Fluorine-free etching solution for Cu, MoNbCu and MTDCuMo and preparation method thereof

By introducing sulfonic acid and its salt compounds and amino acids, especially methylsulfonic acid and cysteine, the substrate damage and residue problems caused by fluorine compounds are solved, and the copper and molybdenum alloy layers are realized. Excellent etching performance and low loss, suitable for the two-layer film structure of liquid crystal displays.

CN118895504APending Publication Date: 2024-11-05SICHUAN HESHENGDA ELECTRONIC TECH CO LTD +1

Patent Information

Application Number
CN202410283592.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The large amount of fluorine compounds used in the existing etching liquid leads to substrate damage and high cost of waste liquid treatment. In addition, the fluorine-free etching liquid produces more residues when etching the molybdenum-containing layer in the pH 2 to 3 areas, affecting the yield of the liquid crystal display.

Method used

Provide a fluorine-free etching solution containing hydrogen peroxide, chelating agent, inhibitor, etchant, sulfonic acid and its salt compounds, amino acids and alkyl amines, especially by simultaneously introducing methylsulfonic acid and cysteine, optimized etching Performance, avoid metal residues, and control etch angles and unilateral losses.

Benefits of technology

Achieve excellent etching performance for copper and MTD alloys, copper and MoNb alloy multilayer films, reduce residue, protect glass substrates, control etch angles and losses, and is suitable for 2000-3000 Åm copper layers and 200-500 Åm molybdenum layers two-layer film structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004738340500000033
    Figure BDA0004738340500000033
  • Figure BDA0004738340500000041
    Figure BDA0004738340500000041
  • Figure BDA0004738340500000042
    Figure BDA0004738340500000042
Patent Text Reader

Abstract

The invention relates to the technical field of etching solutions, in particular to a fluoride-free etching solution for Cu, MoNbCu and MTDCuMo and a preparation method thereof.The fluoride-free etching solution at least comprises, by mass, 12%-25% of hydrogen peroxide, 0.5%-4% of a chelating agent, 0.01%-2% of an inhibitor, 0.1%-5% of an etching agent, 0.1%-3% of sulfonic acid and salt compounds thereof, 0.01%-3% of amino acid, 0.01%-1% of alkylamine and the balance deionized water. According to the present invention, without using a fluorine compound, the etching composition has excellent etching performance on a multilayer film including copper and an MTD alloy, and copper and an MoNb alloy, minimizes residual defects, and does not damage a glass substrate, thereby facilitating etching regeneration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of etching solutions, in particular to a fluorine-free etching solution for Cu, MoNbCu and MTDCuMo and a preparation method thereof. Background Art

[0002] The metal layer on the LCD substrate is usually a two-layer or three-layer structure made of copper or copper alloy and molybdenum, titanium, niobium and its alloy, such as Cu / MoNb, Cu / MTD, Cu / Mo. Generally, an etching liquid is used to make the metal layer produce a predetermined pattern, so it is very important to ensure the etching characteristics of the etching liquid for the yield of the LCD. The current etching liquid usually uses hydrogen peroxide, phosphoric acid, inhibitors, chelating agents and fluorine compounds for etching. In order to suppress residues, a large amount of fluorine is usually added. For example, Taiwan Patent (Grant Announcement No. TWI231275B) discloses a multilayer etching liquid of copper and molybdenum, including hydrogen peroxide, organic acid, phosphate, fluoride, nitrogen-containing additives, etc. However, the introduction of a large amount of fluorine will cause damage to the substrate (glass) and the lower film, affecting the yield of the LCD, and the etching liquid composition with a high fluorine content is expensive in the waste liquid treatment process, and there is a problem of increased manufacturing cost. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo, which has excellent etching performance for multilayer films including copper and MTD alloys, copper and MoNb alloys without using fluorine compounds, minimizes residual defects, and does not damage the glass substrate, thereby facilitating etching regeneration.

[0004] On the one hand, the present invention provides a fluorine-free etching solution for Cu, MoNbCu and MTDCuMo, which comprises, by mass percentage, at least: 12-25% hydrogen peroxide, 0.5-4% chelating agent, 0.01-2% inhibitor, 0.1-5% etching agent, 0.1-3% sulfonic acid and its salt compound, 0.01-3% amino acid, 0.01-1% alkylamine, and deionized water to make up the balance.

[0005] As a preferred technical solution, the fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo comprises at least 14-20% hydrogen peroxide, 1.5-3% chelating agent, 0.1-1% inhibitor, 0.5-3% etching agent, 0.5-2% sulfonic acid and its salt compounds, 0.1-1.5% amino acid, 0.1-0.8% alkylamine, and deionized water to make up the balance.

[0006] Further preferably, the fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo comprises at least, by mass percentage: 17-18% hydrogen peroxide, 2.5-2.8% chelating agent, 0.12-0.2% inhibitor, 1.2-2% etchant, 0.6-0.9% sulfonic acid and its salt compounds, 0.4-0.6% amino acid, 0.4-0.5% alkylamine, and deionized water to make up the balance.

[0007] As a preferred technical solution, the chelating agent is selected from at least one of iminodiacetic acid, nitrotriacetic acid, ethylenediaminetetraacetic acid, diethyl trinitrovaleric acid, aminoformic acid (methylphosphonic acid), (1-hydroxyethane-1,1-decyl)bis(phosphonic acid), ethylenediaminetetraacetic acid (methylphenylpropionic acid), diethyltriaminepentaphenyl (methylphosphonic acid), alanine, glutamic acid, aminobutyric acid, and glycine, preferably iminodiacetic acid.

[0008] As a preferred technical solution, the inhibitor is a heterocyclic aromatic compound and / or a heterocyclic aliphatic compound, preferably at least one of imidazole, pyrazole, triazole, tetrazole, 5-aminotetrazole, 5-methyltetrazole, methyltetrazole, piperazine, methylpiperazine, hydroxyethylpiperazine, pyrrolidine, and alloxan, preferably 5-methyltetrazole.

[0009] As a preferred technical solution, the etching agent is selected from at least one of acetic acid, formic acid, butyric acid, citric acid, glycolic acid, oxalic acid, malonic acid, malic acid, valeric acid, propionic acid, tartaric acid, gluconic acid, and succinic acid, preferably tartaric acid.

[0010] As a preferred technical solution, the sulfonic acid and its salt compounds are selected from at least one of methanesulfonic acid and its salt compounds, ethanesulfonic acid and its salt compounds, p-toluenesulfonic acid and its salt compounds, 2,4-toluenedisulfonic acid and its salt compounds, preferably methanesulfonic acid.

[0011] As a preferred technical solution, the amino acid is selected from at least one of glycine, iminodiacetic acid, alanine, valine, glutamic acid, aspartic acid, glutamine, asparagine, serine, threonine, cysteine, methionine, histidine, phenylalanine, lysine, and arginine, preferably cysteine.

[0012] As a preferred technical solution, the alkylamine compound is selected from at least one of butylamine, pentylamine, octylamine, 2-ethyl-1-butylamine, 2-hexylamine, 2-ethylhexylamine, heptylamine, hexylamine and cyclohexylamine, preferably octylamine.

[0013] The etching solution provided by the present invention overcomes the problem of multiple residues when the fluorine-free etching solution etches the molybdenum-containing layer in the pH range of 2 to 3 by simultaneously introducing sulfonic acid and its salt compounds and amino acids, especially simultaneously introducing methanesulfonic acid and cysteine, and shows excellent residue-free etching performance. At the same time, the etching angle is controlled within the range of 39.2-41.2° and the single-side loss is ensured to be below 0.7 μm. However, the introduction of only one of them or no introduction will result in metal residues.

[0014] On the other hand, the present invention provides a method for preparing a fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo, which is prepared by mixing hydrogen peroxide, a chelating agent, an inhibitor, an etching agent, sulfonic acid and its salt compounds, an amino acid, an alkylamine, and deionized water.

[0015] The etching solution provided by the present invention is a single-dose type, easy to use, and is particularly suitable for etching with a copper layer thickness of 2000-3000 angstroms. Mo-containing layer thickness is 200-500 angstroms Two-layer membrane structure.

[0016] Beneficial Effects

[0017] 1. The present invention provides a fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo, which has excellent etching performance for multilayer films including copper and MTD alloys, copper and MoNb alloys without using fluorine compounds, minimizes residual defects, and does not damage the glass substrate, thereby facilitating etching regeneration.

[0018] 2. The etching solution provided by the present invention overcomes the problem of multiple residues when the fluorine-free etching solution etches the molybdenum-containing layer in the pH range of 2 to 3 by simultaneously introducing sulfonic acid and its salt compounds and amino acids, especially simultaneously introducing methanesulfonic acid and cysteine, and shows excellent residue-free etching performance, while controlling the etching angle within the range of 39.2-41.2° and ensuring that the single-side loss is below 0.7 μm.

[0019] 3. The etching solution provided by the present invention is a single-dose type, easy to use, and is particularly suitable for copper-containing layers with a thickness of 2000-3000 angstroms. Mo-containing layer thickness is 200-500 angstroms Two-layer membrane structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The metal residue results after etching of the embodiments and comparative examples are characterized by SEM. In the figure, ad corresponds to the metal residue results of embodiment 1, comparative example 1, comparative example 2, and comparative example 3, respectively. DETAILED DESCRIPTION

[0021] Examples 1-5 and Comparative Examples 1-3

[0022] Embodiments 1-5 and comparative examples 1-3 of the present invention provide a fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo. The formula is shown in Table 1 in terms of mass percentage.

[0023]

[0024]

[0025] On the other hand, Examples 1-5 and Comparative Examples 1-3 of the present invention provide a method for preparing a fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo, which is prepared by mixing the raw materials according to the formula in Table 1.

[0026] Performance Testing Methods

[0027] 1. The etching solutions provided in the examples and comparative examples are used for etching the Cu / MoNb double-layer film. The etching conditions and etching results are shown in Table 2. Figure 1 .

[0028] Table 2

[0029]

[0030] From the analysis of the above table, it can be seen that compared with Comparative Examples 1, 2, and 3, the etching solutions provided by Examples 1-5 have no metal residue, etching defects such as undercut, and have excellent CD-loss, slope angle, and maximum copper load, and no sediment is placed.

Claims

1. A fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo, characterized in that: Calculated by mass percentage, it at least includes: 12-25% hydrogen peroxide, 0.5-4% chelating agent, 0.01-2% inhibitor, 0.1-5% etching agent, 0.1-3% sulfonic acid and its salt compounds, 0.01-3% amino acid, 0.01-1% alkylamine, and deionized water to make up the balance.

2. A fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo according to claim 1, characterized in that: Calculated by mass percentage, the fluorine-free etching solution for Cu, MoNbCu and MTDCuMo at least comprises: 14-20% hydrogen peroxide, 1.5-3% chelating agent, 0.1-1% inhibitor, 0.5-3% etching agent, 0.5-2% sulfonic acid and its salt compounds, 0.1-1.5% amino acid, 0.1-0.8% alkylamine, and deionized water to make up the balance.

3. A fluorine-free etching solution for Cu, MoNbCu, MTDCuMo according to claim 1 or 2, characterized in that: The chelating agent is selected from at least one of iminediacetic acid, nitrotriacetic acid, ethylenediaminetetraacetic acid, diethyl trinitrovaleric acid, aminoformic acid (methylphosphonic acid), (1-hydroxyethane-1,1-decyl)bis(phosphonic acid), ethylenediaminetetraacetic acid (methylphenylpropionic acid), diethyltriaminepentaphenyl (methylphosphonic acid), alanine, glutamic acid, aminobutyric acid, and glycine.

4. A fluorine-free etching solution for Cu, MoNbCu, MTDCuMo according to claim 3, characterized in that: The inhibitor is a heterocyclic aromatic compound and / or a heterocyclic aliphatic compound.

5. A fluorine-free etching solution for Cu, MoNbCu, MTDCuMo according to claim 4, characterized in that: The inhibitor is selected from at least one of imidazole, pyrazole, triazole, tetrazole, 5-aminotetrazole, 5-methyltetrazole, methyltetrazole, piperazine, methylpiperazine, hydroxyethylpiperazine, pyrrolidine and alloxan.

6. A fluorine-free etching solution for Cu, MoNbCu, MTDCuMo according to claim 5, characterized in that: The etching agent is selected from at least one of acetic acid, formic acid, butyric acid, citric acid, glycolic acid, oxalic acid, malonic acid, malic acid, valeric acid, propionic acid, tartaric acid, gluconic acid, and succinic acid.

7. The fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo according to claim 6, characterized in that: The sulfonic acid and its salt compounds are selected from at least one of methanesulfonic acid and its salt compounds, ethanesulfonic acid and its salt compounds, p-toluenesulfonic acid and its salt compounds, and 2,4-toluenedisulfonic acid and its salt compounds.

8. The fluorine-free etching solution for Cu, MoNbCu, and MTDCuMo according to claim 7, characterized in that: The amino acid is selected from at least one of glycine, iminodiacetic acid, alanine, valine, glutamic acid, aspartic acid, glutamine, asparagine, serine, threonine, cysteine, methionine, histidine, phenylalanine, lysine, and arginine.

9. A method for preparing a fluorine-free etching solution for Cu, MoNbCu, or MTDCuMo according to any one of claims 1 to 8, characterized in that: The preparation method is prepared by mixing hydrogen peroxide, a chelating agent, an inhibitor, an etching agent, sulfonic acid and its salt compounds, an amino acid, an alkylamine and deionized water.

Citation Information

Patent Citations

  • Copper-molybdenum metal etching solution as well as preparation method and application thereof

    CN112663064A

  • Copper etching solution and manufacturing method of array substrate

    CN114045495A

  • Metal etching liquid and preparation method and etching method thereof

    CN114774922A

  • Etching liquid composition

    CN115821264A

  • Copper-based metal film etching solution composition

    CN117604527A

Cited By

  • Cu-MTD alloy etching solution composition and application thereof

    CN121161292A