Sulfonated polyarylene sulfone polymers (sp) having at least bimodal molecular weight distribution
Through the sulfonated polyarylene sulfone polymer with bimodal molecular weight distribution, the production process is simplified and the ion conductivity of the membrane is improved, the complex production and separation problems in the prior art are solved, and efficient hydrogen separation is achieved Effect.
Patent Information
- Application Number
- CN202380023911.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-23
- Publication Date
- 2024-11-05
AI Technical Summary
The existing production methods for sulfonated polyarylene sulfone polymers have long reaction times and complex post-treatment processes. Especially when using a large number of disulfonated monomers, it is difficult to control the degree of sulfonation and separation of products, resulting in the resumption of solvent mixtures. Processing and filter clogging issues.
Using sulfonated polyarylene sulfone polymers with bimodal molecular weight distribution, the molecular weight distribution and sulfonation degree of the polymer are controlled through specific polycondensation reaction methods and solvent systems, simplifying the production process and improving the purity of the product.
The production process is simplified, solvent use and post-treatment steps are reduced, product purity and membrane ion conductivity are improved, and membrane materials are suitable for membrane materials that separate hydrogen from hydrogen-containing gas mixtures.
Smart Images

Figure BDA0005012505570000061 
Figure BDA0005012505570000062 
Figure BDA0005012505570000081
Abstract
Description
[0001] The present invention relates to a sulfonated polyarylene sulfone polymer (sP) having at least a bimodal molecular weight distribution, a method for preparing the sulfonated polyarylene sulfone polymer (sP), a membrane (M) comprising the sulfonated polyarylene sulfone polymer (sP), a method for preparing the membrane (M) and the membrane (M) obtained by the method.
[0002] Politics, society and industry aim to reduce CO2 emissions by decarbonizing industry and mobility. In this context, green hydrogen plays a strategic role due to its ability to replace hydrocarbons in chemical and industrial processes, energy conversion and fuel cell propulsion in mobility applications. Renewable electricity can be used to operate electrolyzers to produce green sustainable hydrogen.
[0003] The key components in electrolyzers and electrodialysis cells are the so-called polymer electrolyte membranes (PEMs), which must meet several requirements. They need to be ion-conducting and separate the gases hydrogen and oxygen at the same time. In addition, the membranes must be robust and stable for long-term operation and lifetime, with constant performance.
[0004] Prior art membranes are mainly based on fluorinated polymers with sulfonic acid side chains (PFSA), which are marketed for example under the trade name Due to the complexity of PFSA production, these polymers are still quite expensive. In addition, the toxicity and persistence of fluorinated chemicals pose several challenges to the production, use and recycling of these materials. Therefore, science and industry try to develop more sustainable solutions to replace PFSA membranes.
[0005] A promising class of materials for these applications is polyarylene sulfone polymers. They belong to the group of high-performance polymers with high thermal resistance, chemical resistance, excellent mechanical properties and durability (EM Koch, H.-M. Walter, Kunststoffe 80 (1990) 1146; E. Kunststoffe 80, (1990) 1149, N. Inchaurondo-Nehm, Kunststoffe 98, (2008) 190).
[0006] In addition to use as engineering plastics, polyarylene sulfone polymers are also used as membrane materials for water treatment (US 9,199,205).
[0007] The polyarylene sulfone polymers can be formed, inter alia, via the hydroxide process, in which a salt is first formed from a dihydroxy component and a hydroxide, or via the carbonate process.
[0008] General information on the formation of polyarylene sulfone polymers by the hydroxide process is found, inter alia, in RN Johnson et al., J. Polym. Sci. A-1 5 (1967) 2375, while the carbonate process is described in JEMcGrath et al., Polymer 25 (1984) 1827.
[0009] Processes for forming polyarylene sulfone polymers from aromatic bishalogen compounds and aromatic bisphenols or their salts in an aprotic solvent in the presence of one or more alkali metal or ammonium carbonates or bicarbonates are known to those skilled in the art and are described, for example, in EP-A 297 363 and EP-A 135 130.
[0010] High performance thermoplastics such as polyarylene sulfone polymers are formed by polycondensation reactions, which are typically carried out in polar aprotic solvents such as DMF (dimethylformamide), DMAc (dimethylacetamide), sulfolane, DMSO (dimethylsulfoxide), and NMP (N-methyl-pyrrolidone) at high reaction temperatures.
[0011] For use as membrane material in water electrolysis, electrodialysis or fuel cells, the polymers must exhibit ion conductivity, which can be achieved by functionalizing the polyarylene sulfone polymers with sulfonic acid groups.
[0012] Sulfonated polyarylene sulfone polymers have been known for decades. Although direct sulfonation of polyarylene sulfone polymers causes side reactions and allows only limited control over the degree of sulfonation, the use of disulfonated aromatic dihalogen sulfones such as sulfonated dichlorodiphenyl sulfone (sDCDPS) as comonomers allows the synthesis of well-defined sulfonated polyarylene sulfone polymers.
[0013] Although sulfonated polyarylene sulfone polymers show several interesting properties for use as ion-conducting membranes in fuel cells, electrodialysis cells or for electrolysis, the main problem that still has to be solved is the production method itself. One challenge is the very long reaction time and large-scale post-processing and separation of such copolymers, especially if a large amount of disulfonated monomers are used. The condensation produces a polymer suspension containing the sulfonated copolymer (sulfonated polyarylene sulfone polymer) and salt. After separation of the salt, precipitation is usually carried out in isopropanol to separate the sulfonated polyarylene sulfone polymer, which causes a large amount of solvent mixture to be reprocessed or disposed of. In addition, a portion of the product is not completely precipitated and can cause clogging of the filter during subsequent separation. In addition, in order to produce a membrane, the sulfonated copolymer must be dissolved again.
[0014] The object of the present invention is therefore to provide a sulfonated polyarylene sulfone polymer (sP) and a process for preparing the sulfonated polyarylene sulfone polymer (sP) which does not retain the disadvantages of the prior art or retains the disadvantages of the prior art only in a reduced form. The process should be easy to implement. The sulfonated polyarylene sulfone polymer (sP) should be suitable for producing membranes, in particular membranes which are able to separate hydrogen from gas mixtures containing hydrogen.
[0015] This object is achieved by a sulfonated polyarylene sulfone polymer (sP) having at least a bimodal molecular weight distribution having at least one first peak (P1) and at least one second peak (P2), wherein the maximum of the first peak (P1) has a relative molecular mass in the range of 800 g / mol to 5 000 g / mol and the maximum of the second peak (P2) has a relative molecular mass in the range of 8 000 g / mol to 300 000 g / mol, wherein the relative molecular mass is determined by gel permeation chromatography using dimethylacetamide as solvent and using narrow distribution poly(methyl methacrylate) as standard.
[0016] Surprisingly, it has been found that sulfonated polyarylene sulfone polymers (sP) having at least a bimodal molecular weight distribution are suitable for preparing membranes (M). Membranes (M) comprising sulfonated polyarylene sulfone polymers (sP) having at least a bimodal molecular weight distribution show improved conductivity compared to membranes (M) comprising sulfonated polyarylene sulfone polymers (sP) having at least a bimodal molecular weight distribution.
[0017] The present invention will be described in more detail below.
[0018] Sulfonated polyarylene sulfone polymer (sP)
[0019] The sulfonated polyarylene sulfone polymers (sP) according to the invention have at least a bimodal molecular weight distribution.
[0020] In the context of the present invention, the term "at least bimodal molecular weight distribution" means that the molecular weight distribution within the sulfonated polyarylene sulfone polymer (sP) according to the present invention may be bimodal, trimodal, tetramodal or pentamodal, or it may contain even higher modalities. However, in a preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) is bimodal.
[0021] The peak state of the molecular weight distribution of the sulfonated polyarylene sulfone polymer (sP) according to the present invention is determined by the number of peaks in the GPC chart.
[0022] Unless otherwise stated, peaks are determined in the gel permeation chromatography (GPC) diagram of the corresponding sulfonated polyarylene sulfone polymer (sP). GPC measurements are performed using dimethylacetamide (DMAc) as solvent and narrow distribution poly(methyl)acrylate (PMMA) as standard. Preferably for GPC, the polymer (sulfonated polyarylene sulfone polymer (sP)) is dissolved in DMAc at a concentration of 4 mg / ml and the solution is then filtered using a 0.2 μm filter. 100 μl of this solution is injected into the system. The flow rate is typically set to 1 ml / min and 4 columns maintained at a temperature of 40°C are used for separation. An RI detector is used as a detector. The system is calibrated from 800 g / mol to 2200200 g / mol. The solvent used may also contain a small amount of salt, preferably LiBr.
[0023] Only those peaks which contribute more than 0.3 area %, preferably more than 0.4 area % to the total peak area in the GPC diagram are taken into account for determining the corresponding peak state. In the context of the present invention, the term "GPC diagram" refers to a diagram obtained by GPC showing the peak intensity on the y-axis relative to the relative molecular mass on the x-axis.
[0024] In other words, a relatively small peak in the baseline with a very low signal-to-noise ratio is not considered as a peak when determining the peak state of the corresponding polymer.
[0025] In the context of the present invention, the term "relative molecular mass" refers to the molecular weight of the sulfonated polyarylene sulfone polymer (sP) determined by GPC, which is set relative to the molecular weight of a narrow distribution poly(meth)acrylate standard with known molecular weight.
[0026] The sulfonated polyarylene sulfone polymer (sP) generally has at least a bimodal molecular weight distribution having at least one first peak (P1) and at least one second peak (P2).
[0027] The relative mass of the first peak (P1) is lower than the relative mass of the second peak (P2).
[0028] The maximum of the first peak (P1) has a relative molecular mass in the range of 800 g / mol to 5 000 g / mol, preferably in the range of 1000 g / mol to 4500 g / mol and more preferably in the range of 1250 g / mol to 4000 g / mol, wherein the relative molecular mass is determined by gel permeation chromatography using dimethylacetamide as solvent and using narrow distribution poly(methyl methacrylate) as standard as described above.
[0029] The maximum of the second peak (P2) has a relative molecular mass in the range of 8 000 g / mol to 300 000 g / mol, preferably in the range of 9 000 g / mol to 275 000 g / mol and more preferably in the range of 10 000 g / mol to 270 000 g / mol, wherein the relative molecular mass is determined by gel permeation chromatography using dimethylacetamide as solvent and using narrow distribution poly(methyl methacrylate) as standard as described above.
[0030] To determine the relative molecular masses of the peak (P1 and P2) maxima, a vertical line was dropped from each maximum to the x-axis of the GPC graph.
[0031] The maximum value of the first peak (P1) preferably shows a lower intensity than the second peak (P2).
[0032] The ratio of the first intensity (I1) to the second intensity (I2) is generally in the range of 1:8 to 1:100, preferably in the range of 1:8 to 1:50, and more preferably in the range of 1:8 to 1:40.
[0033] The term intensity is preferably understood herein as the height of the maximum of a peak in the GPC diagram.
[0034] FIG. 1 shows a preferred embodiment of a GPC diagram of a sulfonated polyarylene sulfone polymer (sP) having a bimodal molecular weight distribution. The intensity is shown on the y-axis. The relative molecular mass is shown on the x-axis. The maximum value of the first peak (P1) has a lower relative molecular weight than the maximum value of the second peak (P2). In order to determine the relative molecular weight of the maximum value of the first peak (P1), a vertical (indicated as I1 in FIG. 1) line (indicated as I1 in FIG. 1) is dropped from the maximum value of the first peak (P1) to the x-axis. The relative molecular weight of the maximum value of the second peak is determined accordingly.
[0035] To determine the intensity of the maxima of peaks (P1) and (P2), the heights of the peaks were measured.
[0036] Therefore, another object of the present invention is a sulfonated polyarylene sulfone polymer (sP), wherein the maximum of the first peak (P1) shows a first intensity (I1), and the maximum of the second peak (P2) shows a second intensity (I2), wherein the ratio of the first intensity (I1) to the second intensity (I2) is in the range of 1:10 to 1:1000.
[0037] The sulfonated polyarylene sulfone polymer (sP) generally has a weight average molecular weight (M) in the range of 20 000 g / mol to 250 000 g / mol, preferably in the range of 30 000 g / mol to 225 000 g / mol and more preferably in the range of 40 000 g / mol to 200 000 g / mol. W ), wherein the weight average molecular weight (M W ) was determined by gel permeation chromatography using dimethylacetamide as solvent and narrow distribution poly(methyl methacrylate) as standard as described above.
[0038] Therefore, another object of the present invention is a sulfonated polyarylene sulfone polymer (sP), wherein the sulfonated polyarylene sulfone polymer (sP) has a weight average molecular weight (M) in the range of 20 000 g / mol to 250 000 g / mol. W ), wherein the weight average molecular weight (M W ) was determined by gel permeation chromatography using dimethylacetamide as solvent and narrow distribution poly(methyl methacrylate) as standard.
[0039] In a preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) comprises 15 mol-% to 80 mol-%, preferably in the range of 20 mol-% to 70 mol-%, and more preferably in the range of 25 mol-% to 65 mol-%, based on the total amount of the sulfonated polyarylene sulfone polymer (sP), of at least one -SO3X 3 The sulfonated repeating unit of the group, wherein X 3 is hydrogen or a cation equivalent.
[0040] Repeat units are preferably understood as meaning units which are derived from an aromatic dihalosulfone and an aromatic dihydroxy compound; for example, repeat units may be derived from a 4,4'-dihydroxybiphenyl and a 4,4'-dichlorodiphenyl sulfone, giving non-sulfonated repeat units, or repeat units may be derived from a 4,4'-dihydroxybiphenyl and a 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid, giving sulfonated repeat units.
[0041] The term repeating unit is known to the person skilled in the art and is also referred to as recurring unit or repeating unit.
[0042] Therefore, another object of the present invention is a sulfonated polyarylene sulfone polymer (sP), wherein the sulfonated polyarylene sulfone polymer (sP) comprises, based on the total amount of the sulfonated polyarylene sulfone polymer (sP), 15 mol-% to 80 mol-% of a sulfonated polyarylene sulfone polymer (sP) comprising at least one -SO3X 3 The sulfonated repeating unit of the group, wherein X 3is hydrogen or a cation equivalent.
[0043] Preferred sulfonated polyarylene sulfone polymers (sP) comprise sulfonated repeating units of the general formula I:
[0044]
[0045] in
[0046] t and q: each independently 0, 1, 2 or 3,
[0047] Q 1 , T and Y 1 : Each independently is a chemical bond or selected from -O-, -S-, -SO2-,
[0048] -S(=O)-, -C(=O)-, -N=N- and -CR a R b -,
[0049] Where R a and R b are independently a hydrogen atom or a C1-C 12 -alkyl, C1-C 12 -alkoxy or C6-C 18 -aryl group, and wherein at least one of Q, T and Y is -SO2-,
[0050] Ar and Ar 1 : Each independently is C6-C 18 Aryl, wherein the C6-C 18 The aryl group is unsubstituted or substituted by at least one substituent selected from the group consisting of: C1-C 12 Alkyl, C1-C 12 Alkoxy, C6-C 18 Aryl, halogen and -SO3X,
[0051] p, m, n and k: are each independently 0, 1, 2, 3 or 4, provided that p, m,
[0052] The sum of n and k is not less than 1, and
[0053] X 3 : is hydrogen or a cation equivalent.
[0054] Therefore, another object of the present invention is a sulfonated polyarylene sulfone polymer (sP), wherein the sulfonated polyarylene sulfone polymer (sP) comprises repeating units of the general formula (I):
[0055]
[0056] in
[0057] t and q: each independently 0, 1, 2 or 3,
[0058] Q 1 , T and Y 1 : Each independently is a chemical bond or selected from -O-, -S-, -SO2-,
[0059] -S(=O)-, -C(=O)-, -N=N- and -CR a R b -,
[0060] Where R a and R b are independently a hydrogen atom or a C1-C 12 -alkyl,
[0061] C1-C 12 -alkoxy or C6-C 18 -aryl group, and wherein Q, T
[0062] At least one of Y is -SO2-,
[0063] Ar and Ar 1 : Each independently is C6-C 18 Aryl, wherein the C6-C 18 The aryl group is unsubstituted or substituted with at least one substituent selected from the following:
[0064] C1-C 12 Alkyl, C1-C 12 Alkoxy, C6-C 18 Aryl, halogen and -
[0065] SO3X,
[0066] p, m, n and k: are each independently 0, 1, 2, 3 or 4, provided that p, m, n and
[0067] The sum of k is not less than 1, and
[0068] X 3 : is hydrogen or a cation equivalent.
[0069] In a preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) comprises at least 80 wt.-%, based on the total weight of the sulfonated polyarylene sulfone polymer (sP), of recurring units of the general formula (I).
[0070] If under the above premise, Q 1 , T or Y 1 is a chemical bond, then this means that the adjacent group on the left-hand side and the adjacent group on the right-hand side are directly connected to each other by a chemical bond.
[0071] R a and R b are independently hydrogen or C1-C 12 alkyl.
[0072] Preferred C1-C 12 Alkyl groups include straight and branched saturated alkyl groups having 1 to 12 carbon atoms. The following moieties are particularly suitable: C1-C6 alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, 2-methylpentyl or 3-methylpentyl, and relatively long chain moieties such as unbranched heptyl, octyl, nonyl, decyl, undecyl, lauryl, and branched analogs thereof.
[0073] C1-C used 12 The alkyl moiety in the alkoxy group includes the alkyl groups having 1 to 12 carbon atoms as defined above. The cycloalkyl moieties preferably used include in particular C3-C 12 Cycloalkyl moieties, for example, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclopropylmethyl, cyclopropylethyl, cyclopropylpropyl, cyclobutylmethyl, cyclobutylethyl, cyclopentylethyl, cyclopentylpropyl, cyclopentylbutyl, cyclopentylpentyl, cyclopentylhexyl, cyclopentylcyclohexylmethyl, -cyclopentyldimethyl, cyclopentyltrimethyl.
[0074] Ar and Ar 1 Each independently is C6-C 18 Aryl. From the starting materials below, Ar is preferably derived from an electron-rich aromatic substance that is very susceptible to electrophilic attack, preferably selected from the group consisting of sulfonated or non-sulfonated hydroquinone, resorcinol, dihydroxynaphthalene, especially 2,7-dihydroxynaphthalene. Ar 1 Preferably, it is unsubstituted C6 or C 12 Arylene group.
[0075] In a preferred embodiment, Ar and Ar of formula (I) 1 Preferably each is independently selected from sulfonated or non-sulfonated 1,4-phenylene, 1,3-phenylene, naphthylene, in particular 2,7-dihydroxynaphthalene.
[0076] Preferred are sulfonated polyarylene sulfone polymers (sP) having one or more of the following structural units (Ia) to (Io):
[0077]
[0078]
[0079] in
[0080] l, k, m, n, o, p are each independently 0, 1, 2, 3 or 4, provided that the sum of l, k, m, n, o and p is ≥ 1, and
[0081] X 3 is hydrogen or a cation equivalent.
[0082] In the context of the present invention, reference to "a cation equivalent" means a cation of a single positive charge or a charge equivalent of a cation carrying two or more positive charges, such as Li, Na, K, Mg, Ca, NH4, preferably Na, K.
[0083] In addition to the preferred building blocks (Ia) to (Io), preference is also given to those structural units in which one or more sulfonated or nonsulfonated 1,4-dihydroxyphenyl units are replaced by resorcinol or dihydroxynaphthalene.
[0084] Copolymers composed of various combinations of structural units or composed of sulfonated and non-sulfonated structural units are also useful.
[0085] In particularly preferred cases, the structural units (Ia), (Ib), (Ig) and (Ik) or copolymers thereof are used as repeating units of the general formula (I).
[0086] In a particularly preferred embodiment, Ar is 1,4-phenylene, t is 1, T is a chemical bond, and Y 1 is -SO2-, q is 0, p is 0, m is 0, n is 1 and k is 1. Sulfonated polyphenylene sulfone composed of the above-mentioned structural repeating units is represented by sPPSU.
[0087] In a particularly preferred embodiment, Ar is 1,4-phenylene, t is 0, Y is -SO2-, q is 0, n is 0 and k is 0. Polyarylene sulfones composed of this listed structural repeating unit are referred to as sulfonated polyetherethersulfones (sPESU).
[0088] In an advantageous embodiment, the sulfonated polyarylene sulfone polymer (sP) comprises:
[0089] The non-sulfonated repeating unit of formula (1)
[0090]
[0091] and the sulfonated repeating unit of formula (2)
[0092]
[0093] Specifically, the sulfonated polyarylene sulfone polymer (sP) consists exclusively of non-sulfonated repeating units of formula (1) and sulfonated repeating units of formula (2).
[0094] In a very advantageous embodiment, the sulfonated polyarylene sulfone polymer (sP) comprises:
[0095] The non-sulfonated repeating unit of formula (1a)
[0096]
[0097] and the sulfonated repeating unit of formula (2a)
[0098]
[0099] Specifically, the sulfonated polyarylene sulfone polymer (sP) consists exclusively of non-sulfonated repeating units of formula (1a) and sulfonated repeating units of formula (2a).
[0100] method
[0101] The sulfonated polyarylene sulfone polymer (sP) according to the present invention is preferably prepared by reacting a reaction mixture (R) comprising an aromatic dihalogen sulfone component, at least one aromatic dihydroxy compound and at least one carbonate compound. G ) conversion. In a preferred embodiment, the reaction mixture (R G ) further comprises at least one aprotic polar solvent.
[0102] The aromatic dihalogen sulfone component is also referred to as component (A). The terms "aromatic dihalogen sulfone component" and "component (A)" in the present invention are used synonymously and thus have the same meaning.
[0103] The at least one aromatic dihydroxy compound is also referred to as component (B). The terms "at least one aromatic dihydroxy compound" and "component (B)" in the present invention are used synonymously and thus have the same meaning.
[0104] The at least one carbonate compound is also referred to as component (C). The terms "at least one carbonate compound" and "component (C)" in the present invention are used synonymously and therefore have the same meaning.
[0105] The at least one aprotic polar solvent is also referred to as component (D). The terms "at least one aprotic polar solvent" and "component (D)" in the present invention are used synonymously and therefore have the same meaning.
[0106] Therefore, another object of the present invention is a process for preparing a sulfonated polyarylene sulfone polymer (sP), which comprises the steps i) subjecting a reaction mixture (R G ) conversion, the reaction mixture comprising as components
[0107] (A) an aromatic dihalogen sulfone component, the aromatic dihalogen sulfone component comprising
[0108] at least one sulfonated aromatic dihalogen sulfone (component (A1)) and at least one non-sulfonated aromatic dihalogen sulfone (component (A2)),
[0109] (B) at least one aromatic dihydroxy compound, and
[0110] (C) at least one carbonate compound.
[0111] Therefore, another object of the present invention is a process in which the reaction mixture (R G )) further comprises at least one aprotic polar solvent (component (D)).
[0112] Reaction mixture (R G ) is a mixture provided for forming a sulfonated polyarylene sulfone polymer (sP). G ) are therefore all components involved in the mixture present before the polycondensation. By the polycondensation of component (A) and component (B), the polycondensation takes place so that the reaction mixture (R G ) is converted into the target product sulfonated polyarylene sulfone polymer (sP).
[0113] In step i), component (A) and component (B) enter into a polycondensation reaction. Component (C) acts as a base to deprotonate the hydroxyl groups of component (B). Component (D), if present, acts as a solvent.
[0114] The mixture obtained after polycondensation containing the target product of sulfonated polyarylene sulfone polymer (sP) is also referred to as product mixture (P G ). The product mixture (P G ) preferably further comprises a halide and preferably at least one aprotic polar solvent (component (D)). G ). During the conversion, component (C) reacts with component (B) to deprotonate component (B). Then, the deprotonated component (B) reacts with component (A), whereby a halide is formed. This process is known to those skilled in the art.
[0115] Reaction mixture (R G ) are preferably reacted simultaneously. The components can be mixed in an upstream step and then reacted. It is also possible to feed the components into a reactor, where they are mixed and then reacted.
[0116] In the process according to the invention, the reaction mixture (R G) are preferably reacted simultaneously in step i). The reaction is preferably carried out in one stage. This means that the deprotonation of component (B) and the condensation reaction between component (A) and component (B) occur in a single reaction stage without isolating intermediate products, such as the deprotonated substance of component (B).
[0117] Furthermore, it is preferred that the reaction mixture (R G ) does not contain toluene or monochlorobenzene. Particularly preferably, the reaction mixture (R G ) does not contain any substance that forms an azeotrope with water.
[0118] The ratio of component (A) to component (B) results in principle from the stoichiometry of the polycondensation reaction which is carried out theoretically with elimination of hydrogen chloride and is established in a known manner by the person skilled in the art.
[0119] Preferably, the ratio of halogen end groups derived from component (A) to phenolic end groups derived from component (B) is adjusted by controlled establishment of an excess of component (A) relative to component (B) as starting compound.
[0120] Preferably, the conversion rate in the polycondensation reaction is at least 0.9.
[0121] Process step i) for preparing the sulfonated polyarylene sulfone polymer (sP) is preferably carried out under the conditions of the so-called "carbonate process". This means that the reaction mixture (R G ) under the conditions of the so-called "carbonate process". The polycondensation reaction is usually carried out at a temperature in the range of 80° C. to 250° C., preferably in the range of 100° C. to 220° C. The upper limit of the temperature is preferably determined by the boiling point of the at least one aprotic polar solvent (component (D)) at standard pressure (1013.25 mbar). The reaction is usually carried out at standard pressure. The reaction is preferably carried out within a time interval in the range of 0.5 hour to 14 hours, in particular 1 hour to 12 hours.
[0122] In a preferred embodiment, in step i), the reaction mixture (R G ) conversion, the reaction mixture comprising
[0123] X mol of an aromatic dihalogen sulfone component (component A), the aromatic dihalogen sulfone component comprising: G ),
[0124] X 1 mol % of at least one sulfonated aromatic dihalogen sulfone (component (A1)), and
[0125] X 2mol.-% of at least one non-sulfonated aromatic dihalogen sulfone (component (A2)), wherein
[0126] X 1 In the range of 15 to 80, and
[0127] X 2 In the range of 20 to 85,
[0128] Y moles of at least one aromatic dihydroxy compound (component (B)),
[0129] Z moles of at least one carbonate compound (component (C)),
[0130] in
[0131] The ratio of X to Y is in the range of 0.95 to 1.05,
[0132] And among them
[0133] Z is in the range of P to Q,
[0134] Where P is calculated according to the following formula:
[0135] P=Y*(1.05+X 1 / 100*1.05),
[0136] And where Q is calculated according to the following formula:
[0137] Q=Y*(1.05+X 1 / 100*1.4).
[0138] More preferably, the molar ratio of component (A) to component (B) is from 0.95 to 1.05, especially from 0.96 to 1.04, most preferably from 0.97 to 1.03.
[0139] In a preferred embodiment, the ratio of X to Y is from 0.95 to 1.05, especially from 0.96 to 1.04, most preferably from 0.97 to 1.03.
[0140] In a preferred embodiment, no G ) isolating the sulfonated polyarylene sulfone polymer (sP) obtained in step i).
[0141] In a preferred embodiment, the product mixture (P G ) is further worked up by steps ii) and iii) as described below.
[0142] Thus, in a preferred embodiment, after step i), a product mixture (P) is obtained comprising the sulfonated polyarylene sulfone polymer (sP), the at least one aprotic polar solvent and the at least one inorganic halide compound. G ), and the method further comprises the following steps
[0143] ii) from the product mixture (P G ) to obtain a solution (S) comprising the sulfonated polyarylene sulfone polymer (sP) and the at least one aprotic polar solvent, and
[0144] iii) separating the at least one aprotic polar solvent from the solution (S) by evaporation to obtain the sulfonated polyarylene sulfone polymer (sP).
[0145] After step iii), the sulfonated polyarylene sulfone polymer (sP) can be further processed, for example by extraction with a solvent, preferably with a polar protic solvent such as water.
[0146] In step ii), from the product mixture (P G ) to remove the inorganic halide compound formed during the condensation reaction in step i). To obtain a solution (S) comprising the sulfonated polyarylene sulfone polymer (sP) and the at least one aprotic polar solvent (component (D)).
[0147] The inorganic halide compounds can be removed by means known in the art, such as filtration, centrifugation, decantation, and the like.
[0148] Therefore, the present invention also provides a method, wherein the method comprises the steps of
[0149] ii) treating the product mixture (P) obtained in step i) G ) is filtered, centrifuged and / or decanted to obtain a solution (S).
[0150] In a preferred embodiment, the solution (S) obtained in step ii) does not contain solid inorganic halide compounds. In a further preferred embodiment, the solution (S) obtained in step ii) contains less than 3 wt%, more preferably less than 1.5 wt% and particularly preferably less than 0.5 wt% of inorganic halide components based on the total weight of the solution (S) obtained in step ii).
[0151] In a more preferred embodiment, the solution (S) obtained in step ii) comprises no solid inorganic compounds.
[0152] In a further preferred embodiment, the solution (S) obtained in step ii) comprises less than 0.4 wt %, more preferably less than 0.3 wt % and particularly preferably less than 0.2 wt % of inorganic components, based on the total weight of the solution (S) obtained in step ii).
[0153] In a preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) in step ii) is not separated from the solution (S).
[0154] In a further preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) in the solution (S) in step ii) remains in dissolved form before step iii) is carried out.
[0155] In a particularly preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) in the process according to the invention remains dissolved until step iii) is carried out.
[0156] In a further particularly preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) is not isolated before carrying out step iii).
[0157] The components used in the process of the present invention for preparing the sulfonated polyarylene sulfone polymer (sP) will be described in more detail hereinafter.
[0158] Component (A)
[0159] Component (A), which is also referred to as the aromatic dihalogen sulfone component, comprises at least one sulfonated aromatic dihalogen sulfone and at least one non-sulfonated aromatic dihalogen sulfone.
[0160] The at least one sulfonated aromatic dihalogen sulfone is also referred to as component (A1). The terms "at least one sulfonated aromatic dihalogen sulfone" and "component (A1)" in the present invention are used synonymously and therefore have the same meaning.
[0161] The at least one non-sulfonated aromatic dihalogen sulfone is also referred to as component (A2). The terms "at least one non-sulfonated aromatic dihalogen sulfone" and "component (A2)" in the present invention are used synonymously and therefore have the same meaning.
[0162] Reference herein to "at least one sulfonated aromatic dihalogen sulfone" is intended to mean exactly one sulfonated aromatic dihalogen sulfone as well as mixtures of two or more sulfonated aromatic dihalogen sulfones. Preferably exactly one sulfonated aromatic dihalogen sulfone is used.
[0163] Reference herein to "at least one non-sulfonated aromatic dihalogen sulfone" is intended to mean exactly one non-sulfonated aromatic dihalogen sulfone as well as mixtures of two or more non-sulfonated aromatic dihalogen sulfones. Preferably exactly one non-sulfonated aromatic dihalogen sulfone is used.
[0164] "X" preferably means the reaction mixture (R G ) in the reaction mixture (R G ) is the total molar amount of the aromatic dihalogen sulfone component (component (A)). In other words, "X" preferably means the molar amount of the aromatic dihalogen sulfone component (component (A)) contained in component (A), preferably in the reaction mixture (R G ) is the sum of the molar amounts of component (A1) and component (A2) contained in the reaction mixture (R G ) in the total molar amount of component (A), "X 1 " means herein the molar amount of component (A1) in mol %, and "X 2 " refers herein to the molar amount of component (A2) in mol %.
[0165] X 1 For example in the range of 15 to 80 mol.-%, preferably in the range of 20 to 70 mol.-%, more preferably in the range of 25 to 65 mol.-%, and most preferably in the range of 27.5 to 62.5 mol.-%, in each case based on the reaction mixture (R G ) is the total molar amount of the aromatic dihalogen sulfone component (component (A)).
[0166] X 2 Typically in the range of 20 mol.-% to 85 mol.-%, preferably in the range of 30 mol.-% to 80 mol.-%, more preferably in the range of 35 mol.-% to 75 mol.-% and most preferably in the range of 37.5 mol.-% to 72.5 mol.-%, in each case based on the reaction mixture (R G ) is the total molar amount of the aromatic dihalogen sulfone component (component (A)).
[0167] X 1 and X 2 The amounts generally add up to 100 mol %.
[0168] Component (A1)
[0169] Component (A1) (which is also referred to as sulfonated aromatic dihalogen sulfone) preferably comprises at least one -SO3X 3 Group.
[0170] Component (A1) preferably contains at least one -SO3X 3 Group. In this article, "at least one -SO3X 3 "Group" means that component (A1) may contain exactly one -SO3X3 group and two or more -SO3X 3 More preferably, component (A1) contains two -SO3X 3 Group.
[0171] General formula - SO3X 3 Contains sulfonic acid functional groups and derivatives of sulfonic acid functional groups such as sulfonates. 3 In the group, X 3 Can be hydrogen and / or a cation equivalent.
[0172] In the context of the present invention, reference to "a cation equivalent" means a cation of a single positive charge or a charge equivalent of a cation with two or more positive charges, such as Li, Na, K, Mg, Ca, NH4, preferably Na, K. Particularly preferred are Na or K.
[0173] Component (A1) is preferably selected from the group consisting of 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid and 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid and derivatives thereof.
[0174] In the context of the present invention, the terms "sulfonic acid" and "-SO3X 3 The term "sulfonic acid" in 4,4'-dichlorodiphenylsulfone-3,3'-disulfonic acid and 4,4'-difluorodiphenylsulfone-3,3'-disulfonic acid means "-SO3X 3 Group", where X 3 is hydrogen or a cation equivalent.
[0175] In one embodiment, component (A1) preferably comprises -SO3X with a cation equivalent 3 Particularly preferably, component (A1) is selected from the group consisting of 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid disodium salt and 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt.
[0176] Therefore, another object of the present invention is a process, wherein component (A1) comprises at least one compound selected from the group consisting of 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid disodium salt and 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt.
[0177] In one embodiment, based on the reaction mixture (R G ) in the total weight of component (A1), component (A1) comprises not less than 70 wt%, preferably not less than 90 wt%, and more preferably not less than 98 wt% of at least one aromatic dihalogen sulfone component, the at least one aromatic dihalogen sulfone component comprising at least one -SO3X selected from the group consisting of 3 Groups: 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid disodium salt and 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt.
[0178] In another particularly preferred embodiment, component (A1) consists essentially of at least one aromatic dihalogen sulfone comprising at least one -SO3X selected from the group consisting of 3 Groups: 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid disodium salt and 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt.
[0179] In these embodiments, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt and 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt are particularly preferred for use as component (A1).
[0180] In another particularly preferred embodiment, component (A1) consists of 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt or 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt.
[0181] Component (A2)
[0182] Component (A2) (which is also referred to as the non-sulfonated aromatic dihalogen sulfone component) preferably does not contain -SO3X 3 Group.
[0183] Preferably, based on the reaction mixture (R G ) in the total weight of component (A2), component (A2) comprises not less than 80% by weight, preferably not less than 90% by weight, and more preferably not less than 98% by weight of at least one aromatic dihalogen sulfone selected from the group consisting of 4,4'-dichlorodiphenyl sulfone and 4,4'-difluorodiphenyl sulfone. The weight percentages related to component (A2) here further relate to the sum of the 4,4'-dichlorodiphenyl sulfone used and the 4,4'-difluorodiphenyl sulfone used.
[0184] Therefore, another object of the present invention is a process in which, based on the reaction mixture (R G ) in the present invention, component (A2) contains not less than 80 wt % of at least one aromatic dihalogen sulfone selected from the group consisting of 4,4'-dichlorodiphenyl sulfone and 4,4'-difluorodiphenyl sulfone, based on the total weight of component (A2) in the present invention.
[0185] In another particularly preferred embodiment, component (A2) consists essentially of at least one aromatic dihalogen sulfone selected from the group consisting of 4,4'-dichlorodiphenyl sulfone and 4,4'-difluorodiphenyl sulfone. In these embodiments, 4,4'-dichlorodiphenyl sulfone is particularly preferred for use as component (A2).
[0186] Preferably, component (A2) is selected from the group consisting of 4,4'-dichlorodiphenyl sulfone and 4,4'-difluorodiphenyl sulfone.
[0187] Component (B)
[0188] Component (B), which is also referred to as an aromatic dihydroxy compound, generally comprises two hydroxyl groups.
[0189] Reference herein to "at least one aromatic dihydroxy compound" is to exactly one aromatic dihydroxy compound as well as mixtures of two or more aromatic dihydroxy compounds. Preferably exactly one aromatic dihydroxy compound is used.
[0190] "Y" preferably means the reaction mixture (R G ) in the reaction mixture (R G ) is the total molar amount of the aromatic dihydroxy compound (component (B)).
[0191] Preferably, component (B) is selected from the group consisting of 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl sulfone, bisphenol A (2,2-bis(4-hydroxyphenyl)propane), 4,4'-dihydroxybenzophenone and hydroquinone. From among the above aromatic dihydroxy components, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl sulfone, bisphenol A are preferred, and 4,4'-dihydroxybiphenyl is particularly preferred.
[0192] Therefore, the present invention also provides a process, wherein component (B) is selected from the group consisting of 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl sulfone, bisphenol A, 4,4'-dihydroxybenzophenone and hydroquinone.
[0193] Preferably, based on the reaction mixture (R G ) in the total weight of component (B), component (B) contains not less than 80 wt%, preferably not less than 90 wt%, and more preferably not less than 98 wt% of 4,4'-dihydroxybiphenyl.
[0194] Therefore, another object of the present invention is a process in which, based on the reaction mixture (R G ) in the total weight of component (B), component (B) contains not less than 80 wt% of 4,4'-dihydroxybiphenyl.
[0195] The percentages by weight relating to component (B) here further relate to the sum of the 4,4′-dihydroxybiphenyl, 4,4′-dihydroxydiphenyl sulfone, bisphenol A (2,2-bis-(4-hydroxyphenyl)-propane), 4,4′-dihydroxybenzophenone and hydroquinone used.
[0196] In another particularly preferred embodiment, component (B) consists essentially of at least one aromatic dihydroxy component selected from the group consisting of 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl sulfone, bisphenol A (2,2-bis(4-hydroxy-phenyl)propane), 4,4'-dihydroxybenzophenone and hydroquinone. In these embodiments, 4,4'-dihydroxybiphenyl, bisphenol A and 4,4'-dihydroxydiphenyl sulfone are particularly preferred for use as component (B), while 4,4'-dihydroxybiphenyl is most preferred.
[0197] Component (C)
[0198] Reaction mixture (R G) comprises at least one carbonate compound as component (C). In this case, the term "at least one carbonate compound" is understood to mean exactly one carbonate compound, and also a mixture of two or more carbonate compounds. The at least one carbonate compound is preferably at least one metal carbonate. The metal carbonate is preferably anhydrous. In this case, the terms "at least one carbonate compound" and "component (C)" are used synonymously and therefore have the same meaning.
[0199] Alkali metal carbonates and / or alkaline earth metal carbonates are preferred as metal carbonates. At least one metal carbonate selected from the group consisting of sodium carbonate, potassium carbonate and calcium carbonate is particularly preferred as metal carbonate. Potassium carbonate is most preferred.
[0200] For example, based on the reaction mixture (R G ), component (C) comprises not less than 50 wt. %, more preferably not less than 70 wt. %, and most preferably not less than 90 wt. % potassium carbonate, based on the total weight of the at least one carbonate component in the composition.
[0201] Therefore, another object of the present invention is a process in which, based on the reaction mixture (R G ) in the present invention, the component (C) contains not less than 50 wt % potassium carbonate, based on the total weight of the component (C) in the present invention.
[0202] In a preferred embodiment, component (C) consists of potassium carbonate. Potassium carbonate having a volume-weighted average particle size of less than 200 μm, more preferably less than 100 μm, even more preferably less than 70 μm, and most preferably less than 50 μm is preferably potassium carbonate. The volume-weighted average particle size of potassium carbonate is determined using a particle size analyzer in a suspension of potassium carbonate in a mixture of chlorobenzene / sulfolane (60 / 40 by weight).
[0203] "Z" preferably means the reaction mixture (R G ) in the reaction mixture (R G ) in the total molar amount of at least one carbonate component (component (C)).
[0204] Z is in the range of P to Q.
[0205] "P" is calculated according to the following formula:
[0206] P=Y*(1.05+X 1 / 100*1.05)
[0207] In this formula, Y is the reaction mixture (R G ) in the molar amount of component (B), and X1 is the reaction mixture (R G ) is the value of the mol % of component (A1) in ).
[0208] "Q" is calculated according to the following formula:
[0209] Q=Y*(1.05+X 1 / 100*1.4)
[0210] In this formula, Y is also the reaction mixture (R G ) in the molar amount of component (B), and X 1 Also the reaction mixture (R G ) is the value of the mol % of component (A1) in ).
[0211] Component (D)
[0212] Reaction mixture (R G ) preferably comprises at least one aprotic polar solvent as component (D). According to the invention, "at least one aprotic polar solvent" is understood to mean exactly one aprotic polar solvent and also mixtures of two or more aprotic polar solvents. In this case, the terms "at least one aprotic polar solvent" and "component (D)" are used synonymously and therefore have the same meaning.
[0213] Suitable aprotic polar solvents are, for example, selected from anisole, dimethylformamide, dimethyl sulfoxide, sulfolane, N-methylpyrrolidone, N-ethylpyrrolidone and N-dimethylacetamide.
[0214] Preferably, component (D) is selected from the group consisting of: N-methylpyrrolidone, N-dimethylacetamide, dimethyl sulfoxide and dimethylformamide. N-methylpyrrolidone is particularly preferred as component (D).
[0215] Preferably, based on the reaction mixture (R G ), component (D) contains not less than 50 wt %, preferably not less than 70 wt %, and more preferably not less than 90 wt % of at least one solvent selected from the group consisting of: N-methylpyrrolidone, N-dimethylacetamide, dimethyl sulfoxide and dimethylformamide. N-methylpyrrolidone is particularly preferred as component (D).
[0216] Therefore, another object of the present invention is a process in which, based on the reaction mixture (R G), based on the total weight of component (D) in the composition, component (D) contains not less than 50 wt % of at least one solvent selected from the group consisting of N-methylpyrrolidone, N-dimethylacetamide, dimethyl sulfoxide and dimethylformamide.
[0217] In a preferred embodiment, component (D) consists of N-methylpyrrolidone, which is also known as NMP or N-methyl-2-pyrrolidone.
[0218] Membrane (M)
[0219] The sulfonated polyarylene sulfone polymer (sP) according to the invention is suitable for preparing membrane (M).The sulfonated polyarylene sulfone polymer (sP) according to the invention can be used in membrane (M).
[0220] Another object of the present invention is therefore also the use of the sulfonated polyarylene sulfone polymer (sP) obtainable by the process of the invention in a membrane (M).
[0221] The membrane (M) can be prepared from the sulfonated polyarylene sulfone polymer (sP) according to the invention by any method known to the person skilled in the art.
[0222] Preferably, the membrane (M) comprising the sulfonated polyarylene sulfone polymer (sP) according to the present invention is prepared by a method comprising the following steps
[0223] i) providing a solution (S) comprising a sulfonated polyarylene sulfone polymer (sP) and at least one solvent,
[0224] ii) separating the at least one solvent from the solution (S) to obtain a membrane (M).
[0225] Therefore, another object of the present invention is a process for preparing a membrane (M) comprising a sulfonated polyarylene sulfone polymer (sP) obtained by the process of the present invention, comprising the following steps
[0226] i) providing a solution (S) comprising the sulfonated polyarylene sulfone polymer (sP) obtained by the process of the present invention and at least one solvent,
[0227] ii) separating the at least one solvent from the solution (S) to obtain a membrane (M).
[0228] In a preferred embodiment, the method for preparing a membrane (M) comprising a sulfonated polyarylene sulfone polymer (sP) according to any one of claims 1 to 5 comprises the following steps
[0229] ii-1) providing the solution (S) obtained in step ii) according to claim 9, said solution comprising the sulfonated polyarylene sulfone polymer (sP) and the at least one aprotic polar solvent, and
[0230] iii-1) separating the at least one aprotic polar solvent from the solution (S) to obtain the membrane (M).
[0231] Another object of the present invention is a membrane (M) comprising a sulfonated polyarylene sulfone polymer (sP).
[0232] Another object of the present invention is a membrane (M) comprising the sulfonated polyarylene sulfone polymer (sP) obtained by the process of the present invention.
[0233] The membrane (M) preferably comprises at least 50 wt% sulfonated polyarylene sulfone polymer (sP), more preferably at least 70 wt% and most preferably at least 90 wt% sulfonated polyarylene sulfone polymer (sP), based on the total weight of the membrane (M).
[0234] The membrane (M) is suitable for separating a gas from a gas mixture, in particular for separating hydrogen from a gas mixture containing hydrogen.
[0235] Therefore, another object of the present invention is the use of the membrane (M) obtained by the process of the present invention for separating gases from gas mixtures.
[0236] The present invention is more particularly illustrated by the following examples without being restricted thereto.
[0237] Components used :
[0238] DCDPS 4,4'-Dichlorodiphenyl sulfone,
[0239] sDCDPS 4,4'-Dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt
[0240] BP 4,4'-dihydroxybiphenyl,
[0241] K2CO3: Potassium carbonate, anhydrous, average particle size 32.6 μm
[0242] NMP: N-Methylpyrrolidone, anhydrous
[0243] The viscosity number VN of the sulfonated polyarylene sulfone polymers (sP) was measured in 0.5% by weight NMP solution in accordance with DIN ISO 1628-1.
[0244] In CDCl3 by 1 H-NMR was used to determine the incorporation rate (incorporation rate) of sDCDPS.
[0245] The molecular weight distribution of the sulfonated polyarylene sulfone polymers with unimodal molecular weight distribution (Comparative Examples C1, C2, C3, C4, C7, C8, C9 and C10) and the sulfonated polyarylene sulfone polymers (sP) with bimodal molecular weight distribution (Examples 5 and 6) was determined by GPC using DMAc as solvent and using narrow distribution PMMA as described above.
[0246] In the case of the comparative example, the precipitated sulfonated polyarylene sulfone polymer was dissolved in NMP at the same concentration (20 wt.%) as the corresponding solution obtained in the inventive example. An appropriate amount of this solution was dissolved in DMAc so that the polymer concentration was 4 mg / ml. Then 100 μl of this solution was injected into the GPC system.
[0247] The isolation of the sulfonated polyarylene sulfone polymer with a monomodal molecular weight distribution is carried out by precipitation of a NMP solution of the sulfonated polyarylene sulfone polymer (sP) into isopropanol at room temperature. The drop height is 0.5 m. The throughput is about 2.5 l / hour. The precipitate obtained is then extracted with water at 85° C. (water throughput 160 l / h) for twenty hours. The material is then heated below the glass transition temperature T g The mixture was dried at a temperature of 100 °C to a residual moisture content of less than 2 wt %.
[0248] Filtration of the product mixture was carried out in a heated metal pressure filter using a filter with a pore size of 5 μm and a N2 pressure of 3 bar. The filter was heated to 60°C to reduce the viscosity of the reaction mixture.
[0249] The yield of sulfonated polyarylene sulfone polymer was determined gravimetrically.
[0250] Comparative Example 1: Sulfonated polyarylene sulfone polymer having a unimodal molecular weight distribution :
[0251] In a 4-liter glass reactor equipped with a thermometer, a gas inlet tube and a Dean-Stark separator, 384.81 g (1.34 mol) of DCDPS, 343.84 g (0.70 mol) of sDCDPS, 372.42 g (2.00 mol) of BP and 400.81 g (2.90 mol) of potassium carbonate having a volume average particle size of 32.6 μm were suspended in 1250 ml of NMP in a nitrogen atmosphere.
[0252] The mixture was heated to 190° C. within one hour. In the following, the reaction time is understood to be the time during which the reaction mixture was kept at 190° C. The water formed in the reaction was removed continuously by distillation, and the losses in NMP were replaced.
[0253] After 8 hours of reaction time, the reaction was stopped by adding 1750 ml of NMP and cooling to room temperature (within one hour). The potassium chloride formed in the reaction was removed by filtration. The polymer solution obtained was precipitated in isopropanol, the resulting polymer precipitate was separated, and then extracted with hot water (85° C.) for 20 h. The precipitate was then dried at 120° C. for 24 h under reduced pressure (<100 mbar).
[0254] Comparative Example 2: Sulfonated polyarylene sulfone polymer having a unimodal molecular weight distribution :
[0255] In a 4-liter glass reactor equipped with a thermometer, a gas inlet tube and a Dean-Stark separator, 370.45 g (1.29 mol) of DCDPS, 368.40 g (0.75 mol) of sDCDPS, 372.42 g (2.00 mol) of BP and 407.72 g (2.95 mol) of potassium carbonate having a volume average particle size of 32.6 μm were suspended in 1250 ml of NMP in a nitrogen atmosphere.
[0256] The mixture was heated to 190° C. within one hour. In the following, the reaction time is understood to be the time during which the reaction mixture was kept at 190° C. The water formed in the reaction was removed continuously by distillation, and the losses in NMP were replaced.
[0257] After 8 hours of reaction time, the reaction was stopped by adding 1750 ml of NMP and cooling to room temperature (within one hour). The potassium chloride formed in the reaction was removed by filtration. The polymer solution obtained was precipitated in isopropanol, the resulting polymer precipitate was separated, and then extracted with hot water (85° C.) for 20 h. The precipitate was then dried at 120° C. for 24 h under reduced pressure (<100 mbar).
[0258] Comparative Example 3; Sulfonated polyarylene sulfone polymer having a unimodal molecular weight distribution :
[0259] In a 4-liter glass reactor equipped with a thermometer, a gas inlet tube and a Dean-Stark separator, 364.69 g (1.27 mol) of DCDPS, 378.26 g (0.77 mol) of sDCDPS, 372.42 g (2.00 mol) of BP and 414.63 g (3.00 mol) of potassium carbonate having a volume average particle size of 32.6 μm were suspended in 1250 ml of NMP in a nitrogen atmosphere.
[0260] The mixture was heated to 190° C. within one hour. In the following, the reaction time is understood to be the time during which the reaction mixture was kept at 190° C. The water formed in the reaction was removed continuously by distillation, and the losses in NMP were replaced.
[0261] After 8 hours of reaction time, the reaction was stopped by adding 1750 ml of NMP and cooling to room temperature (within one hour). The potassium chloride formed in the reaction was removed by filtration. The polymer solution obtained was precipitated in isopropanol, the resulting polymer precipitate was separated, and then extracted with hot water (85° C.) for 20 h. The precipitate was then dried at 120° C. for 24 h under reduced pressure (<100 mbar).
[0262] Comparative Example 4; Sulfonated polyarylene sulfone polymer having a unimodal molecular weight distribution :
[0263] In a 4-liter glass reactor equipped with a thermometer, a gas inlet tube and a Dean-Stark separator, 356.07 g (1.24 mol) of DCDPS, 393.00 g (0.80 mol) of sDCDPS, 372.42 g (2.00 mol) of BP and 421.54 g (3.05 mol) of potassium carbonate having a volume average particle size of 32.6 μm were suspended in 1250 ml of NMP in a nitrogen atmosphere.
[0264] The mixture was heated to 190° C. within one hour. In the following, the reaction time is understood to be the time during which the reaction mixture was kept at 190° C. The water formed in the reaction was removed continuously by distillation, and the losses in NMP were replaced.
[0265] After 8 hours of reaction time, the reaction was stopped by adding 1750 ml of NMP and cooling to room temperature (within one hour). The potassium chloride formed in the reaction was removed by filtration. The polymer solution obtained was precipitated in isopropanol, the resulting polymer precipitate was separated, and then extracted with hot water (85° C.) for 20 h. The precipitate was then dried at 120° C. for 24 h under reduced pressure (<100 mbar).
[0266] Example 5; Sulfonated polyarylene sulfone polymer (sP) having a bimodal molecular weight distribution :
[0267] In a 4-liter glass reactor equipped with a thermometer, a gas inlet tube and a Dean-Stark separator, 384.81 g (1.34 mol) of DCDPS, 343.84 g (0.70 mol) of sDCDPS, 372.42 g (2.00 mol) of BP and 400.81 g (2.90 mol) of potassium carbonate having a volume average particle size of 32.6 μm were suspended in 1250 ml of NMP in a nitrogen atmosphere.
[0268] The mixture was heated to 190° C. within one hour. In the following, the reaction time is understood to be the time during which the reaction mixture was kept at 190° C. The water formed in the reaction was removed continuously by distillation, and the losses in NMP were replaced.
[0269] After a reaction time of 8 hours, the reaction was stopped by adding 1750 ml of NMP and cooling to room temperature (within one hour). The potassium chloride formed in the reaction was removed by filtration. The polymer solution obtained was used for membrane preparation. The polymer content of the solution was 23.9 wt.%.
[0270] Example 6; Sulfonated polyarylene sulfone polymer (sP) having a bimodal molecular weight distribution :
[0271] In a 4-liter glass reactor equipped with a thermometer, a gas inlet tube and a Dean-Stark separator, 370.45 g (1.29 mol) of DCDPS, 368.40 g (0.75 mol) of sDCDPS, 372.42 g (2.00 mol) of BP and 407.72 g (2.95 mol) of potassium carbonate having a volume average particle size of 32.6 μm were suspended in 1250 ml of NMP in a nitrogen atmosphere.
[0272] The mixture was heated to 190° C. within one hour. In the following, the reaction time is understood to be the time during which the reaction mixture was kept at 190° C. The water formed in the reaction was removed continuously by distillation, and the losses in NMP were replaced.
[0273] After a reaction time of 8 hours, the reaction was stopped by adding 1750 ml of NMP and cooling to room temperature (within one hour). The potassium chloride formed in the reaction was removed by filtration. The polymer solution obtained was used for membrane preparation. The polymer content of the solution was 24.0 wt.%.
[0274] Comparative Examples 7, 8, 9 and 10: Sulfonated polymers with unimodal molecular weight distribution :
[0275] A small portion of the polymer solution obtained in Example 5 was precipitated in water (Comparative Example C7), ethanol (Comparative Example C8), methanol (Comparative Example C9) and water / ethanol 1 / 1 (volume ratio) (Comparative Example C10). The polymer obtained was extracted with hot water for 20 h and then dried at 120° C. and then dried at 120° C. under reduced pressure (<100 mbar) for 24 h.
[0276] To prepare the film, a solution of the isolated polymer from Examples C1, C2, C3, C4, C7, C8, C9 and C10 was prepared using a polymer content of 17.5 wt.%. The solutions of Examples 5 and 6 were diluted with NMP to obtain a polymer content of 17.5 wt.%. Films were prepared from these solutions by casting the solution onto a glass plate at a speed of 5 mm / s at a temperature of 60°C with a doctor blade. The glass plate was transferred to a vacuum oven, and the temperature was gradually increased to 100°C and maintained for 12 h. After cooling to room temperature, the plate was placed in a water bath, which caused the film to detach from the glass plate. The wet film was then fixed and vacuum dried at 120°C for 12 h.
[0277] The membranes prepared as described were cut to the required size (i.e. 5×5 cm). For activation, the membranes were immersed in 0.5 M H2SO4 at 80°C for 2 h. Subsequently, the membranes were immersed in deionized water (MiliQ 18.2 MOhm) at 80°C for another 2 h and finally stored in a fresh batch of deionized water at room temperature. To determine the conductivity, the membranes were sandwiched between a 2-well plate equipped with two rectangular gold electrodes (0.25 cm 2 ) in a special teflon cell. Constant pressure is achieved by adjusting the torque of the 4 screws to 4Nm.
[0278] Table 1 :
[0279]
[0280] The membrane with bimodal molecular weight distribution (M) showed higher conductivity.
Claims
1. A sulfonated polyarylene sulfone polymer (sP) having at least a bimodal molecular weight distribution having at least one first peak (P1) and at least one second peak (P2), wherein the maximum of the first peak (P1) has a relative molecular mass in the range of 800 g / mol to 5 000 g / mol and the maximum of the second peak (P2) has a relative molecular mass in the range of 8 000 g / mol to 300 000 g / mol, wherein the relative molecular mass is determined by gel permeation chromatography using dimethylacetamide as solvent and narrow distribution poly(methyl methacrylate) as standard.
2. The sulfonated polyarylene sulfone polymer (sP) according to claim 1, wherein the maximum value of the first peak (P1) shows a first intensity (I1), and the maximum value of the second peak (P2) shows a second intensity (I2), wherein the ratio of the first intensity (I1) to the second intensity (I2) is in the range of 1:10 to 1:1000.
3. The sulfonated polyarylene sulfone polymer (sP) according to claim 1 or 2, wherein the sulfonated polyarylene sulfone polymer (sP) has a weight average molecular weight (MW) in the range of 20 000 g / mol to 250 000 g / mol. W ), wherein the weight average molecular weight (M W ) was determined by gel permeation chromatography using dimethylacetamide as solvent and narrow distribution poly(methyl methacrylate) as standard.
4. The sulfonated polyarylene sulfone polymer (sP) according to any one of claims 1 to 3, wherein the sulfonated polyarylene sulfone polymer (sP) comprises, based on the total amount of the sulfonated polyarylene sulfone polymer (sP), 15 mol-% to 80 mol-% of a sulfonated polyarylene sulfone polymer (sP) comprising at least one -SO3X 3 The sulfonated repeating unit of the group, wherein X 3 is hydrogen or a cation equivalent.
5. The sulfonated polyarylene sulfone polymer (sP) according to any one of claims 1 to 4, wherein the sulfonated polyarylene sulfone polymer (sP) comprises sulfonated repeating units of the general formula (I): in t and q: each independently 0, 1, 2 or 3, Q 1 , T and Y 1 : Each independently is a chemical bond or is selected from -O-, -S-, -SO2-, -S(=O)-, -C(=O)-, -N=N- and -CR a Rb -, where R a and R b are independently a hydrogen atom or a C1-C 12 -alkyl, C1-C 12 -alkoxy or C6-C 18 -aryl group, and wherein at least one of Q, T and Y is -SO2-, Ar and Ar 1 : Each independently is C6-C 18 Aryl, wherein the C6-C 18 The aryl group is unsubstituted or substituted by at least one substituent selected from the group consisting of: C1-C 12 Alkyl, C1-C 12 Alkoxy, C6-C 18 Aryl, halogen and -SO-3X, p, m, n and k: each independently 0, 1, 2, 3 or 4, provided that the sum of p, m, n and k is not less than 1, and X 3 : is hydrogen or a cation equivalent.
6. A method for preparing a sulfonated polyarylene sulfone polymer (sP) according to any one of claims 1 to 5, comprising the steps of i) subjecting a reaction mixture (R G ) conversion, the reaction mixture comprising the following as components (A) an aromatic dihalogen sulfone component, the aromatic dihalogen sulfone component comprising at least one sulfonated aromatic dihalogen sulfone (component (A1)) and at least one non-sulfonated aromatic dihalogen sulfone (component (A2)), (B) at least one aromatic dihydroxy compound, and (C) at least one carbonate compound.
7. The method according to claim 6, comprising the following steps: i) making the reaction mixture (R G ) conversion, the reaction mixture comprising: X mol of an aromatic dihalogen sulfone component (component (A)), the aromatic dihalogen sulfone component comprising: G ) in the total molar amount of the aromatic dihalogen sulfone component (component A)), X 1 mol % of at least one sulfonated aromatic dihalogen sulfone (component (A1)), and X 2 mol % of at least one non-sulfonated aromatic dihalogen sulfone (component (A2)), Where X 1 In the range of 15 to 80, and X 2In the range of 20 to 85, Y moles of at least one aromatic dihydroxy compound (component (B)), Z moles of at least one carbonate compound (component (C)), in The ratio of X to Y is in the range of 0.95 to 1.05, And among them Z is in the range of P to Q, Where P is calculated according to the following formula: P=Y*(1.05+X 1 / 100*1.05), And where Q is calculated according to the following formula: Q=Y*(1.05+X 1 / 100*1.4).
8. The method according to claim 6 or 7, wherein the reaction mixture (R G )) further comprises at least one aprotic polar solvent (component (D)).
9. The process according to any one of claims 6 to 8, wherein after step i), a product mixture (P) comprising the sulfonated polyarylene sulfone polymer (sP), the at least one aprotic polar solvent and the at least one inorganic halide compound is obtained. G ), and wherein the method further comprises the following steps ii) from the product mixture (P G ) to obtain a solution (S) comprising the sulfonated polyarylene sulfone polymer (sP) and the at least one aprotic polar solvent, and iii) separating said at least one aprotic polar solvent from said solution (S) by evaporation to obtain said sulfonated polyarylene sulfone polymer (sP).
10. The process according to any one of claims 6 to 9, wherein component (A1) comprises G ) in an amount of not less than 80 wt % of the total weight of component (A1) in the mixture: at least one compound selected from the group consisting of 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid disodium salt and 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt.
11. The process according to any one of claims 6 to 10, wherein component (A2) comprises a mixture based on the reaction mixture (RG ) in an amount of not less than 80 wt % of at least one aromatic dihalogen sulfone selected from the group consisting of 4,4'-dichlorodiphenyl sulfone and 4,4'-difluorodiphenyl sulfone, based on the total weight of component (A2) in the present invention.
12. The process according to any one of claims 6 to 11, wherein component (B) comprises G ) in the total weight of component (B), not less than 80 wt% of 4,4'-dihydroxybiphenyl.
13. Use of the sulfonated polyarylene sulfone polymer (sP) according to any one of claims 1 to 5 or obtained by the process according to any one of claims 6 to 12 for the preparation of a membrane (M).
14. Membrane (M) comprising a sulfonated polyarylene sulfone polymer (sP) according to any one of claims 1 to 5 or obtained by a process according to any one of claims 6 to 12.
15. A method for preparing a membrane (M) comprising a sulfonated polyarylene sulfone polymer (sP) according to any one of claims 1 to 5, the method comprising the following steps ii-1) providing the solution (S) obtained in step ii) according to claim 9, said solution comprising the sulfonated polyarylene sulfone polymer (sP) and the at least one aprotic polar solvent, and iii-1) separating the at least one aprotic polar solvent from the solution (S) to obtain the membrane (M).