Reversible semimetal-semiconductor transition of unconventional phase WS2 nanosheets

By driving the reversible phase transition of 1T'-WS2 nanosheets through proton insertion and deintercalation in micro-electrochemical devices, the problem of reversible phase transition at the TMD single crystal level has been solved, realizing the reversible conversion from 1T'-WS2 to 1T'd-WS2, which is suitable for applications in transistors and optotransistors.

CN118899335APending Publication Date: 2024-11-05CITY UNIV OF HONG KONG SHENZHEN RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311318275.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-07-26
Filing Date
2023-10-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve highly controllable and reversible phase transitions of transition metal dichalcogenides (TMDs) at the single-crystal level, especially the reversible conversion between the 1T' phase and the 1T'd phase, and conventional embedding methods are prone to structural damage.

Method used

The reversible phase transition of 1T'-WS2 nanosheets is driven by proton insertion and extraction in micro-electrochemical devices. The reversible conversion from 1T'-WS2 to 1T'd-WS2 is achieved by using proton insertion and extraction in the van der Waals gaps of 1T'-WS2 nanosheets. A protective layer is used to avoid direct contact, and the proton insertion and extraction are controlled by the gate voltage.

Benefits of technology

A reversible phase transition at the single-crystal level was achieved for 1T'-WS2 nanosheets, maintaining structural integrity, reversibly modulating conductivity and spectral response, and achieving an on/off ratio >106, making it suitable for applications in transistors and optotransistors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899335A_ABST
    Figure CN118899335A_ABST
Patent Text Reader

Abstract

According to the invention, injection and deintercalation (1e / WS2) of high-concentration electrons in semimetal 1T '-tungsten disulfide (1T'-WS2) are realized through embedding and deintercalation of highly reversible protons, so that reversible phase change of WS2 is induced. The characterization of the system shows that the new phase WS2 after proton embedding has semiconductor characteristics, has a novel unconventional phase, and is expressed as a 1T'd phase. As the lightest and smallest ion, the proton can avoid structural damage to WS2 in the intercalation process, so that highly reversible structural phase change is realized. In a phase change process from 1T '-WS2 to 1T'd-WS2, transmission modulation with an on / off ratio exceeding 106 can be realized. A 1T '-WS2 nanosheet is used as a channel layer to develop a transistor using the advantage of reversible phase change.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 499,753, filed on May 3, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to 1T' phase and 1T' phase of tungsten disulfide (WS2) nanosheets. d Reversible phase transition between phases. Specifically, the present disclosure relates to a highly efficient reversible phase transition strategy through proton intercalation and deintercalation of WS2 nanosheets, and transistors developed based on the strategy. Background Art

[0004] Crystalline phase is an important structural parameter besides size, dimension, morphology and crystal plane that can determine the physicochemical properties of nanomaterials [1], [2]. As one of the powerful strategies for phase engineering of nanomaterials (PEN) [1], phase transitions accompanied by bandgap modulation have been widely explored in various materials due to their great potential in various fundamental studies and applications [3]-[6]. In particular, the phase transitions of transition metal dichalcogenides (TMDs) are of great interest due to their unique crystal phase-dependent electronic structures, which has triggered fundamental studies in catalysis [7]-[8], (opto)electronics [4], [9] and condensed matter physics

[10] -

[12] . The phase transitions of TMDs can be initiated by various methods [1], such as chemical modification

[13] , laser irradiation

[14] and lithium ion intercalation

[15] ,

[16] . Unlike transition metal tellurides, phase transitions in TMDs can only be realized in monolayers or localized domains due to the large energy difference between thermodynamically stable phases (e.g., 2H) and unconventional phases (e.g., 1T and 1T') in other TMDs

[17] . In addition, associated undesirable structural damage, such as amorphization

[19] , vacancy generation

[14] , and composition changes

[20] , can result in poor reversibility of phase transitions. In contrast, reversible phase transitions in TMDs have been demonstrated in transition metal tellurides under electrostatic gating, taking advantage of the relatively small energy difference between the 2H and 1T' phases of transition metal tellurides [4], [5],

[17] ,

[21] . However, a recent study has shown that such strong gate modulation can induce the formation of tellurium (Te) vacancies

[20] . Alternatively, intercalation strategies exploit the layered structure of TMDs to embed various guest species into the van der Waals gaps to achieve phase transitions in bulk crystals [6],

[15] ,

[22] ,

[23] . However, the reported intercalation methods, whether chemical or electrochemical

[15] ,

[24] –

[27] , can only induce phase transitions in localized domains, accompanied by poor structural damage and limited reversibility. Despite these research efforts, highly controllable and reversible phase transitions of TMDs at the single crystal level remain a great challenge. Compared to commonly used guest species such as metal ions

[25] , metal atoms

[28] , and molecules

[29] , the smallest and lightest ions, namely protons, have attracted extensive research attention due to their excellent ability to tune the physicochemical properties of nanomaterials for various applications [3],

[30] –

[32] . For example, proton intercalation has been used to achieve hydrogenation of metal oxides, thereby tuning their properties [3],

[30] ,

[33] ,

[34] . Summary of the invention

[0005] Here we disclose a highly efficient reversible phase transition strategy induced by proton insertion and deinsertion in microelectrochemical devices ( Figure 1Figure 2 (a) shows that high electron injection and extraction densities (about 1e / WS2) during proton insertion and deinsertion can induce a reversible phase transition of semimetallic 1T'-WS2 on single-crystalline nanosheets ( Figure 1 Based on in situ and ex situ characterizations, the structure of 1T'-WS2 after the phase transition was determined to be a new distorted octahedral phase, denoted as 1T' d Impressively, the 1T' d -WS2 can be completely transformed back to 1T'-WS2 after proton deintercalation, indicating that single-crystalline 1T'-WS2 nanosheets achieve reversible phase transition through proton intercalation and deintercalation. d - During the phase transition of WS2, an on / off ratio of >10 was achieved 6 transmission modulation.

[0006] This article also discloses a transistor using the reversible phase change provided by 1T'-WS2. The transistor includes a source electrode, a drain electrode, and a gate electrode, and the 1T'-WS2 nanosheet forms a channel layer connecting the source electrode and the drain electrode. The surface of the 1T'-WS2 nanosheet is covered with a protective layer to avoid direct contact between the proton electrolyte and the source electrode and the drain electrode, and to avoid direct contact between the gate electrode and the 1T'-WS2 nanosheet. A reaction window is opened on the protective layer near the edge of the 1T'-WS2 nanosheet, so that the protons in the proton electrolyte can be embedded or de-embedded under the drive of the gate electrode voltage, and the reversible embedding and de-embedding of the protons can induce a reversible semi-metal-semiconductor phase change of WS2. Thus, the occurrence of a reversible phase change changes the conductivity of the channel layer or the spectral response of the channel layer to light.

[0007] In certain embodiments, the 1T'-WS2 nanosheet includes at least two layers.

[0008] In certain embodiments, the 1T'-WS2 nanosheets are uniformly crystalline.

[0009] In some embodiments, the proton electrolyte is an aqueous proton electrolyte. The aqueous proton electrolyte can be an inorganic acid. The inorganic acid can include sulfuric acid, nitric acid, hydrochloric acid, phosphoric acid, acetic acid, or a combination thereof.

[0010] In certain embodiments, the proton electrolyte is an organic proton electrolyte. The organic proton electrolyte may be bis(trifluoromethane)sulfonyl imide (TFSI) dissolved in liquid polyethylene glycol.

[0011] In certain embodiments, the protic electrolyte is a proton-containing solid electrolyte.

[0012] In certain embodiments, each of the drain electrode and the source electrode comprises gold, chromium, or a combination thereof.

[0013] In certain embodiments, the gate electrode comprises platinum.

[0014] Further disclosed herein is a method for preparing a 1T'd-WS2 nanosheet. The method comprises: providing any embodiment of the disclosed transistor; and applying a gate-source voltage between a gate electrode and a source electrode to form a 1T'd-WS2 nanosheet. d -WS2 nanosheets.

[0015] In certain embodiments, 1T'-WS2 nanosheets and 1T' d Each of the WS2 nanosheets contains at least two layers.

[0016] In certain embodiments, 1T'-WS2 nanosheets and 1T' d Each of the WS2 nanosheets is uniformly crystalline.

[0017] In some embodiments, the gate-source voltage is 1.1V or above.

[0018] Other aspects of the present invention are disclosed by way of illustration in the following embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The above and other objects and features of the present disclosure will become apparent from the following description of the present disclosure when taken in conjunction with the accompanying drawings.

[0020] Figure 1 The reversible phase transition of 1T'-WS2 in a microelectrochemical device is schematically shown, wherein: sub-figure (a) depicts a schematic diagram of a microelectrochemical device for the reversible phase transition of 1T'-WS2 driven by proton insertion and deinsertion, respectively; and sub-figure (b) depicts the reversible phase transition of 1T'-WS2 and 1T' d -Atomic structure model of WS2 during reversible phase transition.

[0021] Figure 2 The construction of microelectrochemical devices used for measurements during electron injection and extraction and the measurement results of these devices are illustrated, wherein: subfigure (a) provides optical images of the microelectrochemical devices: the overall setup with three electrodes in view (i), the high magnification image of the microelectrochemical device with an electrolyte droplet in view (ii), and the device made with a mechanically exfoliated 1T'-WS2 nanosheet in view (iii), in which windows were opened in the polymethyl methacrylate (PMMA) passivation layer so that two opposite edges and the basal plane of the 1T'-WS2 nanosheet were exposed to the electrolyte; and subfigure (b) provides typical drain-source currents (I) measured in the fabricated 1T'-WS2 microelectrochemical devices during charge injection and extraction in 0.5M H2SO4 aqueous solution. ds) and gate current (I g ).

[0022] Figure 3 A phase change characterization of 1T'-WS2 nanosheets is provided, wherein: subfigure (a) plots the in situ Raman characterization of 1T'-WS2 nanosheets during proton embedding and de-embedding in 0.5M H2SO4 aqueous solution; subfigure (b) plots the in situ photoluminescence characterization of 1T'-WS2 nanosheets during proton embedding and de-embedding in 0.5M H2SO4 aqueous solution; subfigure (c) plots the in situ Raman spectra obtained at different gate potentials, showing a highly reversible phase change process; and subfigure (d) plots the percentage of 1T' phase in WS2 nanosheets at different gate potentials.

[0023] Figure 4 Provides 1T'-WS2 and 1T' d -WS2 nanosheet structural characterization, wherein: sub-figure (a) shows the selected area electron diffraction (SAED) pattern of 1T'-WS2 nanosheet obtained by mechanical exfoliation of bulk 1T'-WS2 crystals; sub-figure (b) depicts the high angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image of the nanosheet in sub-figure (a); sub-figure (c) plots the corresponding FFT pattern of the HAADF-STEM image shown in sub-figure (b); sub-figure (d) shows the SAED pattern of 1T'-WS2 nanosheet after proton embedding; sub-figure (e) depicts the Figure (d) shows the HAADF-STEM image of the nanosheet; sub-figure (f) plots the corresponding FFT pattern of the HAADF-STEM image in sub-figure (e); sub-figure (g) depicts the relative displacement of W atoms in the WS2 nanosheet with respect to the 1T' lattice after proton embedding; sub-figure (h) shows the displacement map derived from sub-figure (g), where the displacement of each W atom is represented by a circle; and sub-figure (i) plots the magnitude of the displacements obtained in sub-figure (h) along the horizontal (X) and vertical (Y) directions, with the average magnitudes of W atoms being 0.11, 0.13, 0.03, and 0.11, respectively.

[0024] Figure 5Different types of microelectrochemical devices used in our work are depicted, wherein: sub-figure (a) provides an optical image of the overall setup of a three-electrode microelectrochemical device; sub-figure (b) depicts an electronic device made with mechanically exfoliated 1T'-WS2 nanosheets, which are used in the three-electrode microelectrochemical device shown in sub-figure (a); sub-figure (c) provides an optical image of the overall setup of a four-electrode microelectrochemical device; sub-figure (d) depicts an electronic device made with mechanically exfoliated 1T'-WS2 nanosheets, which are used in the four-electrode microelectrochemical device shown in sub-figure (c); sub-figure (e) provides an optical image of the overall setup of the microelectrochemical device with in situ Raman; and sub-figure (f) provides a high-magnification optical image of the microelectrochemical device shown in sub-figure (e).

[0025] Figure 6 The typical fabrication process of micro-electrochemical devices is shown.

[0026] Figure 7 The equivalent circuit diagram of the three-electrode micro-electrochemical device is depicted.

[0027] Figure 8 Drawn in Figure 2 Gate current measured during the proton insertion and deinsertion processes shown in subfigure (b) of , where subfigures (a) and (b) show the electron injection and electron extraction curves, respectively.

[0028] Fig. 9 The typical electrical characteristics of 1T'-WS2 nanosheets under various conditions are shown, where: Subfigure (a) depicts the typical drain-source current (I) of 1T'-WS2 nanosheets without window (Case I) and with window (Case II) on the substrate swept in 0.5M H2SO4 aqueous solution. ds ) curve; and sub-figure (b) depicts a typical I of 1T'-WS2 nanosheets swept in 0.5M H2SO4 aqueous solution without window (Case I) and with window (Case II) on the substrate. g V g curve.

[0029] Fig.10 Plotted are the typical drain-source currents (I) of 1T'-WS2 nanosheets in microelectrochemical devices tested in electrolytes containing different ions. ds ) and gate current (I g ) curves, wherein: sub-figure (a) depicts the curve of 1T'-WS2 nanosheets tested in lithium ion polymer gel; and sub-figure (b) depicts the curve of 1T'-WS2 nanosheets tested in 0.5M deuterated sulfuric acid solution.

[0030] Fig.11Plot of the I obtained from the cycling test of the 1T'-WS2 microelectrochemical device during proton insertion and deintercalation processes. ds V g curve.

[0031] Fig.12 The equivalent circuit diagram of the four-electrode micro-electrochemical device was drawn.

[0032] Fig.13 The Raman spectra of 1T'-WS2 nanosheets at different gate potentials are plotted, where: Sub-figure (a) provides the Raman spectra of 1T'-WS2 nanosheets at different gate potentials. g =0.81V measured at 1T'-WS2 nanosheet Raman spectrum; and sub-figure (b) provides the V g = 0.82V measured Raman spectrum of 1T'-WS2 nanosheets.

[0033] Fig.14 Plotted are typical drain-source currents (I) of 1T'-WS2 nanosheets in microelectrochemical devices tested in organic proton electrolytes. ds ) and gate current (I g ) curves, where: sub-figure (a) depicts the curve of the micro-electrochemical device swept in an organic protic electrolyte; and sub-figure (b) depicts the curve of the 1T'-WS2 nanosheet before and after proton insertion on a logarithmic scale.

[0034] Fig.15 Raman characterization of 1T'-WS2 nanosheets after proton intercalation in different protic solutions is provided.

[0035] Fig.16 The average intensity distribution of W atoms in 1T'-WS2 nanosheets before the phase transition as shown in sub-figure (a) and after the phase transition as shown in sub-figure (b) are plotted, where the intensity distributions in sub-figures (a) and (b) correspond to Figure 4 The rectangular areas in sub-images (b) and (e).

[0036] Fig.17 Plotted after damping the amplitude of the new superpoint Figure 4 Inverse Fourier transform of the FFT pattern in sub-figure (f).

[0037] Fig.18 Structural characterization of 1T'-WS2 nanosheets after proton embedding is provided, wherein: sub-figure (a) provides a TEM image of 1T'-WS2 nanosheets after proton embedding; and sub-figures (b), (c) and (d) provide SAED patterns of the corresponding areas marked in sub-figure (a).

[0038] Fig.19 The structure of a transistor disclosed herein is exemplarily depicted.

[0039] Fig. 20 Depicted is a diagram showing the preparation of 1T' as disclosed herein d - Flowchart of exemplary steps of the method for WS2 nanosheets.

[0040] Those skilled in the art will appreciate that elements in the figures are illustrated for simplicity and clarity and have not necessarily been drawn to scale. DETAILED DESCRIPTION

[0041] Throughout this disclosure, unless the context requires otherwise, the word "comprise" or variations such as "comprises" or "comprising" will be understood to imply the inclusion of the specified integer or groups of integers but not the exclusion of any other integer or groups of integers. It should also be noted that in this disclosure, particularly in the claims and / or paragraphs, terms such as "comprise", "comprising" or "containing" may have the meanings ascribed to it in patent law; for example, they may mean "includes", "included", "including", etc.; and terms such as "consisting essentially of" and "consists essentially of" have the meanings ascribed to them in patent law, for example, they allow for elements not expressly recited but exclude elements found in the prior art or that affect the basic or novel characteristics of the invention.

[0042] Furthermore, throughout the present disclosure and claims, unless the context requires otherwise, the word "comprise" or variations such as "comprising" or "including", will be understood to imply the inclusion of a stated integer or group of integers but not the exclusion of any other integer or group of integers.

[0043] Unless otherwise expressly stated, the singular as used herein includes the plural (and vice versa). In addition, when the term "about" is used before a quantitative value, the present teachings also include the specific quantitative value itself, unless otherwise specifically stated. As used herein, the term "about" refers to a variation of ±10%, ±7%, ±5%, ±3%, ±1%, or ±0% from the nominal value, unless otherwise stated or inferred.

[0044] Reversible phase transition driven by proton insertion and deinsertion in 1T'-WS2 nanosheets in microelectrochemical devices ( Figure 2 Subgraph (a) of Figure 5 ; Figure 6 ). Figure 7 Shows Figure 2 Subgraph (a) and Figure 5Detailed equivalent circuit diagram of the three-electrode micro-electrochemical device shown in subfigure (a), in which the mechanically exfoliated 1T'-WS2 nanosheets, Pt wires, and evaporated Cr / Au electrodes are used as the channel material, gate electrode, drain electrode, and source electrode, respectively. Figure 2 Subfigure (b) shows the typical drain-source current (I ds ) and gate current (I g ). Initially, when the gate potential (V g ) in the range of 0 to 0.96 V, 1T'-WS2 maintains a stable and high conductivity, which is consistent with the semi-metallic characteristics of 1T'-WS2 under gate control

[35] . g When it exceeds 0.96V, I ds decreased sharply, and I g There is a positive peak in Figure 2 As shown in sub-figure (b), it corresponds to the electron injection into the 1T'-WS2 nanosheet. g Sweep back from 1.4V to 0V, I ds The value increases and eventually reaches the initial current value. g Negative spikes appear ( Figure 2 , sub-figure (b), which corresponds to the electron extraction from the WS2 nanosheet. Figure 2 The gate current distribution in sub-figure (b) of Figure 1 is integrated to calculate the number of injected and extracted electrons. It is found that the number of injected electrons is almost equal to the number of extracted electrons ( Figure 8 ). It is worth mentioning that the electron injection and extraction densities in 1T′-WS2 are both about 1e per chemical formula unit of WS2, which is about 5 times that obtained in the most efficient reversible electron injection and extraction strategy reported previously (i.e., electrostatic electron injection and extraction in MoTe2

[36] ).

[0045] To further elucidate the origin of this significant electrical transport modulation and charge transfer process at the solid electrolyte interface (SEI), a windowless ( Fig. 9 , sub-graph (a), case I) and with window ( Fig. 9 , sub-figure (a), case II) of the micro-electrochemical device. It is worth mentioning that no electrical transport modulation and electron transfer occurred in the device without a window ( Fig. 9 ,Sub-figure (a),Case I; Fig. 9 , sub-figure (b), case I), which indicates the effective passivation effect of the PMMA layer. When the window exposed to the electrolyte is only opened on the basal surface of the 1T'-WS2 nanosheet ( Fig. 9 , sub-figure (a), case II), no electrical transport modulation and electron transfer were observed ( Fig. 9 ,Sub-figure (a),Case II; Fig. 9, sub-figure (b), case II), indicating that electrostatic gating has no effect on the transport modulation of 1T'-WS2 nanosheets

[37] . However, transport modulation and electron transfer can occur in devices where the edge of the nanosheet is partially exposed to the electrolyte ( Figure 2 , sub-figure (b), indicating that the transport modulation and electron transfer originate from the proton insertion and deinsertion in the van der Waals gap of 1T'-WS2 nanosheets through their edges. g When it exceeds 0.96V, Figure 2 The subgraph (b) of I ds The decay slope can reach below 30 mV / dec, which is much lower than the room temperature Boltzmann limit of 60 mV / dec in electrostatic gating

[38] , further confirming that the electrical transport modulation does not come from electrostatic gating. Based on the above experiments and previous on-chip studies on TMD embedding

[27] , it is believed that the charge injection and extraction in aqueous H2SO4 solution can be attributed to the embedding and de-embedding of protons, respectively, which are the only cations in the electrolyte solution and are located in the van der Waals gaps of the layered 1T'-WS2 nanosheets. It is worth mentioning that our results are similar to the phase transitions of metal oxides induced by hydrogenation, in which protons are embedded in their atomic lattices [3],

[30] -

[34] . Our additional experiments in other ion-containing electrolytes show that only proton-containing electrolytes can lead to this reversible electrical transport modulation ( Fig.10 ). In addition, unlike other ionic or molecular intercalations that usually compromise the structural integrity of 2D crystals

[14] -

[16] ,

[20] , proton intercalation and deintercalation are reversible, as demonstrated by cyclic tests ( Fig.11 ).

[0046] Previous studies have highlighted the structural diversity of TMD crystals and the importance of electron injection in modulating their crystal structures [1], [2]. To further understand how much electron injection and extraction density can lead to such large transport modulations, in situ Raman characterization was performed to characterize the structural evolution of 1T'-WS2 during proton insertion and deinsertion ( Figure 5 Sub-figures (e) and (f)). Figure 3 Sub-figure (a) shows the 1T'-WS2 nanosheets before embedding (V g =0V), embedded nanosheets (V g =1.5V) and the deintercalated nanosheets (V g =0 V) in 0.5 M H2SO4 aqueous electrolyte. The 1T'-WS2 nanosheets before embedding show the characteristic Raman spectrum of 1T'-WS2, indicating that the exfoliated nanosheets have high phase purity

[35] . g =1.5 V), the peaks pointing to 1T'-WS2 completely disappear. On the contrary, the peaks at 128, 212, 263, 282, 298, 317 and 407 cm-1 A new set of different Raman peaks appeared at , indicating that the crystal structure of WS2 nanosheets has changed. g When swept back to 0 V, the nanosheets are deintercalated, and the corresponding Raman spectrum is the same as that of the 1T'-WS2 nanosheets before intercalation, indicating that this structural transformation is highly reversible. g = 1.5 V, which is different from the Raman peaks in the previously reported WS2 polymorphs, indicating the formation of a new phase of WS2. Figure 3 As shown in sub-figure (b), there is no PL signal on the 1T'-WS2 nanosheets before embedding, which is due to its semi-metallic nature

[35] . In contrast, the embedded WS2 nanosheets show semiconductor properties. g =1.5V has a strong PL peak of about 650nm ( Figure 3 Subgraph (b) of V g After scanning back to 0V, the loss of PL signal ( Figure 3 Sub-figure (b) shows that the deintercalated nanosheets have transformed from the semiconductor phase to the semi-metallic 1T′ phase, indicating the high reversibility of this phase transition.

[0047] The phase change process can also be visualized in voltage mapping, where V is swept from 0 to 1.5 V in 0.1 V intervals. g The Raman spectra of WS2 nanosheets were recorded during the experiment. To make the phase transition visible, the Raman intensities obtained at different voltages have been normalized. Figure 3 As shown in sub-figure (c), when a constant V in the range of 0 to 0.8 V is applied g When the WS2 nanosheets retain the original 1T' phase, the peaks at 112, 179, 239, 268, 316, and 407 cm -1 Its characteristic peak is shown at g = 0.9 V, the Raman peaks corresponding to 1T'-WS2 disappear, while the peaks at 129, 212, 263, 282, 298, 317 and 407 cm -1 The Raman peak at 1000 nm appears and can be assigned to the new phase. This phase transition process is similar to the I ds The sharp decline is consistent with Figure 2 , sub-figure (b)). Based on the aforementioned PL and Raman spectra, the observed Figure 2 The larger electrical transport modulation shown in sub-figure (b) of can be attributed to the modulation of the electronic band structure from semimetal to semiconductor. The above phase transition is different from the phase transition caused by electrostatic gating, where the phase percentage changes gradually and is closely related to the gate potential [5].

[0048] like Figure 3 As shown in sub-figure (c), when V gThe nanosheets retain the same new phase in the range of 0.9 to 1.5 V. g When scanning back to 0.8 V, the Raman peak indexed to the new phase disappears, and the peak belonging to 1T'-WS2 reappears, indicating that the phase of the WS2 nanosheets transforms back to the original 1T' phase. The percentage of 1T' phase at different voltages is Estimate, where S 1T′ and Indicates that it is assigned to 112cm -1 1T' phase and 128cm -1 New 1T' d The Raman peak area. Figure 3 As shown in sub-figure (d), in V g The percentage of 1T' phase is 100% when the range is from 0 to 0.8V. However, at V g The percentage of 1T' phase approaches about 0% when the range is from 0.9 to 1.5 V. To further determine the V g The phase transition process ranges from 0.8 to 0.9 V. g = 0.81V and 0.82V were subjected to detailed Raman characterization ( Fig.13 ). g = 0.81 V, the Raman spectrum shows the coexistence of the 1T' phase and the new phase ( Fig.13 , sub-graph (a)), and when V g When the voltage slightly increases from 0.81V to 0.82V, the phase of WS2 nanosheets is completely transformed into a new phase ( Fig.13 , sub-figure (b)).

[0049] Highly reversible phase transitions in aqueous proton electrolytes hinder the new 1T' obtained after proton insertion in 1T'-WS2 d Ex situ structural characterization of the phase. To stabilize the embedded structure, we performed proton insertion in an organic proton electrolyte with a slower insertion and deintercalation rate

[39] ,

[40] . Similar to the results obtained in H2SO4 aqueous electrolyte, I ds Keep constant and at V g When the threshold voltage is reached, it starts to decrease (V g =1.1V, Fig.14 , sub-figure (a)). The WS2 nanosheet changes from a high conductance state to a low conductance state. After the embedding process (V g The gate electrode was immediately removed from the electrolyte and the I ds -V ds .like Fig.14 As shown in sub-figure (b), in V ds =0.10V, I dsThe current dropped from 0.24 mA before proton insertion to 7.52 × 10 -8 mA, display on / off ratio>10 6 . With 0.5M H2SO4 aqueous electrolyte ( Figure 2 , sub-figure (b)) compared to the voltage range (0.96 to 1.15 V), the larger embedded voltage range (0.96 to 2.01 V, Fig.14 , sub-figure (a)) is consistent with the slow embedding kinetics in organic electrolytes

[40] . It is also worth mentioning that compared with WS2 nanosheets embedded in H2SO4 aqueous electrolyte, WS2 nanosheets embedded in organic protic electrolytes show similar Raman spectra ( Fig.15 ), suggesting that WS2 nanosheets embedded in aqueous H2SO4 and organic protic electrolytes should have similar structures. Importantly, after proton embedding in organic electrolytes, the nanosheets have a well-maintained low conductivity ( Fig.14 Subfigure (b) in Figure 2 shows that the obtained intercalation compound can be maintained in an organic protic electrolyte, making it possible to characterize the detailed atomic structure using transmission electron microscopy (TEM).

[0050] Atomic resolution HAADF-STEM and SAED were then used to characterize the structural changes of WS2 nanosheets before and after they were embedded in the organic proton electrolyte. Figure 4 As shown in sub-figure (a), the nanosheets before embedding show a typical diffraction pattern of the 1T' phase, which has a lower symmetry than the 1T phase. Rectangular supercell. HAADF-TEM image ( Figure 4 Sub-image (b) shows a zigzag chain consisting of two rows of W atoms, which is a characteristic of the 1T' phase. The distance between WW atoms along the line is 0.32nm ( Fig.16 The corresponding fast Fourier transform (FFT) pattern ( Figure 4 Sub-image (c) of Figure 1 is also consistent with the SAED pattern. After proton insertion, a new set of super reflections appears in the SAED pattern ( Figure 4 The highlighted circles in sub-image (d) of Figure 2 indicate the phase transition from 1T' to a new structure with lower symmetry. The well-preserved zigzag chains ( Figure 4 Sub-image (e) shows a structure similar to 1T'-WS2, but with a slight lattice distortion, as reflected by the super-reflective spots in the corresponding FFT pattern ( Figure 4 Blocking out the amplitudes of all super-reflective spots and taking an inverse Fourier transform enables us to generate a reference image corresponding to the 1T' lattice ( Fig.17) without lattice distortion

[41] . Then we can compare the original image ( Figure 4 sub-image (e)) and the reference image ( Fig.17 ) to quantitatively measure the atomic displacement. Figure 4 The displacement vector field derived in sub-figure (g) of reveals different displacements between two adjacent lines within each zigzag chain, with a larger opposite atomic shift in one line and a smaller shift in the other. The smaller shift is given by Figure 4 The circle in sub-figure (h) shows that the average ( Figure 4 The large opposite shift (shown as a circle) is along

[010] and Its range is as high as about It generates a line of W dimers within the zigzag chain ( Figure 4 The subgraph (g) and Figure 4 Sub-figure (b) of Figure 1 demonstrates a new distorted octahedral structure, denoted as 1T' d , which is distinct from all reported phases in WS2. Impressively, the phase transition can occur throughout the nanosheet, suggesting that the nanosheet has completely transformed from the 1T' phase to the new 1T' d Mutually( Fig.18 ).

[0051] Additional supporting information for the above disclosure is provided in Appendices 1-3.

[0052] In summary, we have demonstrated a reversible phase transition strategy driven by proton insertion and deinsertion to inject and extract electrons into and from 1T'-WS2, respectively. The high electron injection and extraction density (about 1e per formula unit of WS2) driven by proton insertion and deinsertion makes 1T'-WS2 and the new 1T' d A fully reversible phase transition between TMDs and WS2 was confirmed by comprehensive characterizations, including Raman, PL, SAED, and HAADF-STEM. This reversible phase transition driven by proton insertion and deinsertion opens up a new strategy to dynamically control the phase-dependent physicochemical properties of TMDs, which may have potential applications in transistors, memory devices, and neuromorphic computing.

[0053] The advantage of achieving reversible phase changes across a nanosheet of single-crystalline 1T'-WS2 material without causing structural damage to the nanosheet can be used to design transistors for use in electronic and optical applications. One aspect of the present disclosure is to provide a transistor incorporating a 1T'-WS2 nanosheet. Since the reversible phase change occurs across the entire nanosheet rather than being limited to a certain active / single layer or localized domain in the nanosheet, this property can be advantageously exploited to enhance the current handling capability of the transistor and increase the sensitivity of the transistor in response to electrical or optical stimuli.

[0054] Fig.19 The structure of an exemplary transistor 1900 disclosed herein is depicted.

[0055] Transistor 1900 includes a source electrode 1932, a drain electrode 1931, a gate electrode 1933, a 1T'-WS2 nanosheet 1910, and a proton electrolyte 1920. As used herein, a "nanosheet" is a sheet of material having a thickness ranging from 1 to 100 nm. The 1T'-WS2 nanosheet 1910 forms a channel layer of transistor 1900. In addition, the channel layer (i.e., the 1T'-WS2 nanosheet 1910) connects the source electrode 1932 and the drain electrode 1931. Nanosheet 1910 has an edge 1915. Since nanosheet 1910 has a nanometer-scale thickness, edge 1915 has a flat outer edge. Proton electrolyte 1920 is in contact with edge 1915. Proton electrolyte 1920 may contact the entire edge 1915, or more practically as Fig.19 As shown, only a portion of edge 1915 may be contacted. Fig.19 The proton electrolyte 1920 is shown to be in contact with both sides of the edge 1915. In other embodiments, the proton electrolyte 1920 may also be in contact with the edge 1915 on only one side. In order for the proton electrolyte 1920 to contact at least a portion of the edge 1915, when a reaction window is opened on the protective layer near the edge 1915 of the nanosheet 1910, the window needs to cover at least a portion of the edge 1915. The surface of the nanosheet 1910 is covered with a passivation layer (protective layer) to avoid direct contact between the proton electrolyte 1920 and the source electrode 1932 and the drain electrode 1931 and to avoid direct contact between the gate electrode 1933 and the nanosheet 1910. A reaction window can be opened on the protective layer near the edge of the nanosheet 1910. The proton electrolyte 1920 provides a proton reservoir for proton insertion and deinsertion of the nanosheet 1910. In addition, the gate electrode 1933 contacts the proton electrolyte 1920 but does not contact the nanosheet 1910. Therefore, the non-zero gate-source voltage applied between the gate electrode 1933 and the source electrode 1932 generates a voltage difference between the proton electrolyte 1920 and the nanosheet 1910. This voltage difference controls the start of the electron injection process or extraction process, thereby triggering proton insertion or proton deinsertion. Figure 2 As supported by sub-figure (b), the proton electrolyte 1920 can be controlled by the gate-source voltage to perform proton embedding or de-embedding of the nanosheet 1910. The proton embedding or de-embedding of the nanosheet 1910 is used to induce a reversible phase change on the nanosheet 1910, thereby changing the conductivity of the channel layer (i.e., the nanosheet 1910) or the spectral response of the channel layer to light. Figure 2 Subgraph (b) and Figure 3Sub-figure (b) of supports the changes in conductivity and spectral response to light, respectively. Note that the reversible phase transition occurs between the 1T' phase and the 1T' d Between phases. Fig.14 As shown in sub-figure (a) of FIG. 1 , applying a gate-source voltage of 1.1 V or more to transistor 1900 causes nanosheet 1910 to transition from 1T' to 1T' d Note also that if the spectral response of transistor 1900 to light is utilized in an optical application, then transistor 1900 is a phototransistor.

[0056] 1T'-WS2 nanosheets 1910 may be uniformly crystalline. In some embodiments, the crystalline region of the 1T'-WS2 nanosheets 1910 may account for more than 90% of the volume of the 1T'-WS2 nanosheets 1910. In other embodiments, the crystalline region may account for more than 92%, 95%, 97%, 98%, 99%, or 99.9% of the volume of the 1T'-WS2 nanosheets 1910. In certain embodiments, the crystalline region may occupy a volume of the 1T'-WS2 nanosheet 1910 in the range of 70% to 100%, 80% to 100%, 90% to 100%, 90% to 99%, 95% to 100%, 95% to 99%, 96% to 100%, 96% to 99%, 97% to 100%, 97% to 99%, 98% to 100%, 98% to 99%, 99% to 100%, 99.9% to 100%, or any value or range of values ​​within these ranges.

[0057] 1T'-WS2 nanosheets 1910 may include 2-100 layers of 1T'-WS2 nanosheets. In certain embodiments, 1T'-WS2 nanosheets 1910 include 2-90 layers, 2-80 layers, 2-70 layers, 2-60 layers, 2-50 layers, 2-40 layers, 2-30 layers, 2-25 layers, 2-20 layers, 2-15 layers, 2-10 layers, 2-5 layers, 3-30 layers, 3-25 layers, 3-20 layers, 3-15 layers, 3-11 layers, 1-5 layers, 3-5 layers, 1-3 layers, 1-2 layers, or 2-3 layers of 1T'-WS2 nanosheets.

[0058] In some embodiments, the proton electrolyte 1920 is in liquid form. Those skilled in the art will appreciate that techniques for securely containing the liquid proton electrolyte in the transistor 1900 and exposing the liquid proton electrolyte to at least a portion of the edge 1915 are available in the art. As an example, one technique is as follows Figure 2 Layout of the micro-electrochemical device shown in sub-figure (a).

[0059] In some embodiments, the proton electrolyte 1920 is an aqueous proton electrolyte. The aqueous proton electrolyte can be an inorganic acid. The inorganic acid can include sulfuric acid, nitric acid, hydrochloric acid, phosphoric acid, acetic acid, or a combination thereof.

[0060] In certain embodiments, the proton electrolyte 1920 is an organic proton electrolyte. The organic proton electrolyte may include TFSI dissolved in liquid poly(ethylene glycol). In certain embodiments, the liquid poly(ethylene glycol) has an average molecular weight of about 600 amu. The organic proton electrolyte may include TFSI at a concentration of about 0.18 M.

[0061] In certain embodiments, the proton electrolyte 1920 is in solid form. The proton electrolyte 1920 may be a proton-containing solid electrolyte, such as a clay acid electrolyte.

[0062] In some embodiments, the drain electrode 1931 and the source electrode 1932 are made of gold or chromium. It will be understood by those skilled in the art that other conductive materials may be selected to implement the drain electrode 1931 and the source electrode 1932, as long as (1) an ohmic contact can be achieved between the 1T'-WS2 nanosheet 1910 and each of the drain electrode 1931 and the source electrode 1932, and (2) the selected conductive material is inert to WS2.

[0063] In some embodiments, the gate electrode 1933 is made of platinum. Similarly, other conductive materials can be selected to implement the gate electrode 1933. The selected conductive material needs to at least resist corrosion caused by the proton electrolyte 1920.

[0064] Based on the disclosed transistor 1900, a method for preparing 1T' d -WS2 nanosheets approach. Fig. 20 A flow chart showing exemplary steps of the disclosed method is depicted. The method includes steps 2010 and 2020. In step 2010, an embodiment of the disclosed transistor 1900 is provided. In step 2020, a gate-source voltage between the gate electrode 1933 and the source electrode 1932 is applied to the provided embodiment of the transistor 1900. This causes the 1T'-WS2 nanosheet 1910 to change from the 1T' phase to the 1T' phase. d The reversible phase transition of the phase is 1T' d -WS2 nanosheets.

[0065] In certain embodiments, 1T'-WS2 nanosheets and 1T' d -WS2 nanosheets each contain at least two layers.

[0066] In certain embodiments, 1T'-WS2 nanosheets and 1T' d -WS2 nanosheets are each uniformly crystalline.

[0067] In some embodiments, the gate-source voltage is 1.1V or above.

[0068] Without departing from the spirit or essential features of the present invention, the present invention may be implemented in other specific forms. Therefore, the present embodiment should be considered to be illustrative and not restrictive in all aspects. The scope of the present invention is indicated by the appended claims rather than by the preceding description, and therefore all changes falling within the meaning and scope of the equivalents of the claims are intended to be included therein.

[0069] Appendix 1: Synthesis of 1T'-WS2 crystals

[0070] 1T'-WS2 crystals were synthesized according to our previous work

[35] . Specifically, to synthesize 1T'-WS2, K2WO4 and S powders with a molar ratio of 1:4 were ground in a mortar for 10 min to make them uniform. Subsequently, the mixture was transferred to a quartz sample, which was then evacuated to 10 -6 -10 -5 The quartz sample was then heated to 500°C at a heating rate of 1.5°C / min and kept at 500°C in a box furnace for 96 hours. After cooling naturally to room temperature, the precursor was loaded into an alumina crucible and transferred to a tube furnace. After purging with argon (Ar) for 15 minutes, the tube was moved into the preheating furnace zone at 750°C and kept in a hydrogen / argon (H2 / Ar) (20 s.c.cm / 80 s.c.cm) atmosphere for 8 hours. After the reaction was completed, the tube was removed from the heating zone and quickly cooled to room temperature within 10 minutes. The obtained product was washed with Milli-Q water until the pH value of the supernatant was between 7 and 8. The product was then retained in Milli-Q water for 12 hours and immersed in I2 acetonitrile solution (4 mmol, 15 ml) for 24 hours. Afterwards, the product was washed 3 times with acetonitrile and Milli-Q water, respectively. After drying in a vacuum oven at room temperature for 24 h, 1T′-WS2 crystals were obtained and used for device fabrication.

[0071] Appendix 2: Characterization of WS2 with unconventional crystalline phase

[0072] Using Renishaw inVia TM Raman spectra were recorded using a conformal Raman microscope with an excitation wavelength of 532 nm and a low power density of <5 mW / μm 2 Thus, the phase transition of metastable WS2 is avoided. TEM images and SAED patterns were captured using a JEM-2100F (JEOL) transmission electron microscope. SAED patterns and HAADF-STEM images were captured using a JEM-ARM200F (JEOL) TEM equipped with an advanced aberration corrector and a cold field emission gun. All TEMs were operated at an accelerating voltage of 200 kV. Prior to TEM characterization, the phase of the nanosheets was examined by Raman spectroscopy.

[0073] Appendix 3: Device fabrication and characterization

[0074] A set of 32Au contact pads were prefabricated on a 16mm×16mm SiO2(300nm) / Si substrate by conventional photolithography and thermal evaporation. TM Scotch tape was used to mechanically peel 1T'-WS2 nanosheets from our synthesized 1T'-WS2 crystals and transfer them to a prefabricated Si substrate. Then, a low-temperature device fabrication process was used to connect the 1T'-WS2 nanosheets to the prefabricated contact pads. Specifically, PMMA (495, A8, Microchem) was spin-coated on the 1T'-WS2 nanosheets at 3,000 rpm for 40 seconds and baked on a 55°C hotplate for 20 minutes. Then, an electron beam lithography system (TECAN VEGA) was used to define the electrode contacts. Finally, thermally evaporated Cr (8nm) / Au (32nm) was used as the contact electrode. After the lift-off procedure, the device chip was spin-coated with a 1-micron-thick PMMA film to passivate the metal electrodes. Windows were etched on the passivated PMMA layer by electron beam lithography to expose the areas required for testing. A DC voltage V was applied between the drain and source electrodes using a source measurement unit in the Keysight 2902A. ds = 0.1 V to measure the current during the gate control process. Another source measurement unit is used to apply the gate voltage between the Pt wire and the WS2 nanosheet and record the gate current simultaneously.

[0075] like Figure 5 As shown in the figure, three types of microelectrochemical devices were fabricated in this work. In type 1, a three-electrode microelectrochemical device was used for in-situ electrical measurements, during which the drain-source current and the gate current could be collected simultaneously. In type 2, a four-electrode microelectrochemical device consisting of a drain electrode, a source electrode, a gate electrode, and a reference electrode was used for cycle stability testing, which could maintain a stable gate potential at the solid electrolyte interface during long-term cycle testing

[42] . In type 3, a microelectrochemical device with in-situ Raman was used to collect Raman spectra of the nanosheets at different gate potentials.

[0076] like Figure 6 As shown, Au contact pads were prefabricated on SiO2 (300 nm) / Si substrate (16 mm × 16 mm) by conventional photolithography followed by thermal evaporation. The mechanically exfoliated 1T'-WS2 nanosheets were first transferred to the substrate. Then, the drain and source electrodes (Cr (8 nm) / Au (32 nm)) were fabricated by standard electron beam lithography (EBL) process, which contacted the two pre-patterned Au pads. Finally, a thick PMMA passivation layer (about 1 μm) was spin-coated on the device, and a window was opened in the designed PMMA area by EBL.

[0077] like Figure 7 As shown in Figure 1, the equivalent circuit diagram of the three-electrode microelectrochemical device includes two source measurement units (SMUs). SMU 1 is used to measure the voltage (V ds ) and the current flowing through the drain and source electrodes (I ds ) to monitor the transmission modulation, where “High Force” (Force HI) and “Low Force” (ForceLO) are connected to the drain and source electrodes of the TMD nanosheet, respectively. SMU 2 is used to measure the gate voltage (V g ) and gate current (I g ), where “Force HI” and “Force LO” are connected to the gate electrode (Pt line) and ground respectively. SMU 1 and SMU 2 are synchronized, allowing us to record the drain-source and gate current signals simultaneously.

[0078] The total number of transferred electrons is obtained by integrating the scan time and current. Figure 8 As shown, the number of injected electrons (purple area) and extracted electrons are Q1=1.056×10 -8 C and Q2 = 1.048 × 10 -8 C. The small deviation (less than 1%) between Q1 and Q2 may be caused by the noise current during the measurement. The almost equal number of injected and extracted electrons indicates that the electron injection and extraction processes are highly reversible.

[0079] The number of transferred electrons (n) per chemical formula unit of WS2 can be calculated according to the following equation:

[0080]

[0081] as well as

[0082]

[0083] Where A is the area of ​​WS2 nanosheet, d is the thickness of WS2 nanosheet, V 晶胞 =2.1688×10 -28 m 3 is the volume of the WS2 unit cell, Q is the number of injected or extracted electrons, q = 1.60217662 × 10 -19 C is the elementary charge, is the number of transferred electrons, and is the number of chemical formula units of WS2. As a result, the number of electrons injected and extracted per chemical formula unit of WS2 was calculated to be n1 = 0.9857 and n2 = 0.9782, respectively.

[0084] like Fig.10 As shown in subfigure (a) in Figure , the microelectrochemical device was tested in a lithium-ion polymer gel. Briefly, LiClO4 (0.3 g, Sigma-Aldrich) and polyethylene oxide (MW = 100,000, Sigma-Aldrich) were dissolved in 15 mL of anhydrous methanol and stirred at 60 °C for 6 hours. Afterwards, the gel was dropped on the device and then dried in a vacuum oven at 80 °C for 10 minutes to remove the residual solvent before measurement. When the gate voltage was scanned from 0 V to 2 V, a lower conductivity of the 1T'-WS2 nanosheet was observed, indicating that there was no reversible transport modulation. Fig.10 Sub-figure (b) shows the device measured in 0.5 M deuterated sulfuric acid solution. It was found that deuterium ions only produced minimal transport modulation on 1T'-WS2, indicating that deuterium ions cannot play the same role as protons to induce transport modulation.

[0085] Using a four-electrode micro-electrochemical device ( Figure 5 Type 2 in subgraphs (c) and (d) of Fig.12 ) to characterize the cycling stability. The reference electrode (Ag / AgCl) was introduced to maintain a stable interfacial gate potential and avoid the influence of polarization during long-term operation

[42] . During the cycling test, the nanosheets exhibited highly reversible transport modulation.

[0086] like Fig.12 As shown in Figure 1, the equivalent circuit diagram of the four-electrode micro-electrochemical device includes two source measurement units (SMUs). SMU1 is used to measure the drain-source current (I ds ), where “Force HI” and “Force LO” are connected to the drain and source electrodes of the TMD nanosheet, respectively. SMU 2 is used to measure the voltage (V g ) and the current flowing through the gate electrode (I g ), where “Low Sense” (Sense LO) and “Low Force” (Force LO) are connected to the TMD nanosheet. “High Force” (Force HI) and “High Sense” (Sense HI) are connected to the gate electrode (Pt wire) and the reference electrode (Ag / AgCl), respectively. Using such a reference electrode in the cycle test can avoid the influence of polarization and ensure that the voltage applied to the nanosheet is stable in different cycles

[42] .

[0087] At a constant gate potential of 0.81 V, Raman spectra show the original 1T′ phase and the newly emerged 1T′ dWhen the gate potential is slightly increased to 0.82 V, the Raman peak of 1T'-WS2 disappears, and only the newly emerged 1T' d The Raman peak of the phase.

[0088] By dissolving in the average molecular weight (M n ) is 600 in a liquid poly (ethylene glycol) of 0.18 mol L -1 An organic proton electrolyte composed of bis(trifluoromethane)sulfonyl imide (TFSI-) was used as a proton source for intercalation

[39] . Fig.14 As shown in sub-figure (a), the 1T'-WS2 nanosheet shows a large transmission modulation when the gate voltage is swept from 0 to 3 V. When the gate voltage reaches 3 V, the gate electrode is immediately removed from the electrolyte. Then the I ds -V ds curve and record it after embedding. Fig.14 As shown in sub-figure (b), the 1T'-WS2 nanosheets before embedding show good linear characteristics, indicating metallic properties. However, the nanosheets show ultra-low conductivity after the embedding process.

[0089] Raman spectroscopy was used to characterize the 1T'-WS2 nanosheets before and after proton embedding. Fig.15 As shown in Figure 2, the Raman spectrum of the 1T'-WS2 nanosheets before embedding is identical to that of the previously reported 1T'-WS2

[35] , indicating that the phase of the prepared nanosheets is pure 1T'. After embedding in the organic proton electrolyte, the Raman peaks of the nanosheets corresponding to the 1T' phase disappear, and a unique set of peaks assigned to the new 1T' phase appears. d The new peaks of the 1T'-WS2 nanosheets after proton insertion in organic proton electrolytes and 0.5M H2SO4 aqueous solution are similar to those obtained in 1T'-WS2 nanosheets after proton insertion in organic proton electrolytes. d The slight Raman peak shift of the nanosheets can be attributed to the strong electric field during the in situ Raman measurement

[43] ,

[44] .

[0090] Three different regions were selected from the 1T'-WS2 nanosheet after proton embedding ( Fig.18 ).like Fig.18 As shown in sub-figures (b)-(d), the SAED patterns of the three selected areas all show 1T' observed from the same area axis. d The characteristic diffraction spots of the phase indicate that the d complete phase change.

[0091] References

[0092] Listed below is a list of references occasionally cited in the specification. The disclosures of each of these references are incorporated herein by reference in their entirety.

[0093] [1]Chen, Y.; Lai, Z.; Zhang, X.; Fan, Z.; He, Q.; Tan, C.; Zhang, H., Phase engineering of nanomaterials. Nat. Rev. Chem. 2020, 4, 243-256.

[0094] [2]Voiry,D.;Mohite,A.;Chhowalla,M.,Phase engineering of transitionmetal dichalcogenides.Chem.Soc.Rev.2015,44,2702-12.

[0095] [3]Lu, N.; Zhang, P.; Zhang, Q.; Qiao, R.; He, Q.; Li, H.-B.; Wang, Y.; Guo, J.; Zhang, D.; Duan, Z.; Li, Z.; Wang, M. ;Yang,S.;Yan,M.;Arenholz,E.;Zhou,S.;Yang,W.;Gu,L.;Nan,C.-W.;Wu,J.;Tokura,Y.;Yu,P.,Electric-field control of tri-state phase transformation with a selective dual-ion switch. Nature 2017,546,124-128.

[0096] [4]Wang, Y.; Xiao, J.; Chung, T.-F.; Nie, Z.; Yang, S.; Zhang,

[0097] [5]Wang,Y.;Xiao,J.;Zhu,H.;Li,Y.;Alsaid,Y.;Fong,K.Y.;Zhou,Y.;Wang,S.;Shi,W.;Wang,Y.;Zettl,A.;Reed,E.J.;Zhang,X.,Structural phase transition inmonolayer MoTe2 driven by electrostatic doping.Nature 2017,550,487-491.

[0098] [6]Acerce,M.;Voiry,D.;Chhowalla,M.,Metallic 1T phase MoS2nanosheetsas supercapacitor electrode materials.Nat.Nanotechnol.2015,10(4),313-318.

[0099] [7]Yu,Y.;Nam,G.-H.;He,Q.;Wu,X.-J.;Zhang,K.;Yang,Z.;Chen,J.;Ma,Q.;Zhao,M.;Liu,Z.;Ran,F.-R.;Wang,X.;Li,H.;Huang,X.;Li,B.;Xiong,Q.;Zhang,Q.;Liu,Z.;Gu,L.;Du,Y.;Huang,W.;Zhang,H.,High phase-purity 1T′-MoS2-and 1T′-MoSe2-layered crystals.Nat.Chem.2018,10,638-643.

[0100] [8]Voiry,D.;Yamaguchi,H.;Li,J.;Silva,R.;Alves,D.C.;Fujita,T.;Chen,M.;Asefa,T.;Shenoy,V.B.;Eda,G.;Chhowalla,M.,Enhanced catalytic activity instrained chemically exfoliated WS2 nanosheets for hydrogenevolution.Nat.Mater.2013,12,850-5.

[0101] [9]Xu,X.;Pan,Y.;Liu,S.;Han,B.;Gu,P.;Li,S.;Xu,W.;Peng,Y;Han,Z.;Chen,J.;Gao,P.;Ye,Y. single-crystal films of thevan der Waals semiconductor 2H MoTe2.Science 2021,372,195-200.

[0102]

[10] Wang,W.;Kim,S.;Liu,M.;Cevallos,FA;Cava,RJ;Ong,NP,Evidencefor an edge supercurrent in the Weyl superconductor MoTe2.Science 2020,368,534-537.

[0103]

[11] Yuan,Y.;Pan,J.;Wang,X.;Fang,Y.;Song,C.;Wang,L.;He,K.;Ma,X.;Zhang,H.;Huang,F.;Li,W.;Xue,Q.-K. in2M-WS2.Nat.Phy.2019,15,1046-1051.

[0104]

[12] Vaňo,V.;Amini,M.;Ganguli,SC;Chen,G.;Lado,JL;Kezilebieke,S.;Liljeroth,P.,Artificial heavy fermions in a van der Waalsheterostructure.Nature 2021,598-5956.

[0105]

[13] Voiry,D.;Goswami,A.;Kappera,R.;Silva,C.d.C.C.e.;Kaplan,D.;Fujita,T.;Chen,M.;Asefa,T.;Chhowalla,M.,Covalent functionalization of monolayeredtransition metal dichalcogenides by phase engineering.Nat.Chem.2015,7,45-49.

[0106]

[14] Cho,S.;Kim,S.;Kim,J.H.;Zhao,J.;Seok,J.;Keum,D.H.;Baik,J.;Choe,D.-H.;Chang,K.J.;Suenaga,K.;Kim,S.W.;Lee,Y.H.;Yang,H.,Phase patterning for ohmichomojunction contact in MoTe2.Science 2015,349,625-628.

[0107]

[15] Eda,G.;Fujita,T.;Yamaguchi,H.;Voiry,D.;Chen,M.;Chhowalla,M.,Coherent Atomic and Electronic Heterostructures of Single-Layer MoS2.ACS Nano2012,6,7311-7317.

[0108]

[16] Xiong,F.;Wang,H.;Liu,X.;Sun,J.;Brongersma,M.;Pop,E.;Cui,Y.,LiIntercalation in MoS2:In Situ Observation of Its Dynamics and Tuning Opticaland Electrical Properties.Nano Lett.2015,15,6777-6784.

[0109]

[17] Duerloo,KA;Li,Y.;Reed,EJ,Structural phase transitions in two-dimensional Mo-and W-dichalcogenide monolayers.Nat.Commun.2014,5,4214.

[0110]

[18] Lin,Y.-C.;Dumcenco,DO;Huang,Y.-S.;Suenaga,K.,Atomic mechanismof the semiconducting-to-metallic phase transition in single-layeredMoS2.Nat.Nanotechnol.2014,9,391-396.

[0111]

[19] Zhang,X.;Luo,Z.;Yu,P.;Cai,Y.;Du,Y.;Wu,D.;Gao,S.;Tan, C.;Li,Z.;Ren,M.;Osipowicz,T.;Chen,S.;Jiang,Z.;Li,J.;Huang ,Y.;Yang,J.;Chen,Y.;Ang,CY;Zhao,Y.;Wang,P.;Song,L.;Wu,X.;Liu,Z.;Borgna,A.;Zhang,H.,Lithiation-induced morphization of Pd3P2S8 for highly efficient hydrogenevolution.Nat.Catal.2018,1,460-468.

[0112]

[20] Zakhidov,D.;Rehn,DA;Reed,EJ;Salleo,A.,ReversibleElectrochemical Phase Change in Monolayer to Bulk-like MoTe2 by Ionic LiquidGating.ACS Nano 2020,14,2894-2903.

[0113]

[21] Zhang,F.;Zhang,H.;Krylyuk,S.;Milligan,CA;Zhu,Y.;Zemlyanov,DY;Bendersky,LA;Burton,BP;Davydov,AV;Appenzeller,J.,Electrical-field induced structural transition in vertical Mo-Tech and 1-x W x Te2-based resistivememories.Nat.Mater.2019,18,55-61.

[0114]

[22] Zhou,J.;Lin,Z.;Ren,H.;Duan,X.;Shakir,I.;Huang,Y.;Duan,X.,LayeredIntercalation Materials.Adv.Mater.2021,33,2004557.

[0115]

[23] Wu,Y.;Li,D.;Wu,C.-L.;Hwang,HY;Cui,Y.,Electrostatic gating andintercalation in 2D materials.Nat.Rev.Mater.2023,8,41-53.

[0116]

[24] Kappera,R.;Voiry,D.;Yalcin,SE;Branch,B.;Gupta,G.;Mohite,AD;Chhowalla,M.,Phase-engineered low-resistance contacts for ultrathin MoS2transistors.Nat.Mater, 2014,138,131-11.

[0117]

[25] Zeng,Z.;Yin,Z.;Huang,X.;Li,H.;He,Q.;Lu,G.;Boey,F.;Zhang,H.,Single-layer semiconducting nanosheets:high-yield preparation and devicefabrication.Angew.Chem.2011,123,11289-11293.

[0118]

[26] Wang,C.;He,Q.;Halim,U.;Liu,Y.;Zhu,E.;Lin,Z.;Xiao,H.;Duan,X.;Feng,Z.;Cheng,R .;Weiss,NO;Ye,G.;Huang,Y.-C.;Wu,H.;Cheng,H.-C.;Shakir,I.;Liao,L.;Chen,X.;Goddard Iii,WA;Huang,Y.;Duan,X.,Monolayer atomic crystal molecularsuperlattices.Nature2018,555,231-236.

[0119]

[27] He,Q.;Lin,Z.;Ding,M.;Yin,A.;Halim,U.;Wang,C.;Liu,Y.;Cheng,H.-C.;Huang,Y.;Duan,X.,In Situ Probing Molecular Intercalation in Two-Layered Dimensional Semiconductors. Lett.2019,19,6819-6826.

[0120]

[28] Gong,Y.;Yuan,H.;Wu,C.-L.;Tang,P.;Yang,S.-Z.;Yang,A.;Li,G.;Liu,B.;van de Groep,J.;Brongersma,ML;Chisholm,MF;Zhang,S.-C.;Zhou,W.;Cui,Y.,Spatially controlled doping of two-dimensional SnS2 through intercalation forelectronics.Nat.Nanotechnol.2018,13,294-299.

[0121]

[29] Qian,Q.;Ren,H.;Zhou,J.;Wan,Z.;Zhou,J.;Yan,X.;Cai,J.;Wang, P.;Li,B.;Driver,Z.;Li,B.;Duan,X.;Pan,X.;Huang,Y.;Duan,X.,Chiral molecularintercalation superlattices.Nature 2022,606,902-908.

[0122]

[30] Li,L.;Wang,M.;Zhou,Y.;Zhang,Y.;Zhang,F.;Wu,Y.;Wang,Y.;Liu,Y.;Lu, N.;Wang,G.;Peng,H.;Shen,S.;Du,Y.;Zhu,Z.;Nan,C.-W.;Yu,P.,Manipulating theinsulator–metal transition through tip-induced hydrogenation.Nat.Mater.2022,21,1246-1251.

[0123]

[31] Zhao,Q.;Liu,L.;Yin,J.;Zheng,J.;Zhang,D.;Chen,J.;Archer,LA,Proton Intercalation / De-Intercalation Dynamics in Vanadium Oxides for AqueousAluminum Electrochemical Cells.Angew.Chem.Int.Ed.2020,59,3048-3052.

[0124]

[32] Wang,X.;Xie,Y.;Tang,K.;Wang,C.;Yan,C.,Redox Chemistry ofMolybdenum Trioxide for Ultrafast Hydrogen-IonStorage.Angew.Chem.Int.Ed.2018,57,115693-115673.

[0125]

[33] Tan,AJ;Huang,M.;Avci,CO;Büttner,F.;Mann,M.;Hu,W.;Mazzoli,C.;Wilkins,S.;Tuller,HL;Beach,GSD,Magneto-ionic control of magnetism using solid-state proton pump.Nat.Mater.2019,18,35-41.

[0126]

[34] Huang,M.;Hasan,MU;Klyukin,K.;Zhang,D.;Lyu,D.;Gargiani,P.;Valvidares,M.;Sheffels,S.;Churikova,A.; Büttner,F.;Zehner,J.;Caretta,L.;Lee,K.-Y.;Chang,J.;Wang,J.-P.;Leistner,K.;Yildiz,B.;Beach,GSD,Voltage controlof ferrimagnetic order and voltage-assisted writing of ferrimagnetic spintextures.Nat.Nanotechnol.2021,16,981-988.

[0127]

[35] Lai,Z.;He,Q.;Tran,TH;Repaka,DVM;Zhou,DD;Sun,Y.;Xi,S.;Li,Y;Chaturvedi,A.;Tan,C.;Chen,B .;Nam,GH;Li,B.;Ling,C.;Zhai,W.;Shi,Z.;Hu,D.;Sharma,V.;Hu,Z.;Chen,Y.;Zhang,Z.;Yu,Y;Renshaw Wang,X.;Ramanujan,RV;Ma,Y.;Hippalgaonkar,K.;Zhang,H.,Metastable 1T′-phase group VIB transition metaldichalcogenide crystals.Nat.Mater.2021,20,1113-1120.

[0128]

[36] Ye,JT;Zhang,YJ;Akashi,R.;Bahramy,MS;Arita,R.;Iwasa,Y.,Superconducting Dome in a Gate-Tuned Band Insulator.Science2012,338,1193-1196.

[0129]

[37] Perera,M.M.;Lin,M.-W.;Chuang,H.-J.;Chamlagain,B.P.;Wang,C.;Tan,X.;Cheng,M.M.-C.;Tománek,D.;Zhou,Z.,Improved Carrier Mobility in Few-LayerMoS2 Field-Effect Transistors with Ionic-Liquid Gating.ACS Nano 2013,7,4449-4458.

[0130]

[38] Illarionov,Y.Y.;Knobloch,T.;Jech,M.;Lanza,M.;Akinwande,D.;Vexler,M.I.;Mueller,T.;Lemme,M.C.;Fiori,G.;Schwierz,F.;Grasser,T.,Insulators for 2Dnanoelectronics:the gap to bridge.Nat.Commun.2020,11,3385.

[0131]

[39] Li,S.;Li,J.;Wang,Y.;Yu,C.;Li,Y.;Duan,W.;Wang,Y.;Zhang,J.,Largetransport gap modulation in graphene via electric-field-controlled reversiblehydrogenation.Nat.Electron.2021,4,254-260.

[0132]

[40] He,P.;Zhang,X.;Wang,Y.-G.;Cheng,L.;Xia,Y.-Y.,Lithium-IonIntercalation Behavior of LiFePO4 in Aqueous and Nonaqueous Electrolyte Solutions.J.Electrochem.Soc.2008,155,A144.

[0133]

[41] Goodge,B.H.;El Baggari,I.;Hong,S.S.;Wang,Z.;Schlom,D.G.;Hwang,H.Y.;Kourkoutis,L.F.,Disentangling Coexisting Structural Order Through PhaseLock-In Analysis of Atomic-Resolution STEM Data.Microsc.Microanal.2022,28,404-411.

[0134]

[42] Pu,J.;Funahashi,K.;Chen,C.-H.;Li,M.-Y.;Li,L.-J.;Takenobu,T.,Highly Flexible and High-Performance Complementary Inverters of Large-AreaTransition Metal Dichalcogenide Monolayers.Adv.Mater.2016,28,4111-4119.

[0135]

[43] Ayars,E.J.;Hallen,H.D.;Jahncke,C.L.,Electric Field GradientEffects in Raman Spectroscopy.Phy.Rev.Lett.2000,85,4180-4183.

[0136]

[44] Li,L.;Lee,I.;Lim,D.;Kang,M.;Kim,G.-H.;Aoki,N.;Ochiai,Y.;Watanabe,K.;Taniguchi,T.,Raman shift and electrical properties of MoS2 bilayer onboron nitride substrate.Nanotechnol.2015,26,295702。

Claims

1. A transistor, comprising: source electrode, drain electrode and gate electrode; A 1T'-WS2 nanosheet is used as a channel layer, and its two ends are connected to the source electrode and the drain electrode respectively. The surface of the 1T'-WS2 nanosheet is covered with a protective layer to avoid direct contact between the proton electrolyte and the source electrode and the drain electrode, and to avoid direct contact between the gate electrode and the 1T'-WS2 nanosheet. A reaction window is opened on the protective layer near the edge of the 1T'-WS2 nanosheet, so that protons in the proton electrolyte can be embedded and de-embedded under the drive of the gate voltage. The reversible embedding and de-embedding of protons can induce a reversible semi-metal-semiconductor phase transition of WS2, thereby changing the conductivity of the channel layer or the spectral response of the channel layer to light.

2. The transistor according to claim 1, wherein the 1T'-WS2 nanosheet comprises at least two layers.

3. The transistor according to claim 1, wherein the 1T'-WS2 nanosheet is uniformly crystallized. The transistor according to claim 1 , wherein the protonic electrolyte is an aqueous protonic electrolyte. The transistor of claim 4 , wherein the aqueous proton electrolyte is an inorganic acid. 6 . The transistor of claim 5 , wherein the inorganic acid comprises sulfuric acid, nitric acid, hydrochloric acid, phosphoric acid, acetic acid, or a combination thereof. The transistor according to claim 1 , wherein the proton electrolyte is an organic proton electrolyte.

8. The transistor of claim 7, wherein the organic protonic electrolyte is bis(trifluoromethane)sulfonimide (TFSI) dissolved in polyethylene glycol. 9 . The transistor according to claim 1 , wherein the proton electrolyte is a proton-containing solid electrolyte.

10. The transistor of claim 1, wherein each of the drain electrode and the source electrode comprises gold, chromium, or a combination thereof.

11. The transistor of claim 1, wherein the gate electrode comprises platinum.

12. A method for preparing 1T' d - a method for WS2 nanosheets, the method comprising: Providing a transistor according to claim 1; as well as A gate-source voltage is applied between the gate electrode and the source electrode to form the 1T' d -WS2 nanosheets.

13. The method according to claim 12, wherein the 1T'-WS2 nanosheets and the 1T' d Each of the WS2 nanosheets contains at least two layers.