Optical laminate and method for manufacturing optical laminate
By adopting a combined structure of a transparent layer, a porous layer and an adhesive layer in the optical laminate, the problems of thinning and optical performance maintenance of the optical laminate in the prior art are solved, and the effects of thinning thickness and excellent performance are achieved. .
Patent Information
- Application Number
- CN202380028977.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-02-27
- Publication Date
- 2024-11-05
Smart Images

Figure CN118900764A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical layered body and a method for producing the optical layered body. Background Art
[0002] It is known that an optical laminate including a low refractive index layer having a refractive index lower than that of the light guide plate is pasted on a light guide plate for propagating light so as to arbitrarily control the propagation of light in the light guide plate. Currently, research is being conducted on patterning such a low refractive index layer to give the optical laminate a light extraction function. For example, an optical laminate is proposed, which comprises a substrate and a variable refractive index extraction layer disposed on the substrate, and the variable refractive index extraction layer comprises a first region selectively printed with a first substance having a relatively small refractive index, and a second region formed by coating the first substance with a second substance having a relatively large refractive index (for example, refer to patent document 1). The optical laminate described in patent document 1 forms an adhesive layer on the surface of the substrate on the opposite side of the variable refractive index extraction layer, and is pasted to the light guide plate through the adhesive layer. In recent years, the uses of optical products having light guide plates have been continuously diversified, and it is desired to miniaturize optical products and then thin the optical laminate pasted on the light guide plate. However, the optical laminate described in patent document 1 comprises a substrate selectively printed with a first substance, and it is difficult to achieve the thinning of the optical laminate. Although studies have been conducted on thinning the substrate or peeling and removing the substrate from the variable refractive index extraction layer, it is difficult to thin the substrate from the viewpoint of manufacturing stability of the optical laminate, and if the substrate is peeled off, the variable refractive index extraction layer may be damaged. In addition, if the substrate is peeled off and an adhesive layer is directly provided on the variable refractive index extraction layer, the optical performance of the variable refractive index extraction layer cannot be fully maintained.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2014 / 031726 Summary of the invention
[0006] Technical problem to be solved by the invention
[0007] The present invention has been made to solve the above-mentioned conventional problems, and a main object of the present invention is to provide an optical layered body and a method for producing the optical layered body which can achieve a reduced thickness and maintain excellent optical performance.
[0008] Technical solutions for solving technical problems
[0009] The optical laminate of an embodiment of the present invention comprises: a transparent layer having a thickness of 20 μm or less; a porous layer directly provided on one side of the transparent layer in a thickness direction in a predetermined pattern and having a refractive index of 1.25 or less; an adhesive layer arranged on the opposite side of the porous layer relative to the transparent layer and in contact with the transparent layer; and an adhesive layer arranged on the opposite side of the adhesive layer relative to the transparent layer and covering the porous layer.
[0010] In one embodiment, the transparent layer has a barrier function of suppressing the penetration of components constituting the adhesive layer into the porous layer.
[0011] In one embodiment, the porosity of the transparent layer is smaller than the porosity of the porous layer.
[0012] In one embodiment, the adhesive layer has an elastic modulus of 1.0×10 5 (Pa) or more adhesive composition.
[0013] Another aspect of the present invention is a method for manufacturing an optical laminate, which includes: a step of forming a transparent layer having a thickness of less than 20 μm on a substrate; a step of patterning a porous layer having a refractive index of less than 1.25 on the surface of the transparent layer opposite to the substrate; a step of forming an adhesive layer from the side opposite to the transparent layer to cover the porous layer; a step of peeling the substrate from the transparent layer; and a step of forming an adhesive layer on the surface of the transparent layer opposite to the porous layer.
[0014] In one embodiment, a peeling force when the substrate is peeled from the transparent layer is 1 N / 25 mm or less.
[0015] Effects of the Invention
[0016] According to the embodiment of the present invention, an optical layered body that can achieve a reduced thickness and maintain excellent optical performance can be realized. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention.
[0018] Figure 2 Yes Figure 1 A schematic cross-sectional view of an optical product of an optical laminate.
[0019] Figure 3 (a)~ Figure 3 (e) is a schematic cross-sectional view for explaining a method for producing an optical layered body according to one embodiment of the present invention. DETAILED DESCRIPTION
[0020] Embodiments of the present invention will be described below, but the present invention is not limited to these embodiments. First, the overall structure of the optical layered body will be described in outline, and then the components of the optical layered body will be described in detail.
[0021] A. Overall structure of optical laminate
[0022] Figure 1 is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention; Figure 2 Yes Figure 1 A schematic cross-sectional view of an optical product of an optical laminate. The optical laminate 100 shown in the figure comprises: a transparent layer 1 having a thickness of 20 μm or less; a porous layer 2 directly disposed on one side of the transparent layer 1 in a thickness direction in a predetermined pattern and having a refractive index of 1.25 or less; an adhesive layer 4 disposed on the opposite side of the porous layer 2 relative to the transparent layer 1 and in contact with the transparent layer 1; and an adhesive layer 3 disposed on the opposite side of the adhesive layer 4 relative to the transparent layer 1 and covering the porous layer 2. In this configuration, the transparent layer is disposed between the porous layer and the adhesive layer, and the thickness of the transparent layer is 20 μm or less, so that the thickness of the optical laminate can be reduced, and the refractive index of the porous layer can be maintained below the above upper limit. Therefore, the excellent optical performance of the optical laminate can be fully maintained. The thickness of the transparent layer 1 is preferably 10 μm or less, more preferably 5 μm or less, further preferably 4 μm or less, and typically 0.1 μm or more. The porous layer 2 typically has voids inside. The refractive index of the porous layer 2 is preferably less than 1.20, more preferably 1.19 or less, further preferably 1.18 or less, and typically 1.10 or more. Unless otherwise specified, the refractive index refers to the refractive index measured at a wavelength of 550 nm.
[0023] In one embodiment, a portion of one side in the thickness direction of the transparent layer 1 may be exposed from the porous layer 2. The exposed portion is in contact with the adhesive layer 3. Therefore, the adhesive layer 3 is in contact with the porous layer 2 and the transparent layer 1. Thus, it is possible to suppress the peeling of the transparent layer 1 relative to the porous layer 2 during the handling of the laminate before processing. The refractive index of the adhesive layer 3 is typically greater than the refractive index of the porous layer 2. The refractive index of the adhesive layer 3 exceeds 1.25, preferably is 1.4 or more, and is typically 1.7 or less.
[0024] In one embodiment, the transparent layer 1 is a barrier layer 1a having a barrier function to inhibit the components constituting the adhesive layer 4 from penetrating into the porous layer 2. Therefore, the increase in the refractive index of the porous layer can be stably inhibited. The adhesive layer 4 may be a pressure-sensitive adhesive layer or an adhesive layer.
[0025] In one embodiment, the porosity of the transparent layer 1 is smaller than that of the porous layer 2. With this configuration, the barrier performance of the transparent layer 1 can be sufficiently ensured, and the adhesive or pressure-sensitive adhesive constituting the adhesive layer can be stably prevented from entering the voids of the porous layer.
[0026] The porosity of the transparent layer 1 is, for example, less than 15% by volume, preferably less than 10% by volume, and the lower limit is, for example, more than 1% by volume. The porosity of the porous layer 2 is, for example, more than 10% by volume, preferably more than 20% by volume, more preferably more than 30% by volume, and more preferably more than 35% by volume, and for example, less than 60% by volume, preferably less than 55% by volume, more preferably less than 50% by volume, and more preferably less than 45% by volume. If the porosity is within this range, the refractive index of the porous layer can be set to an appropriate range, and the specified mechanical strength can be ensured. The porosity is the value of the porosity calculated by the Lorentz-Lorenz's formula based on the value of the refractive index measured by the ellipsometer.
[0027] In one embodiment, the adhesive layer 3 has an elastic modulus of 1.0×10 5 The elastic modulus of the adhesive constituting the adhesive layer 3 at 23° C. is preferably 1.1×10 5 (Pa) or more, more preferably 1.2×10 5 (Pa) or more. If the elastic modulus of the adhesive is above the above lower limit, the adhesive constituting the adhesive layer can be inhibited from entering the voids of the porous layer. Therefore, the increase in the refractive index of the porous layer can be more stably inhibited. The elastic modulus is determined by reading the value at 23°C when measured at a temperature increase rate of 5°C / min in the range of -50°C to 150°C under a frequency of 1 Hz according to the method described in JIS K7244-1 "Plastics-Test methods for dynamic mechanical properties". The upper limit of the elastic modulus of the adhesive constituting the adhesive layer 3 at 23°C is typically 100×10 5 (Pa) or less.
[0028] The transparent layer, the porous layer, the adhesive layer, and the pressure-sensitive adhesive layer are described in detail below.
[0029] B. Transparent layer
[0030] The transparent layer 1 allows light to pass through. The total light transmittance of the transparent layer 1 is, for example, 70% to 100%, preferably 80% to 99%. If the total light transmittance of the transparent layer is within the above range, excellent transparency of the entire optical laminate can be achieved. As a result, adverse effects in the use of the optical laminate can be suppressed.
[0031] As long as light can be transmitted, the transparent layer 1 can adopt any appropriate structure. As the transparent layer 1, for example, resin films and inorganic films can be listed. As the material of the resin film, for example, there can be listed: polyvinyl alcohol (PVA); (meth) acrylic resins such as polymethyl methacrylate (PMMA); polyvinyl acetal resins; thermoplastic resin materials with polar groups such as polycarbonate resins, polyarylate resins, and polyurethane resins; acrylic hard coating resin materials, epoxy hard coating resin materials, silicone hard coating resin materials and other heat or UV (Ultraviolet) curable resin materials. In addition, (meth) acrylic refers to acrylic and / or methacrylic. The material of the resin film can be used alone or in combination. In addition, the above-mentioned resin film can be composed of resin alone, and other substances can also be added to change the physical properties of the above-mentioned resin film. Specifically, it can be mentioned that a boric acid compound or a silane compound is added to introduce a cross-linked structure into PVA.
[0032] Examples of materials for the inorganic thin film include SiO2, ZTO (zinc tin oxide), ITO (indium tin oxide), IZO (indium zinc oxide), TiO2, Si, ZnO, AZO (aluminum zinc oxide), Al2O3, MgO, MgF2, and SiN. The materials for the inorganic thin film may be used alone or in combination.
[0033] C. Porous layer
[0034] The porous layer 2 is directly disposed on one side of the transparent layer 1 in the thickness direction and has a predetermined pattern shape. The porous layer 2 typically has a plurality of openings 21 defining the pattern. In one embodiment, the porous layer 2 has a gradient pattern in which the opening ratio per unit area increases as it moves toward a predetermined direction orthogonal to the thickness direction of the transparent layer 1. The openings 21 may have any appropriate shape and size. In the case where the porous layer 2 has a gradient pattern, the openings 21 of the same size may be distributed in a manner that becomes sparse as it moves toward a predetermined direction, or the size of the openings 21 may be changed in a manner that becomes larger as it moves toward a predetermined direction.
[0035] The total light transmittance of the porous layer 2 is, for example, 85% to 99%, preferably 87% to 98%, and more preferably 89% to 97%. The haze of the porous layer 2 is, for example, less than 5%, preferably less than 3%. On the other hand, the haze is, for example, 0.1% or more, preferably 0.2% or more. By arranging such a porous layer at a predetermined position, excellent transparency of the entire optical laminate can be achieved. The haze can be measured, for example, by the following method.
[0036] The void layer (porous layer) was cut into a size of 50 mm×50 mm, and placed in a haze meter (manufactured by Murakami Color Research Laboratory: HM-150) to measure the haze value. The haze value was calculated by the following formula.
[0037] Haze (%) = [diffuse transmittance (%) / total light transmittance (%)] × 100 (%)
[0038] The thickness of the porous layer 2 is, for example, 30 nm to 5 μm, preferably 200 nm to 4 μm, more preferably 400 nm to 3 μm, and further preferably 600 nm to 2 μm. If the thickness of the porous layer is within this range, the porous layer can effectively exhibit a total reflection function for light in the visible to infrared regions.
[0039] As long as it has the above-mentioned required characteristics, the porous layer 2 can adopt any appropriate structure. The porous layer is preferably formed by coating or printing. As the material constituting the porous layer, for example, the materials described in International Publication No. 2004 / 113966, Japanese Patent Publication No. 2013-254183, and Japanese Patent Publication No. 2012-189802 can be used. As a representative example, silicon compounds can be listed. As silicon compounds, for example: silicon dioxide compounds; hydrolyzable silanes, and their partial hydrolyzates and dehydrated condensates; silicon compounds containing silanol groups; active silica obtained by contacting silicates with acids or ion exchange resins. Also listed: organic polymers; polymerizable monomers (such as (meth) acrylic monomers and styrene monomers); curable resins (such as (meth) acrylic resins, fluorine-containing resins, and urethane resins). These materials can be used alone or in combination. The porous layer can be formed by applying or printing a solution or dispersion of such a material.
[0040] The size of the void (pore) in the porous layer refers to the major axis diameter of the void (pore) and the major axis diameter of the minor axis diameter. The size of the void (pore) is, for example, 2nm to 500nm. The size of the void (pore) is, for example, more than 2nm, preferably more than 5nm, more preferably more than 10nm, and further preferably more than 20nm. On the other hand, the size of the void (pore) is, for example, less than 500nm, preferably less than 200nm, and more preferably less than 100nm. The range of the size of the void (pore) is, for example, 2nm to 500nm, preferably 5nm to 500nm, more preferably 10nm to 200nm, and further preferably 20nm to 100nm. The size of the void (pore) can be adjusted to the desired size according to the purpose and use.
[0041] The size of the voids (pores) can be quantified by the BET (Brunauer-Emmett-Teller) test method. Specifically, after 0.1 g of sample (the void layer formed) is put into the capillary of the specific surface area measuring device (manufactured by Micromeritics: ASAP2020), it is dried under reduced pressure at room temperature for 24 hours to degas the gas in the void structure. In addition, the adsorption isotherm is drawn by adsorbing nitrogen on the above sample to obtain the pore distribution. In this way, the void size can be evaluated.
[0042] As the porous layer having voids inside, for example, a porous layer having a porous layer and / or an air layer in at least a portion thereof can be cited. The porous layer typically includes aerogel and / or particles (e.g., hollow microparticles and / or porous particles). The porous layer can preferably be a nanoporous layer (specifically, a layer in which 90% or more of the micropores have a diameter of 10 -1 nm~10 3 nm range).
[0043] As the above-mentioned particles, any appropriate particles can be used. The particles are typically composed of silica-based compounds. As the shape of the particles, for example, spherical, plate-like, needle-like, string-like, and grape-like shapes can be listed. As string-like particles, for example, multiple particles with spherical, plate-like, or needle-like shapes are strung together to form beads, short-fiber particles (for example, short-fiber particles described in Japanese Patent Gazette No. 2001-188104), and combinations thereof can be listed. The string-like particles can be linear or branched. As grape-like particles, for example, multiple spherical, plate-like, and needle-like particles are agglomerated to form grape-like strings. The shape of the particles can be confirmed, for example, by observation with a transmission electron microscope.
[0044] An example of the specific composition of the porous layer is described below. The porous layer of this embodiment is composed of one or more structural units that form a fine void structure, and the structural units are chemically bonded to each other via catalysis. As the shape of the structural unit, for example, particles, fibers, rods, and plates can be listed. The structural unit can have only one shape, or it can have a combination of more than two shapes. The following mainly describes the case where the porous layer is a void layer of a porous body in which the above-mentioned fine pore particles are chemically bonded to each other.
[0045] In the void layer forming process, such a void layer can be formed, for example, by chemically bonding microporous particles (porous particles) to each other. In addition, in an embodiment of the present invention, the shape of the "particles" (such as the above-mentioned microporous particles) is not particularly limited, for example, it can be spherical or other shapes. In addition, in an embodiment of the present invention, the above-mentioned microporous particles can be, for example, sol-gel beaded particles, nanoparticles (hollow nano-silica / nano-balloon particles), nanofibers, etc. The microporous particles typically include inorganic substances. As specific examples of inorganic substances, silicon (Si), magnesium (Mg), aluminum (Al), titanium (Ti), zinc (Zn), and zirconium (Zr) can be listed. These can be used alone or in combination of two or more. In one embodiment, the above-mentioned microporous particles are, for example, microporous particles (porous particles) of silicon compounds, and the above-mentioned porous body is, for example, an organosilicon porous body. The microporous particles of the above-mentioned silicon compound, for example, include a pulverized body of a gel-like silicon compound. In addition, as another form of a porous layer having a porous layer and / or an air layer in at least a portion, there is, for example, a void layer: a fibrous substance such as nanofibers, and the fibrous substances are entangled with each other to form voids and form a layer. The method for manufacturing such a void layer is not particularly limited, for example, it is the same as the case of the void layer of a porous body in which the above-mentioned fine pore particles are chemically bonded to each other. As another form, a void layer using hollow nanoparticles or nanoclays, a void layer formed using hollow nano balloons or magnesium fluoride can be listed. The void layer can be a void layer composed of a single constituent substance, or it can be a void layer composed of multiple constituent substances. The void layer can be composed of a single form mentioned above, or it can be composed of multiple forms mentioned above.
[0046] In the present embodiment, the porous structure of the porous body may be, for example, a continuous bubble structure in which the pore structure is continuous. The continuous bubble structure refers, for example, to a state in which the pore structure is three-dimensionally connected in the above-mentioned organic silicon porous body, or it can be said that the internal voids of the pore structure are continuous. The porous body has a continuous bubble structure, and the porosity can be increased. However, in the case of using single bubble particles (particles each having a pore structure) such as hollow silica, a continuous bubble structure cannot be formed. On the other hand, for example, in the case of using silica sol particles (a crushed product of a gel-like silicon compound forming a sol), since the particles have a three-dimensional tree-like structure, a continuous bubble structure can be easily formed by sedimenting and depositing the tree-like particles in a coating film (a coating film of a sol containing a crushed product of a gel-like silicon compound). The porous layer is more preferably a monolithic structure having a continuous bubble structure including a plurality of pores distributed therein. The monolithic structure refers, for example, to a structure including a structure having nano-sized fine voids, and a hierarchical structure of a continuous bubble structure formed by the nano-voids. In the case of forming a monolithic structure, for example, fine voids can be used to impart membrane strength, and coarse connected bubble voids can be used to impart a high porosity, thereby achieving both membrane strength and high porosity. Such a monolithic structure is preferably formed by controlling the pore distribution of the generated void structure in the gel (gel-like silicon compound) in the previous stage of crushing into silica sol particles. In addition, for example, when crushing the gel-like silicon compound, the particle size distribution of the crushed silica sol particles can be controlled to a desired size to form a monolithic structure.
[0047] The porous layer contains, for example, a pulverized product of a gel-like compound as described above, and the pulverized products are chemically bonded to each other. The form of chemical bonding (chemical bonding) between the pulverized products in the porous layer is not particularly limited, and examples thereof include cross-linking, covalent bonding, and hydrogen bonding.
[0048] The volume average particle size of the above-mentioned pulverized material in the porous layer is, for example, 0.05 μm or more, preferably 0.10 μm or more, and more preferably 0.11 μm or more. On the other hand, the volume average particle size is, for example, 1.00 μm or less, preferably 0.90 μm or less, and more preferably 0.50 μm or less. The range of the volume average particle size is, for example, 0.05 μm to 1.00 μm, preferably 0.10 μm to 0.90 μm, and more preferably 0.11 μm to 0.55 μm. The particle size distribution can be measured, for example, by a particle size distribution evaluation device such as a dynamic light scattering method and a laser diffraction method, and an electron microscope such as a scanning electron microscope (SEM) and a transmission electron microscope (TEM). In addition, the volume average particle size is an indicator of the deviation of the particle size of the pulverized material.
[0049] The type of the gel-like compound is not particularly limited. Examples of the gel-like compound include gel-like silicon compounds.
[0050] In addition, in the porous layer (void layer), for example, the silicon atoms contained therein are preferably siloxane-bonded. As a specific example, the proportion of unbonded silicon atoms (i.e., residual silanol) in all silicon atoms contained in the void layer is, for example, less than 50%, preferably less than 30%, and more preferably less than 15%.
[0051] D. Adhesive layer
[0052] The adhesive layer 4 is described in detail later and is provided in order to adhere the optical laminate 100 to an optical component (representatively a light guide plate 10). The adhesive layer 4 is provided on the surface of the transparent layer 1 opposite to the porous layer 2. Since the adhesive layer 4 is not in contact with the porous layer 2, there is no particular restriction on its composition, and any appropriate composition can be adopted. As described above, the adhesive layer 4 can be an adhesive layer or an adhesive layer. When the adhesive layer 4 is an adhesive layer, the adhesive layer 3 is set as the first adhesive layer 3, and the adhesive layer 4 is set as the second adhesive layer 4a to distinguish them.
[0053] Examples of the adhesive constituting the second adhesive layer 4 a include a (meth)acrylic adhesive. The thickness of the second adhesive layer 4 a is, for example, 5 μm or more and 200 μm or less, and preferably 100 μm or less.
[0054] Examples of the adhesive constituting the adhesive layer include a thermosetting adhesive and an ultraviolet curing adhesive. The thickness of the adhesive layer is, for example, 0.1 μm or more and 200 μm or less.
[0055] E. Adhesive layer (first adhesive layer)
[0056] The adhesive layer 3 is described in detail below and is provided for attaching the optical laminate 100 to an optical component. That is, the optical laminate 100 has a double-sided adhesive structure capable of connecting two optical components. In one embodiment, the adhesive layer 3 covers the porous layer 2 in an embedded manner and contacts the transparent layer 1 via the opening 21 possessed by the porous layer 2.
[0057] As the adhesive constituting the adhesive layer 3, any appropriate adhesive can be used as long as it has the characteristics as described above. As an adhesive, an acrylic adhesive (acrylic adhesive composition) can be representatively cited. The acrylic adhesive composition typically contains a (meth) acrylic polymer as a main component (base polymer). In the solid content of the adhesive composition, the (meth) acrylic polymer can be contained in the adhesive composition at a ratio of, for example, 50% by mass or more, preferably 70% by mass or more, and more preferably 90% by mass or more. The (meth) acrylic polymer contains an alkyl (meth) acrylate as a monomer unit as a main component. In addition, (meth) acrylate refers to acrylate and / or methacrylate. As the alkyl of the alkyl (meth) acrylate, for example, a linear or branched alkyl having 1 to 18 carbon atoms can be cited. The average carbon number of the alkyl is preferably 3 to 9. As monomers constituting the (meth) acrylic polymer, in addition to the alkyl (meth) acrylate, copolymer monomers such as carboxyl-containing monomers, hydroxyl-containing monomers, amide-containing monomers, aromatic ring-containing (meth) acrylates, and heterocyclic (meth) acrylates can also be cited. The comonomer is preferably a hydroxyl-containing monomer and / or a heterocyclic (meth)acrylate, more preferably N-acryloylmorpholine. The acrylic adhesive composition preferably contains a silane coupling agent and / or a crosslinking agent. As the silane coupling agent, for example, epoxy-containing silane coupling agents can be cited. As the crosslinking agent, for example, isocyanate crosslinking agents and peroxide crosslinking agents can be cited. The details of such an adhesive layer or acrylic adhesive composition are described, for example, in Patent No. 4140736, and the description of the patent gazette is cited in this specification by reference.
[0058] The thickness of the pressure-sensitive adhesive layer 3 is, for example, 3 μm to 30 μm, or preferably 5 μm to 10 μm. When the thickness of the pressure-sensitive adhesive layer is within such a range, sufficient adhesion can be achieved and the optical laminate can be made thinner.
[0059] F. Method for producing an optical laminate
[0060] Next, a method for producing an optical layered body according to one embodiment will be described.
[0061] Figure 3 (a)~ Figure 3 (e) is a schematic cross-sectional view for explaining a method for producing an optical layered body according to one embodiment of the present invention.
[0062] A method for manufacturing an optical laminate according to one embodiment includes: a step of forming a transparent layer 1 having a thickness of less than 20 μm on a substrate 5; a step of patterning a porous layer 2 having a refractive index of less than 1.25 on a surface of the transparent layer 1 opposite to the substrate 5; a step of forming an adhesive layer 3 from the opposite side of the transparent layer 1 to cover the porous layer 2; a step of peeling the substrate 5 from the transparent layer 1; and a step of forming an adhesive layer 4 on a surface of the transparent layer 1 opposite to the porous layer 2.
[0063] In this method, Figure 3 As shown in (a), first, the transparent layer 1 is formed on the substrate 5 by any appropriate method. The substrate 5 is not particularly limited in its composition as long as it can support the transparent layer 1 and the porous layer 2 in a manner that the patterned formation of the porous layer 2 can be stably implemented. As the substrate 5, any appropriate resin film can be used. Specific examples of materials that serve as the main component of the resin film include: cellulose resins such as triacetyl cellulose (TAC); polyester resins such as polyethylene terephthalate (PET); polyvinyl alcohol; polycarbonate; polyamide; polyimide; polyether sulfone; polysulfone; polystyrene; polynorbornene; polyolefin; (meth)acrylic; acetate. In addition, thermosetting resins or ultraviolet curing resins such as (meth)acrylic, urethane, (meth)acrylic urethane, epoxy, and silicone can also be listed. An inorganic thin film such as a copper oxide film can be provided on the surface of the substrate 5.
[0064] The thickness of the substrate 5 is, for example, more than 5 μm, preferably 10 μm or more, and, for example, 100 μm or less.
[0065] When the transparent layer 1 is composed of a resin film, a solution containing a material of the resin film is applied to the substrate 5 and then the coating is dried to form the transparent layer 1 (resin film). Alternatively, a separately prepared transparent layer (resin film) may be attached to the substrate.
[0066] When the transparent layer 1 is composed of an inorganic thin film, the inorganic thin film material is formed on the substrate 5 by a film forming method such as sputtering to form the transparent layer 1 (inorganic thin film).
[0067] Then, if Figure 3 As shown in (b), the porous layer 2 is patterned on the surface of the transparent layer 1 opposite to the substrate 5 by any appropriate method. That is, the porous layer 2 is patterned on the transparent layer 1 in a state where the transparent layer 1 is supported by the substrate 5. Therefore, the patterning of the porous layer 2 can be stably performed.
[0068] In one embodiment, the process typically includes: a precursor forming step of forming a void structure as a precursor of a porous layer (void layer) on a transparent layer; and a cross-linking reaction step of causing a cross-linking reaction inside the precursor after the precursor forming step. The process further includes a liquid preparation step of making a liquid containing microporous particles (hereinafter sometimes referred to as "microporous particle-containing liquid" or simply "containing liquid"), and a drying step of drying the liquid containing liquid. In the precursor forming step, the microporous particles in the dried body are chemically bonded to each other to form a precursor. The containing liquid is not particularly limited, for example, it is a suspension containing microporous particles. In addition, the following mainly describes the case where the microporous particles are a pulverized product of a gel-like compound, and the void layer is a porous body (preferably a silicone porous body) containing a pulverized product of a gel-like compound. However, in the case where the microporous particles are other than a pulverized product of a gel-like compound, the porous layer can also be formed in the same manner.
[0069] According to the above method, for example, a porous layer (void layer) having a very low refractive index can be formed. The reason for this is, for example, presumed as follows. However, this presumption does not limit the method for forming the porous layer.
[0070] The above-mentioned crushed material is a compound obtained by crushing a gel-like silicon compound, so the three-dimensional structure of the gel-like silicon compound before crushing is in a state of being dispersed into a three-dimensional basic structure. Furthermore, in the above-mentioned method, by coating or printing the crushed material of the gel-like silicon compound on a transparent layer, a precursor of a porous structure based on a three-dimensional basic structure can be formed. That is, according to the above-mentioned method, a new porous structure (three-dimensional basic structure) obtained by coating the crushed material, which is different from the three-dimensional structure of the gel-like silicon compound, can be formed. Therefore, in the void layer finally obtained, for example, a low refractive index that functions to the same extent as the air layer can be achieved. Furthermore, in the above-mentioned method, since the crushed materials are chemically bonded to each other, the three-dimensional basic structure is fixed. Therefore, although the void layer finally obtained is a structure with voids, sufficient strength and flexibility can be maintained. The specific composition and formation method of the porous layer are described, for example, in International Publication No. 2019 / 151073. The records of the gazette are cited in this specification by reference.
[0071] In one embodiment, this step is performed by printing the microporous particle-containing liquid in a predetermined pattern. Examples of the printing method include inkjet printing, gravure printing, and screen printing.
[0072] Then, if Figure 3As shown in (c), an adhesive layer 3 covering the porous layer 2 is formed by any appropriate method. In one embodiment, the adhesive constituting the adhesive layer 3 is applied to a resin film and dried, and after the adhesive layer 3 is formed on the resin film, the adhesive layer 3 is attached to the porous layer 2 and the transparent layer 1 in a manner such that the porous layer 2 is embedded.
[0073] Then, if Figure 3 As shown in (d), the substrate 5 is peeled off from the transparent layer 1. The peeling force when the substrate 5 is peeled off from the transparent layer 1 is preferably 1 N / 25 mm or less, more preferably 0.8 N / 25 mm or less. The peeling force is measured, for example, by the following method.
[0074] The laminated film of the substrate 5 and the transparent layer 1 is sampled in the form of short strips of 50 mm × 140 mm, and the substrate 5 side of the sample is fixed to a glass plate with a double-sided tape. An acrylic adhesive layer (thickness 20 μm) is attached to a PET film (T100: manufactured by Mitsubishi Resin Film Co., Ltd.), and an adhesive tape piece cut into 25 mm × 100 mm is attached to the transparent layer side of the laminated film to be laminated with the PET film. Next, the sample is clamped in an Autograph tensile testing machine (manufactured by Shimadzu Corporation: AG-Xplus) with a distance of 100 mm between the chucks, and then a tensile test is performed at a tensile speed of 0.3 m / min. The average test force of the 50 mm peel test is set as the adhesive peel strength, i.e., the adhesive force. In addition, the bonding force can also be measured by the same measurement method. In the present invention, there is no clear distinction between "adhesive force" and "adhesive force".
[0075] In one embodiment, since the pressure-sensitive adhesive layer 3 is in contact with the transparent layer 1 via the openings 21 of the porous layer 2 , it is possible to suppress the transparent layer 1 from being peeled off from the porous layer 2 as the substrate 5 is peeled off.
[0076] Then, if Figure 3 As shown in (e), an adhesive layer 4 is formed on the surface of the transparent layer 1 opposite to the porous layer 2 by any appropriate method. In one embodiment, a binder or adhesive constituting the adhesive layer 4 is applied to a resin film and dried, and after the adhesive layer 4 is formed on the resin film, the adhesive layer 4 is attached to the transparent layer 1. Alternatively, a binder or adhesive may be applied to the transparent layer and dried to form the adhesive layer.
[0077] In the above manner, an optical laminate having a structure of pressure-sensitive adhesive layer / porous layer / transparent layer / adhesive layer is produced.
[0078] G. Use of optical laminate
[0079] The optical laminate according to the embodiment of the present invention can be typically applied to an optical product 200 having a light guide plate 10, and can extract light propagating in the light guide plate 10 to another optical component. Figure 2 As shown, the optical laminate 100 is bonded to the light guide plate 10 via the adhesive layer 4. Although not shown, other optical components are bonded to the adhesive layer 3 of the optical laminate 100.
[0080] The light guide plate 10 may be typically arranged in a predetermined direction ( Figure 2 The porous layer 2 is preferably configured such that a portion with a relatively small opening area is located on the light source 11 side of the light guide plate 10, and a portion with a relatively large opening area is located on the opposite side of the light source 11. Thus, the optical stack 100 can extract light uniformly from the light guide plate 10, and can transmit the extracted light to another optical component. In addition, as described above, the optical stack 100 is thinned, so that color shift can be suppressed.
[0081] [Example]
[0082] The present invention is specifically described below by way of examples, but the present invention is not limited to these examples. In addition, the measuring methods of various properties are as follows. In addition, unless otherwise specified, the "%" and "part" in the examples are based on mass.
[0083] (1) Refractive index
[0084] Before attaching the adhesive layer to the porous layer, the porous layer was cut into a size of 25 mm × 50 mm after being formed, and the cut porous layer was attached to the surface of a glass plate (thickness: 3 mm) via an adhesive. The back center of the above-mentioned glass plate (about 20 mm in diameter) was fully coated with black marking ink to prepare a sample that would not reflect on the back of the glass plate. The above-mentioned sample was placed in an ellipsometer (manufactured by JA Woollam Japan: VASE) and the refractive index was measured under the conditions of a wavelength of 550 nm and an incident angle of 50 to 80 degrees.
[0085] On the other hand, the refractive index in the adhesive-attached structure is measured by attaching an adhesive layer to the formed porous layer, injecting laser light (λ=407nm) from the transparent layer side using a prism coupler (manufactured by Metricon), calculating the refractive index at 407nm based on the measured value of the total reflection angle, and converting the refractive index at 550nm based on the wavelength dispersion of the refractive index calculated separately by an ellipsometer (manufactured by JA Woollam).
[0086] (2) Optical durability
[0087] The optical laminates obtained in each embodiment and each comparative example were placed in an oven at 65°C and 95% RH (relative humidity) for 1000 hours of heating and humidification durability test. The degree of increase in refractive index from the initial stage after the above heating and humidification durability test was measured, and laminates with an increase of less than 0.05 were marked as ○, and laminates with an increase of more than 0.05 were marked as ×. The results are shown in Table 1.
[0088] [Manufacturing Example 1] Preparation of a coating liquid for forming a porous layer
[0089] (1) Gelation of Silicon Compounds
[0090] 0.95 g of methyltrimethoxysilane (MTMS), a precursor of a silicon compound, was dissolved in 2.2 g of dimethyl sulfoxide (DMSO) to prepare a mixed solution A. 0.5 g of a 0.01 mol / L aqueous oxalic acid solution was added to the mixed solution A, and the mixture was stirred at room temperature (23° C.) for 30 minutes to hydrolyze MTMS, thereby generating a mixed solution B containing tri(hydroxy)methylsilane.
[0091] To 5.5 g of DMSO were added 0.38 g of 28 wt % ammonia water and 0.2 g of pure water, and then the mixed solution B was added and stirred at room temperature (23° C.) for 15 minutes to gel tri(hydroxy)methylsilane, thereby obtaining a mixed solution C containing a gel-like silicon compound.
[0092] (2) Aging treatment
[0093] The mixed solution C containing the gel-like silicon compound prepared as described above was incubated at 40° C. for 20 hours to perform an aging treatment.
[0094] (3) Crushing
[0095] Next, use a spatula to crush the gel-like silicon compound that has been aged as described above into particles of a few mm to a few cm in size. Next, add 40 g of isobutyl alcohol (IBA) to the mixed solution C, stir gently, and let it stand at room temperature for 6 hours to decant the solvent and catalyst in the gel. Solvent replacement is performed by performing the same decantation treatment three times to obtain a mixed solution D. Next, the gel-like silicon compound in the mixed solution D is crushed (high-pressure medium-free crushing). The crushing treatment (high-pressure medium-free crushing) is performed using a homogenizer (manufactured by SMT, trade name "UH-50"). After weighing 1.85 g of the gel-like compound and 1.15 g of IBA in the mixed solution D and placing them in a 5 cc screw-capped bottle, crush them at 50 W and 20 kHz for 2 minutes.
[0096] The gel-like silicon compound in the mixed solution D was pulverized by the pulverization treatment, and the mixed solution D was obtained as a sol solution E of the pulverized product. The volume average particle size indicating the particle size deviation of the pulverized product contained in the sol solution E was confirmed by a dynamic light scattering type Nanotrac particle size analyzer (manufactured by Nikkiso Co., Ltd., UPA-EX150 model), and the result was 0.10 μm to 0.30 μm. Furthermore, 0.062 g of a 1.5 mass % MEK (methyl ethyl ketone) solution of a photobase generator (Wako Pure Chemical Industries, Ltd.: trade name WPBG266) and 0.036 g of a 5 % MEK solution of bis(trimethoxysilyl)hexane were added to 0.75 g of the sol solution E to obtain a coating solution for forming a porous layer.
[0097] [Manufacturing Example 2] Preparation of the first adhesive layer
[0098] 90.7 parts of butyl acrylate, 6 parts of N-acryloylmorpholine, 3 parts of acrylic acid, 0.3 parts of 2-hydroxybutyl acrylate, 0.1 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator and 100 g of ethyl acetate were added to a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube and a cooler, and nitrogen was introduced while slowly stirring to replace the atmosphere with nitrogen. The liquid temperature in the flask was maintained at about 55°C, and a polymerization reaction was performed for 8 hours to prepare an acrylic polymer solution. 0.2 parts of an isocyanate crosslinking agent (Coronate L manufactured by Nippon Polyurethane Industry, an adduct of trimethylolpropane toluene diisocyanate), 0.3 parts of benzoyl peroxide (Nyper BMT manufactured by NOF Corporation), and 0.2 parts of γ-glycidyloxypropylmethoxysilane (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) were added to 100 parts of the solid content of the obtained acrylic polymer solution to prepare an acrylic adhesive solution. Next, the acrylic adhesive solution was applied to one side of a silicone-treated polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., thickness: 38 μm) so that the adhesive layer after drying had a thickness of 10 μm, and dried at 150° C. for 3 minutes to form a first adhesive layer. The elastic modulus of the obtained adhesive was 1.3×10 5 (Pa).
[0099] [Manufacturing Example 3] Preparation of the Second Adhesive Layer
[0100] 99 parts of butyl acrylate, 1 part of 4-hydroxybutyl acrylate, 0.1 part of 2,2'-azobisisobutyronitrile as a polymerization initiator and 100 parts of ethyl acetate were added to a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube and a cooler, and nitrogen was introduced while slowly stirring to replace the atmosphere with nitrogen. The liquid temperature in the flask was kept at about 55°C, and a polymerization reaction was performed for 8 hours to prepare an acrylic polymer solution. 0.1 part of an isocyanate crosslinking agent (Takenate D110N manufactured by Mitsui Takeda Chemical Co., Ltd., trimethylolpropane benzyl diisocyanate), 0.1 part of benzoyl peroxide (Nyper BMT manufactured by NOF Corporation), and 0.2 part of γ-glycidyloxypropylmethoxysilane (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) were added to 100 parts of the solid content of the obtained acrylic polymer solution to prepare a solution of an acrylic adhesive composition. Next, the solution of the acrylic adhesive composition was applied to one side of a polyethylene terephthalate film (release film: manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., MRF38) treated with a silicone release agent, and dried at 150°C for 3 minutes to form a second adhesive layer with a thickness of 12 μm on the release film surface. The elastic modulus of the obtained adhesive was 8.2×10 4 (Pa).
[0101] [Example 1]
[0102] After applying a polyvinyl alcohol (PVA) aqueous solution on a substrate (PET resin film), the coating was dried to form a PVA layer as a transparent layer on the substrate. The thickness of the PVA layer was 3 μm.
[0103] Next, the porous layer-forming coating liquid of Manufacturing Example 1 was pattern-coated on the surface of the PVA layer opposite to the substrate by gravure printing, and the coating was dried. Thus, a patterned porous layer was formed on the PVA layer. The pattern of the porous layer had a gradual distribution in which the opening ratio per unit area became larger as it moved toward one side in the width direction. The refractive index of the porous layer was 1.19. The thickness of the porous layer was 0.9 μm.
[0104] Next, the first pressure-sensitive adhesive layer obtained in Production Example 2 was attached to the porous layer.
[0105] Next, the PET substrate was peeled off from the PVA layer at a peeling angle of 180° and a peeling speed of 300 mm / min. The peeling force at this time was measured using an Autograph tensile tester. The results are shown in Table 1.
[0106] Next, the second pressure-sensitive adhesive layer obtained in Production Example 3 was attached to the surface of the PVA layer opposite to the porous layer.
[0107] In the above manner, an optical laminate having a structure of first pressure-sensitive adhesive layer / porous layer / transparent layer / second pressure-sensitive adhesive layer was obtained.
[0108] [Example 2]
[0109] An optical layered body was obtained in the same manner as in Example 1 except that a polymethyl methacrylate (PMMA) aqueous solution was used instead of the PVA aqueous solution to form a PMMA layer as a transparent layer on the substrate.
[0110] [Example 3]
[0111] An optical laminate was obtained in the same manner as in Example 1 except that an ethanol solution of polyvinyl acetal was used instead of the PVA aqueous solution to form a polyvinyl acetal layer as a transparent layer on the substrate.
[0112] [Example 4]
[0113] An optical laminate was obtained in the same manner as in Example 1 except that a substrate having a CuO sputtered film laminated on a polyethylene terephthalate (PET) film was prepared and a SiO 2 layer as a transparent layer was formed on the CuO sputtered film by sputtering.
[0114] [Example 5]
[0115] An optical layered body was obtained in the same manner as in Example 1 except that the porous layer-forming coating liquid of Production Example 1 was pattern-coated by inkjet printing instead of gravure printing.
[0116] [Comparative Example 1]
[0117] The porous layer-forming coating liquid of Production Example 1 was pattern-coated on a 100 μm-thick substrate (cycloolefin (COP) film; ZF16; manufactured by ZEON Corporation) by gravure printing, and then the coating was dried to form a patterned porous layer on the substrate.
[0118] Next, the first pressure-sensitive adhesive layer obtained in Production Example 2 was attached to the porous layer. Next, the substrate was peeled off from the porous layer, and the second pressure-sensitive adhesive layer obtained in Production Example 3 was attached to the peeled surface.
[0119] In the above manner, an optical laminate having a structure of first pressure-sensitive adhesive layer / porous layer / second pressure-sensitive adhesive layer was obtained.
[0120] [Comparative Example 2]
[0121] The porous layer-forming coating liquid of Production Example 1 was pattern-coated on a substrate (acrylic resin film) having a thickness of 30 μm by gravure printing, and the coating was dried to form a patterned porous layer on the substrate.
[0122] Next, the first adhesive layer obtained in Production Example 2 was attached to the porous layer. Next, the second adhesive layer obtained in Production Example 3 was attached to the surface of the substrate opposite to the porous layer.
[0123] In the above manner, an optical laminate having a structure of first pressure-sensitive adhesive layer / porous layer / substrate / second pressure-sensitive adhesive layer was obtained.
[0124] [Table 1]
[0125] Table 1
[0126]
[0127] As is clear from Table 1, according to the examples of the present invention, by providing a transparent layer having a thickness of 20 μm or less between the patterned porous layer and the adhesive layer, the thickness of the optical laminate can be reduced and excellent optical durability can be achieved.
[0128] [Industrial Applicability]
[0129] The optical layered body according to the embodiment of the present invention can be used for various optical products, and can be particularly suitably used for an optical product including a light guide plate.
[0130] Description of Reference Numerals
[0131] 1: Transparent layer
[0132] 1a: Barrier layer
[0133] 2: Porous layer
[0134] 21: Opening
[0135] 3: Adhesive layer
[0136] 4: Adhesive layer
[0137] 100: Optical laminate
[0138] 200: Optical products
Claims
1. An optical laminate, wherein: have: A transparent layer having a thickness of less than 20 μm; a porous layer, which is directly provided on one surface of the transparent layer in the thickness direction in a predetermined pattern and has a refractive index of 1.25 or less; an adhesive layer disposed on the opposite side of the transparent layer from the porous layer and in contact with the transparent layer; The pressure-sensitive adhesive layer is disposed on the opposite side of the transparent layer from the adhesive layer and covers the porous layer.
2. The optical layered body according to claim 1, wherein: The transparent layer has a barrier function of suppressing the components constituting the adhesive layer from penetrating into the porous layer.
3. The optical laminate according to claim 2, wherein: The porosity of the transparent layer is smaller than the porosity of the porous layer.
4. The optical layered body according to any one of claims 1 to 3, wherein The adhesive layer has an elastic modulus of 1.0×10 5 (Pa) or more adhesive composition.
5. A method for producing an optical laminate, wherein: include: A step of forming a transparent layer having a thickness of 20 μm or less on a substrate; A step of patterning a porous layer having a refractive index of 1.25 or less on a surface of the transparent layer opposite to the substrate; forming a binder layer from the side opposite to the transparent layer with respect to the porous layer so as to cover the porous layer; A step of peeling the substrate from the transparent layer; A step of forming an adhesive layer on a surface of the transparent layer opposite to the porous layer.
6. The method for producing an optical layered body according to claim 5, wherein: The peeling force when the substrate is peeled from the transparent layer is 1 N / 25 mm or less.
Citation Information
Patent Citations
Optical member, and backlight unit and image display device using said optical member
WO2021193789A1