Novel high-molecular nano anti-attrition paste

Through the step-by-step saponification process of the new polymer nano-grinding paste, combined with multiple components, the problem that traditional grinding paste cannot provide long-lasting lubrication protection is solved, and the effect of significantly reducing friction coefficient and improving track safety is achieved.

CN118895176APending Publication Date: 2024-11-05JINAN HERUI ELECTRIC POWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196453.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Traditional grinding paste cannot provide long-lasting lubrication protection under various working conditions, resulting in less obvious reduction in friction coefficient and requires frequent re-coating, which cannot effectively reduce the maintenance cost and safety risks of rail transit systems.

Method used

A new type of polymer nano-grinding cream is adopted to combine various components through a step-by-step saponification process, including base oil, pentaerythritol ester, lithium monohydrate, 12-hydroxystearic acid, stearic acid, sebacic acid and Polytetrafluoroethylene, through physical mixing and chemical saponification reaction, a nano-grinding paste with excellent grinding reduction effect was prepared.

Benefits of technology

Significantly reduces the friction coefficient from 0.4-0.5 to 0.2, providing a lasting lubrication effect, reducing maintenance costs and frequency, and improving track safety and operating efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895176A_ABST
    Figure CN118895176A_ABST
Patent Text Reader

Abstract

The invention discloses a novel polymer nano anti-friction paste in the technical field of nano anti-friction pastes. The novel polymer nano anti-friction paste comprises the following components in percentage by weight: base oil: 30% of LUAN10 and 48% of pentaerythritol ester; auxiliary materials: 2.6% of lithium hydroxide monohydrate, 7% of 12-hydroxystearic acid, 3% of stearic acid, 2% of sebacic acid and 5% of polytetrafluoroethylene; and additives: 12% of T6, 46 per thousand of T7 and 13 per thousand of T32. By physically mixing various components, the anti-friction paste can remarkably reduce the friction coefficient, has a very excellent anti-friction effect, has a lasting lubricating effect, and can keep a low-friction state for a long time, so that the maintenance cost and frequency are reduced, the use amount of materials is reduced, the operation efficiency is also improved, and the anti-friction paste is suitable for large-scale popularization and application. And the maximum value and the average value of the derailment coefficient are both in a small range and are far lower than standard fixed values, so that the safety of the track is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano anti-friction paste, and in particular relates to a novel polymer nano anti-friction paste. Background Art

[0002] Friction reduction technology plays a vital role in rail transportation. Friction not only consumes energy and reduces mechanical efficiency, but also causes premature wear of equipment, increased maintenance costs, and may even cause failures or accidents due to overheating. Especially in high-speed or high-load mechanical systems, effective friction reduction can significantly improve system performance and reliability, reduce downtime, and extend the service life of equipment. In addition, friction reduction can also reduce noise, improve the working environment, and reduce environmental pollution. With the increase in railway transportation volume and traffic density, especially since the speed increase of trains, the side wear of curved rails and the wear of crossing switches have become increasingly serious, which will increase the maintenance cost of the line and affect driving safety.

[0003] Traditional anti-friction pastes may not provide adequate lubrication protection under all working conditions, resulting in an insignificant reduction in the coefficient of friction. Some anti-friction pastes may provide good lubrication in the short term, but their performance will decline rapidly over time and require frequent re-application. Summary of the invention

[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a new type of polymer nano-friction reducing paste.

[0005] In order to achieve the above purpose, the following technical scheme is adopted: a new type of polymer nano anti-friction paste, which includes the following components in weight percentage: base oil: LUAN1020-40%, pentaerythritol ester 35-55%; auxiliary materials: lithium hydroxide monohydrate 2-3%, 12-hydroxystearic acid 5-10%, stearic acid 2-6%, sebacic acid 1-3%, polytetrafluoroethylene 3-6%; additives: T6121-3%, T7461-3‰, T3211-3‰.

[0006] Preferably, the anti-friction paste comprises the following components in weight percentage: base oil: LUAN10 20-35%, pentaerythritol ester 40-50%; auxiliary materials: lithium hydroxide monohydrate 2.2-2.8%, 12-hydroxystearic acid 5.5-8%, stearic acid 2-5%, sebacic acid 1-2.5%, polytetrafluoroethylene 3-5%; additives: T612 1-2.5%, T746 1-2‰, T321 1.5-3‰.

[0007] Preferably, the anti-friction paste comprises the following components in weight percentage: base oil: LUAN10 25-30%, pentaerythritol ester 45-50%; auxiliary materials: lithium hydroxide monohydrate 2.5-2.8%, 12-hydroxystearic acid 6-8%, stearic acid 3-4%, sebacic acid 1.5-2%, polytetrafluoroethylene 3.5-5%; additives: T612 1.5-2%, T746 1.5-2‰, T321 2-3‰.

[0008] Preferably, the anti-friction paste comprises the following components in weight percentage: base oil: LUAN10 30%, pentaerythritol ester 48%; auxiliary materials: lithium hydroxide monohydrate 2.6%, 12-hydroxystearic acid 7%, stearic acid 3%, sebacic acid 2%, polytetrafluoroethylene 5%; additives: T61 22%, T74 61‰, T32 13‰.

[0009] Further, the anti-friction paste is prepared by the following steps:

[0010] S1, add the LUAN10 base oil into the fat making kettle and heat it to 80°C;

[0011] S2, adding the 12-hydroxystearic acid and heating to melt;

[0012] S3, preparing the lithium hydroxide monohydrate into a saturated lithium hydroxide solution, slowly adding 1 / 2 of the saturated lithium hydroxide solution, the temperature is 110° C.;

[0013] S4, after adding the saturated lithium hydroxide solution, the temperature is rapidly raised to 149°C and maintained for 1 hour to completely dehydrate the soap base, and then the material is rapidly cooled to 96°C;

[0014] S5, add the stearic acid, stir for 15 minutes, slowly add 1 / 4 of the saturated lithium hydroxide solution, and heat to 110°C;

[0015] S6, add the sebacic acid, stir for 15 minutes, add the remaining saturated lithium hydroxide solution, control the addition within 45 minutes, saponify the sebacic acid, raise the temperature to 149 ° C and maintain for 1 hour to complete the dehydration;

[0016] S7, first add 13% of the pentaerythritol ester, quickly raise the temperature to 200° C. and maintain for 20 minutes;

[0017] S8, adding 35% of the pentaerythritol ester to rapidly cool the fat base;

[0018] S9, adding the polytetrafluoroethylene, continuing to stir and cool to 66°C;

[0019] S10, adding the T612, T746 and T321, and grinding to obtain the finished product of the anti-friction paste.

[0020] The beneficial effects of the present invention are as follows: the present invention provides a novel polymer nano anti-friction paste, the production method of which is a two-step method, and the saponification process is a step-by-step saponification process, wherein lithium hydroxide is first subjected to saponification reaction with a polymer fatty acid, the temperature is raised to a specified temperature after dehydration, and then the second and third low molecular weight acids (compounding agents) are added to carry out saponification composite reaction, the present invention physically mixes a plurality of components, the anti-friction paste can significantly reduce the friction coefficient, and the friction coefficient is reduced from the original μ=0.4-0.5 to μ=0.2, indicating that it has a very excellent anti-friction effect, after the anti-friction paste is coated on the track, its lubricating effect is long-lasting, and the low friction state can be maintained for a long time, which reduces the maintenance cost and frequency, the maximum value and average value of the derailment coefficient of the track after using the anti-friction paste are both within a small range, and are far lower than the specified value, which helps to improve the safety of the track, the anti-friction paste is used in a small amount but can provide a long-lasting lubricating effect, which not only reduces the amount of material used, but also improves the operating efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a line graph of the derailment coefficient measured before and after lubrication with the new polymer nano-friction reducing paste.

[0022] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0025] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0026] Example

[0027] A new type of polymer nano anti-friction paste

[0028] The anti-friction paste comprises the following components in percentage by weight:

[0029] Base oil: LUAN1030%, pentaerythritol ester 48%; auxiliary materials: lithium hydroxide monohydrate 2.6%, 12-hydroxystearic acid 7%, stearic acid 3%, sebacic acid 2%, polytetrafluoroethylene 5%; additives: T6122%, T7461‰, T3213‰.

[0030] The anti-friction paste is prepared by the following steps:

[0031] S1. Add 30% LUAN10 base oil into the fat making kettle and heat it to 80°C;

[0032] S2, add 7% 12-hydroxystearic acid, heat and melt;

[0033] S3, prepare a saturated lithium hydroxide solution with 2.6% lithium hydroxide monohydrate, and slowly add 1 / 2 of the saturated lithium hydroxide solution at a temperature of 110°C;

[0034] S4. After adding the saturated lithium hydroxide solution, the temperature is rapidly raised to 149°C and maintained for 1 hour to completely dehydrate the soap base, and then the material is rapidly cooled to 96°C;

[0035] S5. Add 3% stearic acid, stir for 15 minutes, slowly add 1 / 4 of the saturated lithium hydroxide solution, and heat to 110°C;

[0036] S6, add 2% sebacic acid, stir for 15 minutes, add the remaining saturated lithium hydroxide solution, control the addition within 45 minutes, saponify the sebacic acid, raise the temperature to 149 ° C and maintain for 1 hour to complete the dehydration;

[0037] S7, first add 13% pentaerythritol ester, quickly raise the temperature to 200°C and maintain for 20 minutes;

[0038] S8, adding 35% of pentaerythritol ester to rapidly cool the fat base;

[0039] S9, add 5% polytetrafluoroethylene, continue stirring and cool to 66°C;

[0040] S10, adding 2% T612, 1‰ T746 and 3‰ T321, grinding to obtain the finished product of the anti-friction paste.

[0041] Results Analysis

[0042] The rails were coated with the novel polymer nano anti-friction paste in the embodiment, and the derailment coefficients of the sections before and after lubrication were measured. Figure 1 .

[0043] Depend on Figure 1It can be seen that the maximum and average values ​​of the derailment coefficients measured before and after lubrication are within a relatively small range. The maximum value before lubrication is 0.255, and the maximum value after lubrication is 0.226, both of which are far less than the specified values.

[0044] After testing, the friction coefficient of the wear surface inside the track was reduced from the original μ=0.4-0.5 to μ=0.2.

[0045] In summary, the invention has small dosage, long durability, excellent wear-reducing effect, and is suitable for promotion and use.

[0046] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0047] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A new type of polymer nano anti-friction paste, Features: The invention comprises the following components in weight percentage: base oil: LUAN10 20-40%, pentaerythritol ester 35-55%; auxiliary materials: lithium hydroxide monohydrate 2-3%, 12-hydroxystearic acid 5-10%, stearic acid 2-6%, sebacic acid 1-3%, polytetrafluoroethylene 3-6%; additives: T612 1-3%, T746 1-3‰, T321 1-3‰.

2. A novel polymer nano-friction reducing paste according to claim 1, Features: The invention comprises the following components in weight percentage: base oil: LUAN10 20-35%, pentaerythritol ester 40-50%; auxiliary materials: lithium hydroxide monohydrate 2.2-2.8%, 12-hydroxystearic acid 5.5-8%, stearic acid 2-5%, sebacic acid 1-2.5%, polytetrafluoroethylene 3-5%; additives: T612 1-2.5%, T746 1-2‰, T321 1.5-3‰.

3. A novel polymer nano-friction reducing paste according to claim 2, Features: The invention comprises the following components in weight percentage: base oil: LUAN10 25-30%, pentaerythritol ester 45-50%; auxiliary materials: lithium hydroxide monohydrate 2.5-2.8%, 12-hydroxystearic acid 6-8%, stearic acid 3-4%, sebacic acid 1.5-2%, polytetrafluoroethylene 3.5-5%; additives: T612 1.5-2%, T746 1.5-2‰, T321 2-3‰.

4. A novel polymer nano-friction reducing paste according to claim 3, Features: The invention comprises the following components in weight percentage: base oil: LUAN10 30%, pentaerythritol ester 48%; auxiliary materials: lithium hydroxide monohydrate 2.6%, 12-hydroxystearic acid 7%, stearic acid 3%, sebacic acid 2%, polytetrafluoroethylene 5%; Additives: T6122%, T7461‰, T3213‰.

5. A novel polymer nano anti-friction paste according to claim 4, Features: The anti-friction paste is prepared by the following steps: S1, add the LUAN10 base oil into the fat making kettle and heat it to 80°C; S2, adding the 12-hydroxystearic acid and heating to melt; S3, preparing the lithium hydroxide monohydrate into a saturated lithium hydroxide solution, slowly adding 1 / 2 of the saturated lithium hydroxide solution, the temperature is 110° C.; S4, after adding the saturated lithium hydroxide solution, the temperature is rapidly raised to 149°C and maintained for 1 hour to completely dehydrate the soap base, and then the material is rapidly cooled to 96°C; S5, add the stearic acid, stir for 15 minutes, slowly add 1 / 4 of the saturated lithium hydroxide solution, and heat to 110°C; S6, add the sebacic acid, stir for 15 minutes, add the remaining saturated lithium hydroxide solution, control the addition within 45 minutes, saponify the sebacic acid, raise the temperature to 149 ° C and maintain for 1 hour to complete the dehydration; S7, first add 13% of the pentaerythritol ester, quickly raise the temperature to 200° C. and maintain for 20 minutes; S8, adding 35% of the pentaerythritol ester to rapidly cool the fat base; S9, adding the polytetrafluoroethylene, continuing to stir and cool to 66°C; S10, adding the T612, T746 and T321, and grinding to obtain the finished product of the anti-friction paste.