High-magnetic-induction non-oriented high silicon steel ultrathin strip and preparation method and application thereof

Through the combination of warm rolling and cold rolling, the problems of non-oriented high-silicon steel thin strips in high magnetic induction and low iron loss are solved, and ultra-thin and high-performance high-silicon steel materials are realized, which simplifies the process and reduces costs. In the fields of motor cores and other fields.

CN118895412AActive Publication Date: 2024-11-05CHINA IRON & STEEL RESEARCH INSTITUTE GROUP CO LTD

Patent Information

Application Number
CN202411022091.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-05
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The existing thin strips of unoriented high-silicon steel are difficult to achieve high magnetic induction and low iron loss at the same time during the preparation process, and there are problems such as complex process, environmental pollution and high cost, especially when obtaining ultra-thin materials.

Method used

By combining warm rolling and cold rolling, a reasonable process route is designed by controlling the rolling temperature, pressure rate and annealing time, a high-magnetic inductance, non-orientation, high-silicon steel ultra-thin belt is realized. Ensure the thickness is ≤0.1mm, the magnetic inductance B50≥1.62T, iron loss P1.0/400<15W/kg, and suppress the formation of unfavorable γ-line texture.

Benefits of technology

It realizes the preparation of high-silicon steel ultra-thin belts with high magnetic inductance, low iron loss and isotropicity. It has simple process, low cost and environmentally friendly, and is suitable for lightweight and high efficiency motor core manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895412A_ABST
    Figure CN118895412A_ABST
Patent Text Reader

Abstract

The invention relates to a high-magnetic-induction non-oriented high silicon steel ultrathin strip as well as a preparation method and application thereof, belongs to the technical field of non-oriented silicon steel, and solves at least one of the following problems of an existing preparation method and an existing product of the non-oriented high silicon steel ultrathin strip: high magnetic induction and low iron loss are difficult to realize while isotropic magnetic performance is maintained; very thin materials are difficult to realize while high isotropic magnetic induction and excellent comprehensive magnetic performance are obtained; the process route is complex, the environment is polluted, and the cost is high. A preparation method of a high-magnetic-induction non-oriented high-silicon steel ultrathin strip comprises the steps that S1, warm rolling is conducted, specifically, a high-silicon steel casting thin plate is subjected to warm rolling to form a warm-rolled plate, oil quenching and acid pickling are conducted after annealing, and an annealed warm-rolled plate is obtained; and S2, cold rolling, wherein the annealed warm-rolled plate is cold-rolled into a cold-rolled plate with the thickness smaller than or equal to 0.1 mm, and annealing is conducted. The method is simple in process route, low in cost and environmentally friendly, and the non-oriented high silicon steel ultrathin strip which is ultrathin in thickness, isotropic, high in magnetic induction and excellent in comprehensive magnetic performance can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of non-oriented silicon steel, and in particular to an ultra-thin strip of high magnetic induction non-oriented high silicon steel and a preparation method and application thereof. Background Art

[0002] Non-oriented high silicon steel strips have broad application prospects in high-end motors used at medium and high frequencies. With the increasing requirements for miniaturization of cores, lightweight design, and high efficiency, it is necessary to improve the magnetic properties of high silicon steel strips and further reduce their thickness.

[0003] The existing preparation methods of high silicon steel strip mainly include: traditional rolling method, non-traditional rolling method (such as chemical vapor deposition method, spray forming method, powder rolling method), however, these preparation methods and the obtained high silicon steel strip have the following problems: according to existing research, in most cases, it is difficult to meet the following magnetic property requirements: that is, to obtain high magnetic induction (such as B) while ensuring a small degree of anisotropy. 50 Reach 1.6 or more) and low iron loss (such as P 1.0 / 400 Less than 15W / kg), high silicon steel thin strip is prone to anisotropy during the preparation process, that is, the magnetic properties vary in different directions. It is a technical challenge to control this difference within a small range while meeting the requirements of high magnetic induction and low iron loss. It is difficult to prepare high silicon steel ultra-thin strips that meet the above magnetic property requirements by traditional rolling methods; only a small part of non-traditional rolling methods can approach the above magnetic property requirements, but there are problems such as complex process routes (such as powder rolling method), limited thickness (such as spray forming method), environmental pollution, and high cost (such as chemical vapor deposition method).

[0004] In summary, for non-oriented high-silicon steel ultra-thin strip, it is necessary to develop a relatively simple, low-cost, environmentally friendly processing technology that can obtain high magnetic induction and excellent comprehensive magnetic properties. Summary of the invention

[0005] In view of the above analysis, the present invention aims to provide a high magnetic induction non-oriented high silicon steel ultra-thin strip and its preparation method and application, so as to solve at least one of the following problems existing in the preparation method of the existing non-oriented high silicon steel strip and its products: (1) it is difficult to achieve high magnetic induction (B 50 >1.6T) and low iron loss (P 1.0 / 400 <15W / kg) while maintaining isotropic magnetic properties; (2) it is difficult to achieve very thin materials (for example: thickness ≤0.1mm) while obtaining high isotropic magnetic induction and excellent comprehensive magnetic properties; (3) the process route is complex, environmentally polluting and costly.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a high magnetic induction non-oriented high silicon steel ultra-thin strip, comprising the following steps:

[0008] S1, warm rolling: preheat the high silicon steel cast sheet with a thickness H0 of 1 to 3 mm to a temperature T1 = 780 to 850°C, and warm roll it into a warm rolled sheet with a thickness H1 of 0.5 to 0.7 mm, and the temperature range of the warm rolling is set to 600 to 750°C;

[0009] The warm rolled sheet is annealed at a temperature of T2 = 800-900°C and a time of t2 = 15-25 min. After annealing, the sheet is oil quenched and pickled to obtain an annealed warm rolled sheet.

[0010] S2, cold rolling: preheat the annealed warm-rolled sheet to a temperature of T3 = 290-310°C, and cold-roll the sheet to a thickness of H2 ≤ 0.1 mm, wherein the temperature range of the cold rolling is set at room temperature to 250°C;

[0011] The cold-rolled sheet is annealed at an annealing temperature of T4=800-900°C and an annealing time of t4=45-90min to obtain a high magnetic induction non-oriented high silicon steel ultra-thin strip.

[0012] Further, in step S1, the total reduction rate R of the warm rolling is a 50-70%, the rolling pass M is 2-4, and the reduction rate of each pass R a1 To R aM Controlled between 20% and 35%.

[0013] Further, in step S2, the total reduction ratio R of the cold rolling is b 80-92%, the rolling pass N is 3-5 times, and the reduction rate of each pass R b1 To R bN Controlled between 15 and 40%.

[0014] Further, in step S2, the first pass reduction rate R of the cold rolling is b1 Controlled at 35-40%, the subsequent pass reduction rate R b2 To R bN Controlled between 15 and 38%.

[0015] Further, in step S1, the annealing time t2=18-22 min; and / or, in step S2, the annealing time t4=50-70 min.

[0016] Further, T2=T4=820-880°C; and / or, T1=780-820°C; and / or, T3=295-305°C.

[0017] Furthermore, in step S2, before annealing, the annealing furnace is first heated to T4, and then the cold-rolled sheet is placed therein.

[0018] Further, in step S1, the preheating to temperature T1 is followed by heat preservation, and the heat preservation time t1 = 20 to 40 minutes; and / or, in step S2, the preheating to temperature T3 is followed by heat preservation, and the heat preservation time t3 = 5 to 10 minutes.

[0019] In a second aspect, the present invention further provides a high magnetic induction non-oriented high silicon steel ultra-thin strip obtained by the preparation method described in the first aspect, wherein the thickness of the high magnetic induction non-oriented high silicon steel ultra-thin strip is ≤0.1 mm, and the magnetic induction B 50 ≥1.62T, iron loss P 1.0 / 400 <15W / kg, the absolute value of the longitudinal and transverse difference of magnetic induction S1 is <2.0%, and the absolute value of the longitudinal and transverse difference of iron loss S2 is <2.0%.

[0020] The present invention also provides the use of the high magnetic induction non-oriented high silicon steel ultra-thin strip obtained by the preparation method as described in the first aspect or the high magnetic induction non-oriented high silicon steel ultra-thin strip as described in the second aspect in a motor.

[0021] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0022] (1) The preparation method provided by the present invention eliminates the hot rolling process, has a simple process route, low cost, and is environmentally friendly, and can produce ultra-thin, isotropic, high magnetic induction, and excellent comprehensive magnetic properties of non-oriented high silicon steel ultra-thin strips; through the tacit cooperation of warm rolling and cold rolling, the plasticization is gradually enhanced to improve the processing performance, and a high magnetic induction non-oriented high silicon steel ultra-thin strip with a thickness of ≤0.1mm is successfully produced; through the reasonable ratio of warm rolling and cold rolling reduction rates, combined with the design of rolling process and annealing system, under the condition of ensuring good processing performance, the unfavorable γ line (plate normal ND / / <111> ) texture formation, obtaining uniform and appropriately sized grain structure, and reducing magnetic anisotropy, so that the obtained high silicon steel ultra-thin strip can exhibit high magnetic induction and low iron loss in all directions, that is, to achieve high magnetic induction B while ensuring that the absolute value of the difference between the iron loss and the longitudinal and transverse directions of the magnetic induction is less than 2%. 50 ≥1.62T, low iron loss P 1.0 / 400<15W / kg. Specifically, the reduction rate of warm rolling (rolling from 1 to 3 mm to 0.5 to 0.7 mm) is used to ensure that a higher cold rolling reduction rate can be achieved in the subsequent process, and a larger cold rolling reduction rate (rolling from 0.5 to 0.7 mm to 0.1 mm and below) is used to effectively suppress the unfavorable γ-line texture after cold rolling annealing; through the carefully designed warm rolling process and annealing system after warm rolling, such as controlling the preheating temperature T1 before warm rolling, the warm rolling temperature range, the annealing temperature T2 after warm rolling, the annealing time t2, and the oil quenching and rapid cooling after annealing, the processability can be guaranteed. At the same time, the unfavorable γ-line texture is suppressed, and a uniform and appropriately grown grain structure is obtained, providing a good foundation for achieving high magnetic induction, low iron loss and isotropy of the final product; through carefully designed cold rolling process and annealing system after cold rolling, such as controlling the preheating temperature T3 before cold rolling and the cold rolling temperature range, as well as the annealing temperature T4 and annealing time t4 after cold rolling, the unfavorable γ-line texture can be suppressed, and a uniform and appropriately sized grain structure can be obtained, thereby improving the magnetic induction and reducing the iron loss while ensuring a very small degree of anisotropy.

[0023] (2) In some preferred embodiments, during the warm rolling process, by selecting a suitable total reduction rate, rolling passes, and controlling the reduction rate of each pass within a suitable range, the isotropy of the material can be further improved and the unfavorable γ-ray texture formation can be reduced while ensuring the processability of the material. This is also conducive to obtaining more uniform and moderately grown coarse grains, thereby providing a better basis for improving the isotropic magnetic properties of the final product.

[0024] (3) In some preferred embodiments, during the cold rolling process, by selecting a suitable total reduction rate, rolling passes, and controlling the reduction rate of each pass within a suitable range, the isotropy of the material can be further improved and the unfavorable γ-ray texture formation can be reduced while ensuring the material processability, which is also conducive to obtaining more uniform and appropriately sized grains, thereby further improving the isotropic magnetic properties of the final product.

[0025] (4) In some preferred embodiments, after warm rolling and cold rolling, by selecting a more suitable annealing temperature and annealing time (such as: T2 = T4 = 820-880°C, t2 = 18-22min, t4 = 50-70min), it is beneficial to further reduce the formation of unfavorable γ-ray texture and obtain a more uniform and appropriately sized grain structure, thereby further improving the magnetic properties of the final product and reducing the difference in anisotropic magnetic properties. Before warm rolling and cold rolling, by selecting a more suitable preheating temperature (such as T1 = 780-820°C; T3 = 295-305°C) and controlling the holding time after reaching the preheating temperature (such as t1 = 20-40min, t3 = 5-10min), it is beneficial to improve the processing performance, reduce the number of rolling passes, improve the processing efficiency, and further improve the anisotropic magnetic properties of the product while ensuring product quality.

[0026] (5) In some preferred embodiments, before annealing after cold rolling, the annealing furnace is first heated to a preset temperature T4 and then the cold-rolled sheet is placed in the annealing furnace. This can reduce the release of stored energy during the heating process of the cold-rolled sheet, is beneficial to suppressing the γ-ray recrystallization texture, and helps to further improve the overall magnetic properties.

[0027] (6) The preparation method of the present invention can obtain an ultra-thin non-oriented high-silicon steel sheet with a thickness of ≤0.1 mm, which has excellent performance in magnetic properties, such as high magnetic induction, low iron loss and low anisotropy, and has broad application prospects, especially in the field of motor core manufacturing that requires lightweight, miniaturization and high efficiency.

[0028] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0030] Figure 1 The microstructure and texture diagram of the non-oriented high silicon steel ultra-thin strip prepared in Example 1 of the present invention, wherein (a) is the microstructure diagram and (b) is the texture diagram;

[0031] Figure 2 The microstructure and texture diagram of the non-oriented high silicon steel ultra-thin strip prepared in Example 2 of the present invention, wherein (a) is the microstructure diagram and (b) is the texture diagram;

[0032] Figure 3 The structure and texture diagram of the high silicon steel strip prepared in Comparative Example 3, wherein (a) is the structure diagram and (b) is the texture diagram;

[0033] Figure 4 The microstructure and texture diagrams of the high silicon steel strip prepared in Comparative Example 6, wherein (a) is the microstructure diagram and (b) is the texture diagram. DETAILED DESCRIPTION

[0034] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0035] In order to solve the hardness and brittleness problem of high silicon steel, the gradual plasticization technology developed in recent years, that is, the three-step rolling method of "hot rolling-warm rolling-cold rolling" plus a reasonable heat treatment process, can produce thin-gauge high silicon steel sheets and strips. Compared with chemical vapor deposition, spray forming, and powder rolling, this technology has the advantages of energy saving and environmental protection, simpler process, and lower cost. However, the current gradual plasticization technology has the following technical bottlenecks: it is difficult to achieve high magnetic induction (B in ultra-thin high silicon steel materials. 50 >1.6T) and low iron loss (P 1.0 / 400 <15W / kg) while maintaining isotropic magnetic properties. "Ultra-thin" in the present invention refers to a thickness specification of ≤0.1mm. The applicant found in the study that the main reason for the above bottleneck is that the process design of the existing gradual plasticization technology is unreasonable, making it difficult to obtain a uniform microstructure and optimized texture while reducing the thickness, resulting in the inability to obtain an isotropic high magnetic induction and high silicon steel ultra-thin strip with excellent comprehensive magnetic properties.

[0036] Based on this, in a first aspect, the present invention provides a method for preparing a high magnetic induction non-oriented high silicon steel ultra-thin strip, comprising the following steps:

[0037] S1, warm rolling: preheat the high silicon steel cast sheet with a thickness H0 of 1 to 3 mm to a temperature T1 = 780 to 850°C, and warm roll it into a warm rolled sheet with a thickness H1 of 0.5 to 0.7 mm, and the temperature range of the warm rolling is set to 600 to 750°C;

[0038] The warm rolled sheet is annealed at an annealing temperature of T2 = 800-900°C and an annealing time of t2 = 15-25 min. After annealing, the sheet is oil quenched and pickled to obtain an annealed warm rolled sheet.

[0039] S2, cold rolling: preheat the annealed warm-rolled sheet to a temperature of T3 = 290-310°C, and cold-roll the sheet to a thickness of H2 ≤ 0.1 mm, wherein the temperature range of the cold rolling is set at room temperature to 250°C;

[0040] The cold-rolled sheet is annealed at an annealing temperature of T4=800-900°C and an annealing time of t4=45-90min to obtain a high magnetic induction non-oriented high silicon steel ultra-thin strip.

[0041] Compared with the prior art, the preparation method provided by the present invention omits the hot rolling process, has a simple process route, low cost and is environmentally friendly; through the tacit cooperation of warm rolling and cold rolling, the plasticization is gradually enhanced to improve the processing performance, and a high magnetic induction non-oriented high silicon steel ultra-thin strip with a thickness of ≤0.1mm is successfully prepared; through the reasonable ratio of warm rolling and cold rolling reduction rates, combined with the design of rolling process and annealing system, the unfavorable γ line (plate normal ND / / ) is effectively suppressed while ensuring good processing performance. <111> ) texture formation, obtaining uniform and appropriately sized grain structure, and reducing magnetic anisotropy, so that the obtained high silicon steel ultra-thin strip can exhibit high magnetic induction and low iron loss in all directions, that is, to achieve high magnetic induction B while ensuring that the absolute value of the difference between the iron loss and the longitudinal and transverse directions of the magnetic induction is less than 2%. 50 ≥1.62T, low iron loss P 1.0 / 400 <15W / kg. Specifically, the reduction rate of warm rolling (rolling from 1 to 3mm to 0.5 to 0.7mm) is used to ensure that a higher cold rolling reduction rate can be achieved in the subsequent process, and a larger cold rolling reduction rate (rolling from 0.5 to 0.7mm to 0.1mm and below) is used to effectively suppress the unfavorable γ line texture after cold rolling annealing; through the carefully designed warm rolling process and annealing system after warm rolling, such as controlling the preheating temperature T1 before warm rolling, the warm rolling temperature range, the annealing temperature T2 after warm rolling, the annealing time t2, and the oil quenching and rapid cooling after annealing, it can be Suppressing the unfavorable γ-line texture and obtaining a uniform and moderately grown grain structure provides a good foundation for achieving high magnetic induction, low iron loss and isotropy of the final product; through carefully designed cold rolling process and post-cold rolling annealing system, such as controlling the preheating temperature T3 before cold rolling and the cold rolling temperature range, as well as the post-cold rolling annealing temperature T4 and annealing time t4, the unfavorable γ-line texture can be suppressed, and a uniform and appropriately sized grain structure can be obtained, thereby improving the magnetic induction and reducing the iron loss while ensuring a very small degree of anisotropy.

[0042] Specifically, in step S1, the initial thickness H0 of the high silicon steel cast sheet is 1-3 mm, and this thickness range is suitable for direct warm rolling without hot rolling thinning, thereby further simplifying the processing steps and reducing energy consumption.

[0043] Specifically, in step S1, the high silicon steel cast sheet is first preheated to a temperature of T1 = 780-850°C. Before warm rolling, the sheet is preheated to a suitable temperature (30-100°C higher than the upper limit of the warm rolling temperature range), which can make the warm rolling process easier, improve processing performance, reduce defects, and make the material deform more uniformly during warm rolling, which helps to obtain a more uniform microstructure, improve the isotropy of magnetic properties, and is conducive to controlling the deformation mechanism of the material, thereby inhibiting the formation of unfavorable γ-ray textures, and promoting a certain degree of recovery of the material during warm rolling, which provides a good foundation for the subsequent formation of uniform grain structure, thereby improving the isotropic magnetic properties of the material. Preferably, T1 = 780-820°C; illustratively, T1 = 790°C, 800°C, 810°C.

[0044] Specifically, in step S1, by controlling the total reduction rate of warm rolling (rolling from 1 to 3 mm to 0.5 to 0.7 mm, i.e., the total reduction rate R a 30% to 83%), which is beneficial to ensure that a higher reduction rate can be achieved in the subsequent cold rolling process, which not only helps to reduce the anisotropy of magnetic properties, thereby providing similar magnetic properties in all directions, but also inhibits the formation of unfavorable γ-line texture and obtains a more uniform grain structure, all of which help to improve the comprehensive magnetic properties of the material.

[0045] Specifically, in step S1, by controlling the warm rolling temperature interval to set it to 600-750°C, the formation of unfavorable γ-ray texture can be suppressed, and a more uniform and moderately grown grain structure can be obtained. The specific principle is: because the nucleation of γ-ray grains mostly occurs at the grain boundary or inside the γ-ray deformation structure, within the above-mentioned appropriate warm rolling temperature interval, it is helpful to form a uniform and moderately grown grain structure. The moderately grown grain structure can reduce the number of grain boundaries, making the deformation structure more uniform, reducing the nucleation and preferential growth of γ-ray grains inside the deformation structure, thereby ensuring that there is no significant γ-ray texture in the organization and texture of the warm-rolled plate, and providing a good basis for suppressing the γ-ray texture in the subsequent cold-rolled annealed plate. Exemplarily, the temperature interval of warm rolling can be set to 625-750°C, 650-750°C, 675-750°C, 700-750°C, 725-750°C.

[0046] Specifically, in step S1, by controlling the annealing system after warm rolling, that is, setting the annealing temperature T2 = 800-900 ° C and the annealing time t2 = 15-25 min, it can promote the acquisition of a relatively coarse grain structure, provide better processing performance for subsequent cold rolling, and provide a better basis for subsequent tissue texture regulation. The specific principle is: using the above-mentioned synergistic T2 and t2, the annealed warm-rolled plate obtains a uniform and appropriately sized grain structure, inhibits the nucleation of fine γ-ray grains at the grain boundary and in the grain during the subsequent cold rolling annealing process, and is beneficial for forming a texture-optimized, uniform and moderately grown grain structure. For magnetic materials, a uniform and moderately grown grain structure helps to reduce the pinning of magnetic domain walls, improve magnetic induction, reduce iron loss, and will not bring about differences in magnetic properties of silicon steel sheets in different directions. Preferably, T2 = 820-880 ° C, t2 = 18-22 min. Exemplarily, T2=830°C, 840°C, 850°C, 860°C, 870°C, t2=19 min, 20 min, 21 min.

[0047] Specifically, in step S1, after annealing, rapid cooling by oil quenching can effectively inhibit the formation of the partially ordered phase B2 and inhibit the transformation of the B2 phase to the DO3 phase, thereby improving the subsequent cold rolling plasticity and providing better processing performance for subsequent cold rolling. Preferably, the quenching oil used for oil quenching includes: at least one of rapid bright quenching oil and environmentally friendly water-soluble quenching liquid.

[0048] It can be understood that the annealed warm-rolled sheet obtained in step S1 is pickled to remove surface oxides and make the surface clean.

[0049] Specifically, in step S2, the annealed warm-rolled plate after pickling is preheated to T3 = 290 ~ 310 ° C. Before cold rolling, the annealed warm-rolled plate is preheated to a suitable temperature (40 ~ 60 ° C higher than the upper limit of the cold rolling temperature range), which helps to improve the processing performance, improve the uniformity of the microstructure, and reduce the formation of unfavorable γ-line texture. The specific principle is: the appropriate preheating temperature can reduce the deformation resistance of the material, make the cold rolling process easier, increase the plasticity of the material, reduce the risk of cracks and fractures during the cold rolling process, and improve the processing performance; the appropriate preheating temperature helps to promote the thermal balance inside the material and reduce the structural inhomogeneity caused by uneven temperature; the appropriate preheating temperature helps to break the deformation structure that may promote the formation of γ-line texture, thereby reducing the formation of unfavorable texture. Preferably, T3 = 295 ~ 305 ° C; illustratively, T3 = 298 ° C, 300 ° C, 302 ° C.

[0050] Specifically, in step S2, by controlling the total reduction rate of cold rolling (rolling from 0.5 to 0.7 mm to 0.1 mm or less, that is, the total reduction rate R b≥80%), that is, a larger cold rolling reduction rate is used, which helps to promote the formation of specific textures, such as α*({h,1,1}<1 / h,1,2>) texture. Due to the competitive relationship between textures, promoting the formation of one texture will naturally inhibit the development of another texture, thereby inhibiting the formation of unfavorable γ-ray texture. The texture characteristics at this time also help to reduce the anisotropy of the material's magnetic properties, and uniformly improve the magnetic induction in all directions while reducing iron loss.

[0051] Specifically, in step S2, by controlling the cold rolling temperature range to be set to room temperature to 250°C, while improving the processing performance, it is beneficial to suppress the formation of unfavorable γ-line texture and promote the acquisition of a more uniform grain structure. The specific principle is: the warm cold rolling reduces the deformation resistance and work hardening of the material, so that the thinner warm-rolled plate can withstand greater deformation without breaking, and the required thickness reduction can be achieved in fewer passes, thereby improving production efficiency; because after the warm rolling annealing process in step S1, the grains are uniform and moderately grown coarse grains, the above cold rolling temperature range can promote the formation of shear bands with a suitable ratio during the silicon steel rolling process, and the shear bands can form dominant shear band η lines during subsequent annealing, thereby forming η lines with a suitable ratio ( <001> / / RD) texture, where the appropriate ratio can improve the magnetic properties (i.e., high magnetic induction, low iron loss) while ensuring that the anisotropy of the magnetic properties is small. Exemplarily, the cold rolling temperature range can be set to 50-250°C, 100-250°C, 150-250°C, 200-250°C.

[0052] Specifically, in step S2, by controlling the annealing system after cold rolling, that is, setting the annealing temperature T4=800-900°C and the annealing time t4=45-90min, the formation of unfavorable γ-line texture after annealing can be suppressed, and it is helpful to obtain a more uniform and appropriately sized grain structure, improve the magnetic properties in all directions, and enhance the plasticity of the final product. The specific principle is: the use of the above-mentioned synergistic T4 and t4 helps to reduce the nucleation inside the γ-line deformation grains caused by cold rolling, helps to reduce the nucleation advantage at the grain boundary, and thus reduces the formation of γ-line texture; by using appropriate T4 and t4, the grain growth rate can be adjusted. The growth rate allows the grains to nucleate uniformly inside the material, reducing the preferential growth of specific grain orientations, thereby forming a uniform and appropriately sized grain structure, while suppressing the γ-ray texture and obtaining a uniform and appropriately sized grain structure helps to improve the magnetic properties of the material and reduce the anisotropy of the magnetic properties; at the same time, a suitable annealing system helps to release the internal stress accumulated during the cold rolling process, reduce the stress concentration area, and the uniform grain structure and reduced internal stress help to improve the plasticity of the obtained strip, making it easier to deform during further processing and forming, reducing the risk of cracks and fractures in practical applications, and improving the yield and reliability. Preferably, T4 = 820 ~ 880 ° C and annealing time t4 = 50 ~ 70 min. Exemplarily, T4 = 830 ° C, 840 ° C, 850 ° C, 860 ° C, 870 ° C, t4 = 55 min, 60 min, 65 min.

[0053] In some preferred embodiments, in step S1, the total reduction ratio R of warm rolling is a 50-70%, the rolling pass M is 2-4, and the reduction rate of each pass R a1 To R aM Controlled at 20% to 35%. During the warm rolling process, by selecting a suitable total reduction rate and rolling passes and controlling the reduction rate of each pass within a suitable range, the isotropy of the material can be further improved while ensuring the processability of the material and reducing the formation of unfavorable γ-ray texture, which is also conducive to obtaining more uniform and moderately grown coarse grains, thereby providing a better basis for improving the isotropic magnetic properties of the final product. For example, the total reduction rate R of warm rolling is a The temperature of the warm rolling is 55%, 60%, and 65%, and the number of warm rolling passes is 2, 3, and 4.

[0054] In some preferred embodiments, in step S2, the total cold rolling reduction ratio R b 80-92%, the rolling pass N is 3-5 times, and the reduction rate of each pass R b1 To R bNIn the cold rolling process, by selecting a suitable total reduction rate and rolling passes and controlling the reduction rate of each pass within a suitable range, the isotropy of the material can be further improved while ensuring the processability of the material and reducing the formation of unfavorable γ-ray texture, which is also conducive to obtaining more uniform and appropriately sized grains, thereby further improving the isotropic magnetic properties of the final product. More preferably, the total reduction rate R b For example, the total reduction ratio R of cold rolling is 83-90%. b It is 84%, 85%, 86%, 87%, 88%, and 89%; the cold rolling passes N are 3, 4, and 5.

[0055] In some preferred embodiments, the first pass reduction rate R of cold rolling is b1 Controlled at 35-40%, the subsequent pass reduction rate R b2 To R bN Controlled at 15-38%. Such a setting has the following benefits: (1) Improving processing performance: A higher reduction rate in the first pass can quickly reduce the thickness of the material. With the first cold rolling, the temperature will drop, and the material will undergo work hardening. Reducing the reduction rate in subsequent passes will help adapt to the increased deformation resistance due to hardening and keep the processing process going smoothly; (2) Improving overall magnetic properties: Related to the temperature range of rolling, a larger deformation in the first pass can promote the formation of favorable textures, while a smaller reduction rate in the subsequent pass can help suppress the development of unfavorable γ-line textures and help obtain a uniform and moderately grown grain structure, thereby optimizing the overall magnetic properties, improving magnetic induction and reducing iron loss, and ensuring that the magnetic properties of the material in all directions are less different. For example, the first cold rolling reduction rate R b1 Controlled at 36%, 37%, 38%, 39%, and the subsequent pass reduction rate R b2 To R bN Controlled at 18%, 20%, 25%, 30%, 35%. In a possible design, the subsequent pass reduction rate R b2 To R bN In descending order.

[0056] In some preferred embodiments, in step S2, before annealing, the annealing furnace is first heated to T4, and then the cold-rolled sheet is placed therein; since the annealing furnace has been pre-heated to T4, the cold-rolled sheet can quickly reach the desired temperature T4 after being placed therein, thereby reducing the release of stored energy during the heating process of the cold-rolled sheet, because once the stored energy is reduced, the unfavorable γ-ray texture will be enhanced, while the favorable texture will be weakened; therefore, quickly heating the cold-rolled sheet to the annealing temperature T4 is beneficial to suppressing the γ-ray recrystallization texture, thereby helping to improve the overall magnetic properties.

[0057] In some preferred embodiments, in step S1, the steel is preheated to temperature T1 and then kept warm for a time of t1=20-40 min; in step S2, the steel is preheated to temperature T3 and then kept warm for a time of t3=5-10 min. The above-mentioned suitable holding time is conducive to improving the processing performance of subsequent warm rolling and cold rolling, and is also conducive to microstructure optimization, reducing unfavorable γ-ray texture, and improving grain uniformity, thereby helping to improve the magnetic properties of the material in all directions (improving magnetic induction and reducing iron loss).

[0058] In some preferred embodiments, during the warm rolling process of step S1, the temperature is raised to T1 and kept for 1 to 2 minutes between passes to ensure that the warm rolling temperature is within the set range, which is beneficial to the smoothness of processing and also beneficial to microstructure control and texture optimization.

[0059] It should be noted that during the cold rolling process of step S2, when the cold rolling temperature range is set to room temperature to 250°C, there is no need to heat the steel sheet in between passes to improve efficiency. In some possible designs, when the lower limit of the cold rolling temperature range is higher than room temperature, for example, it is set to 50-250°C, 100-250°C, 150-250°C, or 200-250°C, the steel sheet is heated to T3 between passes, but no insulation is required.

[0060] Preferably, in steps S1 and S2, the "annealing" is performed under the protection of an inert gas; more preferably, preheating before warm rolling and preheating before cold rolling are also performed under the protection of an inert gas. Exemplarily, the inert gas is nitrogen.

[0061] In a second aspect, the present invention further provides a high magnetic induction non-oriented high silicon steel ultra-thin strip obtained by the preparation method as described above, wherein the thickness H2 of the high magnetic induction non-oriented high silicon steel ultra-thin strip is ≤0.1 mm, and the magnetic induction B 50 ≥1.62T, iron loss P 1.0 / 400 <15W / kg, the absolute value of the longitudinal and transverse difference of magnetic induction S1 is <2.0%, and the absolute value of the longitudinal and transverse difference of iron loss S2 is <2.0%.

[0062] Exemplarily, the thickness of the high magnetic induction non-oriented high silicon steel ultra-thin strip is 0.08 mm, 0.06 mm, 0.05 mm, 0.04 mm, or 0.03 mm.

[0063] In some possible designs, the chemical composition of the high magnetic induction non-oriented high silicon steel ultra-thin strip includes, by weight percentage: Si: 5.5%-6.6%, C≤0.02%, Mn≤0.04%, N≤0.004%, P≤0.01%, S≤0.005%, and the rest is Fe and unavoidable impurities.

[0064] The present invention also provides the use of the high magnetic induction non-oriented high silicon steel ultra-thin strip prepared by the preparation method described in the first aspect or the high magnetic induction non-oriented high silicon steel ultra-thin strip described in the second aspect in a motor; for example: in a motor core.

[0065] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and comparative examples.

[0066] Embodiment 1:

[0067] The present embodiment provides a method for preparing a high magnetic induction non-oriented high silicon steel ultra-thin strip, wherein the chemical composition of the high magnetic induction non-oriented high silicon steel ultra-thin strip comprises, by weight percentage, Si: 6.2%, C: 0.018%, Mn: 0.015%, N: 0.0038%, P: 0.006%, S: 0.004%, and the rest is Fe and unavoidable impurities; the preparation method comprises the following steps:

[0068] S1. Warm rolling: Preheat the high silicon steel cast sheet with a thickness of 1.5 mm to T1 = 800 ° C and keep it warm for 30 minutes, and then warm roll it into a warm rolled sheet with a thickness of 0.6 mm. The warm rolling temperature range is set to 600-750 ° C, the total reduction rate is 60%, the rolling passes are 3 times, and the first pass reduction rate R a1 , the second pass reduction rate R a2 , the third pass reduction rate R a3 They are 33%, 25% and 20% respectively. The strip outlet temperature is detected to be lower than 600℃ between passes. After returning to the furnace and heating to 800℃, it is kept at this temperature for 1.5min and then continues rolling until it is rolled to 0.6mm.

[0069] The warm rolled plate was annealed at T2 = 850 ° C, the annealing time was t2 = 20 min, and after annealing, it was quickly cooled by oil quenching in rapid bright quenching oil 7101 (produced by Yingji Lubrication Technology), and pickled to obtain an annealed warm rolled plate;

[0070] Among them, the main steps of pickling include: first, clean the surface of the warm-rolled plate after oil quenching to remove impurities such as oil and dust to ensure the pickling effect. Subsequently, immerse the cleaned warm-rolled plate in a hydrochloric acid aqueous solution with a concentration of about 20% for pickling. The pickling time is set to 10 minutes. After pickling, rinse with clean water to remove the residual acid and dissolved products on the surface to prevent the acid residue from corroding the silicon steel. Finally, dry the warm-rolled plate, wash it with anhydrous ethanol and store it in a container filled with a desiccant to maintain its surface quality and prevent oxidation;

[0071] S2, cold rolling: the pickled annealed warm rolled sheet is preheated to T3 = 300 ° C and then kept warm for 7 minutes, and then cold rolled into a cold rolled sheet with a thickness of 0.09 mm, wherein the cold rolling temperature range is set at room temperature to 250 ° C, the total reduction rate is 85%, the rolling passes are 4 times, and the first pass reduction rate R b1 The second pass reduction rate is 40%, b2 The third and fourth pass reduction ratios are 38%. b3 and R b4 Both are 36%;

[0072] The cold-rolled sheet is annealed at T4=850°C and the annealing time is t4=60min to obtain a high magnetic induction non-oriented high silicon steel ultra-thin strip.

[0073] The microstructure texture of the non-oriented high silicon steel ultra-thin strip obtained in this embodiment is as follows: Figure 1 As shown, from Figure 1 In (a), the blue-marked grains are {111} (i.e., γ-ray) grains. It can be seen that the proportion of unfavorable γ-ray grains in this embodiment is low. In terms of grain size, there is no abnormal growth of grains (i.e., the size of individual grains exceeds 10 times the average grain size), and the structure is relatively uniform. The same information can be obtained from Figure (1) b. The triangle of the inverse pole figure has a low intensity at {111}, which proves that the proportion of {111} grains is small. Based on the uniform and moderately grown grain structure and the low proportion of unfavorable γ-ray grains, the magnetic properties of this embodiment are as follows: Longitudinal magnetic induction B 50 =1.656T, longitudinal and transverse magnetic induction difference S1 = -0.7%; longitudinal iron loss P 1.0 / 400 =12.7W / kg, longitudinal and transverse iron loss difference S2 = -1.5%; where S1 = (longitudinal magnetic induction B 50 - Transverse magnetic induction B 50 ) / longitudinal magnetic induction B 50 , S2=(longitudinal iron loss P 1.0 / 400 - Transverse iron loss P 1.0 / 400 ) / longitudinal iron loss P 1.0 / 400 It can be seen that the present embodiment can obtain an ultra-thin high-silicon steel sheet with a thickness of ≤0.1 mm, which has excellent performance in magnetic properties, such as high magnetic induction, low iron loss and low anisotropy, and has broad application prospects, especially in the field of motor core manufacturing that requires lightweight, miniaturization and high efficiency.

[0074] Example 2

[0075] The difference between this embodiment and embodiment 1 is that in step S1, a high silicon steel cast sheet with a thickness of 2.0 mm is warm rolled into a warm rolled sheet with a thickness of 0.6 mm, with a total reduction rate of 70%, 4 rolling passes, and a first rolling reduction rate of R a1The second to fourth pass reduction ratio is 35%. a2 , R a3 , R a4 The remaining steps and parameters are the same as those in Example 1.

[0076] The microstructure texture of the non-oriented high silicon steel ultra-thin strip obtained in this embodiment is as follows: Figure 2 As shown, from Figure 2 In (a), the blue-marked grains are {111} (i.e., γ-ray) grains. It can be seen that in this embodiment, the proportion of unfavorable γ-ray grains is relatively low. In terms of grain size, there is no abnormal growth of grains (i.e., the size of individual grains exceeds the average grain size by more than 10 times), and the structure is relatively uniform. The same information can be obtained from Figure (2)b. The triangle of the inverse pole figure has a low intensity at {111}, which proves that the proportion of {111} grains is relatively small.

[0077] Example 3

[0078] The difference between this embodiment and embodiment 1 is that in step S1, a high silicon steel cast sheet with a thickness of 1.0 mm is warm rolled into a warm rolled sheet with a thickness of 0.6 mm, with a total reduction rate of 40%, two rolling passes, and a first and second reduction rate of R a1 , R a2 The remaining steps and parameters are the same as those in Example 1.

[0079] Example 4

[0080] The difference between this embodiment and embodiment 1 is that in step S1, a high silicon steel cast sheet with a thickness of 1.2 mm is warm rolled into a warm rolled sheet with a thickness of 0.6 mm, with a total reduction rate of 50%, two rolling passes, and a first rolling reduction rate of R a1 The second pass reduction rate is 30%, a2 The remaining steps and parameters are the same as those in Example 1.

[0081] Example 5

[0082] The difference between this embodiment and embodiment 1 is that in step S1, the warm rolling temperature range is set to 650-750°C, and if the strip outlet temperature is detected to be lower than 650°C between passes, the strip is returned to the furnace for heating. The remaining steps and parameters are the same as those in embodiment 1.

[0083] Example 6

[0084] The difference between this embodiment and embodiment 1 is that in step S1, the warm rolling temperature range is set to 700-750°C, and if the strip outlet temperature is detected to be lower than 700°C between passes, the strip is returned to the furnace for heating. The remaining steps and parameters are the same as those in embodiment 1.

[0085] Example 7

[0086] The difference between this embodiment and embodiment 1 is that in step S1, the warm rolled sheet is annealed at T2 = 820°C for 22 minutes, and after annealing, the sheet is rapidly cooled by oil quenching in environmentally friendly water-soluble quenching liquid 7201 (produced by Yingji Lubrication Technology). The remaining steps and parameters are the same as those in embodiment 1.

[0087] Example 8

[0088] The difference between this embodiment and embodiment 1 is that in step S1, the warm rolled sheet is annealed at T2 = 880°C for annealing time t2 = 18 min. The remaining steps and parameters are the same as those in embodiment 1.

[0089] Example 9

[0090] The difference between this embodiment and embodiment 1 is that: in step S1, the warm rolled sheet is annealed at T2 = 800°C, and the annealing time t2 = 25 min. The remaining steps and parameters are the same as those in embodiment 1.

[0091] Example 10

[0092] The difference between this embodiment and embodiment 1 is that: in step S1, the warm rolled sheet is annealed at T2 = 900°C, and the annealing time t2 = 15 min. The remaining steps and parameters are the same as those in embodiment 1.

[0093] Embodiment 11

[0094] The difference between this embodiment and embodiment 1 is that in step S2, the cold-rolled sheet with a thickness of 0.1 mm is formed by cold rolling, the total reduction rate is 83%, the rolling passes are 4, and the first pass reduction rate R b1 The second to fourth pass reduction ratio is 40%. b2 , R b3 and R b4 The remaining steps and parameters are the same as those in Example 1.

[0095] Example 12

[0096] The difference between this embodiment and embodiment 1 is that in step S2, a cold-rolled sheet with a thickness of 0.06 mm is formed by cold rolling, the total reduction rate is 90%, the rolling passes are 5, and the reduction rate R from the first pass to the fifth pass is b1 ~R b5 The other steps and parameters are the same as those in Example 1.

[0097] Example 13

[0098] The difference between this embodiment and embodiment 1 is that in step S1, a high silicon steel cast sheet with a thickness of 1.5 mm is warm rolled into a warm rolled sheet with a thickness of 0.5 mm, the total reduction rate is 67%, the rolling passes are 4, and the reduction rates R from the first pass to the fourth pass are a1 ~R a4 33.3%, 25%, 20% and 16.7% respectively; in step S2, the cold-rolled sheet with a thickness of 0.04 mm is formed by cold rolling, the total reduction rate is 92%, the rolling passes are 5, and the first pass reduction rate R b1 The second to fifth pass reduction ratio is 40%. b2 ~R b5 The remaining steps and parameters are the same as those in Example 1.

[0099] Embodiment 14

[0100] The difference between this embodiment and embodiment 1 is that in step S1, a high silicon steel cast sheet with a thickness of 1.5 mm is warm rolled into a warm rolled sheet with a thickness of 0.5 mm, the total reduction rate is 67%, the rolling passes are 4, and the reduction rates R from the first pass to the fourth pass are a1 ~R a4 30%, 25%, 20% and 20% respectively; in step S2, the cold-rolled sheet with a thickness of 0.1 mm is formed by cold rolling, the total reduction rate is 80%, the rolling passes are 4, and the first pass reduction rate R b1 The second pass reduction rate is 40%, b2 The third pass reduction rate is 38%. b3 The fourth pass reduction rate is 30%, b4 The remaining steps and parameters are the same as those in Example 1.

[0101] Embodiment 15

[0102] The difference between this embodiment and embodiment 1 is that in step S2, the cold rolling temperature range is set to 100-250°C, and if the strip outlet temperature is detected to be lower than 100°C between passes, the strip is returned to the furnace for heating. The remaining steps and parameters are the same as those in embodiment 1.

[0103] Example 16

[0104] The difference between this embodiment and embodiment 1 is that in step S2, the cold rolling temperature range is set to 150-250°C, and if the strip outlet temperature is detected to be lower than 150°C between passes, the strip is returned to the furnace for heating. The remaining steps and parameters are the same as those in embodiment 1.

[0105] Embodiment 17

[0106] The difference between this embodiment and embodiment 1 is that in step S2, the cold-rolled sheet is annealed at T4 = 820°C, and the annealing time t4 = 70 min. The remaining steps and parameters are the same as those in embodiment 1.

[0107] Embodiment 18

[0108] The difference between this embodiment and embodiment 1 is that in step S2, the cold-rolled sheet is annealed at T4 = 880°C for annealing time t4 = 50 min. The remaining steps and parameters are the same as those in embodiment 1.

[0109] Embodiment 19

[0110] The difference between this embodiment and embodiment 1 is that in step S2, the cold-rolled sheet is annealed at T4 = 800°C, and the annealing time t4 = 90 min. The remaining steps and parameters are the same as those in embodiment 1.

[0111] Embodiment 20

[0112] The difference between this embodiment and embodiment 1 is that in step S2, the cold-rolled sheet is annealed at T4 = 900°C for annealing time t4 = 45 min. The remaining steps and parameters are the same as those in embodiment 1.

[0113] Embodiment 21

[0114] The difference between this embodiment and embodiment 1 is that in step S2, before annealing, the cold-rolled sheet is placed in an annealing furnace, and then the annealing furnace is heated to an annealing temperature T4 = 850° C. The remaining steps and parameters are the same as those in embodiment 1.

[0115] Comparative Example 1

[0116] The difference between this comparative example and Example 1 is that in step S1, a high silicon steel cast sheet with a thickness of 2.5 mm is warm rolled into a warm rolled sheet with a thickness of 0.35 mm, the total reduction rate is 86%, the rolling passes are 4, and the reduction rate R from the first pass to the third pass is a1 , R a2 , R a3 Both are 40%, the fourth pass reduction rate R a4 In step S2, the cold-rolled sheet is formed into a cold-rolled sheet with a thickness of 0.09 mm, the total reduction ratio is 74%, the number of rolling passes is 4, and the first rolling reduction ratio R b1 The second pass reduction rate is 40%, b2 The third pass reduction rate is 25%. b3 The fourth pass reduction rate is 25%. b4 The remaining steps and parameters are the same as those in Example 1.

[0117] Comparative Example 1 does not adopt the reasonable ratio of the total reduction rate of warm rolling and cold rolling provided by the present invention (i.e., warm rolling from 1 to 3 mm to 0.5 to 0.7 mm, and cold rolling from 0.5 to 0.7 mm to 0.1 mm and below), so the magnetic properties and processing performance are not as good as those of the present invention, which are specifically manifested as follows: Magnetic induction B 50 The absolute value of the difference S1 between the longitudinal and transverse magnetic induction is larger, that is, the degree of anisotropy is greater.

[0118] Comparative Example 2

[0119] The difference between this comparative example and Example 1 is that in step S1, a high silicon steel cast sheet with a thickness of 1.0 mm is warm rolled into a warm rolled sheet with a thickness of 0.8 mm, with a total reduction rate of 20%, one rolling pass, and a reduction rate R a1 In step S2, the cold-rolled sheet is formed into a cold-rolled sheet with a thickness of 0.09 mm, the total reduction ratio is 89%, the number of rolling passes is 5, and the first rolling reduction ratio R b1 The second pass reduction rate is 40%, b2 The third pass reduction rate is 35%. b3 The fourth pass reduction rate is 35%. b4 The fifth pass reduction rate is 35%. b5 The remaining steps and parameters are the same as those in Example 1.

[0120] Comparative Example 2 does not adopt the appropriate range of total reduction rate of warm rolling provided by the present invention (i.e., warm rolling from 1 to 3 mm to 0.5 to 0.7 mm), so the magnetic properties and processing performance are not as good as those of the present invention, which are specifically manifested as follows: Magnetic induction B 50 Low iron loss P 1.0 / 400 The absolute value of the difference between the longitudinal and transverse magnetic induction S1 increases, that is, the degree of anisotropy is large.

[0121] Comparative Example 3

[0122] The difference between this comparative example and Example 1 is that in step S1, the warm rolling temperature range is set to 500-590° C., and the strip outlet temperature is detected to be lower than 500° C. between passes, and the strip is returned to the furnace and heated to 590° C. The remaining steps and parameters are the same as those in Example 1.

[0123] Comparative Example 3 does not adopt the preferred range of warm rolling temperature provided by the present invention (i.e., 600-750°C), so the magnetic properties and processing performance are not as good as those of the present invention, which are specifically manifested as follows: 50 Low iron loss P 1.0 / 400 The absolute value of the difference S1 between the longitudinal and transverse magnetic induction is larger, that is, the degree of anisotropy is greater.

[0124] The microstructure texture of the non-oriented high silicon steel ultra-thin strip obtained in Comparative Example 3 is as follows: Figure 3 As shown, from Figure 3 In (a), the blue-marked grains are {111} (i.e., γ-ray) grains. It can be seen that in this comparative example, the proportion of unfavorable γ-ray grains is relatively high. In terms of grain size, there are more small-sized grains, and the organizational uniformity is not as good as that of the embodiment of the present invention. The above points are not conducive to reducing iron loss. The same information can be obtained from Figure (3)b. The triangle of the inverse pole figure has a higher intensity at {111}, which proves that the proportion of {111} grains is relatively large.

[0125] Comparative Example 4

[0126] The difference between this comparative example and Example 1 is that in step S1, the warm rolled sheet is annealed at T2 = 780° C. The remaining steps and parameters are the same as those in Example 1.

[0127] Comparative Example 4 does not adopt the preferred range of annealing temperature after warm rolling provided by the present invention (i.e., T2 = 800-900°C), so the magnetic properties and processing performance are not as good as those of the present invention, which are specifically manifested as follows: 50 Low iron loss P 1.0 / 400 The absolute value of the difference between the longitudinal and transverse magnetic induction S1 is larger, that is, the degree of anisotropy is larger.

[0128] Comparative Example 5

[0129] The difference between this comparative example and Example 1 is that in step S1, the warm rolled sheet is annealed at T2 = 920° C. The remaining steps and parameters are the same as those in Example 1.

[0130] Comparative Example 5 does not adopt the preferred range of annealing temperature after warm rolling provided by the present invention (i.e., T2 = 800-900°C), so the magnetic properties and processing performance are not as good as those of the present invention, which are specifically manifested as follows: 50 Low iron loss P 1.0 / 400 The absolute value of the difference between the longitudinal and transverse magnetic induction S1 is larger, that is, the degree of anisotropy is larger.

[0131] Comparative Example 6

[0132] The difference between this comparative example and Example 1 is that in step S1, a high silicon steel cast sheet with a thickness of 1.5 mm is warm rolled into a warm rolled sheet with a thickness of 0.3 mm, with a total reduction rate of 80% and a first pass reduction rate of R a1 The second pass reduction rate is 40%, a2 The third and fourth pass reduction ratios are 33.3%. a3 , R a4 In step S2, the cold-rolled sheet is formed into a cold-rolled sheet with a thickness of 0.1 mm, the total reduction rate is 67%, the rolling passes are 3 passes, and the first pass reduction rate R b1 The second pass reduction rate is 40%,b2 The third pass reduction rate is 28%. b3 The remaining steps and parameters are the same as those in Example 1.

[0133] Comparative Example 6 does not adopt the preferred range of total cold rolling reduction provided by the present invention (i.e., rolling from 0.5 to 0.7 mm to ≤ 0.1 mm, total reduction ≥ 80%), so the magnetic properties and processing performance are not as good as those of the present invention, which are specifically manifested as follows: Magnetic induction B 50 The absolute value of the difference S1 between the longitudinal and transverse magnetic induction is larger, that is, the degree of anisotropy is greater.

[0134] The microstructure texture of the non-oriented high silicon steel ultra-thin strip obtained in Comparative Example 6 is as follows: Figure 4 As shown, from Figure 4 In (a), the blue-marked grains are {111} (i.e., γ-ray) grains. It can be seen that in this comparative example, the proportion of unfavorable γ-ray grains is relatively high. The same information can be obtained from Figure (4)b. The triangle of the inverse pole figure has a higher intensity at {111}, which proves that the proportion of {111} grains is relatively large.

[0135] Comparative Example 7

[0136] The difference between this comparative example and Example 1 is that in step S2, the cold rolling temperature is set to room temperature. The remaining steps and parameters are the same as those in Example 1.

[0137] Since Comparative Example 7 does not adopt the strip warm cold rolling temperature range provided by the present invention (ie, room temperature to 250° C.), the processing performance is not as good as that of the present invention, which is specifically manifested in that edge cracking occurs in the strip during the rolling process.

[0138] Comparative Example 8

[0139] The difference between this comparative example and Example 1 is that in step S2, the cold-rolled sheet is annealed at T4 = 780° C. The remaining steps and parameters are the same as those in Example 1.

[0140] Comparative Example 8 does not adopt the preferred range of annealing temperature after cold rolling provided by the present invention (i.e., T4 = 800-900°C), so the magnetic properties and processing performance are not as good as those of the present invention, which are specifically manifested as follows: 50 Low iron loss P 1.0 / 400 The absolute value of the difference S1 between the longitudinal and transverse magnetic induction is larger, that is, the degree of anisotropy is greater.

[0141] Comparative Example 9

[0142] The difference between this comparative example and Example 1 is that in step S2, the cold-rolled sheet is annealed at T4 = 920° C. The remaining steps and parameters are the same as those in Example 1.

[0143] Comparative Example 9 does not adopt the preferred range of annealing temperature after cold rolling provided by the present invention (i.e., T4 = 800-900°C), so the magnetic properties and processing performance are not as good as those of the present invention, which are specifically manifested as follows: 50 Low iron loss P 1.0 / 400 The absolute values ​​of the longitudinal and transverse magnetic induction difference S1 and iron loss difference S2 are larger, that is, the degree of anisotropy is larger.

[0144] Comparative Example 10

[0145] The difference between this comparative example and Example 1 is that the warm-rolled annealed sheet is not subjected to oil quenching treatment, and the remaining steps and parameters are the same as those of Example 1.

[0146] Since Comparative Example 10 does not adopt the preferred operating steps provided by the present invention (ie, oil quenching after annealing in step S1), the processing performance is not as good as that of the present invention, which is specifically manifested in: fracture during rolling.

[0147] In order to more clearly show the parameter variables and performance test results of the above embodiments and comparative examples, see Table 1 and Table 2. Figure 1-2 It can be seen that in Examples 1-21, by adopting the preparation method provided by the present invention, the unfavorable γ line (plate normal ND / / ) is effectively suppressed while ensuring good processing performance. <111> ) texture formation, obtain uniform and appropriately sized grain structure, and achieve high magnetic induction B while ensuring that the absolute value of the difference between the iron loss and the longitudinal and transverse magnetic induction is less than 2%. 50 ≥1.62T, low iron loss P 1.0 / 400 <15W / kg, so that the obtained high silicon steel ultra-thin strip can show excellent magnetic properties in all directions and has good processing performance. The obtained non-oriented high silicon steel thin strip is not only very thin, but also has no defects such as cracking, and has good overall quality.

[0148] From Table 2 and Figure 3-4 It can be seen that, in comparison, the anisotropy degree of comparative examples 1-10 is larger, the magnetic induction is higher, and the overall magnetic properties are not as good as those of the present invention. Moreover, the machinability of some comparative examples is poor, and even edge cracks and fractures occur. Moreover, the unfavorable γ-ray texture accounts for a large proportion in the microstructure, and the uniformity of the grain structure is not as good as that of the present invention. It can be seen that comparative examples 1-10 have decreased overall magnetic properties, machining performance, and product quality due to the failure to adopt the preferred process steps and parameters provided by the present invention.

[0149] Table 1: Specific process parameters and performance results in the preparation methods of Examples 1-21

[0150]

[0151]

[0152]

[0153] Table 2: Specific process parameters and performance results in the preparation methods of Comparative Examples 1-10

[0154]

[0155]

[0156] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for preparing a high magnetic induction non-oriented high silicon steel ultra-thin strip, characterized in that: The following steps are involved: S1, warm rolling: preheat the high silicon steel cast sheet with a thickness H0 of 1 to 3 mm to a temperature T1 = 780 to 850°C, and warm roll it into a warm rolled sheet with a thickness H1 of 0.5 to 0.7 mm, and the temperature range of the warm rolling is set to 600 to 750°C; The warm rolled sheet is annealed at a temperature of T2 = 800-900°C and a time of t2 = 15-25 min. After annealing, the sheet is oil quenched and pickled to obtain an annealed warm rolled sheet. S2, cold rolling: preheat the annealed warm-rolled sheet to a temperature of T3 = 290-310°C, and cold-roll the sheet to a thickness of H2 ≤ 0.1 mm, wherein the temperature range of the cold rolling is set at room temperature to 250°C; The cold-rolled sheet is annealed at an annealing temperature of T4=800-900°C and an annealing time of t4=45-90min to obtain a high magnetic induction non-oriented high silicon steel ultra-thin strip.

2. The preparation method according to claim 1, characterized in that: In step S1, the total reduction ratio R of the warm rolling is a 50-70%, the rolling pass M is 2-4, and the reduction rate of each pass R a1 To R aM Controlled between 20% and 35%.

3. The preparation method according to claim 1, characterized in that: In step S2, the total reduction ratio R of the cold rolling is b 80-92%, the rolling pass N is 3-5 times, and the reduction rate of each pass R b1 To R bN Controlled between 15 and 40%.

4. The preparation method according to claim 3, characterized in that: In step S2, the first pass reduction rate R of the cold rolling is b1 Controlled at 35-40%, the subsequent pass reduction rate R b2 To R bN Controlled between 15 and 38%.

5. The preparation method according to claim 1, characterized in that: In step S1, the annealing time t2=18-22 min; and / or, in step S2, the annealing time t4=50-70 min.

6. The preparation method according to claim 1, characterized in that: T2=T4=820~880°C; and / or, T1=780~820°C; and / or, T3=295~305°C.

7. The preparation method according to claim 1, characterized in that: In step S2, before annealing, the annealing furnace is first heated to T4, and then the cold-rolled sheet is placed therein.

8. The preparation method according to claim 1, characterized in that: In step S1, the preheating to temperature T1 is followed by heat preservation, and the heat preservation time t1 is 20 to 40 minutes; and / or, in step S2, the preheating to temperature T3 is followed by heat preservation, and the heat preservation time t3 is 5 to 10 minutes.

9. A high magnetic induction non-oriented high silicon steel ultra-thin strip obtained by the preparation method as described in any one of claims 1 to 8, characterized in that: The thickness of the high magnetic induction non-oriented high silicon steel ultra-thin strip is ≤0.1mm, and the magnetic induction B 50 ≥1.62T, iron loss P 1.0 / 400 <15W / kg, the absolute value of the longitudinal and transverse difference of magnetic induction S1 is <2.0%, and the absolute value of the longitudinal and transverse difference of iron loss S2 is <2.0%.

10. Use of the high magnetic induction non-oriented high silicon steel ultra-thin strip obtained by the preparation method according to any one of claims 1 to 8 or the high magnetic induction non-oriented high silicon steel ultra-thin strip according to claim 9 in a motor.

Citation Information

Patent Citations

  • Reduction preparing method for high-magnetic-induction grain-oriented silicon steel ultra-thin belt

    CN105385937A

  • High-strength non-oriented silicon steel based on structure inheritance and preparation method of high-strength non-oriented silicon steel

    CN115747444A

  • Short-process preparation method of ultrathin high-silicon steel thin strip

    CN118180341A

  • Method for manufacturing non-oriented silicon steel sheet

    JP2020020005A

  • Method of manufacturing a grain-oriented electromagnetic steel sheet

    US20020011278A1

Cited By

  • Rolling method of elastic alloy strip foil for sensor

    CN119702685A

  • Rolling method for elastic alloy strip foil for sensors

    CN119702685B