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A high elastic PPS used in sealing rings, characterized in that: Calculated by weight percentage, the high elastic PPS is composed of the following components: 74wt% to 94wt% of PPS resin, 1wt% to 5wt% of compatibilizer, 5wt% to 20wt% of toughening agent, 0.1wt% to 0.4wt% of antioxidant, 0.1wt% to 0.3wt% of lubricant and 0.1wt% to 0.3wt% of coupling agent.

2. The high elastic PPS used for sealing ring according to claim 1, characterized in that: The PPS resin is selected from linear PPS resin.

3. The high elastic PPS used for sealing ring according to claim 1, characterized in that: The compatibilizer is POE grafted maleic anhydride.

4. The high elastic PPS used for sealing ring according to claim 1, characterized in that: The toughening agent is selected from ethylene-acrylic acid-methacrylate glycidyl ester or polyethylene terephthalate.

5. The high elastic PPS used for sealing ring according to claim 1, characterized in that: The antioxidant is antioxidant 1010.

6. The high elastic PPS used for sealing ring according to claim 1, characterized in that: The lubricant is selected from ethylene bis stearamide or pentaerythritol stearate.

7. The high elastic PPS used for sealing ring according to claim 1, characterized in that: The coupling agent is silane coupling agent KH560.

8. The high elastic PPS used for sealing ring according to claim 1, characterized in that: Calculated by weight percentage, the high-elastic PPS consists of 79.4wt% of PPS resin, 5wt% of compatibilizer, 15wt% of toughening agent, 0.2wt% of antioxidant, 0.3wt% of lubricant and 0.1wt% of coupling agent; or, calculated by weight percentage, the high-elastic PPS consists of 89.4wt% of PPS resin, 5wt% of compatibilizer, 5wt% of toughening agent, 0.2wt% of antioxidant, 0.3wt% of lubricant and 0.1wt% of coupling agent; or, calculated by weight percentage, the high-elastic PPS consists of 83.4wt% of PPS resin, 1wt% of compatibilizer, 15wt% of toughening agent, 0.2wt% of antioxidant, 0.3wt% of lubricant and 0.1wt% of coupling agent.

9. A method for preparing a high elastic PPS for use in a sealing ring as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Mix the PPS resin and the coupling agent and stir for 10 to 60 minutes; Step 2: Add the compatibilizer, toughening agent, antioxidant and lubricant to step 1 and stir for 10 to 60 minutes to obtain a mixture; Step 3: Finally, the mixture obtained in step 2 is sent to a twin-screw extruder for extrusion and granulation to obtain high-elastic PPS.

10. The preparation method according to claim 9, characterized in that: In step three, the temperature of the twin-screw extruder is set to: 280°C to 300°C for sections 1 to 3, 280°C to 290°C for sections 4 to 6, 270°C to 280°C for sections 7 to 9, and 290°C to 310°C for sections 10 to 12.

Citation Information

Patent Citations

  • Food-grade high-heat-resistance PPS composite material and preparation method thereof

    CN106349695A

  • Spraying-free high-impact PC alloy material with metallic luster and preparation method thereof

    CN107987503A

  • Low-flash high-toughness good-surface polyphenylene sulfide composition as well as preparation method and application thereof

    CN114525032A

  • Manufacturing method of halogen-free flame-retardant reinforced polyphenylene sulfide with high CTI (comparative tracking index) value

    CN117820862A