Catalyst compositions and methods of making and using same
By setting a specific combination of elements on the catalyst support and avoiding the presence of silicon, a catalyst with excellent stability and activity under high temperature and high pressure was prepared, which solved the problem of low propylene yield under low pressure of existing catalysts and realized a highly efficient dehydrogenation process.
Patent Information
- Application Number
- CN202380028887.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-02-27
- Publication Date
- 2024-11-05
AI Technical Summary
Existing catalysts have low propylene yields under low pressure, and more efficient conditions are needed to increase propylene yield in order to improve the efficiency of the dehydrogenation process.
A catalyst composition consisting of 0.001 wt%-6 wt% of Group 8-10 elements and at least 0.5 wt% of Group 2 elements on a support is used to prepare catalyst particles by spray drying and calcination, avoiding the presence of silicon to prolong catalyst lifetime. The particles are then contacted with a hydrocarbon feed at 300°C to 900°C and at an absolute pressure of at least 20 kPa to carry out dehydrogenation, dehydrogenation aromatization and dehydrogenation cyclization.
Maintaining high propylene yield and selectivity through multiple cycles, the catalyst composition exhibits significant stability and activity under high temperature and pressure, thereby improving propylene yield and dehydrogenation process efficiency.
Smart Images

Figure CN118900722A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of U.S. Provisional Application No. 63 / 322,450, filed on March 22, 2022, and U.S. Provisional Application No. 63 / 322,998, filed on March 22, 2022, the disclosures of which are incorporated herein by reference in their entireties.
[0003] field
[0004] The present disclosure relates to catalyst compositions and methods of making and using the catalyst compositions. Background Art
[0005] Catalytic reforming or dehydrogenation, dehydroaromatization and / or dehydrocyclization of alkanes and / or alkylaromatics are endothermic and equilibrium-limited industrially important chemical conversion processes. 12 Reforming or dehydrogenation, dehydroaromatization and / or dehydrocyclization of alkanes and / or alkyl aromatics such as ethylbenzene can be carried out via a variety of different catalyst compositions such as Pt-based, Ni-based, Pd-based, Ru-based, Re-based, Cr-based, Ga-based, V-based, Zr-based, In-based, W-based, Mo-based, Zn-based and Fe-based systems disposed on a support.
[0006] Among existing propane dehydrogenation processes, one process uses an alumina-supported chromium oxide catalyst which provides one of the highest propylene yields of about 50% (55% propane conversion at 90% propylene selectivity) at temperatures of about 560° C. to 650° C. and low pressures of 20 kPa absolute to 50 kPa absolute. It would be desirable to increase the propylene yield without having to operate at such low pressures to increase the efficiency of the dehydrogenation process.
[0007] Therefore, there is a need for improved catalyst compositions and methods of making and using the same. The present disclosure satisfies this need and others.
[0008] Overview
[0009] The present disclosure provides a catalyst composition and a method for preparing and using the catalyst composition. In some embodiments, the catalyst composition may include 0.001wt%-6wt% of the 8th-10th group element disposed on a carrier, based on the weight of the carrier. The carrier may include Al and at least 0.5wt% of the 2nd group element, based on the weight of the carrier. The catalyst composition may be free of Si or may contain <0.5wt%, <0.45wt%, <0.4wt%, <0.35wt%, <0.3wt%, <0.25wt%, <0.2wt%, <0.15wt%, <0.1wt%, <0.05wt%, or <0.01wt% of Si, based on the weight of the carrier.
[0010] In some embodiments, a method for preparing a catalyst composition may include: (I) preparing a slurry or gel comprising Al or a compound thereof, a Group 2 element or a compound thereof, and a liquid medium; (II) spray drying the slurry or gel to produce spray-dried particles comprising Al or a compound thereof and a Group 2 element or a compound thereof; and (III) calcining the spray-dried particles under an oxidizing atmosphere to produce calcined carrier particles, which may contain Al or a compound thereof and a Group 2 element or a compound thereof. The method may also include at least one of the following (i), (ii), and (iii): (i) the Group 8-10 element may be present in the slurry or gel in the form of a compound containing the Group 8-10 element, and the catalyst composition may include catalyst particles, the catalyst particles comprising calcined carrier particles having the Group 8-10 element disposed thereon, (ii) the Group 8-10 element may be deposited on the spray-dried particles by contacting the spray-dried particles with a compound containing the Group 8-10 element to produce spray-dried particles containing the Group 8-10 element, and the catalyst composition may include catalyst particles, the catalyst particles comprising calcined carrier particles having the Group 8-10 element disposed thereon, (iii) the Group 8-10 element may be deposited on the spray-dried particles by contacting the spray-dried particles with a compound containing the Group 8-10 element to produce spray-dried particles containing the Group 8-10 element, and the catalyst composition may include catalyst particles, the catalyst particles comprising calcined carrier particles having the Group 8-10 element disposed thereon, The method further comprises (IV) calcining the calcined carrier particles containing the 8-10 group element to produce a re-calcined carrier particle having the 8-10 group element disposed thereon, wherein the catalyst composition comprises the re-calcined carrier particle. The catalyst particles may contain Group 8-10 elements and at least 0.5 wt % Group 2 elements in an amount of 0.001 wt % to 6 wt %, and the catalyst composition may be Si-free or may contain <0.5 wt %, <0.45 wt %, <0.4 wt %, <0.35 wt %, <0.3 wt %, <0.25 wt %, <0.2 wt %, <0.15 wt %, <0.1 wt %, <0.05 wt % or <0.01 wt % Si, wherein all weight percentage values are based on the weight of the calcined support particles or the re-calcined support particles.
[0011] In some embodiments, a method for upgrading a hydrocarbon-containing feed may include: (I) contacting the hydrocarbon-containing feed with a catalyst composition that may include a Group 8-10 element disposed on a support to perform one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the hydrocarbon-containing feed to produce a coked catalyst composition and an effluent comprising one or more upgraded hydrocarbons and molecular hydrogen. The hydrocarbon-containing feed may include C2-C 16One or more linear or branched alkanes or C4-C 16 One or more cycloalkanes or C8-C 16 The hydrocarbon feed and the catalyst composition may be contacted at a temperature of 300°C to 900°C for a period of ≤3 hours at a hydrocarbon partial pressure of at least 20 kPa absolute, wherein the hydrocarbon partial pressure is any C2-C 16 Alkanes and any C8-C 16 The total partial pressure of alkyl aromatics. The carrier may contain Al and at least 0.5wt% of Group 2 elements, based on the weight of the carrier. The catalyst composition may contain 0.001wt% to 6wt% of Group 8-10 elements, based on the weight of the carrier. The catalyst composition may be Si-free or may contain <0.5wt%, <0.45wt%, <0.4wt%, <0.35wt%, <0.3wt%, <0.25wt%, <0.2wt%, <0.15wt%, <0.1wt%, <0.05wt% or <0.01wt% Si, based on the weight of the carrier. The one or more upgraded hydrocarbons may include at least one of dehydrogenated hydrocarbons, dehydroaromatized hydrocarbons and dehydrocyclized hydrocarbons.
[0012] BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 The C3H6 yield and selectivity for a catalyst composition (Catalyst 1) including Al in the support and containing no Si that maintains its performance over multiple cycles is shown.
[0014] Figure 2 The C3H6 yield and selectivity for a catalyst composition including Al and Si in the support (Catalyst 2) that deactivates rapidly with increasing cycle number are shown.
[0015] Figure 3 The C3H6 yield and selectivity for a catalyst composition (Catalyst 3) including Si in the support and containing no Al that maintains its performance over multiple cycles is shown.
[0016] Figure 4 A plot of the average C3H6 yield versus cycle number for a catalyst composition comprising Al and no Si in the carrier (Catalyst 4) and a catalyst composition comprising Al and 0.45 wt% Si (Catalyst 5) is shown, wherein Catalyst 5 deactivates with increasing cycle number, while Catalyst 4 does not.
[0017] Detailed Description
[0018] Various specific embodiments, variations and examples of the present invention are now described, including preferred embodiments and definitions adopted herein for understanding the claimed invention. Although the following detailed description gives specific preferred embodiments, it should be appreciated by those skilled in the art that these embodiments are exemplary only, and the present invention may be practiced in other ways. For the purpose of determining infringement, the scope of the present invention refers to any one or more of the appended claims, including their equivalents and elements or limitations equivalent to those listed. Any reference to the "invention" may refer to one or more of the inventions defined by the claims, but not necessarily all.
[0019] In the present disclosure, a method is described as comprising at least one "step". It should be understood that each step is an action or operation that can be performed one or more times in the method in a continuous or discontinuous manner. Unless otherwise specified or the context clearly indicates otherwise, the multiple steps in the method can be performed in the order in which they are listed, with or without overlapping with one or more other steps, or in any other order, if the situation permits. In addition, one or more or even all steps can be performed simultaneously with respect to the same or different batches of materials. For example, in a continuous method, while the first step of the method is performed with respect to the raw materials just fed to the starting stage of the method, the second step can be performed simultaneously with the intermediate material obtained by processing the raw materials fed to the method at an earlier time in the first step. Preferably, the steps are performed in the order described.
[0020] Unless otherwise indicated, all numerical values indicating quantities in this disclosure are to be understood in all cases as being modified by the term "about". It should also be understood that the precise numerical values used in this specification and claims constitute specific embodiments. Efforts have been made to ensure the accuracy of the data in the examples. However, it should be understood that any measured data inherently contain a certain level of error due to the limitations of the techniques and / or equipment used to make the measurements.
[0021] Certain embodiments and features are described herein using a set of numerical upper limits and a set of numerical lower limits. It should be understood that the range including the combination of any two values (e.g., the combination of any lower limit value with any upper limit value, the combination of any two lower limits, and / or the combination of any two upper limits) is contemplated unless otherwise specified.
[0022] As used herein, the indefinite article "a" or "an" means "at least one", unless specified to the contrary or the context clearly indicates otherwise. Thus, embodiments using "a reactor" or "a conversion zone" include embodiments in which one, two or more reactors or conversion zones are used, unless specified to the contrary or the context clearly indicates that only one reactor or conversion zone is used.
[0023] The term "hydrocarbon" means (i) any compound consisting of hydrogen and carbon atoms or (ii) any mixture of two or more such compounds of (i). The term "Cn hydrocarbon" (where n is a positive integer) means (i) any hydrocarbon compound containing a total of n carbon atoms in its molecule or (ii) any mixture of two or more such hydrocarbon compounds of (i). Thus, C2 hydrocarbons can be ethane, ethylene, acetylene, or any mixture of at least two of these compounds in any proportion. "Cm to Cn hydrocarbons" or "Cm-Cn hydrocarbons" (where m and n are positive integers and m < n) means any one of Cm, Cm+1, Cm+2, …, Cn-1, Cn hydrocarbons or any mixture of two or more of them. Thus, "C2 to C3 hydrocarbons" or "C2-C3 hydrocarbons" can be any one of ethane, ethylene, acetylene, propane, propylene, propyne, allene, cyclopropane, and any mixture of two or more of them in any proportion between the components. "Saturated C2-C3 hydrocarbons" can be ethane, propane, cyclopropane, or any mixture of two or more of them in any proportion. "Cn+ hydrocarbons" means (i) any hydrocarbon compound containing a total of at least n carbon atoms in its molecule or (ii) any mixture of two or more such hydrocarbon compounds of (i). "Cn- hydrocarbons" means (i) any hydrocarbon compound containing a total of at most n carbon atoms in its molecule or (ii) any mixture of two or more such hydrocarbon compounds of (i). "Cm hydrocarbon stream" means a hydrocarbon stream consisting essentially of Cm hydrocarbons. "Cm-Cn hydrocarbon stream" means a hydrocarbon stream consisting essentially of Cm-Cn hydrocarbons.
[0024] For the purposes of this disclosure, the naming of elements follows the version of the periodic table provided in Appendix V of Hawley's Condensed Chemical Dictionary, 16th Edition, John Wiley & Sons, Inc., (2016) (in the new notation). For example, Group 2 elements include Mg, Group 8 elements include Fe, Group 9 elements include Co, Group 10 elements include Ni, and Group 13 elements include Al. The term "metalloid" as used herein refers to the following elements: B, Si, Ge, As, Sb, Te, and At. In this disclosure, when a given element is indicated as being present, it can be in elemental form or present as any of its compounds, unless the context otherwise requires or is otherwise clearly stated.
[0025] The term "alkane" refers to saturated hydrocarbons. The term "cycloalkane" refers to saturated hydrocarbons containing a cyclic carbon ring in their molecular structure. Alkanes can be linear, branched, or cyclic.
[0026] The term "aromatic hydrocarbon" is to be understood in accordance with its art-recognized scope, which includes alkyl-substituted and unsubstituted monocyclic and polycyclic compounds.
[0027] The term "rich" when used in phrases such as "enriched in X" or "rich in X" means that, relative to an output stream obtained from a device, such as a conversion zone, the stream comprises a higher concentration of material X than that fed to the same device from which the stream is obtained. The term "lean" when used in phrases such as "depleted in X" or "depleted in X" means that, relative to an output stream obtained from a device, such as a conversion zone, the stream comprises a lower concentration of material X than that fed to the same device from which the stream is obtained.
[0028] The term "mixed metal oxide" refers to a composition comprising oxygen atoms and at least two different metal atoms mixed at the atomic scale. For example, a "mixed Mg / Al metal oxide" has O, Mg, and Al atoms mixed at the atomic scale and has a chemical formula of The compositions obtained are substantially the same or equivalent to those obtained with Mg / Al hydrotalcites of the invention, wherein A is a counter anion of negative charge n, x is in the range of >0 to <1, and m ≥ 0. Materials consisting of nm-sized MgO particles and nm-sized Al2O3 particles mixed together are not mixed metal oxides, since the Mg and Al atoms are not mixed on an atomic scale, but on a nm scale.
[0029] The term "selectivity" refers to the yield (based on moles of carbon) of a specified compound in a catalytic reaction. For example, the phrase "an alkane conversion reaction has a 100% selectivity to olefins" means that 100% of the alkanes converted in the reaction (based on moles of carbon) are converted to olefins. When used in conjunction with a specified reactant, the term "conversion" refers to the amount of the reactant consumed in the reaction. For example, when the specified reactant is propane, 100% conversion means that 100% of the propane is consumed in the reaction. In another example, when the specified reactant is propane, if 1 mole of propane is converted to 1 mole of methane and 1 mole of ethylene, the methane selectivity is 33.3% and the ethylene selectivity is 66.7%. The yield (based on moles of carbon) is the conversion multiplied by the selectivity.
[0030] In the present disclosure, “A, B, ... or a combination thereof” means “A, B, ... or any combination of any two or more of A, B, ...”. “A, B, ... or a mixture thereof” means “A, B, ... or any mixture of any two or more of A, B, ...”.
[0031] Catalyst composition
[0032] The catalyst composition may include 0.001 wt%, 0.002 wt%, 0.003 wt%, 0.004 wt%, 0.005 wt%, 0.006 wt%, 0.007 wt%, 0.008 wt%, 0.009 wt%, 0.01 wt%, 0.015 wt%, 0.02 wt%, 0.025 wt%, 0.03 wt%, 0.035 wt%, 0.04 wt%, 0.045 wt%, 0.05 wt%, 0.055 wt%, 0.065 wt%, 0.075 wt%, 0.080 wt%, 0.081 wt%, 0.082 wt%, 0.083 wt%, 0.084 wt%, 0.085 wt%, 0.086 wt%, 0.090 wt%, 0.091 wt%, 0.092 wt%, 0.093 wt%, 0.094 wt%, 0.095 wt%, 0.096 wt%, 0.097 wt%, 0.098 wt%, 0.099 wt%, %. 0.06wt%, 0.065wt%, 0.07wt%, 0.08wt%, 0.085wt%, 0.09wt%, 0.095wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1wt% to 2wt%, 3wt%, 4wt%, 5wt% or 6wt% of the Group 8-10 element disposed on the support, based on the weight of the support. In some embodiments, the catalyst composition may include ≤5.5 wt%, ≤4.5 wt%, ≤3.5 wt%, ≤2.5 wt%, ≤1.5 wt%, ≤1 wt%, ≤0.9 wt%, ≤0.8 wt%, ≤0.7 wt%, ≤0.6 wt%, ≤0.5 wt%, ≤0.4 wt%, ≤0.3 wt%, ≤0.2 wt%, ≤0.15 wt%, ≤0.1 wt%, ≤0.09 wt%, ≤0.08 wt%, ≤0 .07wt%, ≤0.06wt%, ≤0.05wt%, ≤0.04wt%, ≤0.03wt%, ≤0.02wt%, ≤0.01wt%, ≤0.009wt%, ≤0.008wt%, ≤0.007wt%, ≤0.006wt%, ≤0.005wt%, ≤0.004wt%, ≤0.003wt% or ≤0.002wt% of the Group 8-10 element disposed on the carrier, based on the weight of the carrier.
[0033] In some embodiments, the 8-10 group element may be or may include, but is not limited to, Fe, Co, Ni, Ru, Pd, Os, Ir, Pt, combinations thereof, or mixtures thereof. In at least one embodiment, the 8-10 group element may be or may include Pt. If two or more 8-10 group elements are disposed on the support, the catalyst composition may include a total amount of 0.001 wt%, 0.002 wt%, 0.003 wt%, 0.004 wt%, 0.005 wt%, 0.006 wt%, 0.007 wt%, 0.008 wt%, 0.009 wt%, 0.01 wt%, 0.015 wt%, 0.02 wt%, 0.025 wt%, 0.03 wt%, 0.035 wt%, 0.04 wt%, 0.05 wt%, 0.06 wt%, 0.07 wt%, 0.08 wt%, 0.09 wt%, 0.01 ... %, 0.05wt%, 0.055wt%, 0.06wt%, 0.065wt%, 0.07wt%, 0.08wt%, 0.085wt%, 0.09wt%, 0.095wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1wt% to 2wt%, 3wt%, 4wt%, 5wt% or 6wt% of the two or more Group 8-10 elements, based on the weight of the support. In some embodiments, the active component of the catalyst composition capable of reforming or one or more of dehydrogenation, dehydroaromatization and dehydrocyclization of a hydrocarbon-containing feed can be or can include one or more Group 8-10 elements disposed on a support.
[0034] The carrier may be or may include but is not limited to one or more Group 2 elements and aluminum (Al). The Group 2 element may be or may include Be, Mg, Ca, Sr, Ba or a combination thereof or a mixture thereof. In some embodiments, the Group 2 element and / or Al may exist in its elemental form. In other embodiments, the Group 2 element and / or Al may exist in the form of a compound. For example, the Group 2 element and / or Al may exist as an oxide, phosphate, halide, halogenate, sulfate, sulfide, borate, nitride, carbide, aluminate, carbonate, metaphosphate, selenide, tungstate, molybdate, chromite, chromate or dichromate. In some embodiments, a mixture of any two or more compounds comprising the Group 2 element and / or Al may exist in different forms.
[0035] It has been surprisingly and unexpectedly found that when the carrier includes Group 2 elements and Al, the presence of silicon (Si) is harmful to the life of the catalyst composition. More specifically, when the catalyst composition includes Group 2 elements, Al and Si based on the weight of the carrier ≥0.5wt%, the catalyst composition will deactivate rapidly with the increase of the number of cycles. Each cycle at least includes contacting the hydrocarbon-containing feed with the catalyst composition to produce a coked catalyst composition and an effluent that can include one or more upgraded hydrocarbons and molecular hydrogen and contacting the catalyst composition with an oxidant to carry out the combustion of at least a portion of the coke to produce a regenerated catalyst and combustion gases that are lean in coke. Contacting the additional amount of hydrocarbon-containing feed with the regenerated catalyst will start a second cycle. In some embodiments, the catalyst composition may not contain any Si. In other embodiments, the catalyst composition may include <0.5 wt%, <0.45 wt%, <0.4 wt%, <0.35 wt%, <0.3 wt%, <0.25 wt%, <0.2 wt%, <0.15 wt%, <0.1 wt%, <0.09 wt%, <0.08 wt%, <0.07 wt%, <0.06 wt%, <0.05 wt%, <0.04 wt%, <0.03 wt%, 0.02 wt%, <0.01 wt%, <0.007 wt%, <0.005 wt%, <0.003 wt%, <0.001 wt%, <0.0007 wt%, <0.0005 wt%, <0.0003 wt%, or <0.0001 wt% Si based on the weight of the support.
[0036] In some embodiments, the Group 2 element and Al may be in the form of a mixed Group 2 element / Al metal oxide having O, Mg, and Al atoms mixed at the atomic scale. In some embodiments, the support may be or may include the Group 2 element and Al in the form of an oxide or one or more Group 2 element oxides and Al2O3 that may be mixed at the nanoscale. In some embodiments, the support may be or may include oxides of the Group 2 element such as MgO and Al2O3 mixed at the nanoscale.
[0037] In some embodiments, the support may be or may include a first amount of a Group 2 element and Al in the form of a mixed Group 2 element / Al metal oxide and a second amount of a Group 2 element in the form of an oxide of the Group 2 element. In such embodiments, the mixed Group 2 element / Al metal oxide and the Group 2 element oxide may be mixed at the nanoscale, and the Group 2 element and Al in the mixed Group 2 element / Al metal oxide may be mixed at the atomic scale.
[0038] In other embodiments, the support may be or may include a first amount of a Group 2 element and a first amount of Al in the form of a mixed Group 2 element / Al metal oxide, a second amount of a Group 2 element in the form of a Group 2 element oxide, and a second amount of Al in the form of Al2O3. In such embodiments, the mixed Group 2 element / Al metal oxide, the Group 2 element oxide, and Al2O3 may be mixed at the nanoscale, and the Group 2 element and Al in the mixed Group 2 element / Al metal oxide may be mixed at the atomic scale.
[0039] In some embodiments, the carrier may be or may include, but is not limited to, one or more of the following compounds: Mg w Al2O 3+w , where w is a positive number; Ca x Al2O 3+x , where x is a positive number; Sr y Al2O 3+y , where y is a positive number; Ba z Al2O 3+z , where z is a positive number, BeO, MgO, CaO, BaO, SrO, BeCO3, MgCO3, CaCO3, SrCO3, BaCO3, CaZrO3, Ca7ZrAl6O 18 , CaTiO3, Ca7Al6O 18 ,Ca7HfAl6O 18 , BaCeO3, one or more magnesium chromates, one or more magnesium tungstates, one or more magnesium molybdates, combinations thereof, and / or mixtures thereof.
[0040] In some embodiments, if present as a support or as a component of a support, Mg wherein w is a positive number w Al2O 3+w The molar ratio of Mg to Al may be in the range of 0.5, 1, 2, 3, 4, or 5 to 6, 7, 8, 9, or 10. In some embodiments, the Mg w Al2O 3+w It may include MgAl2O4, Mg2Al2O5 or mixtures thereof. If present as a support or as a component of a support, Ca wherein x is a positive number x Al2O 3+x The molar ratio of Ca to Al may be in the range of 1:12, 1:4, 1:2, 2:3, 5:6, 1:1, 12:14 or 1.5:1. x Al2O 3+xIt may include tricalcium aluminate, dodecaluminate heptaaluminate, monocalcium aluminate, monocalcium dialuminate, monocalcium hexaaluminate, dicalcium aluminate, pentacalcium trialuminate, tetracalcium trialuminate or any mixture thereof. If present as a carrier or as a component of a carrier, Sr wherein y is a positive number y Al2O 3+y The molar ratio of Sr to Al may be in the range of 0.05, 0.3 or 0.6 to 0.9, 1.5 or 3. If present as a support or as a component of a support, Ba wherein z is a positive number z Al2O 3+z The molar ratio of Ba to Al may be in the range of 0.05, 0.3 or 0.6 to 0.9, 1.5 or 3.
[0041] In some embodiments, the weight ratio of Group 2 elements to Al in the support can range from 0.001, 0.005, 0.01, 0.05, 0.1, 0.15, 0.2, 0.3, 0.5, 0.7, or 1 to 3, 6, 12.5, 25, 50, 75, 100, 200, 300, 400, 500, 600, 700, 800, 900, or 1,000. In some embodiments, the carrier may include ≥0.5wt%, ≥1wt%, ≥2wt%, ≥2.1wt%, ≥2.5wt%, ≥3wt%, ≥3.5wt%, ≥4wt%, ≥4.5wt%, ≥5wt%, ≥5.5wt%, ≥6wt%, ≥6.5wt%, ≥7wt%, ≥8wt%, ≥9wt%, ≥10wt%, ≥11wt%, ≥12wt%, ≥13wt%, ≥14wt%, ≥15wt%, ≥16wt%, ≥17wt%, ≥18wt%. %, ≥ 19 wt %, ≥ 20 wt %, ≥ 21 wt %, ≥ 22 wt %, ≥ 23 wt %, ≥ 24 wt %, ≥ 25 wt %, ≥ 26 wt %, ≥ 27 wt %, ≥ 28 wt %, ≥ 29 wt %, ≥ 30 wt %, ≥ 35 wt %, ≥ 40 wt %, ≥ 45 wt %, ≥ 50 wt %, ≥ 55 wt %, ≥ 60 wt %, ≥ 65 wt %, ≥ 70 wt %, ≥ 75 wt %, ≥ 80 wt %, ≥ 85 wt % or ≥ 90 wt % of the Group 2 element, based on the weight of the carrier. In some embodiments, the carrier can include a Group 2 element in an amount ranging from 0.5, 1, 1.5, 2, 2.1, 2.3, 2.5, 2.7, 3, 4, 5, 6, 7, 8, 9, 10, 11, 13, 15, 17, 19, 21, 23, or 25 wt% to 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 92.34 wt% based on the weight of the carrier. In some embodiments, the support may include Al in a range from 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.1 wt%, 2.3 wt%, 2.5 wt%, 2.7 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt% or 11 wt% to 15 wt%, 20 wt%, 25 wt%, 30 wt%, 40 wt%, 45 wt% or 50 wt% based on the weight of the support.
[0042] In some embodiments, the molar ratio of the Group 2 element to the one or more Group 8-10 elements, such as Pt, disposed on the support may be from 0.24, 0.5, 1, 10, 50, 100, 300, 450, 600, 800, 1,000, 1,200, 1,500, 1,700, or 2,000 to 3,000, 3,500, 4,000, 4,500, 5,000, 5,500, 6,000, 6,500, 7,000, 7,500, 8,000, 8,500, 9,000, 9,500, 10,000, 11,000, 12,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 31,000, 32,000, 33,000, 34,000, 35,000, 0,000, 15,000, 20,000, 25,000, 30,000, 35,000, 40,000, 45,000, 50,000, 55,000, 60,000, 65,000, 70,000, 75,000, 80,000, 85,000, 90,000, 95,000, 100,000, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000 or 900,000.
[0043] In some embodiments, the catalyst composition may optionally include a promoter disposed on a carrier, based on the weight of the carrier, of up to 10 wt%. In some embodiments, the catalyst composition may include 0.01 wt%, 0.1 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, or 1 wt% to 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt% of a promoter disposed on a carrier, based on the weight of the carrier. The promoter may be or may include, but is not limited to, Sn, Cu, Au, Ag, Ga, Zn, Ge, In, Re, Ag, combinations thereof, or mixtures thereof. In some embodiments, the promoter may be associated with an element of Groups 8-10. For example, the promoter and the Group 8-10 element such as Pt disposed on the support can form a Group 8-10 element-promoter cluster, which can be dispersed on the support. The promoter can improve the selectivity / activity / life of the catalyst composition for a given upgraded hydrocarbon. In some embodiments, when the hydrocarbon-containing feed includes propane, the promoter can improve the propylene selectivity of the catalyst composition.
[0044] In some embodiments, the catalyst composition may optionally include one or more alkali metal elements disposed on a carrier in an amount of up to 5wt%, based on the weight of the carrier. In some embodiments, the catalyst composition may include 0.01wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1wt% to 2wt%, 3wt%, 4wt% or 5wt% of alkali metal elements disposed on a carrier, based on the weight of the carrier. If present, the alkali metal element may be or may include but is not limited to Li, Na, K, Rb, Cs or a combination thereof or a mixture thereof. In at least some embodiments, the alkali metal element may be or may include K and / or Cs. In some embodiments, if present, the alkali metal element may improve the selectivity of the catalyst composition for a given upgraded hydrocarbon.
[0045] In some embodiments, the carrier may further include, but is not limited to, at least one metal element and / or at least one metalloid element and / or at least one compound thereof selected from a group other than Groups 2 and 8-10, wherein the at least one metal element and / or at least one metalloid element is not one of the alkali metal elements or one of the promoter elements. If the carrier further includes a compound comprising the metal element and / or metalloid element selected from a group other than Groups 2 and 8-10, wherein the at least one metal element and / or at least one metalloid element is not one of the alkali metal elements or one of the promoter elements, the compound may be present on the carrier as an oxide, phosphate, halide, halogenate, sulfate, sulfide, borate, nitride, carbide, aluminate, carbonate, metaphosphate, selenide, tungstate, molybdate, chromite, chromate or dichromate. In some embodiments, the at least one metal element and / or at least one metalloid element and / or at least one compound thereof selected from a group other than Groups 2 and 8-10 (wherein the at least one metal element and / or at least one metalloid element is not one of the alkali metal elements or one of the promoter elements) may be or may include but is not limited to one or more rare earth elements, i.e., elements with atomic numbers of 21, 39 or 57-71.
[0046] If the carrier includes at least one metal element and / or at least one metalloid element and / or at least one compound thereof selected from a group other than Groups 2 and 8-10 (wherein the at least one metal element and / or at least one metalloid element is not one of the alkali metal elements or one of the promoter elements), the at least one metal element and / or at least one metalloid element may function as a binder in some embodiments and may be referred to as a "binder". Regardless of the at least one metal element and / or at least one metalloid element and / or at least one compound thereof selected from a group other than Groups 2 and 8-10 (wherein the at least one metal element and / or at least one metalloid element is not one of the alkali metal elements or one of the promoter elements), for clarity and ease of description, the at least one metal element and / or at least one metalloid element selected from a group other than Groups 2 and 8-10 will be further described herein as a "binder". In some embodiments, the carrier can include 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.5 wt%, 1 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt% or 40 wt% to 50 wt%, 60 wt%, 70 wt%, 80 wt% or 90 wt% of the binder, based on the weight of the carrier.
[0047] In some embodiments, suitable compounds that can be used as binders can be or can include, but are not limited to, one or more of the following: B2O3, AlBO3, Al2O3, ZrO2, TiO2, zinc aluminate, ZnO, VO, V2O3, VO2, V2O5, Ga s O t 、In u O v , Mn2O3, Mn3O4, MnO, one or more molybdenum oxides, one or more tungsten oxides, one or more zeolites, and mixtures and combinations thereof, wherein s, t, u and v are positive numbers. If the Group 2 element is in the form of a mixed metal oxide such as a mixed Mg / Al metal oxide, the one or more additional metals in the mixed metal oxide are not considered to be part of the binder. For example, the support may include a mixed Mg / Al metal oxide, such as those obtained by calcining Mg / Al hydrotalcite, and such Al would not be considered to be part of the binder, but the support may also include Al2O3 mixed with the mixed Mg / Al metal oxide on a nanoscale, and the Al2O3 would be considered to be a binder.
[0048] In some embodiments, the catalyst composition may be in the form of catalyst particles or a monolithic structure. In some embodiments, if the catalyst composition is in the form of catalyst particles, the catalyst particles may have a median particle size in the range of 1 μm, 5 μm, 10 μm, 20 μm, 40 μm, or 60 μm to 80 μm, 100 μm, 115 μm, 130 μm, 150 μm, 200 μm, 300 μm, 400 μm, or 500 μm. In some embodiments, the catalyst particles may have a particle size of 0.3 g / cm 3 , 0.4g / cm 3 , 0.5g / cm 3 , 0.6g / cm 3 , 0.7g / cm 3 , 0.8g / cm 3 , 0.9g / cm 3 or 1g / cm 3 Up to 1.1g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 , 1.8g / cm 3 , 1.9g / cm 3 or 2g / cm 3 The apparent loose bulk density in the range of , measured according to a modified ASTM D7481-18 with a 10, 25 or 50 mL measuring cylinder instead of a 100 or 250 mL measuring cylinder. In some embodiments, the catalyst particles may have a one-hour attrition loss of ≤5 wt%, ≤4 wt%, ≤3 wt%, ≤2 wt%, ≤1 wt%, ≤0.7 wt%, ≤0.5 wt%, ≤0.4 wt%, ≤0.3 wt%, ≤0.2 wt%, ≤0.1 wt%, ≤0.07 wt% or ≤0.05 wt%, measured according to ASTM D5757-11 (2017). The morphology of the particles may be substantially spherical, making them suitable for operation in a fluidized bed reactor. In some embodiments, the catalyst particles may have a size and density that conforms to the Geldart A or Geldart B definition of a fluidizable solid.
[0049] In some embodiments, the catalyst particles may have a diameter of 0.1 μm. 2 / g, 1m 2 / g, 10m 2 / g or 100m 2 / g to 500m 2 / g、800m2 / g、1,000m 2 / g or 1,500m 2 The surface area of the catalyst particles can be measured according to the Brunauer-Emmett-Teller (BET) method using a Micromeritics 3Flex instrument at 350°C after degassing the powder for 4 hours using nitrogen adsorption-desorption (temperature of liquid nitrogen, 77K). For more information about the method, see, for example, "Characterization of Porous Solids and Powders: Surface Area, Pore Size and Density", S. Lowell et al., Springer, 2004.
[0050] First method for preparing catalyst particles
[0051] The method for preparing the catalyst composition may include preparing a slurry or gel, which may include grinding, mixing, blending, merging or otherwise contacting the following materials: Al and / or its compounds, Group 2 elements and / or its compounds and a liquid medium. In some embodiments, the preparation of the slurry or gel may also include, but is not limited to, contacting Al or its compounds, Group 2 elements or its compounds and a liquid medium and one or more additives. In other embodiments, the preparation of the slurry or gel may include, but is not limited to, contacting Al or its compounds, Group 2 elements or its compounds, a liquid medium, a binder or a binder precursor and optionally one or more additives.
[0052] In some embodiments, the compound containing Al may be or may include, but is not limited to, Al2O3, Al(OH)2, hydrated aluminum chloride (ACH), layered double hydroxides including Al and Mg, or mixtures thereof. In some embodiments, the compound containing Group 2 elements may be in the form of oxides, hydroxides, hydrated carbonates, salts, clays containing Group 2 elements, layered double hydroxides, phosphates, halides, halides, sulfates, sulfides, borates, nitrides, carbides, aluminates, carbonates, metaphosphates, selenides, tungstates, molybdates, chromites, chromates, dichromates, or mixtures thereof. In some embodiments, the Group 2 element may be or may include Mg, and the compound containing Group 2 elements may be in the form of magnesium oxide, magnesium hydroxide, hydromagnesite (hydrated magnesium carbonate mineral, Mg5(CO3)4(OH)2·4H2O)), magnesium salts, magnesium-containing clays, hydrotalcites (also including layered double hydroxides of Al), organic magnesium compounds, or mixtures thereof. In some embodiments, the Group 2 element and Al may be present as a mixed Group 2 element / Al metal oxide. In some embodiments, the Group 2 element and Al may be present as a mixed Group 2 element / Al layered double hydroxide such as hydrotalcite.
[0053] The liquid medium may be or may include, but is not limited to, water, alcohol, acetone, chloroform, methylene chloride, dimethylformamide, dimethyl sulfoxide, glycerol, ethyl acetate, or any mixture thereof. Illustrative alcohol may be or may include, but is not limited to, methanol, ethanol, isopropanol, or any mixture thereof. If present, the binder may be or may include the above-mentioned binder. If present, the binder precursor may be or may include, but is not limited to, aluminum chlorohydrate, boehmite, pseudoboehmite, gibbsite, bayerite, aluminum nitrate, aluminum chloride, sodium aluminate, alumina sol, or any mixture thereof. Some compounds known in the literature herein as "binders" may also be referred to as fillers, matrix, additives, etc. If present, one or more additives may be or may include, but are not limited to: one or more acids, such as formic acid, lactic acid, citric acid, acetic acid, HNO3, HCl, oxalic acid, stearic acid, carbonic acid, etc.; one or more bases, such as ammonia solution, NaOH, KOH, etc.; inorganic salts, such as nitrates, carbonates, bicarbonates, chlorides, etc.; organic salts, such as acetates, oxalates, formates, citrates, etc.; polymers, such as polyvinyl alcohol, polysaccharides, etc., or any mixture thereof. The additives may help improve the chemical / physical properties of the spray-dried material and / or improve the rheological properties of the slurry / gel to aid spray drying.
[0054] The slurry or gel can be spray dried to produce spray-dried particles containing Group 2 elements and Al. Spray drying refers to a method for producing a dry particulate solid product from a slurry or gel. The method may include spraying or atomizing (e.g., forming small droplets) the slurry or gel into a temperature-controlled gas stream to evaporate the liquid medium from the atomized droplets and produce a particulate solid product. For example, in a spray drying process, the slurry or gel can be atomized into small droplets and mixed with hot air or a hot inert gas such as nitrogen to evaporate the liquid from the droplets. The temperature of the slurry or gel during the spray drying process can generally be close to or higher than the boiling temperature of the liquid. An outlet air temperature of about 60°C to about 120°C can be common.
[0055] The slurry or gel can be atomized with one or more pressure nozzles (e.g., fluid nozzle atomizers), one or more pulse atomizers, one or more high-speed rotating disks (e.g., centrifugal or rotary atomizers), or any other known method. The median particle size, liquid (e.g., water) concentration, apparent loose bulk density, or any combination thereof of the granular solid product prepared by spray drying can be controlled, regulated, or otherwise affected by one or more operating conditions and / or parameters of the spray dryer. Illustrative operating conditions can include, but are not limited to, the feed rate and temperature of the gas stream, the atomizer speed, the feed rate of the slurry or gel via the atomizer, the temperature of the slurry or gel, the size of the droplets, and / or the solid concentration, the spray dryer size, or any combination thereof. It is well known in the art that various operating conditions will vary according to the specific spray drying equipment used, and can be easily determined by those of ordinary skill in the art.
[0056] The spray-dried particles may optionally be calcined in an oxidizing atmosphere such as an air atmosphere to produce calcined support particles comprising Group 2 elements and Al. In some embodiments, the spray-dried particles may be calcined at a temperature ranging from 450°C, 500°C, 525°C, 550°C, 575°C, 600°C, 625°C, 650°C, or 675°C to 700°C, 725°C, 750°C, 775°C, 800°C, 850°C, 900°C, or 950°C. In some embodiments, the spray-dried particles may be calcined at a temperature of ≤950°C, ≤900°C, ≤850°C, ≤800°C, ≤750°C, ≤700°C, ≤650°C, ≤600°C, or ≤550°C, ≤525°C, ≤500°C, ≤475°C, or ≤460°C. In some embodiments, the spray-dried particles can be calcined for a time of ≤240 minutes, ≤180 minutes, ≤120 minutes, ≤90 minutes, ≤60 minutes, ≤45 minutes, ≤30 minutes, ≤25 minutes, ≤20 minutes or ≤15 minutes. In some embodiments, the spray-dried particles can be calcined in the presence of oxygen, such as in an air atmosphere. In some embodiments, the spray-dried particles can be calcined at a temperature of 550°C to 900°C or 550°C to 850°C for a time of ≤240 minutes, ≤180 minutes, ≤120 minutes, ≤90 minutes, ≤60 minutes, ≤45 minutes, ≤30 minutes, ≤25 minutes, ≤20 minutes or ≤15 minutes. In other embodiments, the spray-dried particles are calcined at a temperature of ≤550°C, ≤540°C, ≤530°C, ≤520°C, ≤510°C or ≤500°C for a time of ≤240 minutes, ≤180 minutes, ≤120 minutes, ≤90 minutes, ≤60 minutes, ≤45 minutes, ≤30 minutes, ≤25 minutes, ≤20 minutes or ≤15 minutes.
[0057] The Group 8-10 elements present in the catalyst particles may be introduced via one or more means. In some embodiments, the method of preparing the catalyst composition may include (i) contacting Al and / or its compounds, Group 2 elements and / or its compounds and a liquid medium with Group 8-10 elements and / or its compounds, so that Group 8-10 elements may be present in the slurry or the gel, and the catalyst composition may include catalyst particles comprising calcined carrier particles having Group 8-10 elements disposed thereon. In other embodiments, the method of preparing the catalyst composition may include (ii) depositing Group 8-10 elements and / or its compounds on spray-dried particles by contacting the spray-dried particles with Group 8-10 elements and / or its compounds to produce spray-dried particles containing Group 8-10 elements, and the catalyst composition may include catalyst particles comprising calcined carrier particles having Group 8-10 elements disposed thereon. In other embodiments, the method of preparing a catalyst composition may include (iii) if the spray-dried particles are optionally calcined, depositing a Group 8-10 element or compound thereof on the calcined support particles by contacting the calcined support particles with a Group 8-10 element and / or compound thereof to produce a calcined support particle containing a Group 8-10 element, and the method may optionally further include calcining the calcined support particles containing a Group 8-10 element to produce a re-calcined support particle having a Group 8-10 element disposed thereon, wherein the catalyst composition may include the re-calcined support particle. In some embodiments, the catalyst composition may include calcined support particles containing a Group 8-10 element without the optional additional calcination step. In other embodiments, the method of preparing a catalyst composition may include options (i), (ii), (iii), (i) and (ii), (i) and (iii), (ii) and (iii), or (i), (ii) and (iii). In some embodiments, when the element of Group 8-10 is in the form of a compound, suitable compounds including the element of Group 8-10 may be or may include, but are not limited to, chloroplatinic acid hexahydrate, tetraammineplatinum (II) nitrate, platinum (II) acetylacetonate, platinum (II) bromide, platinum (II) iodide, platinum (II) chloride, platinum (IV) chloride, diammineplatinum (II) dichloride, ammonium tetrachloroplatinate (II), tetraammineplatinum (II) chloride hydrate, tetraammineplatinum (II) hydroxide hydrate, nickel (II) chloride, palladium (II) acetate, palladium (II) nitrate, iron (II) chloride, iron (III) chloride, ruthenium (III) chloride hydrate, rhodium (III) nitrate, or any mixture thereof.
[0058] Optional promoters that may be present in the catalyst particles may be introduced via one or more means. In some embodiments, the method for preparing the catalyst composition may include (iv) contacting at least Al and / or a compound thereof, a Group 2 element and / or a compound thereof, and a liquid medium with a compound comprising a promoter element such that the promoter element is present in the slurry or the gel, and the catalyst composition may include catalyst particles comprising spray-dried and / or calcined carrier particles having the promoter element disposed thereon. In other embodiments, the method for preparing the catalyst composition may include (v) depositing a compound comprising a promoter element on the spray-dried particles to produce spray-dried particles containing the promoter, and the catalyst composition may include catalyst particles comprising spray-dried particles containing the promoter and / or calcined carrier particles having the promoter element disposed thereon. In other embodiments, the method of preparing the catalyst composition may include (vi) if the spray-dried particles are optionally calcined, depositing a compound including a promoter element on the calcined support particles to produce promoter-containing calcined support particles, and the method may further optionally include calcining the promoter-containing calcined support particles to produce re-calcined support particles having the promoter element disposed thereon, wherein the catalyst composition includes the re-calcined support particles. In some embodiments, the catalyst composition may include the promoter-containing, calcined support particles without the optional additional calcination step. In other embodiments, the method of preparing the catalyst composition may include options (iv), (v), (vi), (iv) and (v), (iv) and (vi), (v) and (vi), or (iv), (v) and (vi). In other embodiments, the method may include any one or more of options (i), (ii) and (iii) and any one or more of options (iv), (v) and (iv). The compound including the promoter element can be or can include, but is not limited to, tin (II) oxide, tin (IV) oxide, tin (IV) chloride pentahydrate, tin (II) chloride dihydrate, tin (II) bromide, ammonium hexachlorotin (IV) acid, tin (IV) bromide, tin (II) acetylacetonate, tin (II) acetate, tin (IV) acetate, tin (II) oxalate, silver (I) nitrate, gold (III) nitrate, copper (II) nitrate, gallium (III) nitrate, zinc (II) nitrate, germanium (IV) chloride, indium (III) nitrate, rhenium (VII) oxide, or any mixture thereof.
[0059] If present in the catalyst particles, the alkali metal element may be introduced via one or more means. In some embodiments, the method for preparing the catalyst composition may include (vii) contacting Al and / or its compounds, Group 2 elements and / or their compounds and a liquid medium with a compound comprising an alkali metal element, such that the alkali metal element is present in the slurry or gel, and the catalyst composition may include catalyst particles comprising spray-dried and / or calcined carrier particles having an alkali metal element disposed thereon. In other embodiments, the method for preparing the catalyst composition may include (viii) depositing a compound comprising an alkali metal element on the spray-dried particles to produce spray-dried particles containing an alkali metal element, and the catalyst composition may include catalyst particles comprising spray-dried particles and / or calcined carrier particles having an alkali metal element disposed thereon. In other embodiments, the method of preparing the catalyst composition may include (ix) if the spray-dried particles are optionally calcined, depositing a compound including an alkali metal element on the calcined support particles to produce alkali metal element-containing, calcined support particles, and the method may further optionally include calcining the alkali metal element-containing, calcined support particles to produce re-calcined support particles having an alkali metal element disposed thereon, wherein the catalyst composition includes the re-calcined support particles. In other embodiments, the method of preparing the catalyst composition may include options (vii), (viii), (ix), (vii) and (viii), (vi) and (ix), (viii) and (ix), or (vii), (viii) and (iv). In other embodiments, the method may include any one or more of options (i), (ii) and (iii), any one or more of options (iv), (v) and (iv), and any one or more of options (vii), (viii) and (ix). The compound including the alkali metal element may be or may include, but is not limited to, lithium nitrate, sodium nitrate, potassium nitrate, rubidium nitrate, cesium nitrate, or any mixture thereof.
[0060] In some embodiments, the method for preparing the catalyst composition may optionally include hydrating the calcined support particles to produce hydrated support particles. For example, the calcined support particles may be contacted with water to produce hydrated support particles. In such an embodiment, the method may also include calcining the hydrated support particles to produce a catalyst composition comprising re-calcined support particles. Hydration of the calcined support may be carried out at a temperature ranging from 20°C, 40°C or 60°C to 80°C, 120°C, 140°C, 160°C, 180°C or 200°C. The calcined support may be contacted with water for a time ranging from 1 minute, 5 minutes or 10 minutes to 20 minutes, 40 minutes, 80 minutes, 160 minutes, 6 hours, 12 hours, 24 hours or 48 hours. In some embodiments, anions such as chloride, nitrate, carbonate, bicarbonate, acetate, oxalate, formate and / or citrate may be present during hydration.
[0061] In some embodiments, the method for preparing the catalyst composition may optionally include hydrating the spray-dried particles to produce hydrated spray-dried particles. For example, the spray-dried particles may be contacted with water to produce hydrated spray-dried particles. In such an embodiment, the method may also include calcining the hydrated spray-dried particles to produce a catalyst composition comprising calcined carrier particles. Hydration of the spray-dried particles may be carried out at a temperature ranging from 20°C, 40°C or 60°C to 80°C, 120°C, 140°C, 160°C, 180°C or 200°C. The spray-dried particles may be contacted with water for a time ranging from 1 minute, 5 minutes or 10 minutes to 20 minutes, 40 minutes, 80 minutes, 160 minutes, 6 hours, 12 hours, 24 hours or 48 hours. In some embodiments, anions such as chloride, nitrate, carbonate, bicarbonate, acetate, oxalate, formate and / or citrate may be present during hydration.
[0062] In some embodiments, the method of preparing the catalyst composition may optionally include hydrating the spray-dried particles to produce hydrated spray-dried particles, calcining the hydrated spray-dried particles to produce calcined support particles, hydrating the calcined support particles to produce hydrated calcined support particles, and calcining the hydrated calcined support particles to produce re-calcined support particles. Thus, the catalyst composition may include spray-dried particles, calcined support particles, hydrated spray-dried particles, hydrated spray-dried particles that can be calcined, hydrated calcined support particles, hydrated calcined support particles that can be re-calcined, or any mixture thereof.
[0063] In some embodiments, the catalyst particles produced by hydrating the calcined support particles or spray-dried particles and then calcining the hydrated calcined support particles or hydrated spray-dried particles can produce catalyst particles having an attrition loss after one hour that is less than the attrition loss after one hour of the initial calcined particles or spray-dried particles produced before the hydration step, as measured according to ASTM D5757-11 (2017). In some embodiments, the catalyst particles produced by hydrating the calcined support particles or spray-dried particles and then calcining the hydrated support particles or hydrated support particles can produce catalyst particles having an attrition loss after one hour that is less than 10%, less than 30%, less than 50%, less than 70%, less than 90%, or less than 100% of the attrition loss after one hour of the initial calcined particles produced before the hydration step, as measured according to ASTM D5757-11 (2017).
[0064] Second method for preparing catalyst particles
[0065] In some embodiments, the catalyst composition may be or may include catalyst particles produced only by a spray drying step, such that a slurry is prepared and spray-dried particles are produced therefrom, wherein Group 8-10 elements and optional promoters and / or alkali metal elements are added to the slurry, the spray-dried particles, or a combination thereof. Thus, in some embodiments, a method for preparing a catalyst composition may include: preparing the slurry or gel, which may include Al and / or compounds thereof, Group 2 elements and / or compounds thereof, a liquid medium, and optionally one or more additives as described above; and spray drying the slurry or gel to produce spray-dried support particles comprising at least Al and Group 2 elements. At least one of the following (i) and (ii) may be satisfied: (i) the Group 8-10 element may be present in the slurry or gel in the form of a compound containing the Group 8-10 element, and the catalyst composition may include catalyst particles, the catalyst particles including spray-dried carrier particles having the Group 8-10 element disposed thereon, and (ii) the Group 8-10 element may be deposited on the spray-dried carrier particles by contacting the spray-dried carrier particles with a compound containing the Group 8-10 element to produce spray-dried carrier particles containing the Group 8-10 element, and the catalyst composition may include catalyst particles, the catalyst particles including spray-dried carrier particles having the Group 8-10 element disposed thereon. In some embodiments, at least one of the following (iii) and (iv) may also be satisfied: (iii) a compound comprising a promoter element may be present in the slurry or gel, and the catalyst composition may comprise catalyst particles comprising spray-dried carrier particles having a promoter element disposed thereon, and (iv) a compound that may comprise a promoter element may be deposited on the spray-dried carrier particles to produce promoter-containing, spray-dried carrier particles, and the catalyst composition may comprise catalyst particles comprising spray-dried carrier particles having a promoter element disposed thereon. In some embodiments, the optional one or more alkali metal elements and / or binders may also be added during the synthesis of the catalyst particles as described above.
[0066] In some embodiments, the catalyst particles may be further processed or activated in situ by adding them to a hydrocarbon upgrading process that subjects the catalyst particles to conditions of higher severity to produce catalyst particles having a higher activation level than when the spray-dried particles were first prepared. In some embodiments, when the catalyst particles include catalyst particles that have only been subjected to a spray drying step (a slurry is prepared and spray-dried support particles are produced therefrom, wherein Pt and promoters are added to the slurry, the spray-dried support particles, or a combination thereof), the catalyst particles may be introduced into a reaction zone, a combustion zone, a reduction zone, or any other location within a fluidized hydrocarbon upgrading process, some of which are further described below.
[0067] The preparation of the catalyst composition and the method of adding the Group 8-10 element, one or more promoters such as Sn, optionally one or more alkali metal elements and optionally one or more binders to the catalyst composition have been described above. In some embodiments, the preparation of the slurry or gel, spray drying the slurry, calcining the spray-dried particles and / or hydrated calcined particles, and / or hydration of the calcined support particles or spray-dried particles containing Al and Group 2 elements can also be carried out using one of the known methods reported in the literature, such as U.S. Patent Nos. 4,866,019; 6,028,023; 6,589,902; 6,593,265; 6,800,578; 7,361,264; and 7,417,005; U.S. Patent Application Publication Nos. 2004 / 0029729; 2005 / 000396; and 2016 / 0082424; WO Publication No. WO2008083563A1; and journal publication Wang et al., Ind. Eng. Chem. Res. 2008, 47, 5746–5750; Chubar et al., Ind. Eng. Chem. Res. 2008, 47, 5746–5750; al., Chem. Eng. J. 2013, 234, 284-299; Valente et al., Energy Environ. Sci., 2011, 4, 4096-4107; and Julklang et al., Mater. Lett. 2017, 209, 429-432.
[0068] Without wishing to be bound by theory, it is believed that the support produced via any of the above methods and / or other methods may include (i) Mg and Al mixed together on a nanoscale, (ii) Mg and Al in the form of a mixed Mg / Al metal oxide, or (iii) a combination of (i) and (ii) above.
[0069] The first method of upgrading hydrocarbons
[0070] The first method of upgrading hydrocarbons can include contacting a hydrocarbon-containing feed (first hydrocarbon-containing feed) with a catalyst composition comprising a Group 8-10 element disposed on a carrier to perform one or more of dehydrogenation, dehydrogenation aromatization and dehydrogenation cyclization of at least a portion of the first hydrocarbon-containing feed to produce a coked catalyst composition and an effluent that can contain one or more upgraded hydrocarbons and molecular hydrogen. The catalyst composition and the first hydrocarbon-containing feed can be contacted with each other in any suitable environment, such as one or more reaction or conversion zones disposed in one or more reactors to produce an effluent and a coked catalyst composition. The reaction or conversion zone can be disposed or located in one or more fixed bed reactors, one or more fluidized or moving bed reactors, one or more flow conversion reactors or any combination thereof. The catalyst composition can include 0.001wt% to 6wt% of the Group 8-10 element disposed on a carrier, the carrier including Al and at least 0.5wt% of the Group 2 element and free of Si or containing <0.5wt% of Si, wherein all weight percentage values are based on the weight of the carrier.
[0071] The first hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature in the range of 300° C., 350° C., 400° C., 450° C., 500° C., 550° C., 600° C., 620° C., 650° C., 660° C., 670° C., 680° C., 690° C., or 700° C. to 725° C., 750° C., 760° C., 780° C., 800° C., 825° C., 850° C., 875° C., or 900° C. In some embodiments, the first hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature of at least 620° C., at least 650° C., at least 660° C., at least 670° C., at least 680° C., at least 690° C., or at least 700° C. to 725° C., 750° C., 760° C., 780° C., 800° C., 825° C., 850° C., 875° C., or 900° C. The first hydrocarbon-containing feed can be introduced into the reaction or conversion zone and contacted with the catalyst composition therein for a period of ≤3 hours, ≤2.5 hours, ≤2 hours, ≤1.5 hours, ≤1 hour, ≤45 minutes, ≤30 minutes, ≤20 minutes, ≤10 minutes, ≤5 minutes, ≤1 minute, ≤30 seconds, ≤10 seconds, ≤5 seconds, or ≤1 second or ≤0.5 seconds. In some embodiments, the first hydrocarbon-containing feed can be contacted with the catalyst composition for a period of 0.1 seconds, 0.5 seconds, 0.7 seconds, 1 second, 30 seconds, 1 minute, 5 minutes or 10 minutes to 30 minutes, 50 minutes, 70 minutes, 1.5 hours, 2 hours or 3 hours.
[0072] The first hydrocarbon-containing feed and the catalyst composition may be contacted at a hydrocarbon partial pressure of at least 20 kPa absolute, wherein the hydrocarbon partial pressure is the hydrocarbon partial pressure of any C2-C4 in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16In some embodiments, the hydrocarbon partial pressure during contacting of the first hydrocarbon-containing feed and the catalyst composition can be in the range of 20 kPa absolute, 50 kPa absolute, 70 kPa absolute, 80 kPa absolute, 90 kPa absolute, 95 kPa absolute, 100 kPa absolute, 150 kPa, 200 kPa, 300 kPa absolute, 500 kPa absolute, 750 kPa absolute, or 1,000 kPa absolute to 1,500 kPa absolute, 2,500 kPa absolute, 4,000 kPa absolute, 5,000 kPa absolute, 7,000 kPa absolute, 8,500 kPa absolute, or 10,000 kPa absolute, wherein the hydrocarbon partial pressure is the total partial pressure of the alkyl aromatic hydrocarbons in any C2-C4 hydrocarbons in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 In other embodiments, the hydrocarbon partial pressure during contact of the hydrocarbon-containing feed with the catalyst composition may be in the range of 20 kPa absolute, 50 kPa absolute, 70 kPa absolute, 80 kPa absolute, 90 kPa absolute, 95 kPa absolute, 100 kPa absolute, 150 kPa absolute, 200 kPa absolute, 250 kPa absolute, or 300 kPa absolute to 500 kPa absolute, 600 kPa absolute, 700 kPa absolute, 800 kPa absolute, 900 kPa absolute, or 1,000 kPa absolute, wherein the hydrocarbon partial pressure is the total partial pressure of the alkyl aromatic hydrocarbons in any C2-C4 hydrocarbons in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 Total partial pressure of alkyl aromatics.
[0073] In some embodiments, the first hydrocarbon-containing feed may include at least 60 vol%, at least 65 vol%, at least 70 vol%, at least 75 vol%, at least 80 vol%, at least 85 vol%, at least 90 vol%, at least 95 vol%, or at least 99 vol% of a single C2-C 16 The first hydrocarbon-containing feed and the catalyst composition may be a single C2-C4 hydrocarbon at a pressure of at least 20 kPa absolute, at least 50 kPa absolute, at least 70 kPa absolute, at least 80 kPa absolute, at least 90 kPa absolute, at least 95 kPa absolute, at least 100 kPa absolute, at least 150 kPa absolute, at least 250 kPa absolute, at least 300 kPa absolute, at least 400 kPa absolute, at least 500 kPa absolute, or at least 1,000 kPa absolute. 16 Alkanes such as propane are contacted under pressure.
[0074] The first hydrocarbon feed can be contacted with the catalyst composition in the reaction or conversion zone at any weight hourly space velocity (WHSV) effective to carry out the described upgrading process. In some embodiments, the WHSV can be 0.01 hr -1 、0.1hr -1 , 1hr -1 , 2hr -1 , 5hr -1 、10hr -1 、20hr -1 、30hr -1 or 50hr -1 Up to 100hr -1 、250hr -1 、500hr -1 or 1,000hr -1 In some embodiments, when the hydrocarbon upgrading process includes a fluidized or otherwise moving catalyst composition, the catalyst composition circulation mass flow rate is proportional to any C2-C 16 Alkanes and any C8-C 16 The ratio of the total amount of alkyl aromatic hydrocarbon mass flow rates can range from 1, 3, 5, 10, 15, 20, 25, 30, or 40 to 50, 60, 70, 80, 90, 100, 110, 125, or 150 on a weight to weight basis.
[0075] When the activity of the coked catalyst composition is reduced to below the required minimum amount, the coked catalyst composition or at least a portion thereof can undergo a regeneration process to produce a regenerated catalyst composition. More specifically, the coked catalyst composition can be contacted with one or more oxidants to carry out the combustion of at least a portion of coke, to produce a regenerated catalyst composition and combustion gases lean in coke. The regeneration of the coked catalyst composition can occur in a reaction or conversion zone or in a combustion zone separated from a reaction or conversion zone according to a specific reactor configuration, to produce a regenerated catalyst composition. For example, when using a fixed bed or flow conversion reactor, the regeneration of the coked catalyst composition can occur in a reaction or conversion zone, or when using a fluidized bed reactor or other circulation or fluidized reactor, the regeneration of the coked catalyst composition occurs in a separate combustion zone that can be separated from a reaction or conversion zone.
[0076] In some embodiments, the method may optionally include contacting at least a portion of the regenerated catalyst composition with a reducing gas to produce a regenerated and reduced catalyst composition. An additional amount of hydrocarbon-containing feed may contact at least a portion of the regenerated catalyst composition and / or at least a portion of any regenerated and reduced catalyst composition to produce a re-coked catalyst composition and additional effluent.
[0077] In some embodiments, the cycle time from contacting the hydrocarbon-containing feed with the catalyst composition to contacting the additional amount of hydrocarbon-containing feed with the regenerated catalyst composition can be ≤5 hours, ≤4 hours, ≤3 hours, ≤2 hours, ≤1.5 hours, ≤1 hour, ≤50 minutes, ≤45 minutes, ≤40 minutes, ≤30 minutes, ≤25 minutes, ≤20 minutes, or ≤15 minutes. The first cycle begins when the catalyst composition is contacted with the first hydrocarbon-containing feed, and then the catalyst composition is contacted with at least an oxidizing gas to produce a regenerated catalyst composition or at least an oxidizing gas and an optional reducing gas to produce a regenerated and reduced catalyst composition, and the first cycle ends and the second cycle begins when the regenerated catalyst composition is contacted with the additional amount of the first hydrocarbon-containing feed. If one or more additional feeds (described in more detail below) are used between the first hydrocarbon-containing feed and the oxidizing gas stream, between the oxidizing gas and the reducing gas (if used) stream, between the oxidizing gas and the additional amount of the first hydrocarbon-containing feed stream, and / or between the reducing gas (if used) and the additional amount of the first hydrocarbon-containing feed stream, then the period of time during which such stripping gas is used will be included in the period of time included in the cycle time. Thus, in some embodiments, the cycle time from contacting the first hydrocarbon-containing feed with the catalyst composition in step to contacting the additional amount of the hydrocarbon-containing feed with the regenerated catalyst composition may be ≤ 5 hours.
[0078] The oxidant may be or may include, but is not limited to, O2, O3, CO2, H2O, or mixtures thereof. In some embodiments, an oxidant in an amount in excess of that required to combust 100% of the coke on the catalyst composition may be used to increase the rate of removal of coke from the catalyst composition, such that the time required to remove the coke may be reduced and result in an increased yield of upgraded products produced in a given period of time. Using pure O2 as an oxidant may facilitate capture and sequestration of CO2 produced during combustion in one or more downstream CO2 recovery systems.
[0079] The coked catalyst composition and the oxidant may be contacted with each other at a temperature in the range of 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, or 800°C to 900°C, 950°C, 1,000°C, 1,050°C, or 1,100°C to produce a regenerated catalyst composition. In some embodiments, the coked catalyst composition and the oxidant may be contacted with each other at a temperature in the range of 500°C to 1,100°C, 600°C to 1,000°C, 650°C to 950°C, 700°C to 900°C, or 750°C to 850°C to produce a regenerated catalyst composition.
[0080] In some embodiments, the coked catalyst composition and oxidant can contact each other for a time of ≤2 hours, ≤1 hour, ≤30 minutes, ≤10 minutes, ≤5 minutes, ≤1 minute, ≤30 seconds, ≤10 seconds, ≤5 seconds, or ≤1 second. For example, the coked catalyst composition and oxidant can contact each other for a time of 2 seconds to 2 hours. In some embodiments, the coked catalyst composition and oxidant can contact a time of ≥50 wt %, ≥75 wt %, or ≥90 wt %, or >99% of any coke on the catalyst composition.
[0081] In some embodiments, the time period during which the coked catalyst composition and the oxidant contact each other may be less than the time period during which the catalyst composition contacts the hydrocarbonaceous feed to produce an effluent and the coked catalyst composition. For example, the time period during which the coked catalyst composition and the oxidant contact each other may be at least 90%, at least 60%, at least 30%, or at least 10% shorter than the time period during which the catalyst composition contacts the hydrocarbonaceous feed to produce an effluent. In other embodiments, the time period during which the coked catalyst composition and the oxidant contact each other may be greater than the time period during which the catalyst composition contacts the hydrocarbonaceous feed to produce an effluent and the coked catalyst composition. For example, in some embodiments, the period of time that the coked catalyst composition and the oxidant are in contact with each other can be at least 50%, at least 100%, at least 300%, at least 500%, at least 1,000%, at least 10,000%, at least 30,000%, at least 50,000%, at least 75,000%, at least 100,000%, at least 250,000%, at least 500,000%, at least 750,000%, at least 1,000,000%, at least 1,250,000%, at least 1,500,000%, or at least 1,800,000% longer than the period of time that the catalyst composition is in contact with the hydrocarbon-containing feed to produce the effluent.
[0082] The coked catalyst composition and the oxidant can contact each other at an oxidant partial pressure in the range of 20 kPa absolute, 50 kPa absolute, 70 kPa absolute, 80 kPa absolute, 90 kPa absolute, 95 kPa absolute, 100 kPa absolute, 300 kPa absolute, 500 kPa absolute, 750 kPa absolute, or 1,000 kPa absolute to 1,500 kPa absolute, 2,500 kPa absolute, 4,000 kPa absolute, 5,000 kPa absolute, 7,000 kPa absolute, 8,500 kPa absolute, or 10,000 kPa absolute. In other embodiments, the partial pressure of the oxidant during contact with the coked catalyst composition can be in the range of 20 kPa absolute, 50 kPa absolute, 70 kPa absolute, 80 kPa absolute, 90 kPa absolute, 95 kPa absolute, 100 kPa absolute, 150 kPa absolute, 200 kPa absolute, 250 kPa absolute, or 300 kPa absolute to 500 kPa absolute, 600 kPa absolute, 700 kPa absolute, 800 kPa absolute, 900 kPa absolute, or 1,000 kPa absolute to produce a regenerated catalyst composition.
[0083] Without wishing to be bound by theory, it is believed that at least a portion of the 8-10 Group elements such as Pt disposed on the coked catalyst composition may be agglomerated compared to the catalyst composition before contacting with the first hydrocarbon-containing feed. It is believed that during the combustion of at least a portion of the coke on the coked catalyst composition, at least a portion of the 8-10 Group elements may be redispersed on the carrier. Redispersing at least a portion of any agglomerated 8-10 Group elements may improve the stability of the catalyst composition over many cycles.
[0084] In some embodiments, compared with the 8-10 group elements in the catalyst composition contacted with the first hydrocarbon-containing feed and compared with the 8-10 group elements in the catalyst composition of coking, at least a portion of the 8-10 group elements such as Pt in the regenerated catalyst composition can be in a higher oxidation state. Therefore, as described above, in some embodiments, the method can optionally include contacting at least a portion of the regenerated catalyst composition with a reducing gas to produce a regenerated and reduced catalyst composition. Suitable reducing gas (reducing agent) can be or can include but is not limited to H2, CO, CH4, C2H6, C3H8, C2H4, C3H6, steam or their mixture. In some embodiments, the reducing agent can be mixed with an inert gas such as Ar, Ne, He, N2, CO2, H2O or their mixture. In such an embodiment, compared with the 2nd group elements in the regenerated catalyst composition, at least a portion of the 2nd group elements in the catalyst composition of regeneration and reduction can be reduced to a lower oxidation state, such as a single substance state. In this embodiment, an additional amount of the hydrocarbon-containing feed may be contacted with at least a portion of the regenerated catalyst composition and / or at least a portion of the regenerated and reduced catalyst composition.
[0085] In some embodiments, the regenerated catalyst composition and the reducing gas may be contacted at a temperature ranging from 400° C., 450° C., 500° C., 550° C., 600° C., 620° C., 650° C., or 670° C. to 720° C., 750° C., 800° C., or 900° C. The regenerated catalyst composition and the reducing gas may be contacted for a time ranging from 1 second, 5 seconds, 10 seconds, 20 seconds, 30 seconds, or 1 minute to 10 minutes, 30 minutes, or 60 minutes. The regenerated catalyst composition and the reducing gas may be contacted at a reducing agent partial pressure of 20 kPa absolute, 50 kPa absolute, 70 kPa absolute, 80 kPa absolute, 90 kPa absolute, 95 kPa absolute, 100 kPa absolute, 300 kPa absolute, 500 kPa absolute, 750 kPa absolute, or from 1,000 kPa absolute to 1,500 kPa absolute, 2,500 kPa absolute, 4,000 kPa absolute, 5,000 kPa absolute, 7,000 kPa absolute, 8,500 kPa absolute, or 10,000 kPa absolute. In other embodiments, the partial pressure of the reductant during contact with the regenerated catalyst composition can be in the range of 20 kPa absolute, 50 kPa absolute, 70 kPa absolute, 80 kPa absolute, 90 kPa absolute, 95 kPa absolute, 100 kPa absolute, 150 kPa absolute, 200 kPa absolute, 250 kPa absolute, or 300 kPa absolute to 500 kPa absolute, 600 kPa absolute, 700 kPa absolute, 800 kPa absolute, 900 kPa absolute, or 1,000 kPa absolute to produce a regenerated catalyst composition.
[0086] At least a portion of the regenerated catalyst composition, the regenerated and reduced catalyst composition, the new or fresh catalyst composition, or a mixture thereof can be contacted with an additional amount of the first hydrocarbon-containing feed in a reaction or conversion zone to produce additional effluent and additional coked catalyst composition. As described above, in some embodiments, the cycle time from contacting the hydrocarbon-containing feed with the catalyst composition to contacting the additional amount of the hydrocarbon-containing feed with at least a portion of the regenerated catalyst composition and / or the regenerated and reduced catalyst composition and optionally with a new or fresh catalyst composition can be ≤5 hours.
[0087] In some embodiments, as described above, one or more additional feeds, such as one or more purge fluids, can be used between the first hydrocarbon-containing feed and the oxidant stream, between the oxidant and the optional reducing gas (if used) stream, between the oxidant and the additional first hydrocarbon-containing feed stream and / or between the reducing gas and the additional first hydrocarbon-containing feed stream. The purge fluid can especially purge or otherwise expel undesirable materials such as non-combustible particles including soot from the reactor. In some embodiments, the additional one or more feeds can be inert under dehydrogenation, dehydrogenation aromatization and dehydrogenation cyclization, combustion and / or reduction conditions. Suitable purge fluids can be or can include but are not limited to N2, He, Ar, CO2, H2O, CO2, CH4 or mixtures thereof. In some embodiments, if the method utilizes a purge fluid, the duration or time period of using the purge fluid can be in the range of 1 second, 5 seconds, 10 seconds, 20 seconds, 30 seconds or 1 minute to 10 minutes, 30 minutes or 60 minutes.
[0088] In some embodiments, the catalyst composition can remain sufficiently active and stable after many cycles, such as at least 15, at least 20, at least 30, at least 40, at least 50, at least 60, at least 70, at least 100, at least 125, at least 150, at least 175, or at least 200 cycles, wherein each cycle time lasts ≤5 hours, ≤4 hours, ≤3 hours, ≤2 hours, ≤1 hour, ≤50 minutes, ≤45 minutes, ≤30 minutes, ≤15 minutes, ≤10 minutes, ≤5 minutes, ≤1 minute, ≤30 seconds, or ≤10 seconds. In some embodiments, the cycle time can be from 5 seconds, 30 seconds, 1 minute, or 5 minutes to 10 minutes, 20 minutes, 30 minutes, 45 minutes, 50 minutes, 70 minutes, 2 hours, 3 hours, 4 hours, or 5 hours. In some embodiments, after the catalyst performance stabilizes (sometimes the first few cycles may have poor or better performance, but the performance may eventually stabilize), the process may produce a first upgraded hydrocarbon product, such as propylene yield, with a selectivity of ≥75%, ≥80%, ≥85%, ≥90%, ≥93% or ≥95% to upgraded hydrocarbons (e.g., propylene when the hydrocarbon-containing feed comprises propane) upon initial contact with the first hydrocarbon-containing feed, and may have a second upgraded hydrocarbon product yield with a selectivity of ≥75%, ≥80%, ≥85%, ≥90%, ≥93% or ≥95% to upgraded hydrocarbons, such as propylene, upon completion of the last cycle (at least 15 cycles in total), which may be at least 90%, at least 93%, at least 95%, at least 97%, at least 98%, at least 99%, at least 99.5% or at least 100% of the first upgraded hydrocarbon product yield.
[0089] In some embodiments, when the first hydrocarbon-containing feed comprises propane and the upgraded hydrocarbon comprises propylene, contacting the hydrocarbon-containing feed with the catalyst composition can produce a propylene yield of ≥52%, ≥53%, ≥55%, ≥57%, ≥60%, ≥62%, ≥63%, ≥64%, ≥65%, or ≥66% with a propylene selectivity of ≥75%, ≥80%, ≥85%, ≥90%, ≥93%, or ≥95%. In some embodiments, when the first hydrocarbon-containing feed comprises propane and the upgraded hydrocarbon comprises propylene, contacting the hydrocarbon-containing feed with the catalyst composition can produce a propylene yield of ≥52%, ≥53%, ≥55%, ≥57%, ≥60%, ≥62%, ≥63%, ≥64%, ≥65%, or ≥66% with a propylene selectivity of ≥75%, ≥80%, ≥85%, ≥90%, ≥93%, or ≥95% for at least 15, at least 20, at least 30, at least 40, at least 50, at least 60, at least 70, at least 100 cycles, at least 125 cycles, at least 150 cycles, at least 175 cycles, or at least 200 cycles. In some embodiments, when a hydrocarbon-containing feed comprising at least 70 vol%, at least 75 vol%, at least 80 vol%, at least 85 vol%, at least 90 vol%, or at least 95 vol% propane based on the total volume of the first hydrocarbon-containing feed is contacted at a propane partial pressure of at least 20 kPa absolute, a propylene yield of ≥52%, ≥53%, ≥55%, ≥57%, ≥60%, ≥62%, ≥63%, ≥64%, ≥65%, or ≥66% can be obtained at a propylene selectivity of ≥75%, ≥80%, ≥85%, ≥90%, ≥93%, or ≥95%. In other embodiments, when a hydrocarbon-containing feed comprising at least 70 vol%, at least 75 vol%, at least 80 vol%, at least 85 vol%, at least 90 vol%, or at least 95 vol% propane based on the total volume of the first hydrocarbon-containing feed is contacted at a propane partial pressure of at least 20 kPa absolute, a propylene yield of ≥52%, ≥53%, ≥55%, ≥57%, ≥60%, ≥62%, ≥63%, ≥64%, ≥65%, or ≥66% can be obtained with a propylene selectivity of ≥75%, ≥80%, ≥85%, ≥90%, ≥93%, or ≥95% for at least 15, at least 20, at least 30, at least 40, at least 50, at least 60, at least 70, at least 100 cycles, at least 125 cycles, at least 150 cycles, at least 175 cycles, or at least 200 cycles.It is believed that by further optimizing the support composition and / or adjusting one or more process conditions, the propylene yield can be further increased to ≥67%, ≥68%, ≥70%, ≥72%, ≥75%, ≥77%, ≥80% or ≥82% at a propylene selectivity of ≥75%, ≥80%, ≥85%, ≥90%, ≥93% or ≥95% for ≥15 cycles, ≥20 cycles, ≥30 cycles, ≥40 cycles, ≥50 cycles, ≥60 cycles, ≥70 cycles, ≥100 cycles, ≥125 cycles, ≥150 cycles, ≥175 cycles or ≥200 cycles. In some embodiments, the propylene yields may be obtained for ≥15 cycles, ≥20 cycles, ≥30 cycles, ≥40 cycles, ≥50 cycles, ≥60 cycles, ≥70 cycles, ≥100 cycles, ≥125 cycles, ≥150 cycles, ≥175 cycles, or ≥200 cycles when the catalyst composition is contacted with a hydrocarbon-containing feed at a temperature of ≥620°C, ≥630°C, ≥640°C, ≥650°C, ≥655°C, ≥660°C, ≥670°C, ≥680°C, ≥690°C, ≥700°C, or ≥750°C.
[0090] Systems suitable for carrying out the methods disclosed herein may include systems well known in the art, such as fixed bed reactors disclosed in WO Publication No. WO2017078894; U.S. Patent Nos. 3,888,762; 7,102,050; 7,195,741; 7,122,160; and 8,653,317; and U.S. Patent Application Publication Nos. 2004 / 0082824; fluidized riser reactors and / or downcomer reactors disclosed in 2008 / 0194891; and U.S. Patent No. 8,754,276; U.S. Patent Application Publication No. 2015 / 0065767; and the flow conversion reactor disclosed in WO Publication No. WO2013169461.
[0091] The first hydrocarbon-containing feed may be or may include, but is not limited to, one or more alkanes, such as C2-C 16 Linear or branched alkanes and / or C4-C 16 Cycloalkanes, and / or one or more alkyl aromatics, such as C8-C 16 In some embodiments, the first hydrocarbon-containing feedstock may optionally include 0.1 vol% to 50 vol% steam, based on any C2-C 16 Alkanes and any C8-C 16 In other embodiments, based on any C2-C 16 Alkanes and any C8-C 16The first hydrocarbon-containing feed may include <0.1 vol% steam, based on the total volume of alkylaromatic hydrocarbons, or may be free of steam.
[0092] The C2-C 16 Alkanes can be or can include but are not limited to ethane, propane, normal butane, isobutane, normal pentane, isopentane, normal hexane, 2-methylpentane, 3-methylpentane, 2,2-dimethylbutane, normal heptane, 2-methylhexane, 2,2,3-trimethylbutane, cyclopentane, cyclohexane, methylcyclopentane, ethylcyclopentane, n-propylcyclopentane, 1,3-dimethylcyclohexane or their mixture.For example, the first hydrocarbon-containing feed can include propane that can be dehydrogenated to produce propylene, and / or can be dehydrogenated to produce isobutane of isobutylene.In another example, the first hydrocarbon-containing feed can include liquefied petroleum gas (LP gas), which can be in gas phase when contacting with catalyst composition.In some embodiments, the first hydrocarbon in hydrocarbon-containing feed can be substantially composed of single alkane such as propane. In some embodiments, the hydrocarbon-containing feed may contain ≥50 mol%, ≥75 mol%, ≥95 mol%, ≥98 mol%, or ≥99 mol% of a single C2-C 16 The first hydrocarbon-containing feedstock may contain at least 50%, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, at least 85%, at least 90%, at least 95%, at least 97%, or at least 99% by volume of a single C2-C 16 The alkane, such as propane, is based on the total volume of the first hydrocarbon-containing feed.
[0093] The C8-C 16 The alkyl aromatic hydrocarbons may be or may include, but are not limited to, ethylbenzene, propylbenzene, butylbenzene, one or more ethyltoluenes, or mixtures thereof. In some embodiments, the hydrocarbon-containing feed may contain ≥50 mol%, ≥75 mol%, ≥95 mol%, ≥98 mol%, or ≥99 mol% of a single C8-C 16 The alkyl aromatics, such as ethylbenzene, are based on the total weight of all hydrocarbons in the first hydrocarbon-containing feed. In some embodiments, ethylbenzene can be dehydrogenated to produce styrene. Therefore, in some embodiments, the first method of upgrading hydrocarbons disclosed herein can include propane dehydrogenation, butane dehydrogenation, isobutane dehydrogenation, pentane dehydrogenation, pentane dehydrogenation cyclization to cyclopentadiene, naphtha reforming, ethylbenzene dehydrogenation, ethyltoluene dehydrogenation, etc.
[0094] In some embodiments, the first hydrocarbon-containing feed may be diluted, for example, with one or more diluents such as one or more inert gases. Suitable inert gases may be or may include, but are not limited to, Ar, Ne, He, N2, CO2, CH4, or mixtures thereof. If the hydrocarbon-containing feed includes a diluent, then based on any C2-C4 in the hydrocarbon-containing feed, the first hydrocarbon-containing feed may be diluted with one or more diluents such as one or more inert gases. Suitable inert gases may be or may include, but are not limited to, Ar, Ne, He, N2, CO2, CH4, or mixtures thereof. 16 Alkanes and any C8-C 16 The hydrocarbonaceous feed may contain from 0.1 vol%, 0.5 vol%, 1 vol% or 2 vol% to 3 vol%, 8 vol%, 16 vol% or 32 vol% diluent, based on the total volume of alkyl aromatic hydrocarbons.
[0095] In some embodiments, the first hydrocarbon-containing feed may further comprise H2. In some embodiments, when the first hydrocarbon-containing feed comprises H2, H2 and any C2-C 16 Alkanes and any C8-C 16 The molar ratio of the total amount of alkyl aromatics may be in the range of 0.1, 0.3, 0.5, 0.7 or 1 to 2, 3, 4, 5, 6, 7, 8, 9 or 10.
[0096] In some embodiments, the first hydrocarbon-containing feed may be substantially free of any steam, e.g., <0.1 vol. % steam, based on any C2-C 16 Alkanes and any C8-C 16 In other embodiments, the first hydrocarbon-containing feed may include steam. For example, the first hydrocarbon-containing feed may include 0.1%, 0.3%, 0.5%, 0.7%, 1%, 3%, or 5% to 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, or 50% steam by volume, based on any C2-C8 in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 In other embodiments, the first hydrocarbon-containing feed may contain ≤50 vol%, ≤45 vol%, ≤40 vol%, ≤35 vol%, ≤30 vol%, ≤25 vol%, ≤20 vol%, or ≤15 vol% steam, based on the total volume of C2-C8 alkyl aromatics in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 In other embodiments, the first hydrocarbon-containing feed may contain at least 1 volume %, at least 3 volume %, at least 5 volume %, at least 10 volume %, at least 15 volume %, at least 20 volume %, at least 25 volume %, or at least 30 volume % steam, based on the total volume of any C2-C8 alkyl aromatics in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 The total volume of alkyl aromatics.
[0097] In some embodiments, the first hydrocarbon-containing feed can comprise sulphur.For example, the first hydrocarbon-containing feed can comprise sulphur of 0.5ppm, 1ppm, 5ppm, 10ppm, 20ppm, 30ppm, 40ppm, 50ppm, 60ppm, 70ppm or 80ppm to 100ppm, 150ppm, 200ppm, 300ppm, 400ppm or 500ppm.In other embodiments, the first hydrocarbon-containing feed can comprise sulphur of 1ppm to 10ppm, 10ppm to 20ppm, 20ppm to 50ppm, 50ppm to 100ppm or 100ppm to 500ppm.If present in the first hydrocarbon-containing feed, described sulphur can be or can include but not limited to H2S, dimethyl disulfide, as one or more mercaptans or its any mixture.
[0098] In some embodiments, the first hydrocarbon-containing feed may be substantially free of or free of molecular oxygen. In some embodiments, the first hydrocarbon-containing feed may contain ≤5 mol%, ≤3 mol%, or ≤1 mol% of molecular oxygen (O2). It is believed that providing a first hydrocarbon-containing feed substantially free of molecular oxygen substantially prevents oxidation reactions that would otherwise consume at least a portion of the alkanes and / or alkyl aromatics in the first hydrocarbon-containing feed.
[0099] The second method of upgrading hydrocarbons
[0100] In some embodiments, the method for upgrading hydrocarbons may include the upgrading method disclosed in U.S. Patent Application Publication No. 2021 / 0276932. For example, the method for upgrading hydrocarbons may include (I) contacting a first hydrocarbon-containing feed with a catalyst composition comprising a Group 8-10 element disposed on a support to perform one or more of dehydrogenation, dehydrogenation aromatization, and dehydrogenation cyclization of at least a portion of the first hydrocarbon-containing feed to produce a coked catalyst composition and an effluent that may include one or more upgraded hydrocarbons and molecular hydrogen. The first hydrocarbon-containing feed may include C2-C 16 One or more linear or branched alkanes, or C4-C 16 One or more of cycloalkanes, or C8-C 16 The first hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature of 300° C. to 900° C. at a hydrocarbon partial pressure of at least 20 kPa absolute for a period of ≤ 3 hours, wherein the hydrocarbon partial pressure is the hydrocarbon partial pressure of any C2-C 16 Alkanes and any C8-C 16The total partial pressure of alkyl aromatics. The catalyst composition may include 0.001wt% to 6wt% of a Group 8-10 element disposed on a carrier, the carrier including Al and at least 0.5wt% of a Group 2 element and containing no Si or containing <0.5wt% Si, wherein all weight percentage values are based on the weight of the carrier. The one or more upgrading hydrocarbons may include at least one of a dehydrogenated hydrocarbon, a dehydrogenated aromatized hydrocarbon, and a dehydrogenated cyclized hydrocarbon. The method may also include (II) contacting at least a portion of the coked catalyst composition with an oxidant to burn at least a portion of the coke to produce a regenerated catalyst composition and combustion gases that are depleted in coke. The method may also include (III) contacting an additional amount of the first hydrocarbon-containing feed with at least a portion of the regenerated catalyst composition to produce a re-coked catalyst composition and additional effluent. The cycle time from contacting the first hydrocarbon-containing feed with the catalyst composition in step (I) to contacting the additional amount of the first hydrocarbon-containing feed with the regenerated catalyst composition in step (III) may be ≤5 hours.
[0101] In some embodiments, at least a portion of the Group 8-10 elements in the regenerated catalyst can be in a higher oxidation state compared to the Group 8-10 elements in the catalyst contacted with the first hydrocarbon-containing feed, and the method can also include the following step (IIa) after step (II) and before step (III): contacting at least a portion of the regenerated catalyst with a reducing gas to produce a regenerated and reduced catalyst, wherein at least a portion of the Group 8-10 elements in the regenerated and reduced catalyst are reduced to a lower oxidation state compared to the Group 8-10 elements in the regenerated catalyst, and wherein an additional amount of hydrocarbon-containing feed can be contacted with at least a portion of the regenerated and reduced catalyst.
[0102] The third method of upgrading hydrocarbons
[0103] In some embodiments, the method for upgrading hydrocarbons may include the upgrading method disclosed in U.S. Patent Application Publication No. 2021 / 0276002. For example, the method for upgrading hydrocarbons may include (I) contacting a first hydrocarbon-containing feed with fluidized catalyst particles that may include Group 8-10 elements disposed on a support in a conversion zone to perform one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the first hydrocarbon-containing feed to produce a conversion effluent that may include coked catalyst particles, one or more upgraded hydrocarbons, and molecular hydrogen. The first hydrocarbon-containing feed may include C2-C 16 One or more linear or branched alkanes, C4-C 16 One or more cycloalkanes, C8-C 16The first hydrocarbon-containing feed and the fluidized catalyst particles may be contacted at a temperature of 300° C. to 900° C. for a period of 0.1 second to 2 minutes at a hydrocarbon partial pressure of at least 20 kPa absolute pressure, wherein the hydrocarbon partial pressure is any C2-C 16 Alkanes and any C8-C 16 The total partial pressure of alkyl aromatics. The catalyst particles may include 0.001wt% to 6wt% of Group 8-10 elements disposed on a carrier, the carrier comprising Al and at least 0.5wt% of Group 2 elements and containing no Si or containing <0.5wt% Si, wherein all weight percentage values are based on the weight of the carrier. The one or more upgrading hydrocarbons may include dehydrogenated hydrocarbons, dehydrogenated aromatized hydrocarbons, dehydrogenated cyclized hydrocarbons, or mixtures thereof. The method may also include (II) obtaining a first gaseous stream rich in the one or more upgrading hydrocarbons and the molecular hydrogen from the conversion effluent and a first particle stream rich in the coked catalyst particles. The method may also include (III) contacting at least a portion of the coked catalyst particles in the first particle stream with an oxidant in a combustion zone to carry out combustion of at least a portion of the coke to produce a combustion effluent that may include regenerated catalyst particles and combustion gases that are lean in coke. The method may also include (IV) obtaining a second gaseous stream rich in combustion gases and a second particle stream rich in regenerated catalyst particles from the combustion effluent. The method may further include (V) contacting an additional amount of the first hydrocarbon-containing feed with the fluidized regenerated catalyst particles to produce an additional conversion effluent comprising recoked catalyst particles, additional one or more upgraded hydrocarbons, and additional molecular hydrogen.
[0104] In some embodiments, the method may further include the following step (IVa) after step (IV) and before step (V): contacting at least a portion of the regenerated catalyst particles with a reducing gas to produce regenerated and reduced catalyst particles, wherein an additional amount of hydrocarbon-containing feed may be contacted with the fluidized regenerated and reduced catalyst particles in step (V).
[0105] The fourth method of upgrading hydrocarbons
[0106] In some embodiments, the method for upgrading hydrocarbons may include the first multi-stage upgrading method disclosed in WO Publication No. 2021 / 225747. For example, the upgrading method may be a multi-stage hydrocarbon upgrading method, which may include (I) contacting a first hydrocarbon-containing feed with a first catalyst composition that may include elements of Groups 8-10 disposed on a carrier in a first conversion zone to perform one or more of dehydrogenation, dehydrogenation aromatization, and dehydrogenation cyclization of a portion of the first hydrocarbon-containing feed to produce a first conversion zone effluent that may include one or more upgraded hydrocarbons, molecular hydrogen, and unconverted first hydrocarbon-containing feed. The method may also include (II) contacting the first conversion zone effluent with a second catalyst composition that may include elements of Groups 8-10 disposed on a carrier in a second conversion zone to perform one or more of dehydrogenation, dehydrogenation aromatization, and dehydrogenation cyclization of at least a portion of the unconverted first hydrocarbon-containing feed to produce a second conversion zone effluent that may include an additional amount of one or more upgraded hydrocarbons and molecular hydrogen. The first hydrocarbon-containing feed may include C2-C 16 One or more linear or branched alkanes, C4-C 16 One or more cycloalkanes, C8-C 16 The first hydrocarbon feed and the first catalyst composition may be contacted for a period of 0.1 second to 3 hours at a hydrocarbon partial pressure of at least 20 kPa absolute pressure, wherein the hydrocarbon partial pressure is the hydrocarbon partial pressure of any C2-C 16 Alkanes and any C8-C 16 The first conversion zone effluent and the second catalyst composition may be contacted at a hydrocarbon partial pressure of at least 20 kPa absolute for a period of time ranging from 0.1 second to 3 hours, wherein the hydrocarbon partial pressure is the total partial pressure of any C2-C8 hydrocarbons in the first conversion zone effluent. 16 Alkanes and any C8-C 16 The total partial pressure of alkyl aromatics. The first conversion zone effluent may have a temperature of 300°C to 850°C. The second conversion zone effluent may have a temperature of 350°C to 900°C. The temperature of the second conversion zone effluent may be greater than the temperature of the first conversion zone effluent. The first catalyst composition and the second catalyst composition may have the same composition or different compositions. The first catalyst composition and the second catalyst composition each contain 0.001wt% to 6wt% of Group 8-10 elements disposed on a carrier, the carrier containing Al and at least 0.5wt% of Group 2 elements and containing no Si or containing <0.5wt% Si, wherein all weight percentage values are based on the weight of the carrier. The one or more upgraded hydrocarbons may include dehydrogenated hydrocarbons, dehydroaromatized hydrocarbons, dehydrocyclized hydrocarbons, or mixtures thereof.
[0107] In some embodiments, at least one of the first catalyst composition and the second catalyst composition can be arranged in a fixed bed. In some embodiments, the first conversion zone and the second conversion zone can be arranged in a fixed bed reactor. In some embodiments, the first conversion zone and the second conversion zone can be arranged in a flow conversion reactor. In some embodiments, at least one of the first catalyst and the second catalyst can be in the form of fluidized catalyst particles. In some embodiments, the first catalyst and the second catalyst can be in the form of fluidized catalyst particles. In some embodiments, the first and second conversion zones can be substantially adiabatic.
[0108] In some embodiments, the method may further include the following steps after step (I) and before step (II): (Ia) contacting the first conversion zone effluent with one or more intermediate catalyst compositions that may include elements of Groups 8-10 disposed on a carrier in one or more intermediate conversion zones to perform one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of a portion of the unconverted hydrocarbonaceous feed in the first conversion zone effluent to produce one or more coked intermediate catalysts and one or more intermediate conversion zone effluents having one or more intermediate temperatures that may include unconverted hydrocarbonaceous feed and additional amounts of one or more upgraded hydrocarbons and molecular hydrogen, wherein the last intermediate conversion zone effluent is contacted with a second catalyst in a second conversion zone in step (II). In some embodiments, if the method includes the optional step (Ia), the one or more intermediate temperatures of the one or more intermediate conversion zone effluents may be higher than the temperature of the first conversion zone effluent, and the temperature of the second conversion zone effluent may be higher than the one or more intermediate temperatures of the one or more intermediate conversion zone effluents.
[0109] In some embodiments, contacting the hydrocarbon-containing feed with the first catalyst can produce a coked first catalyst, and contacting the first conversion zone effluent with the second catalyst can produce a coked second catalyst, and the method can also include step (III), which step (III) can include contacting the coked first catalyst, the coked second catalyst, or both the coked first catalyst and the coked second catalyst with an oxidant to burn at least a portion of the coke to produce combustion gases and regenerate the first catalyst, regenerate the second catalyst, or regenerate the first catalyst and regenerate the second catalyst. In some embodiments, in step (III), the coked first catalyst particles, the coked second catalyst particles, or both the coked first catalyst particles and the coked second catalyst particles and the oxidant can be contacted at a temperature of 580°C to 1,100°C, preferably 650°C to 1,000°C, more preferably 700°C to 900°C, or more preferably 750°C to 850°C. In some embodiments, the method may also include (IV) contacting at least a portion of any regenerated first catalyst, at least a portion of any regenerated second catalyst, or at least a portion of any regenerated first catalyst and at least a portion of any regenerated second catalyst with a reducing gas to produce a regenerated and reduced first catalyst, a regenerated and reduced second catalyst, or both the regenerated and reduced first catalyst and the regenerated and reduced second catalyst.
[0110] Fifth method for upgrading hydrocarbons
[0111] In other embodiments, the method for upgrading hydrocarbons may include a second multi-stage upgrading method disclosed in WO Publication No. 2021 / 225747. For example, the multi-stage hydrocarbon upgrading method may include (I) contacting a first hydrocarbon-containing feed with a first plurality of fluidized catalyst particles that may include elements of Groups 8-10 disposed on a carrier in a first conversion zone to perform one or more of dehydrogenation, dehydrogenation aromatization, and dehydrogenation cyclization of a first portion of the first hydrocarbon-containing feed to produce a first conversion zone effluent that may include coked first catalyst particles, one or more upgraded hydrocarbons, molecular hydrogen, and unconverted first hydrocarbon-containing feed. The method may also include (II) contacting the first conversion zone effluent with a second plurality of fluidized catalyst particles that may include Pt and a promoter disposed on a carrier in a second conversion zone to perform one or more of dehydrogenation, dehydrogenation aromatization, and dehydrogenation cyclization of at least a portion of the unconverted first hydrocarbon-containing feed to produce a second conversion zone effluent that may include coked second catalyst particles, an additional amount of upgraded hydrocarbons, and an additional amount of molecular hydrogen. The first hydrocarbon-containing feed may include C2-C 16 One or more linear or branched alkanes, C4-C 16 One or more cycloalkanes, C8-C 16The first hydrocarbon-containing feed and the first plurality of fluidized catalyst particles may be contacted for a period of 0.1 second to 2 minutes at a hydrocarbon partial pressure of at least 20 kPa absolute, wherein the hydrocarbon partial pressure is the hydrocarbon partial pressure of any C2-C 16 Alkanes and any C8-C 16 The first conversion zone effluent and the second plurality of fluidized catalyst particles may be contacted at a hydrocarbon partial pressure of at least 20 kPa absolute for a period of time ranging from 0.1 seconds to 2 minutes, wherein the hydrocarbon partial pressure is the total partial pressure of any C2-C8 hydrocarbons in the first conversion zone effluent. 16 Alkanes and any C8-C 16 The total partial pressure of alkyl aromatics. The first conversion zone effluent may have a temperature of 300°C to 850°C. The second conversion zone effluent may have a temperature of 350°C to 900°C. The temperature of the second conversion zone effluent may be greater than the temperature of the first conversion zone effluent. The first plurality of fluidized catalyst particles and the second plurality of fluidized catalyst particles may each contain 0.001wt% to 6wt% of Group 8-10 elements disposed on a carrier, the carrier containing Al and at least 0.5wt% of Group 2 elements and containing no Si or containing <0.5wt% Si, wherein all weight percentage values are based on the weight of the carrier. The one or more upgraded hydrocarbons may include dehydrogenated hydrocarbons, dehydrogenated aromatic hydrocarbons, dehydrogenated cyclized hydrocarbons, or mixtures thereof. The method may also include (III) obtaining a first gaseous stream rich in upgraded hydrocarbons and molecular hydrogen from the second conversion zone effluent and a first particle stream rich in coked first catalyst particles and coked second catalyst particles. The method may also include (IV) splitting the first particle stream into a second particle stream and a third particle stream. The method may also include (V) recycling the second stream of particles to the first conversion zone as a first plurality of fluidized particles. The method may also include (VI) contacting the third stream of particles with an oxidant in the combustion zone to burn at least a portion of the coke to produce a combustion effluent that may include regenerated catalyst particles lean in coke and combustion gases. The method may also include (VII) obtaining a second gaseous stream rich in combustion gases and a fourth stream of particles rich in regenerated catalyst particles from the combustion effluent. The method may also include (VIII) recycling the fourth stream of particles to the second conversion zone as a second plurality of fluidized catalyst particles.
[0112] In some embodiments, the method may further include the following step (VIIa) after step (VII) and before step (VIII): contacting at least a portion of the fourth particle stream with a reducing gas to produce regenerated and reduced catalyst particles, wherein the regenerated and reduced catalyst particles can be recycled to the second conversion zone as a second plurality of fluidized catalyst particles in step (VIII). In some embodiments, step (IV) may optionally include separating a fifth particle stream from the first particle stream, and the method may optionally include contacting the fourth particle stream with the fifth particle stream to produce a combined particle stream.
[0113] In some embodiments, the method may optionally include the following step (Ia) after step (I) and before step (II): contacting the first conversion zone effluent with one or more intermediate multiple fluidized catalyst particles comprising elements of Groups 8-10 disposed on a carrier in one or more intermediate conversion zones to perform one or more of dehydrogenation, dehydrogenation aromatization and dehydrogenation cyclization of a portion of the unconverted hydrocarbon-containing feed in the first conversion zone effluent to produce one or more coked intermediate multiple fluidized catalyst particles and one or more intermediate conversion zone effluents that may have one or more intermediate temperatures and may contain unconverted hydrocarbon-containing feed and an additional amount of one or more upgraded hydrocarbons and molecular hydrogen, wherein the last intermediate conversion zone effluent may be contacted with a second catalyst in a second conversion zone in step (II).
[0114] The sixth method for upgrading hydrocarbons
[0115] In some embodiments, the method for upgrading hydrocarbons may include the upgrading method disclosed in U.S. Patent Application No. 63 / 062,084. For example, the upgrading method may include (I) introducing a first hydrocarbon-containing feed into a reaction zone, wherein the first hydrocarbon-containing feed may include C2-C 16 One or more linear or branched alkanes, C4-C 16 One or more cycloalkanes, C8-C 16 The method may further include (II) contacting the first hydrocarbon-containing feed with a catalyst composition disposed in a reaction zone and comprising an element of Groups 8 to 10 disposed on a support to perform at least one of dehydrogenation, dehydroaromatization and dehydrocyclization of at least a portion of the first hydrocarbon-containing feed to produce a coked catalyst composition and a first effluent that may comprise one or more upgraded hydrocarbons and molecular hydrogen. The first hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature of 300° C. to 900° C. at a hydrocarbon partial pressure of at least 20 kPa absolute for a period of 1 minute to 90 minutes, wherein the hydrocarbon partial pressure is any C2-C 2-hydroxy- ... 16 Alkanes and any C8-C16 The total partial pressure of alkyl aromatics. The catalyst composition may include 0.001 wt% to 6 wt% of a Group 8-10 element disposed on a carrier, the carrier including Al and at least 0.5 wt% of a Group 2 element and being free of Si or containing <0.5 wt% Si, wherein all weight percentage values are based on the weight of the carrier. The method may also include (III) stopping the introduction of a first hydrocarbon-containing feed into the reaction zone; (IV) introducing an oxidant into the reaction zone; (V) contacting the oxidant with the coked catalyst composition to burn at least a portion of the coke to produce a regenerated catalyst composition depleted in coke and a second effluent comprising combustion gases, wherein the oxidant and the coked catalyst composition are contacted for a period of 1 minute to 90 minutes; and (VI) stopping the introduction of the oxidant into the reaction zone. The method may also include (VII) introducing a reducing gas into the reaction zone; (VIII) contacting the reducing gas with the regenerated catalyst composition to produce a regenerated and reduced catalyst composition and a third effluent, wherein the reducing gas and the regenerated catalyst composition are in contact for a period of 0.1 seconds to 90 minutes; and (IX) stopping the introduction of the reducing gas into the reaction zone. The method may also include (X) introducing an additional amount of the first hydrocarbon-containing feed into the reaction zone and (XI) contacting the additional amount of the first hydrocarbon-containing feed with the regenerated and reduced catalyst composition to produce a re-coked catalyst composition and an additional first effluent. The additional amount of the first hydrocarbon-containing feed and the regenerated and reduced catalyst composition may be contacted at a temperature of 300° C. to 900° C. at a hydrocarbon partial pressure of at least 20 kPa absolute for a period of 1 minute to 90 minutes, wherein the hydrocarbon partial pressure is any C2-C 16 Alkanes and any C8-C 16 Total partial pressure of alkyl aromatics.
[0116] In some embodiments, the method may optionally include the following steps after step (III) and before step (IV): (III a1 ) introducing a stripping gas into the reaction zone to remove at least a portion of any residual hydrocarbon-containing feed, the first effluent, or both from the reaction zone; (III) a2 ) removing at least a portion of any residual hydrocarbon-containing feed, effluent, or both from the reaction zone by subjecting the reaction zone to a pressure less than atmospheric pressure; or step (III) a1 ) and (III a2 In some embodiments, the method may optionally include the following steps after step (VI) and before step (VII): (VI a1 ) introducing a stripping gas into the reaction zone to remove any residual oxidant, the second effluent, or at least a portion of both from the reaction zone; (VI a2) removing any residual oxidant, the second effluent, or at least a portion of both from the reaction zone by subjecting the reaction zone to a pressure less than atmospheric pressure; or step (VI a1 ) and (VI a2 ) combination.
[0117] In some embodiments, the method may optionally include the following steps after step (IX) and before step (X): a1 ) introducing a stripping gas into the reaction zone to remove at least a portion of any residual reducing gas, the third effluent, or both from the reaction zone;
[0118] (IX a2 ) removing any residual reducing gas, the third effluent, or at least a portion of both from the reaction zone by subjecting the reaction zone to a pressure less than atmospheric pressure; or step (IX) a1 ) and (IX a2 ) combination.
[0119] In some embodiments, step (IV) of the method may optionally include introducing a fuel into a reaction zone along with an oxidant; and burning at least a portion of the fuel in the reaction zone to generate heat, wherein the heat heats the reaction zone to a temperature of ≥580°C, ≥620°C, ≥650°C, ≥680°C, ≥710°C, ≥740°C, ≥770°C, ≥800°C, ≥850°C, ≥900°C or ≥1,000°C.
[0120] The seventh method of upgrading hydrocarbons
[0121] In some embodiments, the method of upgrading hydrocarbons may include the upgrading method disclosed in U.S. Patent Application No. 63 / 195,966. For example, the method may include (I) contacting a first hydrocarbon-containing feed with a catalyst composition that may include a Group 8-10 element disposed on a support to perform one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the hydrocarbon-containing feed to produce an at least partially passivated catalyst composition that may include a Group 8-10 element disposed on a support and contaminants and an effluent that may include one or more upgraded hydrocarbons and molecular hydrogen. The first hydrocarbon-containing feed may include C2-C 16 One or more linear or branched alkanes, or C4-C 16 One or more cycloalkanes, C8-C 16One or more of alkyl aromatic hydrocarbons or their mixtures. The catalyst composition may include 0.001wt% to 6wt% of a Group 8-10 element disposed on a carrier, the carrier including Al and at least 0.5wt% of a Group 2 element and being free of Si or containing <0.5wt% of Si, wherein all weight percentage values are based on the weight of the carrier. The first hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature of 300°C to 900°C. The one or more upgraded hydrocarbons may include at least one of a dehydrogenated hydrocarbon, a dehydrogenated aromatized hydrocarbon, and a dehydrogenated cyclized hydrocarbon. The method may also include (II) heating the at least partially passivated catalyst composition using a heated gas mixture to produce a precursor catalyst composition, the heated gas mixture may contain H2O at a concentration greater than 5 mol%, based on the total moles in the heated gas mixture. The method may also include (III) providing an oxidizing gas that may contain up to 5 mol% of H2O, based on the total moles in the oxidizing gas. The method may also include (IV) contacting the procatalyst composition with the oxidizing gas at an oxidation temperature of 620°C to 1,000°C for a duration of at least 30 seconds to produce an oxidized procatalyst composition. The method may also include (V) obtaining a regenerated catalyst composition from the oxidized procatalyst composition. The method may also include (VI) contacting an additional amount of the first hydrocarbon-containing feed with at least a portion of the regenerated catalyst composition to produce an additional at least partially passivated catalyst composition and additional effluent. In some embodiments, the heated gas mixture may be produced by burning a fuel with an oxidizing gas. In some embodiments, the fuel may include at least one of H2, CO, and a hydrocarbon, and the oxidizing gas may include O2. In some embodiments, the oxidizing gas may be or may include, but is not limited to, O2, O3, CO2, or a mixture thereof, and may include up to 5 mol % of H2O.
[0122] Eighth method for upgrading hydrocarbons
[0123] In some embodiments, the method for upgrading hydrocarbons may include the upgrading method disclosed in U.S. Patent Application No. 63 / 232,959. For example, the method for upgrading hydrocarbons may include (I) contacting a first hydrocarbon-containing feed with a fluidized dehydrogenation catalyst particle that may include a Group 8-10 element disposed on a carrier in a conversion zone to dehydrogenate at least a portion of the hydrocarbon-containing feed to produce a conversion effluent that may include coked catalyst particles and one or more dehydrogenated hydrocarbons. The fluidized dehydrogenation catalyst particles may include 0.001 wt% to 6 wt% of a Group 8-10 element disposed on a carrier, the carrier including Al and at least 0.5 wt% of a Group 2 element and containing no Si or containing <0.5 wt% Si, wherein all weight percentage values are based on the weight of the carrier. The first hydrocarbon-containing feed may include C2-C 16 One or more linear or branched alkanes, C4-C 16 One or more cycloalkanes, C8-C 16 One or more of the alkyl aromatic hydrocarbons or their mixtures. Based on any C2-C 16 Alkanes and any C8-C 16 The first hydrocarbon feed can be fed at 0.1 hr. -1 Up to 1,000hr -1 The fluidized dehydrogenation catalyst particles are in contact with any C2-C 16 Alkanes and any C8-C 16The weight ratio of the total amount of aromatic hydrocarbons can be in the range of 3 to 100. The first hydrocarbon-containing feed and the catalyst particles can be contacted at a temperature of 600° C. to 750° C. The method can also include (II) separating a first particle stream rich in the coked catalyst particles and a first gaseous stream rich in one or more dehydrogenated hydrocarbons from the conversion effluent. The method can also include (III) contacting at least a portion of the coked catalyst particles in the first particle stream with an oxidant and a fuel in a combustion zone to burn at least a portion of the coke, thereby producing a combustion effluent that can contain coke-depleted catalyst particles and combustion gases. The dehydrogenation activity of the coke-depleted catalyst particles can be less than the dehydrogenation activity of the coked catalyst particles. The method can also include (IV) separating a second particle stream rich in coke-depleted catalyst particles and a second gaseous stream rich in combustion gases from the combustion effluent. The method may also include (V) contacting at least a portion of the coke-depleted catalyst particles in the second particle stream with an oxidizing gas in an oxygen soaking zone at an oxidation temperature of 620° C. to 1,000° C. for a duration of at least 30 seconds to produce conditioned catalyst particles whose activity may be less than that of the coked catalyst particles. The method may also include (VI) contacting at least a portion of the conditioned catalyst particles with a reducing gas in a reduction zone to produce regenerated catalyst particles whose dehydrogenation activity may be greater than that of the coked catalyst particles. The method may also include (VII) contacting an additional amount of hydrocarbon-containing feed with at least a portion of the regenerated catalyst particles in a conversion zone to produce an additional amount of conversion effluent, which may contain re-coked catalyst particles and an additional amount of one or more dehydrogenated hydrocarbons. The method may also include (VIII) cooling the first gaseous stream to produce a cooled gaseous stream. The method may also include (IX) compressing at least a portion of the cooled gaseous stream to produce a compressed gaseous stream. The method may also include (X) separating products from the compressed gaseous stream.
[0124] In some embodiments, the first gaseous stream rich in one or more dehydrogenated hydrocarbons may also include the catalyst particles of coking entrained. In such embodiments, step (VIII) may include: (VIIIa) contacting the first gaseous stream with the first quenching medium, transferring heat from the first gaseous stream to the first heat transfer medium indirectly, or a combination thereof, to produce the cooled gaseous stream, and (VIIIb) contacting the cooled gaseous stream with the second quenching medium in a quench tower, (VIIIc) recovering from the quench tower a slurry stream of at least a portion of the third gaseous stream of one or more dehydrogenated hydrocarbons and the second quenching medium that may be included in the liquid phase and the catalyst particles of coking entrained, and step (IX) may include compressing at least a portion of the third gaseous stream to produce a compressed gaseous stream. In some embodiments, the conversion effluent may also include benzene, and the method may further include (XI) taking out a benzene product stream from the quench tower.
[0125] Ninth method for upgrading hydrocarbons
[0126] In some embodiments, the method of upgrading alkanes and / or alkyl aromatics may include the method disclosed in U.S. Patent Application No. 63 / 231,939. For example, the method of upgrading hydrocarbons may include (I) contacting a first hydrocarbon-containing feed with fluidized dehydrogenation catalyst particles that may include Group 8-10 elements disposed on a carrier in a conversion zone to dehydrogenate at least a portion of the first hydrocarbon-containing feed to produce a conversion effluent that may include coked catalyst particles and one or more dehydrogenated hydrocarbons. The fluidized dehydrogenation catalyst particles may include contaminants and 0.001 wt% to 6 wt% of Group 8-10 elements disposed on a carrier, the carrier including Al and at least 0.5 wt% of Group 2 elements and containing no Si or containing <0.5 wt% Si, wherein all weight percentage values are based on the weight of the carrier. The method may also include (II) separating from the conversion effluent a first stream rich in the coked catalyst particles and poor in the one or more dehydrogenated hydrocarbons and a second stream rich in the one or more dehydrogenated hydrocarbons and containing entrained coked catalyst particles. The method may also include (III) contacting the second stream with the first quench medium to produce a cooled second stream. The method may also include (IV) contacting the cooled second stream with the second quench medium in a quench tower. The method may also include (V) recovering from the quench tower a slurry stream of a gaseous stream that may contain one or more dehydrogenated hydrocarbons, a condensed first quench medium stream, and at least a portion of the second quench medium that may be contained in the liquid phase and entrained coked catalyst particles. The method may also include (VI) recycling at least a portion of the condensed first quench medium to step (III). The method may also include (VII) separating at least a portion of the entrained coked catalyst particles from the slurry stream to provide a recovered second quench medium stream and a recovered entrained coked catalyst particle stream. The method may also include (VIII) recycling at least a portion of the recovered second quench medium stream to step (IV).
[0127] In some embodiments, the method may also include (IX) contacting at least a portion of the coked catalyst particles in the first stream and at least a portion of the coked catalyst particles in the recovered entrained catalyst particles stream with an oxidant and, optionally, a fuel in a combustion zone to combust at least a portion of the coke and, if present, the fuel to produce a combustion effluent that may include regenerated catalyst particles depleted in coke and combustion gases; (X) separating the combustion gas stream and the regenerated catalyst particles stream; and (XI) contacting an additional amount of the first hydrocarbon-containing feed with the fluidized regenerated catalyst particles from the regenerated catalyst particles stream to produce an additional conversion effluent comprising re-coked catalyst particles and additional one or more dehydrogenated hydrocarbons.
[0128] In some embodiments, the method may optionally further include (XII) transporting at least a portion of the recovered entrained catalyst particle stream to a metal recovery facility; and (XIII) recovering at least a portion of Group 8-10 elements from the coked catalyst particles in the recovered entrained coked catalyst particle stream. In some embodiments, the method may further include (XIV) cooling the slurry stream to produce a cooled slurry stream before step (VII). In some embodiments, the conversion effluent may also include benzene, and the method may further include (XV) taking out a benzene product stream from a quench tower.
[0129] The tenth method for upgrading hydrocarbons
[0130] In some embodiments, the method of upgrading alkanes may include the method disclosed in U.S. Patent Application No. 63 / 222,733. For example, the method of dehydrogenating alkanes may include introducing a first hydrocarbon-containing feed containing one or more alkanes such as propane into a reactor, and the reactor may include a catalyst composition disposed therein that may include a Group 8-10 element disposed on a carrier. The catalyst composition may include contaminants and 0.001 wt% to 6 wt% of a Group 8-10 element disposed on a carrier, the carrier including Al and at least 0.5 wt% of a Group 2 element and containing no Si or containing <0.5 wt% Si, wherein all weight percentage values are based on the weight of the carrier. The method may also include contacting the first hydrocarbon-containing feed with the catalyst composition in a reactor to form a high temperature dehydrogenation product, the high temperature dehydrogenation product comprising at least a portion of the catalyst composition. The method may also include separating at least a portion of the catalyst composition from the high temperature dehydrogenation product in a primary separation device and in a secondary separation device downstream of the primary separation device and in fluid communication with the primary separation device. The method may also include combining the high temperature dehydrogenated product with a quench stream after the high temperature dehydrogenated product leaves the secondary separation device to cool the high temperature dehydrogenated product and form an intermediate temperature dehydrogenated product, wherein the quench stream comprises hydrocarbons. The method may also include cooling the intermediate temperature dehydrogenated product to form a cooled dehydrogenated product.
[0131] In some embodiments, the quench stream may include liquid hydrocarbons, and the intermediate temperature product may be entirely in the gas phase. In some embodiments, the merging of the high temperature dehydrogenated product with the quench stream may be performed in the plenum section of the reactor. In some embodiments, the method may further include further cooling the cooled dehydrogenated product with a heat exchanger or a secondary quench stream downstream of the reactor, wherein the quench stream may include at least a portion of the cooled dehydrogenated product after further cooling by a heat exchanger or a secondary quench stream.
[0132] It should be understood that the second to tenth methods for upgrading hydrocarbons may include the same or similar process conditions as described for the first method for upgrading hydrocarbons, such as operating temperature, pressure, time intervals of certain steps, WHSV, etc., which will be apparent to those skilled in the art.
[0133] Recovery and application of the first upgraded hydrocarbons
[0134] In some embodiments, the first upgraded hydrocarbon produced by any one of the first to tenth hydrocarbon upgrading methods may include at least one upgraded hydrocarbon such as olefins, water, unreacted hydrocarbons, molecular hydrogen, etc. The first upgraded hydrocarbon can be recovered or obtained via any convenient method, such as by one or more conventional methods. Such a method may include cooling and / or compressing the effluent to condense at least a portion of any water and any heavy hydrocarbons that may be present, leaving olefins and any unreacted alkanes or alkyl aromatics mainly in the gas phase. Olefins and unreacted alkanes or alkyl aromatics can then be removed from the reaction product in one or more separator drums. For example, one or more splitters or distillation towers can be used to separate the dehydrogenated product from the unreacted first hydrocarbon-containing feed.
[0135] In some embodiments, recovered olefins such as propylene can be used to produce polymers, for example, recovered propylene can be polymerized to produce polymers having segments or units derived from recovered propylene, such as polypropylene, ethylene-propylene copolymers, etc. Recovered isobutylene can be used, for example, to produce one or more of the following: oxygenates such as methyl tert-butyl ether, fuel additives such as dimerized isobutylene, synthetic elastomeric polymers such as butyl rubber, etc.
[0136] Method for regenerating catalyst
[0137] In some embodiments, the method for regenerating the catalyst composition may include the regeneration method disclosed in U.S. Patent Application No. 63 / 195,966. For example, the regeneration method may be used to regenerate an at least partially passivated catalyst composition, which may include contaminants and 0.001 wt% to 6 wt% of Group 8-10 elements disposed on a carrier, the carrier including Al and at least 0.5 wt% of Group 2 elements and containing no Si or containing <0.5 wt% Si, wherein all weight percentage values are based on the weight of the carrier. In some embodiments, the contaminant may be or may include coke. The method may include (I) heating the at least partially passivated catalyst composition using a heated gas mixture to produce a precursor catalyst composition, the heated gas mixture may contain H2O at a concentration greater than 5 mol%, based on the total moles in the heated gas mixture. The method may also include (II) providing an oxidizing gas that may contain up to 5 mol% of H2O, based on the total moles in the oxidizing gas. The method may also include (III) contacting the procatalyst composition with an oxidizing gas at an oxidation temperature of 620°C to 1,000°C for a duration of at least 30 seconds, preferably at least 1 minute, preferably at least 5 minutes, to produce an oxidized procatalyst composition. The method may also include (IV) obtaining a regenerated catalyst composition from the oxidized procatalyst composition. In some embodiments, the heated gas mixture may be produced by burning a fuel with an oxidizing gas. In some embodiments, the fuel may include at least one of H2, CO, and a hydrocarbon, and the oxidizing gas may include O2. In some embodiments, the oxidizing gas may be or may include, but is not limited to, O2, O3, CO2, or a mixture thereof, and may contain up to 5 mol % of H2O.
[0138] Eleventh method for upgrading hydrocarbons
[0139] The eleventh method of upgrading hydrocarbons may include contacting a hydrocarbon-containing feed (a second hydrocarbon-containing feed) with a catalyst composition comprising an 8-10 group element disposed on a carrier to reform at least a portion of the second hydrocarbon-containing feed to produce a coked catalyst composition and an effluent that may include carbon monoxide and molecular hydrogen. The catalyst composition may include 0.001wt% to 6wt% of a 8-10 group element disposed on a carrier, the carrier including Al and at least 0.5wt% of a 2nd group element and containing no Si or containing <0.5wt% Si, wherein all weight percentage values are based on the weight of the carrier. The catalyst composition and the second hydrocarbon-containing feed may contact each other in any suitable environment such as one or more reaction or conversion zones disposed in one or more reactors to produce an effluent and a coked catalyst composition. The reaction or conversion zone may be disposed or located in one or more fixed bed reactors, one or more fluidized beds or moving bed reactors, one or more flow conversion reactors or any combination thereof. For clarity and ease of description, the reforming reaction will be discussed in the context of a fluidized bed reactor, but it should be understood that a fixed bed reactor, a reverse flow or moving bed reactor or any other reactor may be used to carry out the reforming of the second hydrocarbon-containing feed.
[0140] The reforming reaction can be used to produce reformed hydrocarbons via a continuous reaction process or a discontinuous reaction process. In some embodiments, the reaction process may include a reforming step and a regeneration step, such as an exothermic reaction, which are continuously operated while the fluidized catalyst composition is transported between the reforming and regeneration zones of the reactor. The endothermic reaction may include hydrocarbon reforming in the presence of the catalyst composition. Fresh hydrocarbons and regenerated fluidized catalyst particles may enter the reforming zone. After spending a period of time in the reforming zone, the hydrocarbons may be at least partially converted into reformed products, which may leave the reforming zone together with the spent catalyst composition. The reformed products and unreacted feed may be separated from the spent catalyst by one or more separation devices. While the reformed products and unreacted feed from the separation device are further purified downstream, the spent catalyst may be sent to the regeneration zone for regeneration. The exothermic regeneration reaction may be a reaction of an oxidant and an optional fuel under combustion conditions to produce a regenerated catalyst and flue gas. After regeneration, the regenerated catalyst may be separated from the flue gas by one or more separation devices, and may be transported back to the reforming zone, adding more hydrocarbon feed to enter the reforming zone to trigger more reforming reactions. The reforming step may convert CO2 and / or H2O and hydrocarbons such as CH4 into a synthesis gas comprising H2 and CO. The regeneration step may burn reactants such as coke and / or optional fuel and oxidant disposed on the spent catalyst to generate heat for heating the regenerated catalyst, which may provide heat that can be used to drive the reforming reaction. In some embodiments, the catalyst may be heated to an average temperature of 600°C, 700°C, or 800°C to 1,000°C, 1,300°C, or 1,600°C during the regeneration step.
[0141] Illustrative fuels may be or may include, but are not limited to, hydrocarbons, such as methane, ethane, propane, butane, pentane, or hydrocarbon-containing streams such as natural gas, molecular hydrogen, and / or other combustible compounds. The oxidant may be or may include O2. In some embodiments, the oxidant may be or may include air, O2-rich air, O2-depleted air, or any other suitable O2-containing stream.
[0142] The regeneration of catalyst can correspond to removing coke from catalyst particles. In some embodiments, during reforming, a portion of the feed introduced into the reforming zone can form coke. This coke may potentially hinder the catalytic site (e.g., metal site) of the catalyst. During regeneration, at least a portion of the coke produced during reforming can be removed as CO or CO2. The regeneration of catalyst can also correspond to the redispersion of any agglomerated active phase of catalyst such as the 8th-10th group element.
[0143] The second hydrocarbon-containing feed may be or may include but is not limited to one or more reformable C1-C 16In some embodiments, the second hydrocarbon-containing feedstock may be or may include methane, ethane, propane, butane, pentane or a mixture thereof. In some embodiments, the second hydrocarbon-containing feedstock may be exposed to the catalyst composition at a pressure less than 35 kPa-a. For example, the second hydrocarbon-containing feedstock may be exposed to the catalyst composition at a pressure of 0.7 kPa-a, 2 kPa-a, 3.5 kPa-a, 5 kPa-a or 10 kPa-a to 15 kPa-a, 20 kPa-a, 25 kPa-a or 30 kPa-a. In other embodiments, the second hydrocarbon-containing feedstock may be exposed to the catalyst composition at a pressure of 35 kPa-a to 15 MPa-a. In still other embodiments, the second hydrocarbon-containing feed can be exposed to the catalyst composition at a pressure of 0.7 kPa-a, 2 kPa-a, 5 kPa-a, 20 kPa-a, 35 kPa-a, 50 kPa-a, or 100 kPa-a to 200 kPa-a, 1 MPa-a, 3 MPa-a, 5 MPa-a, 10 MPa-a, or 15 MPa-a. In still other embodiments, the second hydrocarbon-containing feed can be exposed to the catalyst composition at a pressure of less than 2.8 MPa-a, less than 2.5 MPa-a, less than 2.2 MPa-a, or less than 2 MPa-a.
[0144] The reforming reaction of the second hydrocarbon-containing feed such as CH4 can occur in the presence of H2O (steam reforming), in the presence of CO2 (dry reforming), or in the presence of both H2O and CO2 (double reforming). Examples of the stoichiometry of steam reforming, dry reforming, and double reforming of CH4 are shown in equations (1)-(3).
[0145] (1) Dry reforming: CH4+CO2=2CO+2H2
[0146] (2) Steam reforming: CH4+H2O=CO+3H2
[0147] (3) Double reorganization: 3CH4+2H2O+CO2=4CO+8H2
[0148] As shown in equations (1)-(3), dry reforming can produce a lower H2 to CO ratio than steam reforming. Reforming reactions performed with steam alone can typically produce a syngas having a H2:CO molar ratio of about 3, such as 2.5 to 3.5. In contrast, reforming reactions performed with CO2 alone can typically produce a syngas having a H2:CO molar ratio of about 1 or even lower. By using a combination of CO2 and H2O during reforming, the reforming reaction can be controlled to produce a variety of H2 to CO ratios in the resulting syngas.
[0149] The reforming reaction of the second hydrocarbonaceous feed can also be carried out or partially carried out in the presence of O2, the latter of which is generally referred to as a partial oxidation reaction. Examples of stoichiometric partial oxidation and full oxidation are shown in equations (4) and (5).
[0150] (4) Partial oxidation: CH4+0.5O2=CO+2H2
[0151] (5) Complete oxidation: CH4+2O2=CO2+2H2O
[0152] In the partial oxidation of methane, a certain degree of complete oxidation of methane may be inevitable. In such a reaction, CO2 and H2O produced in the complete oxidation of methane can further reform methane via one or more of reactions (1) to (3).
[0153] It should be noted that the ratio of H2 to CO in the syngas may also depend on the water-gas shift equilibrium. Although the stoichiometry in equations (1)-(4) shows a ratio of approximately 1-3, the equilibrium amount of H2 and CO in the syngas may be different from the reaction stoichiometry. The equilibrium amount may be determined based on the water-gas shift equilibrium, which is based on the concentrations of H2, CO, CO2, and H2O involved in the reaction shown in equation (6).
[0154] (6)H2O+CO←→H2+CO2
[0155] In some embodiments, the catalyst composition may also be used as a water-gas shift catalyst. Thus, if the reaction environment for producing H2 and CO also includes H2O and / or CO2, the initial stoichiometry from the reforming reaction may change based on the water-gas shift equilibrium. However, this equilibrium is also temperature dependent, with higher temperatures favoring the production of CO and H2O. As a result, the ratio of H2 to CO produced when forming synthesis gas is limited by the water-gas shift equilibrium at the reaction zone temperature when the synthesis gas is produced.
[0156] The ability to adjust the H2:CO molar ratio of the synthesis gas provides a flexible method that can be combined with various synthesis gas upgrading methods. Illustrative synthesis gas upgrading methods can include but are not limited to Fischer-Tropsch methods, methanol and / or other alcohols (e.g., one or more C1-C4 alcohols) synthesis, fermentation methods, separation methods that can separate hydrogen to produce rich H2 products, dimethyl ether and combinations thereof. These synthesis gas upgrading methods are well known to those of ordinary skill in the art. In some embodiments, the upgraded product can include but is not limited to methanol, synthetic crude oil, diesel, lubricants, waxes, olefins, dimethyl ether, other chemicals or any combination thereof.
[0157] Systems suitable for carrying out reforming of the second hydrocarbon-containing feed may include systems well known in the art, such as fixed bed reactors disclosed in WO Publication No. WO2017078894; U.S. Patent Nos. 3,888,762; 7,102,050; 7,195,741; 7,122,160; and 8,653,317 and U.S. Patent Application Publication Nos. 2004 / 0082824; 2008 / 0194891, fluidized riser reactors and / or downcomer reactors disclosed; and U.S. Patent Nos.: 7,740,829; 8,551,444; 8,754,276; 9,687,803 and 10,160,708 and flow conversion reactors disclosed in U.S. Patent Application Publication Nos. 2015 / 0065767 and 2017 / 0137285 and WO Publication No. WO2013169461.
[0158] Feed and Energy
[0159] The hydrocarbon feed described herein can be derived from fossil fuels or non-fossil fuel resources. For example, propane can be a product or by-product of a method using biomass as a feed. The fuel described in this work can also be derived from fossil fuels or non-fossil fuel resources. For example, methane or H2 can be a product or by-product of a method using biomass as a feed. The fuel described in this work can also be made from renewable energy such as renewable electricity. For example, renewable electricity can be used to produce H2 via water electrolysis. The energy used in the method described in this article can also be provided directly by an electric heater by renewable electricity instead of fuel. Example
[0160] The foregoing discussion can be further described in conjunction with the following non-limiting examples. Catalyst compositions 1-5 were prepared according to the following procedure.
[0161] Catalyst composition 1 - Al(OH)3( S-11) and calcined Mg-Al hydrotalcite ( MG70 / 170) was mixed in deionized water to form a slurry. The slurry was ground and The spray dried particles were calcined in air at 550°C for 4 hours to produce calcined carrier particles containing a nominal 50 wt% MG70 / 170 and 50wt% derived from The calcined support particles were impregnated with an aqueous solution comprising tin(IV) chloride pentahydrate, chloroplatinic acid hexahydrate and deionized water by equal volume impregnation. The impregnated material was allowed to equilibrate at room temperature for 120 hours in a closed container, then it was dried in air at 110°C for 6 hours and calcined in air at 800°C for 12 hours. The final product contained a nominal 0.3 wt% Pt and 1.5 wt% Sn, based on the weight of the support particles.
[0162] Catalyst composition 2 - colloidal SiO2 ( AS-40) (50 g) and calcined Mg-Al hydrotalcite ( MG70 / 170) (22 g) was mixed in deionized water (236 ml) to form a slurry. The slurry was ground and The spray dried particles were calcined in air at 550°C for 4 hours to produce calcined carrier particles containing a nominal 50 wt% MG70 / 170 and 50wt% derived from The calcined support particles were impregnated with an aqueous solution comprising tin(IV) chloride pentahydrate, chloroplatinic acid hexahydrate and deionized water by equal volume impregnation. The impregnated material was allowed to equilibrate at room temperature for 120 hours in a closed container, then it was dried at 110° C. in air for 6 hours and calcined at 800° C. in air for 12 hours. The final product contained a nominal 0.3 wt% Pt and 1.5 wt% Sn based on the weight of the support particles.
[0163] Catalyst composition 3 - In an agate ball mill cup, a 2 / 1 (wt / wt) Mg / Si mixed metal oxide was prepared by adding MgO (8.04 g) (Acros), SiO2 (4.03 g) (Sigma-Aldrich), deionized water (10 g) and 3 agate balls. The material was ball milled at a speed of 500 rpm for 70 hours. The lid was sealed to reduce the evaporation of water during the ball milling process. After ball milling, a thick paste was obtained. The paste was calcined at 200°C in air for 4 hours and then calcined at 800°C in air for 4 hours to obtain a carrier. In a glass bottle, chloroplatinic acid hexahydrate (0.0296 g) (Sigma Aldrich) and tin (IV) chloride pentahydrate (0.0365 g) (Sigma Aldrich) were dissolved in deionized water (1.4319 g) to obtain a dark orange transparent solution (Pt / Sn solution). The 2 / 1 Mg / Si mixed metal oxide support (2.8178 g) was added to a 50 mL plastic bottle, followed by the dropwise addition of the Pt / Sn solution (1.2704 g). The material was mixed using a small laboratory shaker until a uniform light orange powder was obtained. The metal impregnated catalyst was dried in air at 120° C. for 4 hours, then calcined in air at 800° C. for 12 hours. The final product contained a nominal 0.33 wt % Pt and 0.33 wt % Sn, based on the weight of the support. Without wishing to be bound by theory, it is believed that part of the Mg and Si are mixed on an atomic scale, i.e., part of the Mg and Si are in the form of mixed Mg / Si metal oxides, and part of the Mg and part of the Si are mixed on a nanoscale.
[0164] Catalyst composition 4 - Preparation A catalyst composition comprising 40 wt% aluminum chlorohydrate solution (ACH) (42 g), calcined Mg-Al hydrotalcite ( MG70 / 170) (97 g), dehydrated tin (II) chloride (3 g) and 3.1 wt% tetraammine platinum (II) nitrate solution (10 g). The slurry was ground and The catalyst was spray dried on a B-290 mini spray dryer to produce spray dried particles. The spray dried particles were calcined in air at 800°C for 12 hours to produce a catalyst composition containing nominally 0.3 wt% Pt and 1.5 wt% Sn on 90:10 MG70 / 170:Al2O3.
[0165] Catalyst Composition 5 - Catalyst composition 4 was impregnated with an aqueous solution of tetramethylammonium silicate. The impregnated material was allowed to equilibrate at room temperature for 24 hours in a closed container, then it was dried in air at 110°C for 6 hours and calcined in air at 800°C for 12 hours. The final product contained nominally 0.3 wt% Pt, 0.45 wt% Si, and 1.5 wt% Sn.
[0166] Examples using the catalyst compositions 1-5 described above
[0167] Fixed bed experiments using catalysts were conducted at about 100 kPa absolute pressure using catalyst compositions 1-5. The composition of the reactor effluent was measured using a gas chromatograph (GC). The concentration of each component in the reactor effluent was then used to calculate the C3H6 yield and selectivity. The C3H6 yield and selectivity reported in these examples are calculated based on carbon moles.
[0168] In each example, 0.3 g of catalyst was mixed with an appropriate amount of quartz diluent and loaded into a quartz reactor. The amount of diluent was such that the catalyst bed (catalyst + diluent) overlapped with the isothermal zone of the quartz reactor and the catalyst bed remained substantially isothermal during the run. The dead volume of the reactor was filled with quartz chips / rods.
[0169] The process steps using catalyst compositions 1 and 2 are as follows: 1. The system is flushed with an inert gas. 2. Dry air at a flow rate of 83.9 sccm is passed through the bypass of the reaction zone while the inert gas is passed through the reaction zone. The reaction zone is heated to a regeneration temperature of 800°C. 3. Dry air at a flow rate of 83.9 sccm is then passed through the reaction zone for 10 minutes to regenerate the catalyst. 4. The system is flushed with an inert gas. 5. A H2-containing gas containing 10 vol% H2 and 90 vol% Ar is passed through the bypass of the reaction zone at a flow rate of 46.6 sccm for a period of time while the inert gas is passed through the reaction zone. The H2-containing gas is then passed through the reaction zone at 800°C for 3 seconds. 6. The system is flushed with an inert gas. During this process, the temperature of the reaction zone is varied from 800°C to a reaction temperature of 670°C. 7. A hydrocarbon-containing (HC gas) feed having a flow rate of 17.6 sccm and comprising 81 vol% C3H8, 9 vol% inert gas (Ar or Kr) and 10 vol% steam was passed through the bypass of the reaction zone for a period of time while the inert gas was passed through the reaction zone. The hydrocarbon-containing feed was then passed through the reaction zone at 670° C. for 10 minutes. Once the feed was switched from the bypass of the reaction zone to the reaction zone, GC sampling of the reaction effluent was started. The above process steps were repeated cyclically.
[0170] In this application Figure 1-3The C3H6 yield and C3H6 selectivity of various catalyst compositions are shown as a function of time. Figure 1 , 2 In Figures 3 and 4, the horizontal axis represents time (in hours), and the vertical axis represents C3H6 yield (the lower set of data, represented by solid squares) and C3H6 selectivity (the upper set of data, represented by solid circles), expressed in carbon mol%.
[0171] Figure 1 and 2 The C3H6 yield and selectivity are shown respectively for catalyst compositions 1 and 2. Catalyst composition 2, which includes 50 wt% SiO2, deactivates rapidly as the number of cycles increases, but catalyst composition 1, which does not include any SiO2, does not deactivate rapidly.
[0172] The process steps using catalyst composition 3 are as follows: 1. The system is flushed with an inert gas. 2. Dry air at a flow rate of 83.9 sccm is passed through a bypass of the reaction zone while an inert gas is passed through the reaction zone. The reaction zone is heated to a regeneration temperature of 800°C. 3. Dry air at a flow rate of 83.9 sccm is then passed through the reaction zone for 15 minutes to regenerate the catalyst. 4. The system is flushed with an inert gas while cooling to 620°C. 5. A H2-containing gas containing 10 vol% H2 and 90 vol% Ar is passed through a bypass of the reaction zone at a flow rate of 46.6 sccm for a period of time while an inert gas is passed through the reaction zone. The H2-containing gas is then flowed through the reaction zone at 620°C for 60 seconds. 6. The system is flushed with an inert gas. 7. A hydrocarbon-containing (HC gas) feed having a flow rate of 17.6 sccm and comprising 81 vol% C3H8, 9 vol% inert gas (Ar or Kr) and 10 vol% steam was passed through the bypass of the reaction zone for a period of time while the inert gas was passed through the reaction zone. The hydrocarbon-containing feed was then passed through the reaction zone at 620° C. for 10 minutes. Once the feed was switched from the bypass of the reaction zone to the reaction zone, GC sampling of the reaction effluent was started. The above process steps were repeated cyclically.
[0173] Figure 3 The C3H6 yield and selectivity for catalyst composition 3 are shown (x-axis, time (hours); y-axis, carbon mol %; upper set of data points are C3H6 selectivity; lower set of data points are C3H6 yield). Figure 1 –3 shows that Si leads to rapid deactivation of the catalyst only when Al is present.
[0174] The process steps for using catalyst compositions 4 and 5 are as follows: 1. The system is flushed with an inert gas. 2. A 90% air and 10% H2O mixture at a flow rate of 93.2 sccm is passed through the bypass of the reaction zone while the inert gas is passed through the reaction zone. The reaction zone is heated to a regeneration temperature of 800°C. 3. The 90% air and 10% H2O mixture at a flow rate of 93.2 sccm is then passed through the reaction zone for 1 minute, followed by a flow rate of 83.9 sccm of dry air through the reaction zone for 10 minutes to regenerate the catalyst. 4. The system is flushed with an inert gas. 5. A H2-containing gas containing 10 vol% H2 and 90 vol% Ar is passed through the bypass of the reaction zone at a flow rate of 46.6 sccm for a period of time while the inert gas is passed through the reaction zone. The H2-containing gas is then flowed through the reaction zone at 800°C for 3 seconds. 6. The system is flushed with an inert gas. During this process, the temperature of the reaction zone is varied from 800°C to a reaction temperature of 655°C. 7. A hydrocarbon-containing (HC gas) feed having a flow rate of 17.6 sccm and comprising 81 vol% C3H8, 9 vol% inert gas (Ar or Kr) and 10 vol% steam was passed through the bypass of the reaction zone for a period of time while the inert gas was passed through the reaction zone. The hydrocarbon-containing feed was then passed through the reaction zone at 655° C. for 10 minutes. Once the feed was switched from the bypass of the reaction zone to the reaction zone, GC sampling of the reaction effluent was started. The above process steps were repeated cyclically.
[0175] Figure 4 The average C3H6 yield per cycle versus cycle number is shown for catalyst compositions 4 and 5, respectively (solid circle data points are C3H6 yield for catalyst composition 4; solid square data points are average C3H6 yield for catalyst composition 5). Catalyst composition 5, which includes 0.45 wt% Si, deactivates as the number of cycles increases, while catalyst composition 4, which does not include any Si, does not deactivate.
[0176] List of implementation plans
[0177] The present disclosure may further include the following non-limiting embodiments.
[0178] A1. A method for upgrading hydrocarbons, the method comprising: (I) contacting a hydrocarbon feed with a catalyst composition comprising an element of Group 8 to 10 disposed on a carrier to reform at least a portion of the hydrocarbon feed to produce a coked catalyst composition and a synthesis gas comprising H2 and CO, wherein: the hydrocarbon feed comprises one or more C1-C 16A hydrocarbon and a mixture of H2O, CO2 or H2O and CO2, wherein the hydrocarbon-containing feed and the catalyst composition are contacted at a temperature of 400°C or higher, the carrier comprises Al and at least 0.5wt% of a Group 2 element, the catalyst composition comprises 0.001wt% to 6wt% of a Group 8-10 element, the catalyst composition does not contain Si or contains <0.5wt%, <0.45wt%, <0.4wt%, <0.35wt%, <0.3wt%, <0.25wt%, <0.2wt%, <0.15wt%, <0.1wt%, <0.05wt%, or <0.01wt% Si, wherein all weight percentage values are based on the weight of the carrier.
[0179] A2. The method described in A1 further includes (II) contacting at least a portion of the coked catalyst composition with an oxidant to burn at least a portion of the coke, thereby producing a coke-depleted regenerated catalyst composition and combustion gas.
[0180] A3. The method described in A2 further includes (III) contacting the fuel with the oxidant and the catalyst composition to burn at least a portion of the fuel.
[0181] A4. The method described in A2 or A3, which also includes (IV) contacting an additional amount of the hydrocarbon-containing feed with at least a portion of the regenerated catalyst composition to produce a re-coked catalyst composition and additional effluent.
[0182] A5. The method of any one of A1 to A4, wherein the hydrocarbon-containing feed is contacted with the catalyst composition in a fluidized bed reactor.
[0183] A6. The method of any one of A1 to A4, wherein the hydrocarbon-containing feed is contacted with the catalyst composition in a fixed bed reactor.
[0184] A7. The method of any one of A1 to A4, wherein the hydrocarbon-containing feed is contacted with the catalyst composition in a flow shift reactor.
[0185] A8. The method of any one of A1 to A7, wherein the catalyst composition comprises 0.001wt%, 0.001wt%, 0.01wt%, 0.1wt%, 0.15wt% or 0.2wt% to 0.4wt%, 0.6wt%, 0.8wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt% or 6wt% of the Group 8-10 element, based on the weight of the carrier.
[0186] A9. The method of any one of A1 to A8, wherein the Group 8-10 element comprises Pt.
[0187] A10. The method of any one of A1 to A9, wherein the catalyst composition further comprises a promoter disposed on the carrier and measured at a maximum of 10 wt % based on the weight of the carrier, wherein the promoter comprises Sn, Cu, Au, Ag, Ga, Zn, Ge, In, Re, Ag, a combination thereof, or a mixture thereof.
[0188] A11. The method of any one of A1 to A10, wherein the catalyst composition further comprises an alkali metal element disposed on the carrier, measured at a maximum of 5 wt% based on the weight of the carrier, the alkali metal element comprising Li, Na, K, Rb, Cs, a combination thereof, or a mixture thereof.
[0189] A12. The process of any of A1 to A11, wherein the catalyst composition is in the form of particles having a size and particle density meeting the Geldart A or Geldart B definition of fluidizable solids.
[0190] A13. The method of any one of A1 to A12, wherein the weight ratio of the Group 2 element to Al in the support is in the range of from 0.001, 0.01, 0.1 or 1 to 6, 12.5, 100 or 1,000.
[0191] A14. The method of any one of A1 to A13, wherein: the Group 2 element comprises Mg, and at least a portion of the Mg is in the form of MgO or a mixed metal oxide comprising Mg.
[0192] A15. The method of any one of A1 to A14, wherein: the Group 2 element comprises Mg, and at least a portion of the Mg and at least a portion of the Al are in the form of a mixed Mg / Al metal oxide.
[0193] A16. The method of any one of A1 to A15, wherein: the Group 2 element includes Mg, at least a portion of the Mg and at least a portion of the Al are in the form of a mixed Mg / Al metal oxide, and the weight ratio of Mg to Al in the mixed Mg / Al metal oxide is in the range of from 0.001, 0.01, 0.1 or 1 to 6, 12.5, 100 or 1,000.
[0194] A17. The method of any one of A1 to A16, wherein: at least a portion of the Group 2 elements are in the form of oxides of the Group 2 elements, at least a portion of Al is in the form of Al2O3, and the oxides of the Group 2 elements and Al2O3 are mixed on a nanoscale.
[0195] A18. The method of any one of A1 to A17, wherein: the Group 2 element includes Mg, at least a portion of the Mg is in the form of MgO, at least a portion of the Al is in the form of Al2O3, and the oxides MgO and Al2O3 are mixed on a nanoscale.
[0196] A19. The method of any one of A1 to A18 further includes at least one of the following steps: reacting at least a portion of the synthesis gas in the presence of a Fischer-Tropsch catalyst under effective Fischer-Tropsch conditions to produce an upgraded product, wherein the Fischer-Tropsch catalyst comprises a shift Fischer-Tropsch catalyst or a non-shift Fischer-Tropsch catalyst; subjecting at least a portion of the synthesis gas to a fermentation process to produce alcohols, organic acids or mixtures thereof; contacting at least a portion of the synthesis gas with a catalyst to produce at least one C1-C4 alcohol; and separating H2 from the synthesis gas to produce an H2-rich product.
[0197] B1. A method for preparing a catalyst composition, the method comprising: (I) preparing a slurry or gel comprising Al and / or a compound thereof, a Group 2 element and / or a compound thereof and a liquid medium; and (II) spray drying the slurry or gel to produce spray-dried carrier particles comprising at least Al and a Group 2 element, wherein at least one of the following (i) and (ii) is satisfied: (i) the Group 8-10 element is present in the slurry or gel in the form of a compound containing the Group 8-10 element, and the catalyst composition comprises catalyst particles, the catalyst particles comprising spray-dried carrier particles having the Group 8-10 element disposed thereon, and (ii) spray-dried particles are contacted with a compound containing the Group 8-10 element to produce a spray-dried carrier containing the Group 8-10 element. The invention relates to a catalyst composition comprising a catalyst particle, the catalyst particle comprising a spray-dried carrier particle having a Group 8-10 element disposed thereon, wherein: the catalyst particle comprises 0.001 wt % to 6 wt % of a Group 8-10 element disposed on a carrier, the carrier comprising Al and at least 0.5 wt % of a Group 2 element and containing no Si or containing <0.5 wt %, <0.45 wt %, <0.4 wt %, <0.35 wt %, <0.3 wt %, <0.25 wt %, <0.2 wt %, <0.15 wt %, <0.1 wt %, <0.05 wt % or <0.01 wt % Si, based on the weight of the spray-dried carrier particle.
[0198] B2. The method described in B1, which also includes at least one of the following (iii) and (iv): (iii) a compound containing a promoter element is present in the slurry or gel, and the catalyst composition contains catalyst particles, the catalyst particles containing spray-dried carrier particles having a promoter element disposed thereon, and (iv) the compound containing the promoter element is deposited on the spray-dried carrier particles to produce promoter-containing, spray-dried carrier particles, and the catalyst composition contains catalyst particles, the catalyst particles containing spray-dried carrier particles having a promoter element disposed thereon, wherein: the promoter element contains Sn, Cu, Au, Ag, Ga, Zn, Ge, In, Re, Ag or a combination thereof or a mixture thereof.
[0199] B3. The method of B2, wherein the spray-dried carrier particles contain up to 10 wt % of the promoter element, based on the weight of the spray-dried carrier particles.
[0200] B4. The method described in any one of B1-B3, wherein the compound containing elements of Groups 8 to 10 is present in the slurry or gel.
[0201] B5. The method described in any one of B1-B4, wherein the compound containing elements of Groups 8 to 10 is deposited onto the spray-dried carrier particles.
[0202] B6. The method of any one of B2-B5, wherein the compound containing the promoter element is present in the slurry or gel.
[0203] B7. A method as described in any one of B2-B6, wherein the compound containing the promoter element is deposited onto the spray-dried carrier particles.
[0204] B8. The method described in any one of B1-B7, wherein: the Group 2 element includes Mg, and at least a portion of the Group 2 element and at least a portion of Al in the spray-dried carrier particles are in the form of a mixed Mg / Al metal oxide.
[0205] B9. The method described in any one of B1-B8, which also includes: (III) calcining the spray-dried carrier particles under an oxidizing atmosphere to produce calcined carrier particles, wherein the catalyst composition comprises catalyst particles, the catalyst particles comprising the calcined carrier particles, which contain Al and Group 2 elements and have Group 8-10 elements and optional promoter elements arranged thereon.
[0206] B10. The method described in B9 further includes: (IV) hydrating the calcined carrier particles after step (III) to produce hydrated carrier particles; and (V) calcining the hydrated carrier particles to produce a catalyst composition comprising re-calcined carrier particles, wherein the catalyst particles produced via steps (IV) and (V) have an attrition loss after one hour that is lower than the attrition loss after one hour of the calcined particles produced in step (III), measured according to ASTM D5757-11 (2017).
[0207] Various terms have been defined above. If a term used in a claim is not defined above, it should be given the broadest definition persons in the relevant art have given that term as reflected in at least one printed publication or issued patent. In addition, all patents, test procedures, and other documents cited in this application are fully incorporated by reference to the extent this disclosure is consistent with this application and for all jurisdictions in which such incorporation is permitted.
[0208] While the foregoing is directed to embodiments of the present invention, other and further embodiments of the invention may be devised without departing from the basic scope thereof, and the scope of the invention is determined by the claims that follow.
Claims
1. A catalyst composition comprising 0.001 wt% to 6 wt% of a Group 8-10 element disposed on a carrier, wherein: The support comprises Al and at least 0.5 wt% of a Group 2 element, The catalyst composition contains no Si or <0.5 wt% Si, and All weight percent values are based on the weight of the carrier. 2 . The catalyst composition of claim 1 , wherein a weight ratio of the Group 2 element to Al in the carrier is in the range of from 0.001 to 1,000.
3. The catalyst composition according to claim 1 or claim 2, wherein: Group 2 elements include Mg, and At least a portion of the Mg is in the form of MgO or a mixed metal oxide containing Mg.
4. The catalyst composition according to claim 1 or claim 2, wherein: Group 2 elements include Mg, and At least a portion of the Mg and at least a portion of the Al are in the form of a mixed Mg / Al metal oxide.
5. The catalyst composition of claim 1, wherein: Group 2 elements include Mg, At least a portion of the Mg and at least a portion of the Al are in the form of a mixed Mg / Al metal oxide, and A weight ratio of Mg to Al in the mixed Mg / Al metal oxide ranges from 0.001 to 1,000.
6. The catalyst composition of claim 1 or claim 2, wherein: at least a portion of the Group 2 element is in the form of an oxide of the Group 2 element, At least a portion of the Al is in the form of Al2O3, and The Group 2 element oxide and Al2O3 are mixed on a nanometer scale.
7. The catalyst composition of claim 1 or claim 2, wherein: Group 2 elements include Mg, At least a portion of the Mg is in the form of MgO, At least a portion of the Al is in the form of Al2O3, and The oxides MgO and Al2O3 are mixed on a nanoscale.
8. The catalyst composition of any one of claims 1-7, wherein the catalyst comprises 0.01 wt% to 0.15 wt% of a Group 8-10 element or compound thereof disposed on a support, based on the weight of the support.
9. The catalyst composition of any one of claims 1-8, wherein the Group 8-10 element comprises Pt.
10. The catalyst composition of any one of claims 1-9, further comprising a promoter disposed on a support in an amount of up to 10 wt% based on the weight of the support, wherein the promoter comprises Sn, Cu, Au, Ag, Ga, a combination thereof, or a mixture thereof.
11. The catalyst composition of any one of claims 1 to 10, further comprising an alkali metal element disposed on a carrier in an amount of up to 5 wt% based on the weight of the carrier, comprising Li, Na, K, Rb, Cs, or a combination thereof or a mixture thereof.
12. The catalyst composition of any one of claims 1-11, wherein the catalyst composition is in the form of particles having a size and particle density that conforms to the Geldar t A or Geldar t B definition of a fluidizable solid.
13. A method for preparing a catalyst composition, the method comprising: (I) preparing a slurry or gel comprising Al or a compound thereof, a Group 2 element or a compound thereof, and a liquid medium; (II) spray drying the slurry or gel to produce spray-dried particles comprising Al or a compound thereof and a Group 2 element or a compound thereof; and (III) calcining the spray-dried particles under an oxidizing atmosphere to produce calcined support particles comprising Al or a compound thereof and a Group 2 element or a compound thereof, Wherein at least one of the following (i), (ii) and (iii) is satisfied: (i) the Group 8-10 element is present in the slurry or gel in the form of a compound containing the Group 8-10 element, and the catalyst composition comprises catalyst particles comprising calcined support particles having the Group 8-10 element disposed thereon, (ii) depositing a Group 8-10 element on the spray-dried particles by contacting the spray-dried particles with a compound containing a Group 8-10 element to produce spray-dried particles containing a Group 8-10 element, and the catalyst composition comprises catalyst particles comprising calcined support particles having the Group 8-10 element disposed thereon, and (iii) depositing a Group 8-10 element on the calcined support particles by contacting the calcined support particles with a compound containing a Group 8-10 element to produce a calcined support particle containing a Group 8-10 element, and the method further comprises (IV) calcining the calcined support particle containing a Group 8-10 element to produce a re-calcined support particle having the Group 8-10 element disposed thereon, wherein the catalyst composition comprises the re-calcined support particle, wherein: The catalyst particles contain Group 8-10 elements in an amount of 0.001 wt % to 6 wt %, The catalyst particles contain at least 0.5 wt% of a Group 2 element, The catalyst composition contains no Si or <0.5 wt% Si, and All weight percent values are based on the weight of the calcined support particles or the re-calcined support particles.
14. The method of claim 13, wherein at least one of the following (iv), (v) and (vi) is satisfied: (iv) a compound comprising a promoter element is present in the slurry or gel and the catalyst composition comprises catalyst particles comprising calcined support particles having the promoter element disposed thereon, (v) depositing a compound comprising a promoter element on the spray-dried particles to produce promoter-containing spray-dried particles, and the catalyst composition comprises catalyst particles comprising calcined support particles having the promoter element disposed thereon, and (vi) depositing a compound comprising a promoter element on the calcined support particles to produce promoter-containing calcined support particles, and the method further comprises (v) calcining the promoter-containing calcined support particles to produce re-calcined support particles having the promoter element disposed thereon, wherein the catalyst composition comprises the re-calcined support particles, wherein: The promoter element comprises Sn, Cu, Au, Ag, Ga, a combination thereof or a mixture thereof, and The catalyst particles contain promoter elements in an amount of up to 10 wt %, based on the weight of the calcined support particles or the re-calcined support particles.
15. The method of claim 13 or claim 14, wherein the spray-dried particles are calcined at a temperature in the range of 550°C to 900°C for a time of ≤ 45 minutes.
16. The method of claim 13 or claim 14, wherein the spray-dried particles are calcined at a temperature of <550°C for a time of ≤45 minutes.
17. The method of any one of claims 13 to 16, wherein the compound containing elements of Groups 8 to 10 is present in the slurry or the gel.
18. The method of any one of claims 13-17, wherein the compound containing Group 8-10 elements is deposited on the spray-dried particles.
19. The method of any one of claims 14 to 18, wherein the compound comprising a promoter element is present in the slurry or the gel.
20. The method of any one of claims 14-19, wherein the compound comprising a promoter is deposited on the spray-dried particles.
21. The method of any one of claims 13-20, further comprising: (IV) hydrating the calcined support particles after step (III) to produce hydrated support particles; and (V) calcining the hydrated support particles to produce a catalyst comprising re-calcined support particles, wherein the catalyst particles produced via steps (IV) and (V) have an attrition loss after one hour that is lower than the attrition loss after one hour of the calcined particles produced in step (III), as measured according to ASTM D5757-11 (2017).
22. The method of any one of claims 13-21, wherein: Group 2 elements include Mg, and At least a portion of the Group 2 element and at least a portion of the Al are in the form of a mixed Mg / Al metal oxide.
23. A method for upgrading hydrocarbons, the method comprising: (I) contacting a hydrocarbonaceous feed with a catalyst composition comprising a Group 8-10 element disposed on a support to perform one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the hydrocarbonaceous feed to produce a coked catalyst composition and an effluent comprising one or more upgraded hydrocarbons and molecular hydrogen, wherein: The hydrocarbon feed comprises C2-C 16 One or more linear or branched alkanes or C4-C 16 One or more cycloalkanes or C8-C 16 One or more of alkyl aromatic hydrocarbons or mixtures thereof, The hydrocarbonaceous feed and the catalyst composition are contacted at a temperature in the range of 300° C. to 900° C. under a hydrocarbon partial pressure of at least 20 kPa absolute for a period of time of ≤ 3 hours, wherein the hydrocarbon partial pressure is any C2-C 16 Alkanes and any C8-C 16 The total partial pressure of alkyl aromatics, The support comprises Al and at least 0.5 wt % of a Group 2 element, The catalyst composition comprises an element of Group 8 to 10 in an amount of 0.001 wt % to 6 wt %, The catalyst composition contains no Si or contains <0.5 wt% Si, All weight percentage values are based on the weight of the carrier, and The one or more upgraded hydrocarbons include at least one of dehydrogenated hydrocarbons, dehydroaromatized hydrocarbons, and dehydrocyclized hydrocarbons.
24. The method of claim 23, further comprising: (II) contacting at least a portion of the coked catalyst with an oxidant to effect combustion of at least a portion of the coke to produce a coke-depleted regenerated catalyst and combustion gases; and (III) contacting an additional amount of hydrocarbon-containing feed with at least a portion of the regenerated catalyst to produce a recoked catalyst and an additional effluent, wherein the cycle time from contacting the hydrocarbon-containing feed with the catalyst particles in step (I) to contacting the additional amount of hydrocarbon-containing feed with the regenerated catalyst in step (III) is ≤ 5 hours.
25. The method of claim 23 or claim 24, wherein: Group 2 elements include Mg, and At least a portion of the Group 2 element and at least a portion of the Al are in the form of a mixed Mg / Al metal oxide.
Citation Information
Patent Citations
Dehydrogenation catalyst and process
CN102741200A
Dehydrogenation catalyst and process
CN106238045A
Method for preparation of light alkene by dehydrogenation from relative paraffin
CN1098399A
Processes for Upgrading Alkanes and Alkyl Aromatic Hydrocarbons
US20210276002A1
Processes for Upgrading Alkanes and Alkyl Aromatic Hydrocarbons
US20210276932A1