Preparation method of polyamide 56 draw textured yarn
By adjusting the crystallinity and orientation of polyamide 56 textured yarn and optimizing the production process, the problems of production stability and fiber mechanical property deviation in polyamide 56 textured yarn were solved, achieving efficient and environmentally friendly production and improving dyeing uniformity and mechanical properties.
Patent Information
- Application Number
- CN202411238586.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-30
- Publication Date
- 2024-11-05
AI Technical Summary
There are discrepancies in the production stability, fiber mechanical properties, and dyeing properties of existing polyamide 56 textured yarn.
By adjusting the crystallinity and orientation of polyamide 56 elastic yarn and optimizing process parameters such as hot stretching, shaping, and false twisting, polyamide 56 elastic yarn is prepared using a biological method. C-type, D-type, or PU-type false twisting friction pads are used to control tension and winding speed, thus preparing polyamide 56 elastic yarn with high crystallinity and high orientation.
It improves the production stability and fiber mechanical properties of polyamide 56 textured yarn, reduces the breakage rate, improves dyeing uniformity, reduces production costs, and reduces environmental pollution.
Smart Images

Figure BDA0005028500040000122 
Figure BDA0005028500040000123 
Figure BDA0005028500040000131
Abstract
Description
[0001] This application is a divisional application. The application number of the parent application is 2021104825200, the application date is April 30, 2021, and the name of the invention is "A polyamide 56 elastic yarn and its preparation method". Technical Field
[0002] The invention relates to a polyamide 56 stretch yarn and a preparation method thereof. Background Art
[0003] The bio-based polyamide 56 raw materials and processing process are green and environmentally friendly. The prepared fibers have better moisture absorption and quick-drying properties (the official moisture regain of 6% is closer to cotton, while the official moisture regain of ordinary nylon is 4-5%), skin-friendliness, wear resistance, good softness, and easy dyeing at low temperatures, etc., and can be widely used in the field of clothing filaments.
[0004] Currently, the clothing field includes pre-oriented yarn (POY), stretched yarn (DTY), fully drawn yarn, medium-oriented yarn, and highly oriented yarn. The stretched yarn has good fluffiness and elasticity and is widely used in the clothing field.
[0005] Patent application document CN 103966681A discloses a POY-DTY production method for nylon 56DTY (polyamide 56 plus stretch yarn). In the process, the temperature of the deformation hot box is 210-235°C, the D / Y ratio is 1.1-1.5, and the drafting multiple is 1.1-1.3. The obtained nylon 56DTY has production stability, fiber mechanical properties and dyeing performance deviations. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the defects of existing polyamide 56 stretch yarn production stability, fiber mechanical properties and dyeing performance deviation, and to provide a polyamide 56 stretch yarn with excellent production stability, fiber mechanical properties and dyeing performance and a preparation method thereof.
[0007] The present invention solves the above technical problems through the following technical solutions:
[0008] The present invention provides a polyamide 56 stretch yarn, wherein the crystallinity of the polyamide 56 stretch yarn is ≥70.0%, and / or the orientation degree of the polyamide 56 stretch yarn is ≥80.0%.
[0009] Preferably, the crystallinity of the polyamide 56 elastic yarn is 70.0% to 85.0%, preferably 73.0% to 85.0%, for example 82.5%, 80.2%, 79.7%, 79.5%, 77.4%, 76.8%, 76.5%, 75.8%, 75.5%, 75.4%, 75.0%, 74.9%, 74.2%.
[0010] Preferably, the orientation degree of the polyamide 56 elastic yarn is 80.0% to 95%, preferably 83.0% to 92%, for example 90.3%, 89.7%, 88.4%, 88.2%, 86.5%, 85.9%, 85.4%, 84.9%, 84.5%, 84.3%, 84.2%, 84.0%, 83.5%.
[0011] Preferably, the breaking strength of the polyamide 56 plus elastic yarn is 3.8-5.2 cN / dtex, preferably, the breaking strength of the polyamide 56 plus elastic yarn is 4.0-5.0 cN / dtex, more preferably 4.1-4.8 cN / dtex, further more preferably 4.2-4.6 cN / dtex, for example 4.3 cN / dtex or 4.4 cN / dtex.
[0012] Preferably, the coefficient of variation of the breaking strength of the polyamide 56 elastic yarn is ≤3%, more preferably ≤2.5%, further preferably ≤2%, and further more preferably ≤1.5%, for example 1.3%, 1% or 0.8%.
[0013] Preferably, the elongation at break of the polyamide 56 elastic yarn is 20-35%, more preferably 22-33%, further more preferably 24-30%, further more preferably 26-28%, for example 26.2%, 26.6% or 27%.
[0014] Preferably, the coefficient of variation of the elongation at break of the polyamide 56 elastic yarn is ≤5%, more preferably ≤4%, further more preferably ≤3%, further more preferably ≤2%, for example 1.3% or 1.6%.
[0015] Preferably, the broken wire rate of the polyamide 56 elastic wire is ≤5%, more preferably ≤4%, further preferably ≤3%, further more preferably ≤2%, for example 1.8%.
[0016] Preferably, the dyeing double A ratio of the polyamide 56 stretch yarn is ≥95%, more preferably ≥96%, further preferably ≥97%, further more preferably ≥98%, for example, 98.5%, 99% or 99.2%.
[0017] The present invention provides a method for preparing a polyamide 56 stretch yarn, which comprises the following steps:
[0018] (1) passing the polyamide 56 pre-oriented yarn through a yarn guide and passing through the first roller;
[0019] (2) Then it is subjected to heat stretching, shaping, false twisting, and passes through the second roller;
[0020] (3) After being processed by a network nozzle, it passes through the third roller and is wound to obtain the final product;
[0021] Wherein, the false twist friction plate is a C-type disc, a D-type disc or a PU-type disc.
[0022] In the present invention, the polyamide 56 pre-oriented yarn can be conventional in the art. The specification of the polyamide 56 pre-oriented yarn is preferably 20-200 dtex / 7-144f, for example, 93dtex / 68f. The breaking strength of the polyamide 56 pre-oriented yarn is preferably 3.0-3.8 cN / dtex, for example, 3.6 cN / dtex. The elongation of the polyamide 56 pre-oriented yarn is preferably 65-95%, more preferably 68-90%, and further more preferably 73-85%, for example, 76.5%. A wire cutter is also included between the wire guide and the first roller.
[0023] In the present invention, the heat stretching equipment can adopt conventional heat stretching equipment in the art. The heat stretching equipment is preferably a hot box. The temperature of the heat stretching is preferably 170-200°C; more preferably 175-195°C, further preferably 180-190°C, further more preferably 183-188°C, for example 185°C. The multiple of the heat stretching is preferably 1.25-1.40; more preferably 1.27-1.38, further more preferably 1.29-1.36, further more preferably 1.31-1.34, for example 1.32.
[0024] In the present invention, the shaping operation can be conventional in the art, preferably using a cooling plate for cooling and shaping. The shaping temperature is preferably room temperature.
[0025] In the present invention, the false twisting device generally adopts a false twister.
[0026] In the present invention, the friction plate is preferably a D-type plate or a PU-type plate; more preferably a PU-type plate.
[0027] The thickness of the friction plate is preferably ≤10 mm, more preferably 6-9 mm.
[0028] When the friction plate is a C-type disc, the spacing of the friction plate is preferably ≥0.65mm, more preferably 0.7-0.8mm, and further preferably 0.75mm. When the friction plate is the D-type disc or the PU-type disc, the spacing of the friction plate is preferably ≥0.5mm, more preferably ≥0.6mm, further preferably 0.7-0.8mm, and further more preferably 0.75mm. The friction coefficient of the friction plate is preferably ≤1.0, more preferably ≤0.9, further preferably ≤0.8, and further more preferably ≤0.7, for example 0.65.
[0029] Preferably, the D / Y ratio of the false twist is 1.6 to 2.2, preferably 1.65 to 2.1, more preferably 1.70 to 2.0, and even more preferably 1.75 to 1.9. Those skilled in the art know that the D / Y ratio refers to the ratio of the surface speed of the friction disk to the speed of the yarn leaving the false twister.
[0030] Preferably, the T2 processing tension of the false twist is controlled to be 0.8 to 1.1 times of the T1 processing tension; preferably 0.84 to 1.08 times, more preferably 0.88 to 1.06 times, more preferably 0.90 to 1.04 times, for example 0.95 times. Those skilled in the art know that T1 refers to the twisting tension during the false twisting process; T2 refers to the untwisting tension during the false twisting process.
[0031] In the present invention, those skilled in the art are aware of detecting tensions at different positions, such as the T1 processing tension and the T2 processing tension, by means of an online tension monitor. Preferably, after the false twisting, the yarn passes through the second roller via an online tension monitor.
[0032] Preferably, the winding speed is 500-800 m / min; more preferably 520-750 m / min, further more preferably 540-700 m / min, further more preferably 560-650 m / min, for example 600 m / min.
[0033] In the present invention, those skilled in the art are aware that a wire break sensor and an oil tanker are generally provided before the winding. The wire break sensor is used to record the number of wire breakages to detect the wire breakage rate. The oil tanker is used for oiling, and the oiling operation can be performed according to the conventional art.
[0034] The present invention provides a polyamide 56 stretch yarn produced by the polyamide 56 stretch yarn preparation method.
[0035] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0036] The reagents and raw materials used in the present invention are commercially available.
[0037] The positive and progressive effects of the present invention are:
[0038] The raw materials for the production of the polyamide 56 stretch yarn of the present invention are made by biological methods, are green materials, do not rely on petroleum resources, do not cause serious pollution to the environment, and can reduce the emission of carbon dioxide and reduce the generation of the greenhouse effect. The polyamide 56 stretch yarn of the present invention has good mechanical properties and dyeing uniformity. The polyamide 56 stretch yarn of the present invention can be produced by using conventional polyamide 6 and polyamide 66 stretching equipment while adjusting the false twist friction plate and processing technology, and the broken wire rate is greatly reduced, the production efficiency is improved, the production cost is reduced, and the fiber mechanical performance index is more stable. DETAILED DESCRIPTION
[0039] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0040] In the following embodiments of the present invention, the polyamide 56 pre-oriented yarn used has a specification of 93dtex / 68f, a breaking strength of 3.6cN / dtex, and an elongation of 76.5%; and the texturizing equipment used is an eFK PA texturizing machine.
[0041] Example 1
[0042] Preparation of polyamide 56 stretch yarn
[0043] First, the polyamide 56 pre-oriented yarn is passed through a yarn guide to the first roller, and is heat-stretched in a hot box. Then, it is cooled and shaped using a cooling plate, and a certain twist is obtained through a false twister. Then, it is passed through an online tension detector and the second roller, and then through a network nozzle to add a network. Subsequently, it passes through the third roller, a broken wire sensor, and an oil tanker to add oil, and finally is wound to obtain the polyamide 56 elastic yarn.
[0044] The friction plate used by the false twister is a C-type disk with a thickness of 6 mm, a spacing of 0.75 mm, and a friction coefficient of 0.65.
[0045] The temperature of the hot box is 185°C.
[0046] The stretching ratio is 1.32.
[0047] The D / Y ratio is 1.75.
[0048] The T2 processing tension is controlled to be 0.95 of the T1 tension.
[0049] The winding speed is 600 m / min.
[0050] Example 2
[0051] Preparation of polyamide 56 stretch yarn
[0052] The preparation method of the polyamide 56 with elastic wire is the same as that of Example 1, except that the friction plate adopts a D-type disk with a spacing of 0.5 mm.
[0053] Example 3
[0054] Preparation of polyamide 56 stretch yarn
[0055] The preparation method of the polyamide 56 with elastic wire is the same as that of Example 2, except that the friction plate adopts a D-type disk with a spacing of 0.75 mm.
[0056] Example 4
[0057] Preparation of polyamide 56 stretch yarn
[0058] The preparation method of the polyamide 56 with elastic wire is the same as that of Example 1, except that the friction plate adopts a PU type disk with a thickness of 9 mm and a spacing of 0.5 mm.
[0059] Example 5
[0060] Preparation of polyamide 56 stretch yarn
[0061] The preparation method of the polyamide 56 with elastic wire is the same as that of Example 4, except that the friction plate adopts a PU type disk with a thickness of 9 mm and a spacing of 0.75 mm.
[0062] Example 6
[0063] Preparation of polyamide 56 stretch yarn
[0064] The preparation method of the polyamide 56 stretch yarn is the same as that of Example 1, except that the temperature of the hot box is 195°C.
[0065] Example 7
[0066] Preparation of polyamide 56 stretch yarn
[0067] The preparation method of the polyamide 56 stretched yarn is the same as that of Example 1, except that the stretching ratio is 1.27.
[0068] Example 8
[0069] Preparation of polyamide 56 stretch yarn
[0070] The preparation method of the polyamide 56 with elastic wire is the same as that of Example 1, except that the spacing between the friction plates is 0.65 mm.
[0071] Example 9
[0072] Preparation of polyamide 56 stretch yarn
[0073] The preparation method of the polyamide 56 with elastic wire is the same as that of Example 2, except that the friction plate spacing is 0.65 mm.
[0074] Example 10
[0075] Preparation of polyamide 56 stretch yarn
[0076] The preparation method of the polyamide 56 with elastic wire is the same as that of Example 1, except that the friction coefficient of the C-type disc friction plate is 0.8.
[0077] Embodiment 11
[0078] Preparation of polyamide 56 stretch yarn
[0079] The preparation method of the polyamide 56 stretch yarn is the same as that of Example 1, except that the D / Y ratio is 1.65.
[0080] Example 12
[0081] Preparation of polyamide 56 stretch yarn
[0082] The preparation method of the polyamide 56 stretch yarn is the same as that in Example 1, and the T2 processing tension is controlled to be 0.84 of the T1 tension.
[0083] Example 13
[0084] Preparation of polyamide 56 stretch yarn
[0085] The preparation method of the polyamide 56 stretch yarn is the same as that in Example 1, and the winding speed is 750 m / min (upper limit).
[0086] Comparative Example 1
[0087] Preparation of polyamide 56 stretch yarn
[0088] The preparation method of the polyamide 56 with elastic wire is the same as that of Example 1, except that the friction plate adopts a C-type disk with a spacing of 0.5 mm.
[0089] Comparative Example 2
[0090] Preparation of polyamide 56 stretch yarn
[0091] The preparation method of the polyamide 56 with elastic wire is the same as that of Example 1, except that the friction plate adopts a C-type disk with a spacing of 0.6 mm.
[0092] Comparative Example 3
[0093] Preparation of polyamide 56 stretch yarn
[0094] The preparation method of the polyamide 56 with elastic yarn is the same as that of Example 1, except that the friction plate adopts a C-type disk with a friction coefficient of 1.1.
[0095] Comparative Example 4
[0096] Preparation of polyamide 56 stretch yarn
[0097] The preparation method of the polyamide 56 with elastic yarn is the same as that of Example 1, except that the friction plate adopts a C-type disk and the hot box temperature is 210°C.
[0098] Comparative Example 5
[0099] Preparation of polyamide 56 stretch yarn
[0100] The preparation method of the polyamide 56 elastic wire is the same as that of Example 1, except that the friction plate uses a C-type disk and the T2 processing tension is controlled to be 0.5 of the T1 tension.
[0101] Comparative Example 6
[0102] Preparation of polyamide 56 stretch yarn
[0103] The preparation method of the polyamide 56 with elastic yarn is the same as that of Example 1, except that the friction plate uses a C-type disk and the D / Y ratio is 1.5.
[0104] Comparative Example 7
[0105] Preparation of polyamide 56 stretch yarn
[0106] The preparation method of the polyamide 56 elastic yarn is the same as that of Example 1, except that the friction plate uses a C-type disk and the stretching ratio is 1.1.
[0107] Comparative Example 8
[0108] Preparation of polyamide 56 stretch yarn
[0109] The preparation method of the polyamide 56 elastic yarn is the same as that of Example 1, except that the friction plate adopts a C-type disk and the winding speed is 850m / min.
[0110] Comparative Example 9
[0111] Preparation of polyamide 56 stretch yarn
[0112] The preparation method of the polyamide 56 with elastic yarn is the same as that of Example 1, except that the friction plate uses a D-type disk and the temperature of the hot box is 220°C.
[0113] Comparative Example 10
[0114] Preparation of polyamide 56 stretch yarn
[0115] The preparation method of the polyamide 56 elastic wire is the same as that of Example 1, except that the friction plate uses a D-type disk and the T2 processing tension is controlled to be 0.6 of the T1 tension.
[0116] Comparative Example 11
[0117] Preparation of polyamide 56 stretch yarn
[0118] The preparation method of the polyamide 56 elastic yarn is the same as that of Example 1, except that the friction plate adopts a PU disc with a thickness of 9 mm, and the T2 processing tension is controlled to be 0.5 of the T1 tension.
[0119] Comparative Example 12
[0120] Preparation of polyamide 56 stretch yarn
[0121] The preparation method of the polyamide 56 elastic wire is the same as that of Example 1, except that the friction plate uses a D-type disk, the hot box temperature is 210° C., and the T2 processing tension is controlled to be 0.5 of the T1 tension.
[0122] Comparative Example 13
[0123] Preparation of polyamide 56 stretch yarn
[0124] The preparation method of the polyamide 56 elastic yarn is the same as that of Example 1, except that the friction plate uses a C-type disk, the hot box temperature is 220° C., the D / Y ratio is 1.3, and the stretching multiple is 1.1.
[0125] Comparative Example 14
[0126] Preparation of polyamide 56 stretch yarn
[0127] The preparation method of the polyamide 56 elastic yarn is the same as that of Example 1, except that the friction plate uses a D-type disk, the hot box temperature is 215° C., the D / Y ratio is 1.4, and the stretching multiple is 1.2.
[0128] Comparative Example 15
[0129] Preparation of polyamide 56 stretch yarn
[0130] The preparation method of the polyamide 56 elastic yarn is the same as that of Example 1, except that the friction plate uses a PU disk with a thickness of 9 mm, the hot box temperature is 220° C., the D / Y ratio is 1.4, and the stretch multiple is 1.2.
[0131] Comparative Example 16
[0132] Preparation of polyamide 6 stretch yarn
[0133] The preparation method of the polyamide 6 stretch yarn is the same as that of Comparative Example 1.
[0134] Effect Example 1
[0135] In this effect example, the following tests were conducted on the polyamide 56 stretch yarn parameters in Examples 1 to 5 and Comparative Examples 1 to 16:
[0136] (1) Breaking strength and breaking strength variation coefficient:
[0137] Measured according to GB / T 14344.
[0138] (2) Elongation at break, coefficient of variation of elongation at break:
[0139] Measured according to GB / T 14344.
[0140] (3) Double A dyeing rate:
[0141] Dyeing double A rate = ((weight of fibers with dyeing uniformity ≥ 4.5) / total weight of all dyed fibers) × 100%.
[0142] Dyeing uniformity (gray card) / grade: FZ / T 50008 Test method for dyeing uniformity of nylon filament.
[0143] (4) Wire breakage rate:
[0144] Manual statistics.
[0145] (5) Crystallinity:
[0146] The fiber samples were analyzed using a D / max-2550PC X-ray diffractometer produced by Rigaku Corporation of Japan, with a Cu target wavelength of The voltage is 20-40kV, the current is 10-450mA, and the measurement angle 2θ ranges from 5 to 40°. The polyamide 56 fiber samples used to test crystallization are first fully cut and the sample mass is greater than 0.2g; the polyamide 56 fiber samples used to test microcrystalline orientation are combed neatly, with a bundle length of 30mm for testing. Origin and other software are used for data processing to analyze and calculate the crystallinity and orientation of the fiber.
[0147] The formula for calculating crystallinity is:
[0148]
[0149] Among them, ∑I c is the total diffraction integrated intensity of the crystalline part; ∑I a is the integrated scattering intensity of the amorphous part.
[0150] (6) Orientation degree: Sonic orientation measuring instrument.
[0151] The results are shown in Table 1.
[0152] Table 1 Comparison of various properties of fibers in the embodiments of the present invention
[0153]
[0154]
Claims
1. A method for preparing a polyamide 56 stretch yarn, comprising the following steps: (1) passing the polyamide 56 pre-oriented yarn through a yarn guide and passing through the first roller; (2) Then it is subjected to heat stretching, shaping, false twisting, and passes through the second roller; (3) After being processed by a network nozzle, it passes through the third roller and is wound to obtain the final product; in, The false twist friction plate is a C-type plate, a D-type plate or a PU-type plate, the thickness of the friction plate is ≤10 mm, and the friction coefficient of the friction plate is ≤1.
0.
2. The preparation method according to claim 1, wherein The friction plate is a D-type plate or a PU-type plate; And / or, the friction plate has a thickness of 6 to 9 mm; And / or, the friction coefficient of the friction plate is ≤0.9; And / or, the temperature of the heat stretching is 170-200°C; And / or, the thermal stretching multiple is 1.25 to 1.40; And / or, the D / Y of the false twist is 1.6 to 2.2; And / or, the T2 processing tension of the false twist is controlled to be 0.8 to 1.1 times of the T1 processing tension; And / or, the winding speed is 500-800 m / min.
3. The preparation method according to claim 1, wherein The friction plate is a PU type disc; And / or, the temperature of the heat stretching is 175-195°C; And / or, the thermal stretching multiple is 1.27 to 1.38; And / or, the D / Y of the false twist is 1.65 to 2.1; And / or, the T2 processing tension of the false twist is controlled to be 0.84 to 1.08 times of the T1 processing tension; And / or, the winding speed is 520-750 m / min.
4. The preparation method according to claim 1, wherein The friction coefficient of the friction plate is ≤0.8; And / or, the temperature of the heat stretching is 180-190°C; And / or, the thermal stretching multiple is 1.29 to 1.36; And / or, the D / Y of the false twist is 1.70 to 2.0; And / or, the T2 processing tension of the false twist is controlled to be 0.88 to 1.06 times of the T1 processing tension; And / or, the winding speed is 540-700 m / min.
5. The preparation method according to claim 1, wherein The friction coefficient of the friction plate is ≤0.7; And / or, the temperature of the heat stretching is 183-188°C; And / or, the thermal stretching multiple is 1.31 to 1.34; And / or, the D / Y of the false twist is 1.75 to 1.9; And / or, the T2 processing tension of the false twist is controlled to be 0.90 to 1.04 times of the T1 processing tension; And / or, the winding speed is 560-650 m / min.
6. The preparation method according to claim 1, wherein The friction coefficient of the friction plate is 0.65 to 0.8; And / or, the temperature of the heat stretching is 183-185°C; And / or, the thermal stretching multiple is 1.32 to 1.36; And / or, the T2 processing tension of the false twist is controlled to be 0.95 to 1.04 times of the T1 processing tension; And / or, the winding speed is 560-600 m / min.
7. The preparation method according to claim 1, wherein The friction plate is a C-shaped plate, and the spacing between the friction plates is ≥0.65mm; Alternatively, the friction plate is the D-type plate or the PU-type plate, and the spacing between the friction plates is ≥0.5 mm.
8. The preparation method according to claim 1, wherein The friction plate is a C-shaped plate, and the spacing between the friction plates is 0.7-0.8 mm; Alternatively, the friction plate is the D-type plate or the PU-type plate, and the spacing between the friction plates is ≥0.6 mm.
9. The preparation method according to claim 1, wherein The friction plate is a C-shaped plate, and the spacing between the friction plates is 0.75mm to 0.8mm; Alternatively, the friction plate is the D-type plate or the PU-type plate, and the spacing between the friction plates is 0.7-0.8 mm.
10. The preparation method according to claim 1, wherein: The friction plate is the D-type plate or the PU-type plate, and the spacing between the friction plates is 0.75 mm to 0.8 mm; And / or, a wire cutter is further included between the wire guide and the first roller; And / or, the heat stretching device is a heat box; And / or, the shaping is performed by cooling with a cooling plate; And / or, the shaping temperature is room temperature. And / or, a broken wire sensor and an oil tanker are provided before the winding.
Citation Information
Patent Citations
Denier / superfine denier nylon master granule, preoriented yarn (POY) and draw textured yarn (DTY) stretch yarn and preparation method thereof
CN101724265A
Spun-dyed black polyamide yarn, false-twisted yarn, covered elastomer yarn, and leg knit
CN104220653A
Polyamide 56 fiber with low boiling water shrinkage rate and preparation method and application of polyamide 56 fiber
CN112410916A