Curable resin composition

By using a curable resin composition consisting of a specific combination of epoxy compounds and oxobutane compounds, the problem of insufficient adhesion and light-blocking properties of light-blocking ink under high temperature and high humidity conditions is solved, and a coating film with high light-blocking properties, stable adhesion and high hardness is achieved.

CN118900866APending Publication Date: 2024-11-05TAIYO HOLDINGS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380027924.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-24
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing light-blocking inks have difficulty maintaining good adhesion and curing properties under high temperature and high humidity conditions, resulting in insufficient light-blocking properties and the hardness of the cured coating film cannot meet the requirements.

Method used

By employing a combination of epoxy compounds, oxetane compounds, photoacid generators, and black colorants in specific mass ratios, including alicyclic epoxy compounds with and without intramolecular ester bonds, the viscosity and mixing amount are optimized to improve the curability and adhesion of the coating film.

Benefits of technology

It maintains stable sealing and high light-blocking properties under high temperature and high humidity conditions, while forming a high-hardness cured coating film, thus improving manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005044247410000051
    Figure BDA0005044247410000051
  • Figure BDA0005044247410000061
    Figure BDA0005044247410000061
  • Figure BDA0005044247410000062
    Figure BDA0005044247410000062
Patent Text Reader

Abstract

[Problem] To provide a black light-shielding curable resin composition for inkjet use, which has excellent surface curability in addition to high light-shielding properties, exhibits stable adhesion under high-temperature and high-humidity conditions, and provides a cured coating film having high hardness after curing. [Solution] A curable resin composition comprising (A) an epoxy compound, (B) an oxetane compound, (C) a photoacid generator, and (D) a black colorant, the epoxy compound (A) comprising (a) an alicyclic epoxy compound having an ester bond in the molecule and (b) an alicyclic epoxy compound not having an ester bond in the molecule at a mass ratio in the numerical range from 5: 100 to 30: 100.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a curable resin composition. Background Art

[0002] In the shading member of the display mounted on the PC or mobile device, the influence of the backlight must be suppressed as much as possible, and therefore, high shading properties are required. Therefore, as the material of such shading member, shading ink for forming a black matrix is ​​used. In addition, on the other hand, from the perspective of manufacturing efficiency, the technology of manufacturing the shading member by applying such shading ink to a substrate using an inkjet method has attracted much attention.

[0003] As a technique for applying ink by inkjet method, for example, Patent Document 1 proposes a technique of using an active energy ray-curable ink containing a photocationic polymerization initiator, a polyfunctional epoxy compound, a monofunctional alicyclic epoxy compound, and an oxetane compound for inkjet recording.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2010-106254 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] Here, in particular, smartphones and smart watches are not only used at room temperature, but are also expected to be used in various environments such as summer and in cars. Therefore, the light-shielding ink used is expected to have high reliability. For example, it is also necessary for the light-shielding ink to have not only high light-shielding properties, but also to maintain high adhesion to the substrate under high temperature and high humidity, good curing properties, and high hardness of the cured coating film formed after curing.

[0009] However, in general, light-shielding inks are added with high concentrations of light-shielding pigments, which have the characteristic of high OD values. Therefore, when the light-shielding ink is applied to a substrate using an inkjet method, the light used to photo-cure the light-shielding ink film formed on the substrate will inevitably not easily reach the bottom of the film. As a result, the curability of the entire film is insufficient, and the hardness of the cured film itself and the adhesion to substrates such as glass and metal will be impaired.

[0010] In this regard, the active energy ray curable ink proposed in Patent Document 1 uses an alicyclic epoxy compound having an ester bond in the molecule, but it is assumed that when the pigment concentration is increased, it is difficult for light to fully reach the bottom of the coating film. Therefore, the curability of the coating film is insufficient, and it is estimated that it is difficult to maintain the adhesion of the cured coating film to the substrate when it is left under high temperature and high humidity conditions, and the hardness of the cured coating film after the ink is cured cannot meet the required level.

[0011] Therefore, in view of the above viewpoints, the present invention aims to provide a curable resin composition which has high light-shielding properties, good surface curing properties, exhibits stable adhesion under high temperature and high humidity conditions, and provides a cured coating film having high hardness after curing.

[0012] Solutions for solving problems

[0013] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by using a curable resin composition containing two epoxy compounds having respective structural characteristics, an oxetane compound, a photoacid generator and a black colorant at a mass ratio within a specific numerical range, thereby completing the present invention.

[0014] That is, this problem can be solved more specifically by the following curable resin composition:

[0015] It contains: (A) an epoxy compound, (B) an oxetane compound, (C) a photoacid generator and (D) a black colorant,

[0016] The (A) epoxy compound includes (a) an alicyclic epoxy compound having an ester bond in the molecule and (b) an alicyclic epoxy compound not having an ester bond in the molecule at a mass ratio in the numerical range of 5:100 to 30:100.

[0017] The curable resin composition of the present invention can be used in an inkjet process. In this case, in a more preferred embodiment, from the viewpoint of smooth discharge from an inkjet nozzle, the viscosity is preferably in the range of 5 to 20 mPa·s at 50° C., and more preferably in the range of 5 to 15 mPa·s at 50° C.

[0018] The viscosity can be measured, for example, using a cone-plate viscometer (TVE-33H manufactured by Toki Sangyo Co., Ltd.).

[0019] A more preferred embodiment relates to a curable resin composition, wherein the (b) alicyclic epoxy compound having no ester bond in the molecule has a bifunctional epoxy group.

[0020] In another preferred embodiment, the curable resin composition is provided, wherein the black colorant (D) is carbon black and is contained in an amount of 5 parts by mass or more relative to 100 parts by mass of the total of the epoxy compound (A) and the oxetane compound (B).

[0021] Another preferred embodiment relates to a curable resin composition, wherein the mass ratio of the (B) oxetane compound to the (A) epoxy compound is in a numerical range of 2:100 to 40:100.

[0022] Another preferred embodiment relates to a curable resin composition, wherein the epoxy compound (A) comprises (a) an alicyclic epoxy compound having an ester bond in the molecule and (b) an alicyclic epoxy compound not having an ester bond in the molecule at a mass ratio in the numerical range of 8:100 to 25:100. By limiting the ratio of the compounding amount of the alicyclic epoxy compound having an ester bond in the molecule (a) to the above range, a cured coating film having excellent adhesion can be produced even after being left under high temperature and high humidity conditions. It is envisaged that by making the compounding amount of the alicyclic epoxy compound having an ester bond in the molecule (a) to be greater than the lower limit of the above mass ratio, the softness of the coating film based on the hydrolysis of the ester bond can be appropriately maintained, the internal stress of the coating film can be suppressed, and the initial adhesion can be improved. In addition, it is conceivable that by setting the blending amount of the alicyclic epoxy compound (a) having an ester bond in the molecule to be below the upper limit of the above mass ratio, deterioration of the coating film due to hydrolysis of the coating film after being left under high temperature and high humidity conditions can be suppressed, and the physical properties of the coating film after photocuring such as adhesion can be maintained.

[0023] Another preferred embodiment relates to a curable resin composition, wherein the mass ratio of the (B) oxetane compound to the (A) epoxy compound is in a numerical range of 10:100 to 20:100.

[0024] By limiting the ratio of the amount of compounding of (B) oxetane compound to the above-mentioned scope, the curability of the coating surface and the bottom can be well balanced. By making the ratio of the above-mentioned amount of compounding to be above the lower limit, the viscosity of the cured coating after photocuring becomes good. In addition, by making the ratio of the above-mentioned amount of compounding to be below the upper limit, the crosslinking density of the cured coating is appropriately maintained, and flexibility is maintained, and the adhesion after being placed under the pencil hardness and high temperature and humidity conditions can be improved.

[0025] Still another preferred embodiment relates to a curable resin composition further comprising an alkoxyanthracene derivative as a photosensitizer.

[0026] In view of suitability as a black light shielding agent for smartphones and the like, a more preferred embodiment of the curable resin composition of the present invention is as follows: the OD value of the cured coating film at a film thickness of 10 to 20 μm is preferably 4 or more, more preferably 5 or more.

[0027] The OD value can be calculated based on the formula OD value = -log10 (T / 100) by measuring the amount of transmitted light using a transmission densitometer (model: X-Rite 361T; light source wavelength 400 to 800 nm; manufactured by SAKATAINX CORPORATION), for example.

[0028] Effects of the Invention

[0029] The curable resin composition of the present invention having the above-mentioned structure has the following advantages: not only has high light-shielding properties, but also has good curing properties on the coating surface, exhibits stable adhesion under high temperature and high humidity conditions, and forms a cured coating with high hardness. Furthermore, the curable resin composition of the present invention is also suitable for inkjet applications, and therefore has the advantage of good manufacturing efficiency in the manufacture of various displays.

[0030] Furthermore, the curable resin composition of the present invention can be expected to be particularly suitable for use as a black light-shielding material for displays, for example, due to the above-mentioned properties. DETAILED DESCRIPTION

[0031] [(A) Epoxy compound]

[0032] The curable resin composition of the present invention contains (A) an epoxy compound to improve the hardness of the formed cured product (cured coating film). In particular, in order to improve the adhesion to the substrate even when the curable resin composition of the present invention is exposed to a harsh environment of higher temperature and higher humidity, two epoxy compounds, namely, (a) an alicyclic epoxy compound having an ester bond in the molecule and (b) an alicyclic epoxy compound not having an ester bond in the molecule, are used as the epoxy compound (A).

[0033] When an epoxy compound is used in a curable resin composition having a high OD value, an alicyclic epoxy compound is usually used as one of the components of the epoxy compound due to its high reactivity. In particular, from the perspective of improving the surface curability or curability when using a curable resin composition, an alicyclic epoxy compound having an ester bond is used in the customary manner. However, even if a curable resin composition containing such an alicyclic epoxy compound having an ester bond is used for a display of a smartphone or the like that is exposed to a harsh environment of higher temperature and humidity, there is also a disadvantage that the adhesion to the substrate becomes insufficient.

[0034] Therefore, in the present invention, as the epoxy compound (A), two epoxy compounds, namely, (a) an alicyclic epoxy compound having an ester bond in the molecule and (b) an alicyclic epoxy compound not having an ester bond in the molecule, are used, and not only that, but these two epoxy compounds are contained in the curable resin composition at a mass ratio of 5:100 to 30:100, preferably 8:100 to 25:100, thereby avoiding the above-mentioned disadvantages. By limiting the ratio of the compounding amount of the alicyclic epoxy compound having an ester bond in the molecule (a) to the above-mentioned range, the influence of deterioration caused by the hydrolysis of the ester on the coating film after photocuring is suppressed, and the flexibility and curability of the coating film are taken into account, thereby achieving excellent adhesion.

[0035] Hereinafter, (a) an alicyclic epoxy compound having an ester bond in the molecule and (b) an alicyclic epoxy compound not having an ester bond in the molecule contained in the (A) epoxy compound used as one of the components of the curable resin composition of the present invention will be described.

[0036] [(a) Alicyclic epoxy compound having an ester bond in the molecule]

[0037] In the present invention, the alicyclic epoxy compound refers to a compound having one or more aliphatic ring structures in the molecule, wherein two carbon atoms and an oxygen atom in the aliphatic ring form a further ring to form an epoxy group.

[0038] Furthermore, (a) the alicyclic epoxy compound having an ester bond in the molecule means a compound in which the alicyclic epoxy compound further has an ester bond in its chemical structure.

[0039] As such (a) alicyclic epoxy compounds having an ester bond in the molecule, for example, preferably there can be mentioned compounds having the following structures:

[0040]

[0041]

[0042] (where n1 represents an integer from 1 to 30)

[0043]

[0044] (wherein A represents an alkylene group having 1 to 8 carbon atoms; n2 represents an integer of 1 to 30)

[0045]

[0046] As the (a) alicyclic epoxy compound having an ester bond in the molecule, a commercially available product may be used, and preferred examples thereof include Celloxide 2021P and Celloxide 2081 (both manufactured by Daicel Corporation).

[0047] (a) The alicyclic epoxy compound having an ester bond in the molecule may, of course, be used alone or in combination of two or more.

[0048] [(b) Alicyclic Epoxy Compound Having No Ester Bond in the Molecule]

[0049] In the present invention, (b) an alicyclic epoxy compound having no ester bond in the molecule means an alicyclic epoxy compound described in the section (a) an alicyclic epoxy compound having an ester bond in the molecule which has no ester bond in the molecule, for example, an alicyclic epoxy compound having an ether bond instead of an ester bond.

[0050] Examples of the alicyclic epoxy compound (b) having no ester bond in the molecule include compounds having the following structure:

[0051]

[0052]

[0053] As (b) an alicyclic epoxy compound having no ester bond in the molecule, commercially available products may of course be used, and preferred examples include limonene dioxide (LDO) (manufactured by SYMRISE), THI-DE, DE-102 and DE-103 (manufactured by JXT Genergy Co., Ltd.), X-40-2678 and X-40-2669 (manufactured by Shin-Etsu Chemical Co., Ltd.), EHPE-3150 and CELLOXIDE 2000 (manufactured by Daicel Corporation), and KR-470 (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0054] Moreover, among the alicyclic epoxy compounds (b) having no ester bond in the molecule, those having a bifunctional epoxy group are more preferred in the present invention.

[0055] Such (b) alicyclic bifunctional epoxy compounds having no ester bond in the molecule have a total of two of the following structural formulas in the molecule:

[0056]

[0057] The ethylene oxide group shown and / or the following structural formula:

[0058]

[0059] The cyclohexenyloxy compound shown.

[0060] Examples of commercially available products include THI-DE, DE-102, and DE-103 (manufactured by JXTG Energy Co., Ltd.), X-40-2678, and X-40-2669 (manufactured by Shin-Etsu Chemical Co., Ltd.), and the like.

[0061] (b) The alicyclic epoxy compound having no ester bond in the molecule may, of course, be used alone or in combination of two or more.

[0062] The total content of the alicyclic epoxy compound (a) having an ester bond in the molecule in the curable resin composition of the present invention is preferably 3 to 60 parts by mass, more preferably 3 to 30 parts by mass, based on 100 parts by mass of the total of the epoxy compound (A) and the oxetane compound (B), from the viewpoint of curability and viscosity.

[0063] The total content of the (b) alicyclic epoxy compound having no ester bond in the molecule is preferably 30 to 90 parts by mass, more preferably 40 to 80 parts by mass, based on 100 parts by mass of the total of the (A) epoxy compound and the (B) oxetane compound, from the viewpoint of adhesion to the substrate.

[0064] However, the respective contents of the two types of alicyclic epoxy compounds (a) and (b) need to be adjusted to a ratio within the above-mentioned specific numerical range.

[0065] [Other epoxy compounds]

[0066] The curable resin composition of the present invention may, of course, contain epoxy compounds other than (a) and (b) as the epoxy compound (A), such as non-alicyclic epoxy compounds, as other epoxy compounds for the purpose of further improving the properties of the curable resin composition of the present invention or imparting new properties, in addition to the above-mentioned (a) alicyclic epoxy compound having an ester bond in the molecule and (b) an alicyclic epoxy compound not having an ester bond in the molecule.

[0067] The other epoxy compounds that can be used in the present invention are commonly used and sufficient, so not all of them are listed here, but as preferred examples, Denacol EX-212 and Denacol EX-121 (both manufactured by Denacol Co., Ltd.), and KBM-403 (manufactured by Shin-Etsu Silicone Co., Ltd.) are mentioned.

[0068] The total content of such other epoxy compounds when contained is preferably 130 parts by mass, more preferably 3 to 20 parts by mass, based on 100 parts by mass of the total of the (A) epoxy compound (including the epoxy compounds (a) and (b) and other epoxy compounds) and the (B) oxetane compound.

[0069] [(B) Oxetane compound]

[0070] In the curable resin composition of the present invention, from the viewpoint of improving the hardness of the cured product, an oxetane compound (B) is contained as a thermosetting resin. However, in the present invention, the content of the oxetane compound (B) is adjusted in a manner such that the total amount of the epoxy compound (A), that is, the total amount of the alicyclic epoxy compound (a) having an ester bond in the molecule, the alicyclic epoxy compound (b) not having an ester bond in the molecule, and other epoxy compounds becomes a mass ratio in a specific numerical range. Specifically, the content of the oxetane compound (B) is adjusted in a manner such that the mass ratio of the oxetane compound (B) to the epoxy compound (A) becomes a numerical range of 2:100 to 40:100, preferably a numerical range of 10:100 to 20:100.

[0071] Such (B) oxetane compound is not limited to a monofunctional one, and a polyfunctional one can also be used.

[0072] Examples of the monofunctional (B) oxetane compound include 3-methyloxetane, 3-ethyloxetane, 3-hydroxymethyloxetane, 3-methyl-3-hydroxymethyloxetane, and 3-ethyl-3-hydroxymethyloxetane.

[0073] In addition, as the polyfunctional (B) oxetane compound, in addition to bis[(3-methyl-3-oxetanylmethoxy)methyl]ether, bis[(3-ethyl-3-oxetanylmethoxy)methyl]ether, 1,4-bis[(3-methyl-3-oxetanylmethoxy)methyl]benzene, 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, (3-methyl-3-oxetanyl)methyl acrylate, (3- In addition to polyfunctional oxetanes such as (3-ethyl-3-oxetanyl)methyl ester, (3-methyl-3-oxetanyl)methyl methacrylate, (3-ethyl-3-oxetanyl)methyl methacrylate, and oligomers or copolymers thereof, etherified products of oxetane alcohol and resins having hydroxyl groups such as novolac resins, poly(p-hydroxystyrene), Cardo-type bisphenols, calixarene, resorcinol calixarene, or silsesquioxane can also be mentioned. In addition, copolymers of unsaturated monomers having an oxetane ring and alkyl (meth)acrylates can also be mentioned.

[0074] As the (B) oxetane compound, a commercially available product may be used, of course, and for example, OXT-101, OXT-121, OXT-212, and OXT-221 (manufactured by Toagosei Co., Ltd.) are preferred.

[0075] The curable resin composition of the present invention may, of course, contain one kind alone or two or more kinds of the above-mentioned (B) oxetane compound.

[0076] The content of the (B) oxetane compound is preferably 3 to 40 parts by mass, more preferably 8 to 30 parts by mass, based on 100 parts by mass of the total of the (A) epoxy compound and the (B) oxetane compound, from the viewpoint of hardness of the cured product.

[0077] However, the content of the oxetane compound (B) needs to be adjusted so that the mass ratio to the mass of the epoxy compound (A) contained falls within the above-mentioned specific numerical range.

[0078] The total amount of the epoxy compound (A) and the oxetane compound (B) is preferably 25 to 95% by mass, more preferably 35 to 90% by mass, based on the mass of the curable resin composition of the present invention.

[0079] [(C) Photoacid generator]

[0080] The curable resin composition of the present invention contains (C) a photoacid generator as a compound capable of generating a substance that initiates cationic polymerization by ultraviolet irradiation.

[0081] Examples of the photoacid generator (C) include onium salts such as diazonium salts, iodonium salts, bromonium salts, chloroonium salts, sulfonium salts, selenonium salts, pyrylium salts, thiopyranium salts, and pyridinium salts; halogenated compounds such as tris(trihalomethyl)-s-triazine and its derivatives; 2-nitrobenzyl sulfonic acid esters; iminosulfonates; 1-oxo-2-naphthoquinonediazosulfonate derivatives; N-hydroxyimidesulfonates; tris(methylsulfonyloxy)benzene derivatives; bissulfonyldiazomethanes; sulfonylcarbonylalkanes; sulfonylcarbonyldiazomethanes; disulfone compounds, etc.

[0082] These (C) photoacid generators can be used alone or in combination of two or more.

[0083] As the (C) photoacid generator, commercially available products may be used, for example, CPI-100P, CPI-200K, CPI-101A (all manufactured by San-Apro), Cyracure photocuring initiator UVI-6990, Cyracure photocuring initiator UVI-6992, Cyracure photocuring initiator UVI-6976 (all manufactured by Dow Chemical Japan Co., Ltd.), Adeka Optomer SP-150, Adeka Optomer SP-152, Adeka Optomer SP-170, Adeka Optomer SP-172 (all manufactured by Asahi Denka Kogyo Co., Ltd.), CI-5102, CI-2855 (all manufactured by Nippon Soda Co., Ltd.), Sanaid SI-60L, Sanaid SI-80L, Sanaid SI-100L, Sanaid SI-110L, Sanaid SI-180L, Sanaid SI-201 SI-110, SAN AID SI-145, SAN AID SI-150, SAN AID SI-160, SAN AID SI-180 (all manufactured by Sanshin Chemical Industry Co., Ltd.), Esacure 1064, Esacure 1187 (all manufactured by Lambertye), Ominicat 432, Ominicat 440, Ominicat 445, Ominicat 550, Ominicat 650, Ominicat BL-550, Ominicat 250 (manufactured by IGM Resin Inc.), RHODORSIL PHOTOINITIATOR 2074 (manufactured by Rhodia Japan Co., Ltd.), WPI-113, WPI-116, WPI-169, WPI-170 (manufactured by Wako Pure Chemical Industries, Ltd.), and the like.

[0084] Among these, CPI-100P, CPI-101A, CPI-200K, CPI-210S, or Ominicat 250, WPI-113, WPI-116, WPI-169, and WPI-170, which are aromatic iodonium salts, are preferred.

[0085] The content of the photoacid generator (C) in the curable resin composition is preferably 5 to 30 parts by mass, more preferably 7 to 15 parts by mass, based on 100 parts by mass of the total of the epoxy compound (A) and the oxetane compound (B).

[0086] [(D) Black colorant]

[0087] Generally, from the viewpoint of use as a black light-shielding agent, the curable resin composition of the present invention preferably contains (D) a black colorant, and particularly preferably a black pigment. Typically, a black pigment such as carbon black is preferably used, but within the scope of the viewpoint of use that does not greatly deviate, a black dye or a colorant having other colors may be used, and of course, it may further contain other than carbon black.

[0088] Examples of black pigments include, in addition to carbon black, inorganic pigments such as ferrosoferric oxide (Fe 3 O 4 ), black titanium oxide, copper manganese black, copper chrome black, and cobalt black, and organic pigments such as cyanine black and aniline black.

[0089] In addition, examples of colorants having other colors include well-known and commonly used red, blue, green, and yellow pigments or dyes.

[0090] The content of the black colorant (D) in the curable resin composition of the present invention is adjusted in consideration of the use of the cured product to be formed, but from the viewpoint of the balance between the curability and adhesion of the coating film, it is preferably 5 parts by mass or more, and more preferably 5 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the total of the epoxy compound (A) and the oxetane compound (B).

[0091] [Photosensitizer]

[0092] In order to further improve photosensitivity, the curable resin composition of the present invention preferably further contains a photosensitizer.

[0093] The photosensitizer is preferably a compound that becomes excited by light of wavelength 350nm to 450nm. Examples include polynuclear aromatics such as pyrene, perylene, triphenylene, and anthracene; xanthenes such as fluorescein, eosin, erythrosine, rhodamine B, and diiodoeosin; xanthenes such as xanthone, thioxanthone, dimethylthioxanthone, and diethylthioxanthone; cyanines such as thiocarbocyanine and oxacarbocyanine; merocyanines such as merocyanine and methyl merocyanine; rhodanines; oxonols; thiazines such as thionine, methylene blue, and toluidine blue; acridines such as acridine orange, chloroflavin, and acrylflavin; acridones such as acridone and 10-butyl-2-chloroacridone; anthraquinones; squaric acid pigments; styrenes; basic styrenes; coumarins such as 7-diethylamino-4-methylcoumarin. Among these, anthracene compounds are preferred, and alkoxyanthracene derivatives are particularly preferred.

[0094] Of course, these photosensitizers may be used in combination of two or more types.

[0095] As the photosensitizer, commercial products may be used. As such examples, preferably alkoxyanthracene derivatives such as Anthracure (registered trademark) UVS-1101 (diethoxyanthracene; manufactured by Kawasaki Chemical Industries, Ltd.), Anthracure (registered trademark) UVS-1221 (dipropoxyanthracene; manufactured by Kawasaki Chemical Industries, Ltd.), and Anthracure (registered trademark) UVS-1331 (dibutoxyanthracene; manufactured by Kawasaki Chemical Industries, Ltd.) may be cited.

[0096] The content of the photosensitizer is 0.1 to 2.0 parts by mass, preferably 0.2 to 1.0 parts by mass, based on 1 part by mass of the photoacid generator.

[0097] [Other ingredients]

[0098] In addition, the curable resin composition of the present invention may also contain other ingredients such as solvents, reactive diluents, dispersants, thickeners, surfactants, antioxidants, plasticizers, flame retardants, antistatic agents, leveling agents, defoamers and antibacterial agents within the range of not damaging its characteristics. As a reactive diluent that can reduce the viscosity of the curable resin composition of the present invention, a photoreactive diluent is preferred. As a photoreactive diluent, (meth) acrylates, vinyl ethers, ethylene derivatives, styrene, chloromethylstyrene, α-methylstyrene, maleic anhydride, dicyclopentadiene, N-vinyl pyrrolidone, N-vinyl formaldehyde, dimethylbenzene dioxetane, oxetane alcohol, 3-ethyl-3-(phenoxymethyl)oxetane, resorcinol diglycidyl ether, etc., have unsaturated double bonds, oxetane groups, and epoxy compounds. Among these, (meth) acrylates are preferred.

[0099] [Solidified product and method for producing the same]

[0100] The curable resin composition of the present invention is applied to a target portion of a substrate by an inkjet method and then cured to form a cured product.

[0101] As the inkjet printing method, a piezoelectric method of an on-demand method is suitable, but it should not be particularly limited. As suitable wavelengths, 365nm, 385nm, 395nm, 405nm, etc. in the ultraviolet region can be cited, but it should not be particularly limited.

[0102] Curing is performed by irradiating the applied composition with active energy rays.

[0103] As the irradiation light source of the active energy ray, LED, low-pressure mercury lamp, medium-pressure mercury lamp, high-pressure mercury lamp, ultra-high-pressure mercury lamp, xenon lamp, metal halide lamp, etc. are suitable. In addition, electron beam, α ray, β ray, γ ray, X-ray, neutron beam, etc. can also be used. It should be noted that the irradiation light source is 1 or more than 2. When there are more than 2, of course, light sources with different wavelengths can be combined and used.

[0104] The exposure dose of active energy rays is usually 10 to 10000 mJ / cm 2 , preferably 20 to 2000 mJ / cm 2 , more preferably 100 to 2000 mJ / cm 2 within the range.

[0105] Hereinafter, the present invention will be specifically described with reference to Examples and Comparative Examples, but the present invention is of course not limited to the following Examples.

[0106] In addition, unless otherwise specified, "parts" and "%" indicated are based on mass.

[0107] Example

[0108] The respective components were blended in the amounts described in Table 1 below and pre-mixed in a stirrer to prepare curable resin compositions of Examples 1 to 10 and Comparative Examples 1 to 4.

[0109] In addition, the numerical value of the compounding amount in a table|surface shows a mass part unless otherwise specified.

[0110] [Table 1]

[0111]

[0112] ※ The components corresponding to the numbers in Table 1 are as follows.

[0113] 1) (a) Alicyclic epoxy compound having an ester bond in the molecule: Celloxide 2021P (manufactured by Daicel Corporation) Chemical name: 3,4-epoxycyclohexylmethyl (3,4-epoxy)cyclohexylcarboxylate

[0114] 2) (a) Alicyclic epoxy compound having an ester bond in the molecule: Celloxide 2081 (manufactured by Daicel Corporation) Chemical name: ε-caprolactone-modified 3,4-epoxycyclohexylmethyl 3',4'-epoxycyclohexylcarboxylate

[0115] 3) (b) Alicyclic epoxy compound having no ester bond in the molecule: LDO (manufactured by SYMRISE) Chemical name: Limonene dioxide

[0116] 4) (b) Alicyclic epoxy compound having no ester bond in the molecule: THI-DE (manufactured by JXTG Energy Co., Ltd.) Chemical name: tetrahydroindene dioxide

[0117] 5) Other epoxy compounds: Denacol EX-212 (manufactured by Nagase ChemteX Corporation) Chemical name: 1,6-hexanediol diglycidyl ether

[0118] 6) Other epoxy compounds: Denacol EX-121 (manufactured by Nagase ChemteX Corporation) Chemical name: 2-ethylhexyl glycidyl ether

[0119] 7) Other epoxy compounds: KBM-403 (manufactured by Shin-Etsu Chemical Co., Ltd.) Silane coupling agent having an epoxy group as an organic functional group Chemical name: 3-glycidoxypropyltrimethoxysilane

[0120] 8) (B) Monofunctional oxetane compound: OXT-212 (manufactured by Toagosei Co., Ltd.) Chemical name: 2-ethylhexyloxetane

[0121] 9) (B) Difunctional oxetane compound: OXT-221 (manufactured by Toagosei Co., Ltd.) Chemical name: 3-ethyl-3{[(3-ethyloxetane-3-yl)methoxy]methyl}oxetane

[0122] 10) Photosensitizer: Anthracure UVS-1331 (manufactured by Kawasaki Chemical Industries, Ltd.)

[0123] Chemical name: 9,10-dibutoxyanthracene

[0124] 11) (C) Photoacid generator: CPI-100P (solid content 50%) (manufactured by San-Apro)

[0125] Chemical name: Diphenyl-(4-phenylthio)phenylsulfonium hexafluoro-λ5-phosphate

[0126] 12) (C) Photoacid generator: Ominicat 250 (manufactured by IGM Resin Inc.)

[0127] Chemical name: 4-isobutylphenyl (4-methylphenyl) iodonium hexafluorophosphate (solid content 75%)

[0128] 13) (D) Black colorant: Pigment black 7 (carbon black)

[0129] A cured product (cured coating film) having a film thickness of 5 μm was obtained from the obtained curable resin compositions of Examples 1 to 10 and Comparative Examples 1 to 4. The cured products were measured for cross-cutting, pencil hardness, and dryness to touch after UV curing as described below.

[0130] The viscosity of the curable resin compositions of Examples 1 to 10 and Comparative Examples 1 to 4 was measured at an ink temperature of 50° C. and 100 rpm using a cone and plate viscometer (TVE-33H manufactured by Toki Sangyo Co., Ltd.), and the results were all within the range of 5 to 20 mPa·s.

[0131] [Preparation of test substrate]

[0132] Under the following conditions, the curable resin compositions of Examples 1 to 10 and Comparative Examples 1 to 4 were drawn on a substrate using an inkjet printer and then UV cured to prepare test substrates. It should be noted that a glass substrate (110 mm×160 mm, 1 mm thick) was used as the substrate.

[0133] ·Based on the drawing conditions of inkjet printer

[0134] Cured film thickness: 5μm

[0135] Device: A piezoelectric inkjet printer (Fuji Film Co., Ltd. material printer DMP-2831 (head temperature 50°C)) was used.

[0136] UV curing conditions

[0137] LED-UV lamp (FireEdge FE400 manufactured by Phoseon TECHNOLOGY)

[0138] Exposure: 1500mJ / cm 2

[0139] Wavelength: 365nm

[0140] [Scratch]

[0141] In accordance with JIS K 5600-5-6 1999, the cured coating films on each test substrate of the curable resin composition of Examples 1 to 10 and Comparative Examples 1 to 4 obtained in [Preparation of Test Substrates] were cut with a grid guide at 1 mm intervals to prepare 25 grids (5×5) with a width of 1 mm in both the vertical and horizontal directions, and a transparent adhesive tape (width 25±1 mm) was attached to the portion of the grid cut into the cured coating film. The tape was firmly rubbed with fingers so that the cured coating film was transparent and visible, and adhered, and was reliably peeled off within 0.5 to 1.0 seconds at an angle close to 60 degrees within 5 minutes (tape peeling), and the state of the grid was investigated.

[0142] The cross-cut was subjected to two conditions in total: after the cured coating film was prepared, it was allowed to stand at 23°C and 50% RH for 3 hours (initial adhesion) and after it was allowed to stand in a constant temperature and humidity chamber (ESPEC CORP. LHL-114) at 85°C and 85% relative humidity for 240 hours (85°C and 85% RH adhesion).

[0143] The evaluation criteria are as follows: When the evaluation criteria are other than "△" and "×", the adhesion between the cured coating film and the test substrate is good, and when the evaluation criteria are "◎", the adhesion is particularly good.

[0144] ◎: The mesh remains 100% intact after peeling, with no gaps

[0145] 0: The mesh adhesion after peeling is 100% unchanged, and small gaps can be seen at the intersection of the mesh

[0146] △: The mesh adhesion after peeling is 100% unchanged, and peeling occurs at the intersection of the mesh

[0147] ×: The mesh after peeling is not 100% attached.

[0148] The results are shown in Table 2 below.

[0149] [Pencil hardness]

[0150] The pencil hardness of the surface of the cured coating film on each test substrate of the curable resin composition of Examples 1 to 10 and Comparative Examples 1 to 4 obtained in [Preparation of Test Substrates] was measured in accordance with JIS K 5600-5-41999 and evaluated as follows. When the evaluation criteria are other than "×", it means that the hardness of the cured coating film is high, and when the judgment criteria are "◎", it means that the hardness is particularly high.

[0151] ◎: H or above

[0152] 0:HB

[0153] ×: B or below

[0154] The results are shown in Table 2 below.

[0155] [Dryness to touch after UV curing (adhesiveness test)]

[0156] The dryness to touch of the cured coating films on the test substrates of the curable resin compositions of Examples 1 to 10 and Comparative Examples 1 to 4 obtained in [Preparation of Test Substrates] was evaluated as follows. When the evaluation criteria are other than "×", the curability of the surface of the cured coating film is good, and when the evaluation criteria are "◎", the curability of the surface of the cured coating film is particularly good.

[0157] ◎: No marks left even when touched with fingers

[0158] ○: Touching with a finger leaves a slight mark, but there is no problem in practical use

[0159] ×: It is sometimes sticky when touched with fingers, and the pigment component remains on the fingers

[0160] The results are shown in Table 2 below.

[0161] [OD value]

[0162] The OD values ​​of the cured coating films on the test substrates of the curable resin compositions of Examples 1 to 10 and Comparative Examples 1 to 4 prepared in the same manner were measured as follows, except that the film thickness after curing was changed to 10 μm or 20 μm.

[0163] The cured coating film side of the glass substrate was directed toward a measuring device and attached to a transmission density meter (manufactured by SAKATA INX CORPORATION, model: X-Rite 361T, light source wavelength: 400 to 800 nm) to evaluate the OD value.

[0164] As a result, the OD value of each Example and each Comparative Example with a film thickness of 10 μm after curing was 4 or more and 6 or less, and the OD value of each Example and each Comparative Example with a film thickness of 20 μm after curing was 6 or more.

[0165] This is an OD value sufficient for use as a black sunscreen.

[0166] The film thickness after curing was 10 μm or 20 μm as follows: in the same manner as in [Preparation of Test Substrate], drawing was performed with an inkjet printer at 5 μm intervals, followed by UV curing and stacking to a predetermined film thickness.

[0167] [Table 2]

[0168]

[0169] The evaluation results of the OD values ​​and the results shown in Table 2 show that in each example using the curable resin composition of the present invention, in addition to high light-shielding properties, the surface curing properties are also good.

[0170] Stable adhesion under high temperature and high humidity conditions is exhibited, and a cured film with high hardness after curing can be formed. In addition, in Examples 1, 3, 5, and 6, the mass ratio of the alicyclic epoxy compound having an ester bond in the molecule (a) to the alicyclic epoxy compound not having an ester bond in the molecule (b) is set to a more preferred range of 8:100 to 25:100, and the mass ratio of the oxetane compound (B) to the aforementioned epoxy compound (A) is set to a more preferred range of 10:100 to 20:100, and each evaluation result is the best result within the evaluation criteria. In particular, the cross-cut (85°C 85%RH adhesion) and pencil hardness under high temperature and high humidity conditions are better than those of the Examples.

[0171] In contrast, in Comparative Examples 1 and 2, where the mass ratio of (a) the alicyclic epoxy compound having an ester bond in the molecule to (b) the alicyclic epoxy compound not having an ester bond in the molecule was 43:100 to 50:100, which was outside the range, and Comparative Example 3, which did not contain (a) the alicyclic epoxy compound having an ester bond in the molecule, the cross-cut (initial adhesion) was slightly inferior to that of the Examples, and the cured coating film was peeled off in the cross-cut under high temperature and high humidity conditions (85°C 85% RH adhesion), which was the worst result within the evaluation criteria. In addition, the pencil hardness of Comparative Examples 1 to 3 was also the worst result within the evaluation criteria.

[0172] In Comparative Example 4, although the evaluation result of the cross-cut was good, the pencil hardness and the tackiness were the worst results in the evaluation criteria.

Claims

1. A curable resin composition comprising: (A) an epoxy compound, (B) an oxetane compound, (C) a photoacid generator, and (D) a black colorant, The (A) epoxy compound comprises a mass ratio in a numerical range of 5:100 to 30:

100. (a) an alicyclic epoxy compound having an ester bond in the molecule and (b) an alicyclic epoxy compound not having an ester bond in the molecule. 2 . The curable resin composition according to claim 1 , which has a viscosity of 5 to 20 mPa·s at 50° C.

3. The curable resin composition according to claim 1, wherein The (b) alicyclic epoxy compound having no ester bond in the molecule has a bifunctional epoxy group.

4. The curable resin composition according to claim 1 or 2, wherein The (D) black colorant is carbon black, and is contained in an amount of 5 parts by mass or more based on 100 parts by mass of the total of the (A) epoxy compound and the (B) oxetane compound.

5. The curable resin composition according to any one of claims 1 to 3, wherein The mass ratio of the (B) oxetane compound to the (A) epoxy compound is in the range of 2:100 to 40:

100.

6. The curable resin composition according to claim 5, wherein The (A) epoxy compound includes (a) an alicyclic epoxy compound having an ester bond in the molecule and (b) an alicyclic epoxy compound not having an ester bond in the molecule at a mass ratio in a numerical range of 8:100 to 25:

100.

7. The curable resin composition according to claim 6, wherein The mass ratio of the (B) oxetane compound to the (A) epoxy compound is in the range of 10:100 to 20:100.

Citation Information

Patent Citations

  • Active energy beam-curable ink and ink-jet recording method using active energy beam-curable ink