Modification structure for lithium metal negative electrode, lithium metal negative electrode and preparation method and application of lithium metal negative electrode
By using lithium-philic amidic acid modified layer in lithium metal batteries, combining polymers, amidic acid and lithium-philic materials, the problems of lithium dendrites growth and electrolyte interface stability are solved, and the cycle stability and energy density of lithium metal batteries are improved. Extend battery life and enhance safety.
Patent Information
- Application Number
- CN202410929839.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-11
AI Technical Summary
During the deposition process, lithium dendrites are disorderly grown due to uneven current distribution, forming a thick solid electrolyte interface, increasing the internal resistance and safety risks of the battery, and the repeated deposition and peeling lead to a shortening of the battery life.
The lithium-philic amidic acid modified layer is used to form a modified structure with high thermodynamic stability and low nucleation overpotential through the combination of polymer, amidic acid and lithium-philic material, which improves the transmission and diffusion rate of lithium ions and ensures uniform interface contact on the negative electrode surface and Wettability and bonded with lithium metal by mechanical rolling or electrospinning process.
It significantly improves the cycle stability, energy density and Coulomb efficiency of lithium metal batteries, reduces battery internal resistance, extends battery life and enhances safety.
Smart Images

Figure CN118899403A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of new energy technology, and specifically relates to a modified structure for a lithium metal negative electrode, a lithium metal negative electrode, and a preparation method and application thereof. Background Art
[0002] Lithium metal has a high theoretical capacity (e.g., up to 3860 mAh g -1 ) and a lower standard redox potential (-3.040V) are considered to be one of the most ideal negative electrode materials. However, due to the uneven current distribution during the deposition process of lithium metal batteries and the irreversible side reactions with the electrolyte, it is easy to cause the disordered growth of lithium dendrites and the formation of a thicker solid electrolyte interface (SEI) film. In addition, the repeated deposition and stripping of lithium metal will cause the battery volume to expand and the internal resistance of the battery to increase, which will shorten the battery life and increase the potential safety hazards of the battery.
[0003] At present, the main strategies to solve the above technical problems include constructing artificial solid electrolyte interface, current collector modification, diaphragm improvement and electrolyte additive improvement, etc. Among them, artificial solid electrolyte interface refers to the artificial construction of a stable and functional solid layer on the electrode surface through specific process means to simulate and optimize the naturally formed solid electrolyte interface. Existing artificial solid electrolyte interfaces usually have problems such as insufficient thermodynamic stability and low conductivity, and there is still room for improvement in inhibiting the growth of lithium dendrites and reducing side reactions. Summary of the invention
[0004] In order to solve all or part of the above technical problems, the present invention provides the following technical solutions:
[0005] One of the purposes of the present invention is to provide a modified structure for a lithium metal negative electrode, the modified structure comprising a lithium-philic amide acid modification layer, the raw materials of the lithium-philic amide acid modification layer comprising a polymer, an amide acid and a lithium-philic material; the adsorption energy between the lithium-philic material and lithium atoms is lower than -2.0 eV, and the lithium-philic material can at least reduce the nucleation overpotential of lithium metal.
[0006] The amide acid is an amide organic substance generated by the reaction of reactants containing amide and carboxylic acid, which can form Li3N with high thermodynamic stability, high Li+ conductivity and inhibition of lithium dendrite growth in situ after the first charge of the lithium metal battery, thereby promoting ion transmission and protecting the lithium metal surface in the lithium metal battery; and, the present invention forms lithium-philic sites during the charging and discharging process of the lithium metal battery by adding lithium-philic materials, thereby improving the lithium diffusion rate and ensuring uniform interface contact and good wettability on the negative electrode surface; wherein the role of the polymer is to increase the Young's modulus of the modified layer, forming a stable structure to resist the volume expansion of the lithium metal negative electrode during the charging and discharging process; and there is a synergistic effect between the raw materials of the lithium-philic amide acid modification layer. When the lithium-philic material and the amide acid are used simultaneously, the lithium ion migration number can be increased, the adsorption energy of lithium metal and amide acid can be enhanced, and the lithium ion diffusion rate and transmission speed can be increased.
[0007] In some embodiments, in the raw materials, the mass ratio of the polymer, the amide acid, and the lithium-philic material is 1-10: 1-5: 1-5. If the content of the amide acid is too low, the amount of Li3N in the generated SEI film is small, and the migration speed of lithium ions cannot be accelerated. If the content of the amide acid is too high, the SEI film is brittle and cannot resist the volume expansion of the lithium metal battery during the charging and discharging process. If the content of the lithium-philic material is too low, the overpotential of the lithium metal battery is not significantly reduced. If the content of the lithium-philic material is too high, the first cycle will consume excessive lithium metal and electrolyte, reducing the first cycle coulomb efficiency and discharge capacity.
[0008] In some embodiments, the polymer includes one or more combinations of polyethylene terephthalate (PET), polyacrylonitrile (PAN), polyetheretherketone (PEEK), polymethyl methacrylate (PMMA), polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), polyvinylpyrrolidone (PVP), polyhydroxyalkanoate (PHA), cellulose, and protein, but is not limited thereto. The cellulose includes but is not limited to cellulose acetate (CA).
[0009] In some embodiments, the weight average molecular weight of the polymer is greater than 200,000.
[0010] In some embodiments, the amide acid includes one or more of asparagine, alanine amide, phenylalanine amide, malonyl glutamine, tryptophan amide, valinamide, phenylmalonamide, and arabinamide. The amide acid has good chemical stability and is not easily affected by reactions such as hydrolysis and oxidation. The formed modified layer has high thermodynamic stability, high Li+ conductivity, and good performance in inhibiting the growth of lithium dendrites.
[0011] In some embodiments, the lithium-philic material includes one or a combination of metal elements, alloys, metal oxides, and carbon materials.
[0012] In some preferred embodiments, the metal element includes one or more of gold, silver, and antimony, the alloy includes lithium aluminum alloy, the carbon material includes graphene oxide and / or three-dimensional carbon nanotubes, and the metal oxide includes antimony tin oxide, zinc oxide and / or copper oxide.
[0013] In some embodiments, the size of the lithium-philic material is nanometer-sized, preferably 10 to 100 nm.
[0014] In some embodiments, the raw material further includes an organic solvent.
[0015] In some preferred embodiments, the organic solvent includes one or more of trifluoroacetic acid (TFA), dimethylformamide (DMF), dimethylacetamide (DMA), tetrahydrofuran, acetone, ethanol, acetic acid, and CH2C12.
[0016] In some embodiments, the thickness of the lithium-philic amic acid modification layer is 2 μm to 10 μm.
[0017] In some embodiments, the modified structure further includes a substrate.
[0018] In some preferred embodiments, the substrate includes copper foil, aluminum foil, stainless steel foil, nickel foil or lithium foil.
[0019] A second object of the present invention is to provide a lithium metal negative electrode, which includes a lithium metal substrate and a modified structure for a lithium metal negative electrode as described in any one of the technical solutions, wherein the modified structure for a lithium metal negative electrode is combined with lithium metal.
[0020] In some embodiments, the lithium-philic amide acid modification layer and lithium metal are arranged in a stacked manner; or, the metallic lithium is filled inside the lithium-philic amide acid modification layer.
[0021] In an embodiment containing a substrate, the substrate, the lithium-philic amic acid modified layer, and metallic lithium are arranged in a stacked manner; or, the substrate and the lithium-philic amic acid modified layer are arranged in a stacked manner, and the lithium-philic amic acid modified layer is filled with metallic lithium.
[0022] The third object of the present invention is to provide a method for preparing a lithium metal negative electrode modified with a lithium-philic amide acid, comprising:
[0023] Providing a precursor solution containing a polymer, an amic acid, and a lithium-philic material, wherein the adsorption energy between the lithium-philic material and lithium metal is lower than -2.0 eV, which can at least reduce the nucleation overpotential of lithium metal;
[0024] The precursor solution is prepared into a lithium-philic amide acid modification layer and combined with lithium metal to obtain a lithium-philic amide acid modified lithium metal negative electrode; or, the lithium-philic amide acid modification layer is directly formed on the lithium metal to obtain a lithium-philic amide acid modified lithium metal negative electrode.
[0025] In some embodiments, in the precursor solution, the mass ratio of polymer, amic acid, and lithium-philic material is 1N10: 1N5: 1 to 5. In a preferred embodiment, the mass ratio of polymer, amic acid, and lithium-philic material is 8:1:1.
[0026] In some embodiments, the polymer includes one or a combination of polyethylene terephthalate, polyacrylonitrile, polyetheretherketone, polymethyl methacrylate, polyvinylidene fluoride, polyethylene oxide, polyvinyl pyrrolidone, polyhydroxyalkanoate, cellulose acetate, protein, and cellulose.
[0027] In some embodiments, the weight average molecular weight of the polymer is greater than 200,000.
[0028] In some embodiments, the amide acid includes one or a combination of asparagine, alanineamide, phenylalanineamide, malonylglutamine, tryptophanamide, valineamide, phenylmalonamide, and arabinamide.
[0029] In some embodiments, the lithium-philic material includes one or a combination of metal elements, alloys, metal oxides, and carbon materials.
[0030] In some preferred embodiments, the metal element includes one or more of gold, silver, and antimony, the alloy includes lithium aluminum alloy, the carbon material includes graphene oxide and / or three-dimensional carbon nanotubes, and the metal oxide includes zinc oxide and / or copper oxide.
[0031] In some embodiments, the lithium-philic material has a size of nanometer scale.
[0032] In some preferred embodiments, the size of the lithium-philic material is 10-100 nm.
[0033] In some embodiments, the thickness of the lithium-philic amic acid modification layer is 2 μm to 10 μm.
[0034] In some embodiments, the method for preparing the precursor solution includes: mixing and stirring the polymer, amic acid, lithium-philic material and organic solvent under an inert atmosphere to obtain the precursor solution.
[0035] In some embodiments, the method for preparing the precursor solution specifically includes: adding the polymer, amic acid, and lithium-philic material into an organic solvent, and stirring evenly to obtain the precursor solution.
[0036] In some embodiments, the stirring speed is 400-1000 rpm / min.
[0037] In some embodiments, the stirring time is 12 to 24 hours.
[0038] In a typical embodiment, the precursor solution is obtained by stirring at a rotation speed of 1000 rpm / min for 12 hours.
[0039] In some embodiments, the organic solvent includes one or a combination of trifluoroacetic acid (TFA), dimethylformamide (DMF), dimethylacetamide (DMA), tetrahydrofuran, acetone, ethanol, acetic acid, and CH2Cl2.
[0040] In some embodiments, preparing the precursor solution into a lithium-philic amide acid modification layer specifically includes: coating the precursor solution on the surface of a substrate and drying it to form the lithium-philic amide acid modification layer; or, forming the lithium-philic amide acid modification layer on the substrate using an electrospinning process.
[0041] In a typical embodiment, the coating speed is 15 m / min. In the electrospinning process, the feed rate of the precursor solution is 1 mL h -1 .
[0042] In some embodiments, the method of combining the lithium-philic amide acid modification layer with lithium metal includes one or more of mechanical rolling, injecting molten metal lithium, and electrochemical deposition.
[0043] In a typical embodiment, the mechanical rolling pressure used to bond the lithium-philic amic acid modification layer to the lithium metal is 10 MPa.
[0044] In some embodiments, the method of directly forming the lithium-philic amide acid modification layer on the lithium metal comprises an electrospinning process.
[0045] In some embodiments, the substrate includes copper foil, aluminum foil, stainless steel foil, nickel foil or lithium foil, but is not limited thereto.
[0046] A fourth object of the present invention is to provide a lithium metal negative electrode modified with a lithium-philic amide acid obtained by the preparation method described in any one of the technical solutions.
[0047] A fifth object of the present invention is to provide a modified structure for a lithium metal negative electrode as described in any technical solution or an application of the lithium metal negative electrode in the preparation of a lithium metal battery.
[0048] The sixth object of the present invention is to provide a lithium metal battery, comprising a positive electrode, a negative electrode, an electrolyte and a separator, wherein the negative electrode comprises the modified structure for the lithium metal negative electrode described in any technical solution, or the negative electrode is the lithium metal negative electrode described in any technical solution.
[0049] Compared with the prior art, the present invention has at least the following technical effects:
[0050] (1) The raw material for the modified structure provided by the present invention contains amide acid, which has good chemical stability and is not easily affected by reactions such as hydrolysis and oxidation. In addition, during the first charging process of the lithium metal battery, the amide acid can in situ form Li3N with high thermodynamic stability, high Li+ conductivity and the ability to inhibit lithium dendrite growth on the negative electrode surface, thereby promoting ion transport and protecting the lithium metal surface during the operation of the lithium metal battery;
[0051] (2) The raw material for modifying the structure provided by the present invention contains a lithium-philic material, which is easy to form an alloy or a lithium-carbon composite material with lithium during the charge and discharge process of the lithium metal battery, thereby improving the lithium diffusion rate and ensuring uniform interface contact and good wettability of the negative electrode;
[0052] (3) The lithium metal battery provided by the present invention has good battery cycle stability, high energy density and coulombic efficiency, and low impedance. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0054] Figure 1 is a scanning electron microscope image of the lithium-philic amic acid modified layer in Example 1 of the present invention;
[0055] Figure 2 is a comparison diagram of the coulombic efficiency curves of the lithium metal batteries in Example 1 of the present invention and Comparative Example 1;
[0056] Figure 3 It is a comparison chart of the cycle performance curves of the lithium metal batteries of Example 1N5 of the present invention and Comparative Examples 1 to 4. DETAILED DESCRIPTION
[0057] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention. The specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.
[0058] Unless otherwise specified, the raw materials and reagents used in the specific embodiments of the present invention are all commercially available.
[0059] Example 1
[0060] This embodiment provides a lithium metal anode modified with a lithium-philic amide acid and a preparation method thereof, which are specifically as follows:
[0061] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 13% was prepared: polyvinylidene fluoride (PVDF, weight average molecular weight of 400000), aspartamide (purchased from Aladdin), and nanosilver with a particle size of 5nm in a mass ratio of 8:1:1 were added to a dimethylformamide (DMF) solution in sequence, and stirred at a speed of 2000r / min for 12h to obtain a uniform precursor solution after it was fully dissolved;
[0062] The uniform precursor solution obtained above was transferred to the electrospinning needle tube and electrospun on a copper foil substrate, where the solution feed rate was 1 mL h -1 , the applied voltage was 23 kV, the distance between the spinneret tip and the copper foil substrate was 10 cm, the temperature was 35 ° C, the relative humidity was 30%, and a lithium-philic asparagine amide modification layer with a thickness of 3 μm on the copper foil substrate was obtained. Figure 1 is a scanning electron microscope image of the lithium-philic amic acid modified layer;
[0063] The obtained lithium-philic asparagine amide modified layer and a 100 μm lithium sheet were mechanically rolled at a mechanical rolling pressure of 10 MPa to obtain a lithium metal negative electrode containing the lithium-philic asparagine amide modified layer.
[0064] In this example, the lithium metal negative electrode containing the lithium-philic asparagine amide modification layer obtained above was assembled into a lithium metal battery, and the electrochemical performance test was performed. The specific lithium metal battery production process is as follows:
[0065] Positive electrode preparation: LiNi 0.8 Co 0.1 Mn 0.1O2, conductive agent (sp), and binder (PVDF) materials are mixed evenly in a ratio of 98:1:1, and then a solvent is added to stir into a slurry; the stirred slurry is evenly coated on a copper foil with a coating machine and dried to form a positive electrode sheet, which is then baked in a dryer at 85°C to remove moisture and keep the electrode sheet dry; after drying, the electrode sheet is compacted by a roller press and a roller press, and finally cut into the specifications required by the battery of this embodiment for standby use;
[0066] Preparation of negative electrode sheet: In a glove box filled with argon (water and oxygen content are both less than 0.1 ppm), the lithium metal negative electrode sheet containing the lithium-philic amic acid modification layer prepared above is punched out by a die-cutting machine into the specifications required by the battery of this embodiment and set aside for use;
[0067] Electrolyte preparation: 1 M lithium bis(fluorosulfonyl)imide (LiFSI) was dissolved in equal volumes of 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) to obtain a lithium metal battery electrolyte.
[0068] Battery cell preparation: The prepared positive electrode sheet, negative electrode sheet and a polyethylene separator with a thickness of 16 μm are prepared into a battery cell through a lamination process, and the battery cell is loaded into an aluminum-plastic film shell, and the tab welding and side sealing operations are performed. Then, the electrolyte is injected in a glove box filled with argon gas (the water and oxygen content are both less than 0.1 ppm). After packaging, the battery cell is left to stand, formed, degassed, aged and divided into different volumes to finally obtain a lithium metal battery.
[0069] The lithium metal battery has an energy density of 400wh / kg at 25°C, a coulombic efficiency of >98.5%, a cycle number of >280 cycles at a 0.3 / 0.5C rate, and a battery internal resistance of <16mΩ.
[0070] Example 2
[0071] This embodiment provides a lithium metal anode modified with a lithium-philic amide acid and a preparation method thereof, which are specifically as follows:
[0072] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 13% was prepared: polyethylene terephthalate (PET, weight average molecular weight of 250,000), alanine amide (purchased from McLean), and nano zinc oxide powder with a particle size of 10 nm were added to a tetrahydrofuran solution in a mass ratio of 1:8:1 in sequence, and stirred at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after it was fully dissolved;
[0073] The precursor solution obtained above was evenly coated on a 12 μm copper foil by spin coating process to form a lithium-philic alanine amide modification layer with a thickness of 3 μm;
[0074] The obtained lithium-philic alaninamide modified layer was mechanically rolled with a 80 μm lithium sheet at a mechanical rolling pressure of 15 MPa to obtain a lithium metal negative electrode containing a lithium-philic alaninamide modified layer.
[0075] In this example, the lithium metal negative electrode containing the lithium-philic alaninamide modification layer obtained above is assembled into a lithium metal battery for electrochemical performance testing. The specific lithium metal battery manufacturing process is the same as that in Example 1.
[0076] The lithium metal battery obtained in this embodiment has an energy density of 400wh / kg at 25°C, a coulombic efficiency of >98.8%, a cycle number of >290 cycles at 0.3 / 0.5C rate, a cycle number of >200 cycles at 1C rate, and a battery internal resistance of <16mΩ.
[0077] Example 3
[0078] This embodiment provides a lithium metal anode modified with a lithium-philic amide acid and a preparation method thereof, which are specifically as follows:
[0079] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 13% was prepared: polymethyl methacrylate (PMMA, weight average molecular weight of 200,000), phenylalanine amide (purchased from MacLean) and nano zinc oxide with a particle size of 10 nm were added to a dimethylformamide (DMF) solution in a mass ratio of 8:1:0.5 in sequence, and stirred at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after it was fully dissolved;
[0080] The uniform precursor solution obtained above was transferred to the electrospinning needle tube and electrospun on a copper foil substrate, where the solution feed rate was 0.5 mL h -1 , the applied voltage was 23 kV, the distance between the spinneret tip and the copper foil substrate was 10 cm, the temperature was 35° C., the relative humidity was 30%, and a lithium-philic phenylalanine amide modification layer with a thickness of 5 μm was obtained on the copper foil substrate;
[0081] The molten lithium operation is carried out under an inert gas atmosphere to prevent lithium from reacting with oxygen in the air. The molten lithium is injected into the lithium-philic phenylalaninamide modification layer, and the layer is left to stand and wait for molding to obtain a modified composite lithium metal negative electrode.
[0082] In this example, the composite lithium metal negative electrode prepared by the above method is assembled into a lithium metal battery to conduct an electrochemical performance test. The specific lithium metal battery manufacturing process is the same as that of Example 1.
[0083] The lithium metal battery has an energy density of 400wh / kg at 25°C, a coulombic efficiency of >98.8%, a cycle number of >280 at a rate of 0.3 / 0.5C, and a battery internal resistance of <15mΩ.
[0084] Example 4
[0085] This embodiment provides a lithium metal anode modified with a lithium-philic diamide acid and a preparation method thereof, as follows
[0086] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 15% was prepared: polyethylene oxide (PEO, weight average molecular weight of 200,000), asparagine (purchased from McLean), phenylalanine amide (purchased from McLean) and nanosilver with a particle size of 5 nm were added to a dimethylformamide (DMF) solution in a mass ratio of 1:8:0.5:0.5 in sequence, and stirred at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after the precursor solution was fully dissolved;
[0087] The precursor solution was uniformly coated on a 12 μm copper foil by a doctor blade coating process to form a 5 μm thick lithium-philic diamic acid modified layer.
[0088] The modified layer containing the copper foil current collector obtained in the above step is paired with a pure lithium electrode by using the method of electrochemical deposition of metallic lithium. 1M lithium bis(fluorosulfonyl)imide (LiFSI) is dissolved in an electrolyte of equal volumes of 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME). Lithium is deposited into the modified layer by constant current charge and discharge, thereby obtaining a lithium metal negative electrode containing a lithium-philic bisamic acid modified layer.
[0089] In this embodiment, a lithium metal negative electrode sheet containing a lithium-philic diamide acid modification layer is assembled into a lithium metal battery for electrochemical performance testing. The specific lithium metal battery manufacturing process is the same as in Example 1.
[0090] The lithium metal battery has an energy density of 400wh / kg at 25°C, a coulombic efficiency of >98.5%, a cycle number of >270 cycles at a 0.3 / 0.5C rate, and a battery internal resistance of <16mΩ.
[0091] Example 5
[0092] This embodiment provides a lithium metal anode modified with a lithium-philic amide acid and a preparation method thereof, which are specifically as follows:
[0093] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 15% was prepared: polyetheretherketone (PEEK, weight average molecular weight of 200000), alanylglutamine (purchased from McLean) in a mass ratio of 9:1:0.5, and nano-tin antimony oxide with a particle size of 15nm were added to a dimethylacetamide (DMA) solution in sequence, and stirred at a speed of 2000r / min for 12h to obtain a uniform precursor solution after it was fully dissolved;
[0094] The uniform precursor solution obtained above was transferred to the electrospinning needle tube and electrospun on a stainless steel foil substrate, where the solution feeding rate was 1 mL h -1 , the applied voltage was 23 kV, the distance between the spinneret tip and the stainless steel foil substrate was 10 cm, the temperature was 35° C., the relative humidity was 30%, and a malonyl-glutamine modified layer with a thickness of 5 μm loaded on the substrate was obtained.
[0095] The method of electrochemically depositing metallic lithium is adopted to compound the malonylglutamine modified layer with lithium metal to obtain a lithium metal negative electrode sheet containing the malonylglutamine modified layer.
[0096] In this example, the composite lithium metal negative electrode prepared by the above method is assembled into a lithium metal battery to conduct an electrochemical performance test. The specific lithium metal battery manufacturing process is the same as that of Example 1.
[0097] The lithium metal battery has an energy density of 400wh / kg at 25°C, a coulombic efficiency of >99%, a cycle number of >290 cycles at a 0.3 / 0.5C rate, and a battery internal resistance of <16mΩ.
[0098] Example 6
[0099] This embodiment provides a lithium metal anode modified with a lithium-philic amide acid and a preparation method thereof, which are specifically as follows:
[0100] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 13% was prepared: polyethylene terephthalate (PET, weight average molecular weight of 250,000), tryptophan amide (purchased from Aladdin), and graphene oxide in a mass ratio of 2:7:1 were added to a dimethylformamide (DMF) solution in sequence, and stirred at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after it was fully dissolved;
[0101] The precursor solution obtained above was uniformly coated on a 12 μm copper foil by a spray coating process to obtain a lithium-philic tryptophan amide modification layer;
[0102] The obtained lithium-philic tryptophan amide modified layer was mechanically rolled with a 80 μm lithium sheet at a mechanical rolling pressure of 105 MPa to obtain a lithium metal negative electrode containing a lithium-philic tryptophan amide modified layer.
[0103] In this example, the composite lithium metal negative electrode prepared by the above method is assembled into a lithium metal battery to conduct an electrochemical performance test. The specific lithium metal battery manufacturing process is the same as that of Example 1.
[0104] The lithium metal battery has an energy density of 400wh / kg at 25°C, a coulombic efficiency of >98.5%, a cycle number of >280 cycles at a 0.3 / 0.5C rate, and a battery internal resistance of <16mΩ.
[0105] Example 7
[0106] This embodiment provides a lithium metal anode modified with a lithium-philic amide acid and a preparation method thereof, which are specifically as follows:
[0107] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 13% was prepared: polyvinylpyrrolidone (PVP, weight average molecular weight of 250,000), polyvinylidene fluoride (PVDF), valinamide (purchased from MacLean), and nano copper oxide with a particle size of 5 nm were added to a dimethylformamide (DMF) solution in a mass ratio of 4:4:1:1 in sequence, and stirred at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after it was fully dissolved;
[0108] The above uniform precursor solution was transferred to the electrospinning needle tube and electrospun on a copper foil substrate, where the solution feed rate was 1 mL h -1 , the applied voltage was 23 kV, the distance between the spinneret tip and the current collector was 12 cm, the temperature was 35° C., and the relative humidity was 30%, to obtain a lithium-philic valinamide modified layer with a thickness of 3 μm supported on the substrate.
[0109] The obtained lithium-philic valinamide modified layer and a 50 μm lithium sheet were mechanically rolled at a mechanical rolling pressure of 10 MPa to obtain a lithium metal negative electrode containing a lithium-philic valinamide modified layer.
[0110] In this example, the composite lithium metal negative electrode prepared by the above method is assembled into a lithium metal battery to conduct an electrochemical performance test. The specific lithium metal battery manufacturing process is the same as that of Example 1.
[0111] The lithium metal battery has an energy density of 400wh / kg at 25°C, a coulombic efficiency of >99%, a cycle number of >270 cycles at a 0.3 / 0.5C rate, and a battery internal resistance of <16mΩ.
[0112] Example 8
[0113] This embodiment provides a lithium metal anode modified with a lithium-philic amide acid and a preparation method thereof, which are specifically as follows:
[0114] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 13% was prepared: cellulose acetate (CA, weight average molecular weight of 600000), phenylmalonamide (purchased from MacLean) and nano-tin antimony oxide with a particle size of 15nm were added to an acetone solution in order at a mass ratio of 9:1:1:1, and stirred at a speed of 2000r / min for 12h to obtain a uniform precursor solution after the precursor solution was fully dissolved;
[0115] The uniform precursor solution obtained above was transferred to the electrospinning needle tube and electrospun on a copper foil substrate, where the solution feed rate was 0.8 mL h -1 , the applied voltage was 23 kV, the distance between the spinneret tip and the current collector was 10 cm, the temperature was 35° C., and the relative humidity was 30%, to obtain a lithium-philic phenylmalonamide modified layer with a thickness of 5 μm loaded on the substrate.
[0116] The obtained lithium-philic phenylmalonamide modified layer and a 100 μm lithium sheet were mechanically rolled at a mechanical rolling pressure of 10 MPa to obtain a lithium metal negative electrode containing the lithium-philic phenylmalonamide modified layer.
[0117] In this example, the composite lithium metal negative electrode prepared by the above method is assembled into a lithium metal battery to conduct an electrochemical performance test. The specific lithium metal battery manufacturing process is the same as that of Example 1.
[0118] The lithium metal battery has an energy density of 400wh / kg at 25°C, a coulombic efficiency of >98.5%, a cycle number of >280 cycles at a 0.3 / 0.5C rate, and a battery internal resistance of <16mΩ.
[0119] Example 9
[0120] This embodiment provides a lithium metal anode modified with a lithium-philic amide acid and a preparation method thereof, which are specifically as follows:
[0121] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 13% was prepared: polyacrylonitrile (PAN, weight average molecular weight of 150,000), arabinamide (purchased from Aladdin), and lithium aluminum alloy were added to a dimethylformamide (DMF) solution in a mass ratio of 2:7:1 in sequence, and stirred at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after it was fully dissolved;
[0122] The precursor solution obtained above was uniformly coated on a 12 μm copper foil by a doctor blade coating process to obtain a lithium-philic tryptophan amide modification layer with a thickness of 5 μm;
[0123] The obtained lithium-philic tryptophan amide modified layer was mechanically rolled with a 80 μm lithium sheet at a mechanical rolling pressure of 100 MPa to obtain a lithium metal negative electrode containing a lithium-philic arabinamide modified layer.
[0124] In this example, the composite lithium metal negative electrode prepared by the above method is assembled into a lithium metal battery to conduct an electrochemical performance test. The specific lithium metal battery manufacturing process is the same as that of Example 1.
[0125] The lithium metal battery has an energy density of 400wh / kg at 25°C, a coulombic efficiency of >98.8%, a cycle number of >265 cycles at a 0.3 / 0.5C rate, and a battery internal resistance of <16mΩ.
[0126] Example 10
[0127] This embodiment provides a lithium metal anode modified with a lithium-philic amide acid and a preparation method thereof, which are specifically as follows:
[0128] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 12% was prepared: silk protein (weight average molecular weight of 25000), arabinamide (purchased from Aladdin), and three-dimensional carbon nanotubes with a mass ratio of 2:7:1 were added to a dimethylformamide (DMF) solution in sequence, and stirred at a speed of 2000r / min for 12h to obtain a uniform precursor solution after it was fully dissolved;
[0129] The precursor solution obtained above was uniformly coated on a 12 μm copper foil by a coating process to obtain a lithium-philic tryptophan amide modification layer with a thickness of 5 μm;
[0130] The obtained lithium-philic tryptophan amide modified layer was mechanically rolled with a 80 μm lithium sheet at a mechanical rolling pressure of 105 MPa to obtain a lithium metal negative electrode containing a lithium-philic arabinamide modified layer.
[0131] In this example, the composite lithium metal negative electrode prepared by the above method is assembled into a lithium metal battery to conduct an electrochemical performance test. The specific lithium metal battery manufacturing process is the same as that of Example 1.
[0132] The lithium metal battery has an energy density of 400wh / kg at 25°C, a coulombic efficiency of >98.5%, a cycle number of >280 cycles at a 0.3 / 0.5C rate, and a battery internal resistance of <16mΩ.
[0133] Comparative Example 1
[0134] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 13% was prepared: polyvinylidene fluoride was added to a dimethylformamide (DMF) solution and stirred at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after it was fully dissolved;
[0135] The above-mentioned uniform precursor solution was transferred to the electrospinning needle tube and electrospun on a copper foil substrate, where the solution feed rate was 1 mL h -1 , the applied voltage was 23 kV, the distance between the spinneret tip and the current collector was 10 cm, the temperature was 35 ° C, the relative humidity was 30%, and a polymer modified layer with a thickness of 5 μm was obtained;
[0136] The obtained polymer modified layer and a 100 μm lithium sheet were mechanically rolled at a mechanical rolling pressure of 10 MPa to obtain a modified composite lithium metal negative electrode, and the negative electrode sheet was assembled into a lithium metal battery according to the battery assembly method in the above Example 1.
[0137] Comparative Example 2
[0138] In an argon glove box (water and oxygen contents were all less than 0.1 ppm), a precursor solution with a solid content of 13% was prepared: polyacrylonitrile was added to a dimethylformamide (DMF) solution and stirred at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after it was fully dissolved;
[0139] The precursor solution was uniformly coated on a 12 μm copper foil by a doctor blade coating process to prepare a polymer modified layer with a thickness of 5 μm.
[0140] The obtained polymer modified layer and a 100 μm lithium sheet were mechanically rolled at a mechanical rolling pressure of 10 MPa to obtain a modified composite lithium metal negative electrode, and the negative electrode sheet was assembled into a lithium metal battery according to the battery assembly method in the above Example 1.
[0141] Comparative Example 3
[0142] In an argon glove box (water and oxygen contents were all <0.1ppm), a precursor solution with a solid content of 15% was prepared: polyethylene oxide (PEO) was added to a dimethylformamide solution and stirred at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after it was fully dissolved;
[0143] The precursor solution was evenly coated on a 12 μm copper foil using a blade coating process to form a polymer modification layer with a thickness of 5 μm.
[0144] The modified layer is composited with lithium metal using an electrochemical deposition method to obtain a composite lithium metal negative electrode, and the negative electrode sheet is assembled into a lithium metal battery according to the battery assembly method in the above-mentioned Example 1.
[0145] Comparative Example 4
[0146] Step 1, in an argon glove box (water and oxygen contents are all less than 0.1 ppm), prepare a precursor solution with a solid content of 16%: add polyetheretherketone (PEEK) into dimethylacetamide (DMA) solution, and stir at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after it is fully dissolved;
[0147] Step 2, transferring the uniform precursor solution in step 1 to the electrospinning needle tube, and performing electrospinning on a copper foil substrate, wherein the solution feed rate is 1.2 mL h-1; the applied voltage is 25 kV; the distance between the spinneret tip and the current collector is 10 cm; the temperature is 35°C; and the relative humidity is 30%.
[0148] Step 3, injecting molten lithium into the above-mentioned polymer modified layer to obtain a composite lithium metal negative electrode, and assembling the negative electrode sheet into a lithium metal battery according to the battery assembly method in the above-mentioned embodiment 1.
[0149] Comparative Example 5
[0150] In an argon glove box (water and oxygen contents were all less than 0.1 ppm), a precursor solution with a solid content of 14% was prepared: polyethylene terephthalate (PET) was added to a tetrahydrofuran (THF) solution and stirred at a speed of 2000 r / min for 12 h to obtain a uniform precursor solution after it was fully dissolved;
[0151] The precursor solution obtained above was evenly coated on a 12 μm copper foil by spin coating to form a modified layer with a thickness of 3 μm;
[0152] The obtained polymer modified layer and a 100 μm lithium sheet were mechanically rolled at a mechanical rolling pressure of 10 MPa to obtain a modified composite lithium metal negative electrode, and the negative electrode sheet was assembled into a lithium metal battery according to the battery assembly method in the above Example 1.
[0153] Comparative Example 6
[0154] The difference between Comparative Example 6 and Example 1 is that the precursor solution does not contain asparagine, and the rest is the same as Example 1.
[0155] Comparative Example 7
[0156] The only difference between Comparative Example 7 and Example 1 is that the precursor solution does not contain nanosilver, and the rest is the same as Example 1.
[0157] Figure 2 is a comparison diagram of the coulombic efficiency curves of the lithium metal batteries in Example 1 and Comparative Example 1; Figure 3It is a comparison diagram of the cycle performance curves of the lithium metal batteries of Examples 1 to 5 of the present invention and Comparative Examples 1 to 4. It can be seen that the coulombic efficiency and cycle performance of the lithium metal battery containing the lithium-philic amic acid modification layer are significantly improved.
[0158] Detection Methods
[0159] The soft-pack lithium metal batteries prepared in the above-mentioned embodiments and comparative examples were respectively compared to perform cycle capacity and internal resistance tests, and the test methods are as follows:
[0160] 1) Cycle capacity test: At 25°C, charge the soft-pack battery to 4.3V at 0.2C constant current and constant voltage, with a cut-off current of 0.05C; then leave it for 10 minutes; then discharge it to 3.0V at 0.5C constant current, and record the number of cycles when the capacity decays to 80% of the nominal capacity;
[0161] 2) Internal resistance detection: Under 25° C., the soft-pack lithium metal batteries prepared in Example 1 and Comparative Example 1 were tested for internal resistance using an internal resistance meter, and the internal resistance data were recorded.
[0162] Results Analysis
[0163] The electrochemical properties of the soft-pack lithium metal batteries prepared in the above examples and comparative examples are shown in Table 1:
[0164] Table 1 Comparison of electrochemical performance of lithium metal batteries
[0165]
[0166]
[0167] In summary, the lithium metal negative electrode modified with the lithium-philic amide acid provided by the present invention can inhibit the growth of lithium dendrites, reduce the side reactions between the electrolyte and the metal negative electrode, and effectively extend the cycle life of the lithium metal battery. The amide acid selected by the present invention has good chemical stability, is not easily affected by reactions such as hydrolysis and oxidation, and can form Li3N with high thermodynamic stability, high Li+ conductivity and inhibition of lithium dendrite growth in situ after the first charge of the lithium metal battery, which can promote ion transport and protect the lithium metal surface in the lithium metal battery; at the same time, the lithium-philic substance is very easy to form an alloy with lithium during the charge and discharge process of the lithium metal battery, providing a high lithium diffusion rate to ensure uniform interface contact and good wettability.
[0168] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0169] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0170] Although the present invention has been described with reference to illustrative embodiments, it will be understood by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.
Claims
1. A modified structure for a lithium metal negative electrode, characterized in that: The modified structure includes a lithium-philic amide acid modification layer, the raw materials of which include polymers, amide acid and lithium-philic materials; the adsorption energy between the lithium-philic material and lithium atoms is lower than -2.0 eV, and the lithium-philic material can at least reduce the nucleation overpotential of lithium metal.
2. The modified structure for lithium metal negative electrode according to claim 1, characterized in that: In the raw materials, the mass ratio of the polymer, the amic acid, and the lithium-philic material is 1-10:1-5:1-5; And / or, the polymer includes one or a combination of polyethylene terephthalate, polyacrylonitrile, polyetheretherketone, polymethyl methacrylate, polyvinylidene fluoride, polyethylene oxide, polyvinyl pyrrolidone, polyhydroxyalkanoate, cellulose, and protein; and / or, at least part of the polymer has a weight average molecular weight of 200,000 or more; And / or, the amide acid includes one or a combination of asparagine, alanineamide, phenylalanineamide, malonylglutamine, tryptophanamide, valinamide, phenylmalonamide, and arabinamide; And / or, the lithium-philic material comprises a combination of one or more of a metal element, an alloy, a metal oxide or a carbon material; preferably, the metal element comprises one or more of gold, silver or antimony, the alloy comprises a lithium aluminum alloy, the carbon material comprises graphene oxide and / or a three-dimensional carbon nanotube, and the metal oxide comprises zinc oxide and / or copper oxide; And / or, the size of the lithium-philic material is nanometer-scale, preferably 10 to 100 nm; And / or, the raw material further comprises an organic solvent, preferably, the organic solvent comprises one or more of trifluoroacetic acid, dimethylformamide, dimethylacetamide, tetrahydrofuran, acetone, ethanol, acetic acid or CH2Cl2; And / or, the thickness of the lithium-philic amic acid modification layer is 2 μm to 10 μm; And / or, the modified structure further comprises a substrate, preferably, the substrate comprises copper foil, aluminum foil, stainless steel foil, nickel foil or lithium foil.
3. A lithium metal negative electrode, comprising a lithium metal substrate, characterized in that: The lithium metal negative electrode further comprises the modified structure for the lithium metal negative electrode according to claim 1 or 2, and the modified structure for the lithium metal negative electrode is combined with the lithium metal.
4. A method for preparing a lithium metal negative electrode modified with a lithium-philic amide acid, characterized in that: include: Providing a precursor solution containing a polymer, an amic acid and a lithium-philic material, wherein the adsorption energy between the lithium-philic material and lithium atoms is lower than -2.0 eV, and the lithium-philic material can at least reduce the nucleation overpotential of lithium metal; The precursor solution is prepared into a lithium-philic amic acid modified layer, and combined with lithium metal to obtain a lithium-philic amic acid modified lithium metal negative electrode; Alternatively, a lithium-philic amide acid modification layer is directly formed on the lithium metal to obtain a lithium-philic amide acid modified lithium metal negative electrode.
5. The preparation method according to claim 4, characterized in that: In the precursor solution, the mass ratio of polymer, amic acid and lithium-philic material is 1-10:1-5:1-5; And / or, the polymer includes one or a combination of polyethylene terephthalate, polyacrylonitrile, polyetheretherketone, polymethyl methacrylate, polyvinylidene fluoride, polyethylene oxide, polyvinyl pyrrolidone, polyhydroxyalkanoate, cellulose acetate, protein, and cellulose; and / or, at least part of the polymer has a weight average molecular weight of 200,000 or more; And / or, the amide acid includes one or a combination of asparagine, alanineamide, phenylalanineamide, malonylglutamine, tryptophanamide, valinamide, phenylmalonamide, and arabinamide; And / or, the lithium-philic material comprises a combination of one or more of a metal element, an alloy, a metal oxide or a carbon material; preferably, the metal element comprises one or more of gold, silver or antimony, the alloy comprises a lithium aluminum alloy, the carbon material comprises graphene oxide and / or a three-dimensional carbon nanotube, and the metal oxide comprises zinc oxide and / or copper oxide. And / or, the size of the lithium-philic material is nanometer-scale, preferably 10 to 100 nm; And / or, the thickness of the lithium-philic amic acid modification layer is 2 μm to 10 μm.
6. The preparation method according to claim 4, characterized in that: The method for preparing the precursor solution comprises: mixing and stirring the polymer, amic acid, lithium-philic material and organic solvent under an inert atmosphere to obtain the precursor solution; Preferably, the stirring speed is 400-1000 rpm / min; Preferably, the stirring time is 12 to 24 hours; Preferably, the organic solvent comprises one or a combination of trifluoroacetic acid, dimethylformamide, dimethylacetamide, tetrahydrofuran, acetone, ethanol, acetic acid or CH2Cl2.
7. The preparation method according to claim 4, characterized in that: The step of preparing the precursor solution into a lithium-philic amic acid modification layer specifically includes: coating the precursor solution on a substrate surface and drying to form the lithium-philic amic acid modification layer; or, forming the lithium-philic amic acid modification layer on a substrate using an electrospinning process; and / or, the method of combining the lithium-philic amic acid modified layer with lithium metal comprises one or more of mechanical rolling, injection of molten lithium, and electrochemical deposition; And / or, the method of directly forming the lithium-philic amide acid modification layer on the lithium metal comprises electrospinning or coating.
8. A lithium metal negative electrode modified with a lithium-philic amide acid obtained according to the preparation method according to any one of claims 4 to 7.
9. Use of the modified structure for lithium metal negative electrode according to any one of claims 1 to 2 or the lithium metal negative electrode according to claim 3 or 8 in the preparation of lithium metal batteries.
10. A lithium metal battery comprising a positive electrode, a negative electrode, an electrolyte and a separator, characterized in that: The negative electrode comprises the modified structure for lithium metal negative electrode according to claim 1 or 2, or the negative electrode is the lithium metal negative electrode according to claim 3 or 8.
Citation Information
Patent Citations
Organic lithium-philic composite negative electrode taking three-dimensional conductive carbon material as substrate and preparation method of organic lithium-philic composite negative electrode
CN111952567A
Three-dimensional conductive carbon negative electrode material modified by organic lithium-philic coating as well as preparation method and application thereof
CN113725435A
Preparation method of three-dimensional organic framework composite material, lithium metal negative electrode and battery
CN114335550A
Lithium metal negative electrode modified by sustainable flexible protective layer and preparation method of lithium metal negative electrode
CN116706000A
Anode for lithium ion secondary battery, lithium ion secondary battery and method of manufacturing anode for lithium ion secondary battery
JP2011249058A
Cited By
Modification structure for negative electrode, lithium metal negative electrode containing modification structure for negative electrode and application of lithium metal negative electrode
CN122552525A
A modification structure for a negative electrode, a lithium metal negative electrode including the modification structure for a negative electrode, and applications
CN122552525B