Resin composition and molded article

By using a thermoplastic non-fluoro resin, a first tetrafluoroethylene-based polymer and a second tetrafluoroethylene-based polymer in the resin composition, the problem of insufficient affinity between the fluoroethylene-based resin and other resins is solved, and the problem of insufficient affinity between the fluoroethylene-based resin and other resins is achieved. It improves wear resistance and heat resistance, and is suitable for improving friction characteristics of automobiles and aircraft components.

CN118900895APending Publication Date: 2024-11-05AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028703.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-22
Filing Date
2023-03-16
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The affinity of fluorine-based resins and other resins is insufficient, resulting in poor mixing properties, making it difficult to impart thermoplastic non-fluorine resins with wear resistance and other properties in high melting point or high heat resistance fluorine-based resins, especially in automobiles and aircraft components. and fuel consumption challenges.

Method used

Using a resin composition, including a thermoplastic non-fluoro resin, a first tetrafluoroethylene-based polymer and a second tetrafluoroethylene-based polymer having a melting point above 260°C and lower than the second tetrafluoroethylene-based polymer, by The mixed powder of the first tetrafluoroethylene-based polymer and the second tetrafluoroethylene-based polymer is melt-kneaded with a thermoplastic non-fluoro resin to form a molded body with excellent wear resistance and heat resistance.

Benefits of technology

It is achieved to improve the dispersed particle size density of fluororesin in the molded body, form a matrix structure, enhance wear resistance and heat resistance, and meet the needs of automobile and aircraft components for friction characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005049907730000151
    Figure BDA0005049907730000151
  • Figure BDA0005049907730000171
    Figure BDA0005049907730000171
Patent Text Reader

Abstract

Provided are a resin composition capable of forming a molded article having excellent wear characteristics and heat resistance, and a molded article. A resin composition containing a thermoplastic non-fluororesin, a first tetrafluoroethylene polymer, and a second tetrafluoroethylene polymer having a melting point of 260 DEG C or higher but lower than the melting point of the first tetrafluoroethylene polymer, the total mass of the thermoplastic non-fluororesin, the first tetrafluoroethylene polymer, and the second tetrafluoroethylene polymer being equal to or greater than the total mass of the thermoplastic non-fluororesin, the first tetrafluoroethylene polymer, and the second tetrafluoroethylene polymer, and the total mass of the thermoplastic non-fluororesin, the first tetrafluoroethylene polymer, and the second tetrafluoroethylene polymer being equal to or greater than the total mass of the second tetrafluoroethylene polymer. The present invention relates to a resin composition which contains 4.0-32.0 mass% of a first tetrafluoroethylene polymer and 0.5-10.0 mass% of a second tetrafluoroethylene polymer, and which is obtained by melt-kneading a powder mixture of first particles of the first tetrafluoroethylene polymer and second particles of the second tetrafluoroethylene polymer with a powder of a thermoplastic non-fluororesin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition and a molded article. Background Art

[0002] Fluorine-based resins such as polytetrafluoroethylene have various properties such as excellent heat resistance, insulation, chemical resistance, water repellency, wear resistance and other friction characteristics. They are used in a wide range of applications such as the food industry, chemical industry, automobile parts, and semiconductor fields by utilizing these properties. By adding a fluorine-based resin to a heat-resistant thermoplastic non-fluorine-based resin called a super engineering plastic and subjecting the mixture to molding, a molded product having highly superior physical properties of both resins can be easily obtained (see Patent Document 1). Prior art literature Patent Literature

[0003] Patent Document 1: Japanese Patent Application Publication No. 2013-227504 Summary of the invention Technical problem to be solved by the invention

[0004] However, fluorine-based resins have insufficient affinity with other resins and lack miscibility. This tendency is particularly evident in fluorine-based resins with high tetrafluoroethylene unit content, high melting point or high heat resistance. It is not easy to impart physical properties such as wear resistance of fluorine-based resins to other resins such as thermoplastic non-fluorine-based resins. From the perspective of improving fuel efficiency and quietness, resin parts for automobiles, airplanes, etc. are required to have reduced friction. An object of the present invention is to provide a resin composition capable of forming a molded article having excellent friction characteristics such as wear resistance and heat resistance, and a molded article. Solutions to technical problems

[0005] The present invention has the following embodiments. [1] A resin composition comprising a thermoplastic non-fluorine resin, a first tetrafluoroethylene polymer, and a second tetrafluoroethylene polymer having a melting point of 260° C. or higher and lower than the melting point of the first tetrafluoroethylene polymer, With respect to the total mass of the thermoplastic non-fluorine resin, the first tetrafluoroethylene polymer and the second tetrafluoroethylene polymer, the first tetrafluoroethylene polymer accounts for 4.0 to 32.0 mass %, and the second tetrafluoroethylene polymer accounts for 0.5 to 10.0 mass %, The resin composition is obtained by melt-kneading a mixed powder of first particles of a first tetrafluoroethylene-based polymer and second particles of a second tetrafluoroethylene-based polymer with a powder of a thermoplastic non-fluorine resin. [2] The resin composition according to [1], wherein the first tetrafluoroethylene-based polymer is polytetrafluoroethylene. [3] The resin composition according to [1] or [2], wherein the second tetrafluoroethylene-based polymer contains units based on at least one comonomer selected from perfluoro(alkyl vinyl ether), hexafluoropropylene and fluoroalkylethylene. [4] The resin composition according to any one of [1] to [3], wherein the second tetrafluoroethylene polymer has an oxygen-containing polar group. [5] The resin composition as described in any one of [1] to [4], wherein the melting point of the first tetrafluoroethylene polymer is higher than 320°C and lower than 380°C, and the melting point of the second tetrafluoroethylene polymer is higher than 260°C and lower than 320°C. [6] The resin composition according to any one of [1] to [5], wherein the difference between the melting point of the first tetrafluoroethylene polymer and the melting point of the second tetrafluoroethylene polymer is 20° C. or more and 60° C. or less. [7] The resin composition according to any one of [1] to [6], wherein the average particle size of the first particles is 1 to 100 μm. [8] The resin composition according to any one of [1] to [7], wherein the average particle size of the first particles is larger than the average particle size of the second particles. [9] The resin composition according to any one of [1] to [8], wherein the ratio of the average particle size of the first particles to the average particle size of the second particles is 2 to 50 in terms of a particle size ratio expressed as first particles / second particles.

[10] The resin composition according to any one of [1] to [9], wherein the content of the first particles is greater than the content of the second particles.

[11] The resin composition according to any one of [1] to

[10] , wherein the content ratio of the first particles to the second particles is 55 / 45 to 99 / 1 in terms of mass ratio expressed as first particles / second particles.

[12] The resin composition according to any one of [1] to

[11] , wherein the melting point of the thermoplastic non-fluorine resin is not less than the melting point of the second tetrafluoroethylene polymer and less than the melting point of the first tetrafluoroethylene polymer.

[13] The resin composition described in any one of [1] to

[12] , wherein the total content of the thermoplastic non-fluorine resin, the first tetrafluoroethylene polymer and the second tetrafluoroethylene polymer is 60.0% by mass or more relative to the total content of the resin composition.

[14] The resin composition according to any one of [1] to

[13] , wherein the content of the thermoplastic non-fluorine resin is 65.0 to 95.0% by mass based on the total mass of the resin composition.

[15] A molded article formed from the resin composition according to any one of [1] to

[14] . Effects of the Invention

[0006] According to the present invention, a resin composition capable of forming a molded product having excellent friction characteristics such as wear resistance and heat resistance, and a molded product can be provided. DETAILED DESCRIPTION

[0007] The meanings and definitions of the terms used in the present invention are as follows: "Non-fluorine" means containing no fluorine atoms. "Melting point" refers to the temperature corresponding to the maximum of the melting peak of a polymer as measured by differential scanning calorimetry (DSC). "Melt-formable" means exhibiting melt flowability. “Exhibiting melt fluidity” means that the polymer has a melt flow rate of 0.1 to 1000 g / 10 minutes at a temperature 20° C. or higher than the melting point of the polymer. The "melt flow rate" is the melt flow rate (MFR) specified in JIS K 7210-1:2014 (corresponding to the international standard ISO 1133-1:2011). Hereinafter, the melt flow rate is also referred to as MFR. The "glass transition temperature" is a temperature corresponding to the maximum value of the tan δ peak measured by the dynamic viscoelasticity measurement (DMA) method. Hereinafter, the glass transition temperature is also referred to as Tg. The "average particle size" is the particle size at the point where the cumulative volume reaches 50% in the cumulative distribution curve with the total volume of the particle size distribution calculated on a volume basis as 100%, that is, the volume basis cumulative 50% diameter (D50). The D50 of the particles is obtained by dispersing the particles in water and analyzing them using a laser diffraction / scattering method using a laser diffraction / scattering particle size distribution measuring device (manufactured by Horiba, Ltd., LA-920 measuring instrument). Hereinafter, the average particle size is also referred to as D50. The “average dispersed particle size” is the maximum diameter (domain size) of the domain (dispersed particles) of the first tetrafluoroethylene polymer measured from the SEM image by freeze-cutting the resin composition or its molded body and observing the cross section with a scanning electron microscope (hereinafter also referred to as SEM), and is the value obtained by averaging 20 values ​​arranged in order from the largest domain size in the image. The “arithmetic mean roughness Ra” is measured in accordance with JIS B0601:1994 with a measurement length of 4.0 mm, a measurement speed of 0.30 mm / s, and a cutoff value λc of 0.8 mm. The "unit" in a polymer refers to an atomic group based on a monomer formed by polymerization of the monomer. The unit may be a unit formed directly by a polymerization reaction, or a unit in which a part of the unit is converted into another structure by treating the polymer. Hereinafter, the unit based on monomer a is also referred to as "monomer a unit". " to " indicating a numerical range means that the numerical values ​​described before and after it are included as the lower limit and the upper limit.

[0008] The resin composition of the present invention (hereinafter also referred to as "the present composition") comprises a thermoplastic non-fluororesin, a first tetrafluoroethylene polymer (hereinafter also referred to as "the first F polymer"), and a second tetrafluoroethylene polymer having a melting point of 260°C or higher and lower than the melting point of the first tetrafluoroethylene polymer (hereinafter also referred to as "the second F polymer"), wherein the first tetrafluoroethylene polymer accounts for 4.0 to 32.0% by mass and the second tetrafluoroethylene polymer accounts for 0.5 to 10.0% by mass relative to the total mass of the thermoplastic non-fluororesin, the first tetrafluoroethylene polymer and the second tetrafluoroethylene polymer, and the resin composition is obtained by melt-kneading a mixed powder of first particles of the first tetrafluoroethylene polymer (hereinafter also referred to as "the first particles") and second particles of the second tetrafluoroethylene polymer (hereinafter also referred to as "the second particles") with powder of the thermoplastic non-fluororesin. The present composition is excellent in frictional properties such as wear resistance and heat resistance, and a molded body having the above properties can be easily obtained from the present composition. The reason for this is not necessarily clear, but it is considered as follows.

[0009] In the present composition, a mixed powder containing first particles and second particles, both of which are fluorine-based resins, is prepared in advance, and the mixed powder is used when melt-kneading with a powder of a thermoplastic fluorine-based resin. In other words, the first F polymer and the second F polymer, which are different types of fluorine-based resins, are used in a state where they are agglomerated or affinity-bound to each other and interact with each other. At this time, since the second F polymer has a lower melting point than the first F polymer, it is considered that it starts to flow while maintaining an affinity with the first F polymer during melt kneading, and smoothly becomes affinity with the thermoplastic non-fluororesin. As a result, it is considered that in the obtained molded body, the first F polymer is dispersed in the thermoplastic non-fluororesin or the second F polymer, the dispersed particle size of the fluororesin as a whole becomes small and dense, and a strong matrix structure is formed between the fluororesin as a whole and the thermoplastic non-fluororesin. Therefore, it is considered that even if the blending amounts of the first F polymer and the second F polymer relative to the thermoplastic non-fluororesin are small, the physical properties attributed to the fluororesin, such as abrasion resistance, can be highly imparted to the molded article produced from the composition. This mechanism of action is more likely to be more prominent in the case of the preferred embodiment of the present invention described later in relation to the thermoplastic non-fluorine resin, the particle sizes of the first particles and the second particles, or when the melting point of the thermoplastic non-fluorine resin is high and close to the first F polymer.

[0010] Examples of the thermoplastic non-fluorine resin include polyamide, polyetheramide, polyetherimide, thermoplastic polyimide, polyamideimide, aromatic polyester, semi-aromatic polyester, aromatic polyesteramide, unmodified or modified polyphenylene ether (PPE), polyarylene sulfide (e.g., polyphenylene sulfide (PPS)), polyarylene sulfone (e.g., polysulfone (PSU), polyethersulfone (PESU), polyarylene sulfone (PPSU), polyarylene etherketone (e.g., PEK, PEKK, PEEKK, etc.), polyacetal, and polycarbonate. The above-mentioned thermoplastic non-fluorine resins are classified as heat-resistant resins. The melting point of the thermoplastic non-fluorine resin is preferably 150° C. or higher, more preferably 240° C. or higher. The upper limit of the melting point of the thermoplastic non-fluorine resin is not particularly limited, and is, for example, 420° C. The thermoplastic non-fluorine resin may be used alone or in combination of two or more. Among them, polyamide, polyamideimide, polyaryletherketone and polyarylethersulfide are preferred, and polyamide is more preferred, from the viewpoint of low friction and excellent friction characteristics such as heat resistance and wear resistance of the present composition and a molded article formed therefrom.

[0011] Examples of polyamide include aliphatic polyamides such as polyamide 6 (PA6), polyamide 11 (PA11), polyamide 12 (PA12), polyamide 46 (PA46), polyamide 66 (PA66), polyamide 610 (PA610), polyamide 612 (PA612), polyamide 1010 (PA1010), polyamide 6 / 66 copolymer (PA6 / 66), polyamide 6 / 66 / 610 copolymer (PA6 / 66 / 610); semi-aromatic polyamides such as polyamide 6T, polyamide 9T, polyamide 10T, polyamide 11T, polyamide MXD6 (MXD6), polyamide 6T / 66 copolymer; and aromatic polyamides. Here, T represents terephthalic acid. These may be used alone or in combination of two or more. Among them, from the viewpoint of heat resistance, semi-aromatic polyamide resins are preferred, and polyamide 9T, polyamide 10T, and polyamide 11T are more preferred.

[0012] In the case where the second F polymer described later has an oxygen-containing polar group, from the viewpoint of being able to further improve the affinity between the thermoplastic non-fluorine resin and the second F polymer, it is preferred that the thermoplastic non-fluorine resin has a functional group such as an amino group or a hydroxyl group that can react with the oxygen-containing polar group. The functional group may be contained in the main chain, side chain or terminal of the thermoplastic non-fluorine resin.

[0013] The melting point of the thermoplastic non-fluorine resin is preferably higher than 265° C., more preferably at least 280° C., and further preferably at least 300° C. The upper limit of the melting point of the thermoplastic non-fluorine resin is, for example, 420° C. or less. The melting point of the thermoplastic non-fluorine resin is preferably not less than the melting point of the second F polymer described below and lower than the melting point of the first F polymer. When the melting point of the thermoplastic non-fluorine resin is within the above range, the above-mentioned action mechanism is more likely to be exhibited, and the present composition and a molded article formed therefrom are likely to be excellent in friction properties such as wear resistance and heat resistance.

[0014] The first F polymer and the second F polymer are each a polymer containing a unit (hereinafter also referred to as a “TFE unit”) based on tetrafluoroethylene (hereinafter also referred to as “TFE”). The first F polymer is preferably polytetrafluoroethylene (PTFE) containing 99.5 mol% or more of TFE units relative to all units constituting the first F polymer. That is, the first F polymer may be a homopolymer of TFE, or a copolymer containing less than 0.5 mol% of TFE relative to all units and other monomer units copolymerizable with TFE.

[0015] The melting point of the first F polymer is preferably 310 to 390° C., more preferably higher than 320° C. and lower than 380° C. If the first F polymer is PTFE that does not show a melting point, for example, PTFE that does not deform even when heated to 400° C. and left to stand, the thermal decomposition starting temperature of 390° C. is regarded as the melting point of the first F polymer.

[0016] As the second F polymer, there can be mentioned a polymer containing TFE units and ethylene-based units (ETFE), a polymer containing TFE units and propylene-based units, a polymer containing TFE units and ethylene-based units and propylene-based units (EFEP), a polymer containing TFE units and perfluoro(alkyl vinyl ether) (PAVE)-based units (PAVE units) (PFA), a polymer containing TFE units and hexafluoropropylene-based units (FEP), and a polymer containing TFE units and fluoroalkylethylene (FAE)-based units. As PAVE, preferred are CF2=CFOCF3 (hereinafter also referred to as "PMVE"), CF2=CFOCF2CF3, CF2=CFOCF2CF2CF3 (hereinafter also referred to as "PPVE"), CF2=CFOCF2CF2CF2CF3, CF2=CFO(CF2)8F, and more preferred are PMVE or PPVE. Examples of FAE include CH2=CH(CF2)2F, CH2=CH(CF2)3F, CH2=CH(CF2)4F, CH2=CF(CF2)3H and CH2=CF(CF2)4H. The second F polymer is preferably a polymer containing units based on at least one comonomer selected from PAVE, hexafluoropropylene and FAE, more preferably PFA and FEP, and further preferably PFA. These polymers may also contain units based on other comonomers.

[0017] The second F polymer preferably has a functional group. Examples of the functional group include oxygen-containing polar groups such as hydroxyl-containing groups, carbonyl-containing groups, cyclic acetal groups, diol residues, and epoxy groups; and nitrogen-containing polar groups such as amino groups. Among them, the second F polymer preferably has an oxygen-containing polar group, more preferably has a hydroxyl-containing group or a carbonyl-containing group, and further preferably has a carbonyl-containing group. In this case, the affinity with the thermoplastic non-fluorine resin in the present composition can be easily improved. The hydroxyl group-containing group is preferably a group containing an alcoholic hydroxyl group, more preferably -CF2CH2OH and -C(CF3)2OH. The carbonyl-containing group is preferably a carboxyl group, an alkoxycarbonyl group, an amide group, an isocyanate group, a carbamate group (-OC(O)NH2), an anhydride residue (-C(O)OC(O)-), an imide residue (-C(O)NHC(O)-, etc.), a formyl group, a haloformyl group (-C(=O)-X (wherein X is a halogen atom), a carbamate group (-NHC(O)O-), an oxalyl group (-NH-C(O)-C(O)-NH2) and a carbonate group (-OC(O)O-), and an anhydride residue is more preferred. In the case where the second F polymer has an oxygen-containing polar group, the number of oxygen-containing polar groups in the second F polymer is 6 The number of carbon atoms in the main chain is preferably 10 to 5000, and more preferably 100 to 3000. In addition, the number of oxygen-containing polar groups in the F polymer can be quantified by the composition of the polymer or by the method described in International Publication No. 2020 / 145133.

[0018] The oxygen-containing polar group may be contained in the unit based on the monomer in the second F polymer, or may be contained in the terminal group of the main chain of the second F polymer, and is preferably contained in the unit based on the monomer in the second F polymer. As a form in which the oxygen-containing polar group is contained in the terminal group of the main chain of the second F polymer, there can be exemplified a second F polymer having an oxygen-containing polar group as a terminal group derived from a polymerization initiator, a chain transfer agent, etc., and a second F polymer obtained by subjecting a polymer having a TFE unit to plasma treatment or electrolysis off-line treatment. As the monomer having a carbonyl group, itaconic anhydride (hereinafter also referred to as IAH), citraconic anhydride (hereinafter also referred to as CAH), and 5-norbornene-2,3-dicarboxylic anhydride (hereinafter also referred to as "NAH") are preferred, and NAH is more preferred.

[0019] The second F polymer is preferably a polymer having a carbonyl group containing TFE units and PAVE units, more preferably a polymer containing TFE units, PAVE units and units based on monomers having carbonyl groups and containing 90 to 99 mol%, 0.99 to 9.97 mol%, and 0.01 to 3 mol% of these units in order relative to all units. As a specific example of the second F polymer, the polymer described in International Publication No. 2018 / 16644 can be cited.

[0020] The melting point of the second F polymer is 260°C or higher and lower than the melting point of the first F polymer. When the melting point of the second F polymer is 260°C or higher, the heat resistance of the present composition is excellent. The melting point of the second F polymer is preferably 275°C or higher, more preferably 280°C or higher. The melting point of the second F polymer is preferably 350°C or lower, more preferably 320°C or lower. When the melting point of the second F polymer is 350°C or lower, the moldability of the present composition is excellent. The melting point of the second F polymer can be adjusted by the ratio of the TFE unit, the ratio of the comonomer unit, and the like.

[0021] The glass transition temperature of the second polymer F is preferably 50° C. or higher, more preferably 75° C. or higher. The glass transition temperature of the second polymer F is preferably 150° C. or lower, more preferably 125° C. or lower. The melt flow rate (MFR; 372° C., load 49 N) of the second F polymer is preferably 1 to 100 g / 10 min, more preferably 3 to 50 g / 10 min.

[0022] In the present composition, as described above, the melting point of the second F polymer is 260° C. or higher and lower than the melting point of the first F polymer. In addition, it is preferred that the melting point of the first F polymer is higher than 320° C. and lower than 380° C., and the melting point of the second F polymer is 260° C. or higher and lower than 320° C. Furthermore, it is preferred that the difference between the melting points of the first F polymer and the second F polymer is 20° C. or higher and 75° C. or lower, and more preferably 20° C. or higher and 60° C. or lower. When the melting points of the first F polymer and the second F polymer satisfy the above relationship, the first F polymer and the second F polymer as fluorine-based resins can easily improve their dispersibility in the thermoplastic non-fluorine resin by the above-mentioned action mechanism, and the molded body formed from the present composition can easily have excellent friction properties such as wear resistance and heat resistance.

[0023] The average particle size (D50) of the first particles as a raw material of the present composition is larger than the average particle size (D50) of the second particles. The D50 of the first particles is preferably 1 to 100 μm, more preferably 10 to 75 μm. The D50 of the second particles is preferably 0.1 to 50 μm, more preferably 1 to 10 μm. The ratio of D50 of the first particles to D50 of the second particles is preferably 2 to 50, more preferably 5 to 25. In this case, the molded article formed from the present composition tends to have excellent friction properties such as wear resistance and heat resistance due to the above-mentioned action mechanism.

[0024] In the present composition, the content of the first particles is preferably greater than the content of the second particles. Specifically, the content of the first particles to the content of the second particles is preferably 55 / 45 to 99 / 1, more preferably 70 / 30 to 99 / 1, and further preferably 80 / 20 to 95 / 5 in terms of mass ratio expressed as first particles / second particles. When the content ratio of the first particles to the second particles is within the above range, the wear resistance improvement effect brought about by the first F polymer and the dispersibility improvement effect brought about by the second F polymer will be fully manifested, and the friction characteristics such as wear resistance and heat resistance of the present composition and the molded body formed from the present composition are likely to be excellent.

[0025] In the present composition, the first F polymer is 4.0 to 32.0% by mass, preferably 7.0 to 26.0% by mass, and more preferably 10.0 to 20.0% by mass relative to the total mass of the thermoplastic non-fluorine resin, the first F polymer, and the second F polymer. When the content of the first F polymer is within the above range, the friction characteristics such as wear resistance of the first F polymer can be easily improved. In addition, in the present composition, the second F polymer is 0.5 to 10.0% by mass, preferably 0.75 to 5.0% by mass, and more preferably 1.0 to 3.5% by mass, relative to the total mass of the thermoplastic non-fluorine resin, the first F polymer, and the second F polymer. If the second F polymer is above the above lower limit, the dispersibility of the first F polymer is good, and if it is below the above upper limit, the excellent properties (mechanical properties, etc.) of the thermoplastic non-fluorine resin are easily exhibited.

[0026] The content of the thermoplastic non-fluorine resin is preferably 65.0 to 95.5% by mass, more preferably 70.0 to 90.0% by mass, and further preferably 75.0 to 85.0% by mass relative to the total weight of the present composition. When the content of the thermoplastic non-fluorine resin is above the above lower limit, the excellent properties (mechanical properties, etc.) of the thermoplastic non-fluorine resin are easily exhibited, and when it is below the above upper limit, the friction properties such as wear resistance of the present composition are excellent.

[0027] The total content of the thermoplastic non-fluorine resin, the first F polymer and the second F polymer is preferably 60.0% by mass or more, preferably 65.0% by mass or more, more preferably 70.0% by mass or more, and may be 100% by mass, relative to the entire composition. When the total content of the thermoplastic non-fluorine resin, the first F polymer and the second F polymer is 60.0% by mass or more, the moldability of the composition and the friction characteristics such as wear resistance and heat resistance of the molded body formed from the composition are likely to be excellent.

[0028] In the present composition, preferably, the thermoplastic non-fluorine resin is 65.0 to 95.5% by mass, the first F polymer is 4.0 to 32.0% by mass, and the second F polymer is 0.5 to 10.0% by mass, relative to the total mass of the present composition. More preferably, the thermoplastic non-fluorine resin is 70.0 to 90.0% by mass, the first F polymer is 7.0 to 26.0% by mass, and the second F polymer is 0.75 to 5.0% by mass. Still more preferably, the thermoplastic non-fluorine resin is 75.0 to 85.0% by mass, the first F polymer is 10.0 to 20.0% by mass, and the second F polymer is 1.0 to 3.5% by mass.

[0029] In the present composition, the first F polymer is dispersed in the thermoplastic non-fluorine resin or the second F polymer by the above-mentioned mechanism of action. In the present composition, the average dispersed particle size of the first F polymer is preferably 1.0 to 40.0 μm, more preferably 3.0 to 30.0 μm, and further preferably 5.0 to 20 μm. When the average dispersed particle size of the first F polymer is within the above-mentioned range, the present composition and the molded article formed from the present composition tend to have excellent friction characteristics such as wear resistance and heat resistance.

[0030] The composition may further contain fillers, plasticizers, weathering agents, antioxidants, heat stabilizers, lubricants, antistatic agents, whitening agents, colorants, conductive agents, release agents, surface treatment agents, flame retardants and other materials as required within the range not impairing the effects of the present invention. Among them, it is preferred that the present composition contains carbon fibers, glass fibers, and the like as inorganic fillers from the viewpoint of being able to improve the mechanical properties of a molded body molded from the present composition.

[0031] When the composition is formed into a molded body (hereinafter also referred to as molded body M) of 80 mm × 80 mm × 1 mm in thickness by press molding at 320° C., preheating for 8 minutes, and pressurizing at a pressure of 5 MPa for 3 minutes, the arithmetic mean roughness Ra of the surface of the molded body M is preferably 0.08 μm or less. When the arithmetic mean roughness Ra of the surface of the molded body M is 0.08 μm or less, friction characteristics such as wear resistance are more excellent. The arithmetic mean roughness Ra of the surface of the molded body M is more preferably 0.05 μm or less, and further preferably 0.03 μm or less. The lower limit of the arithmetic mean roughness Ra of the surface of the molded body M is not particularly limited, and is, for example, 0.01 μm. In addition, the wear loss measured on the molded body M is preferably within 0.005 cm 3 Below, more preferably 0.0025cm 3 When the wear amount is below the above upper limit, the present composition can be used in applications requiring friction characteristics such as wear resistance. Furthermore, the dynamic friction coefficient measured for the molded body M is preferably 0.35 or less, more preferably 0.3 or less. When the dynamic friction coefficient is below the above upper limit, the present composition can be used for applications requiring friction characteristics such as wear resistance. The wear amount and the dynamic friction coefficient were measured by the Matsubara friction measurement method in accordance with JIS K 7218 as described later in Examples.

[0032] The present resin composition is obtained by melt-kneading a mixed powder of first particles and second particles with a powder of a thermoplastic non-fluorine resin. The mixed powder of the first particles and the second particles can be prepared in advance using a mixer such as a tumble mixer or a Henschel mixer. The melt-kneading can be carried out using a known melt-kneading machine such as a Banbury mixer, a roll, a Brabender, a single-screw kneading extruder, a double-screw kneading extruder, or a kneader. The mixed powder of the first and second particles, the thermoplastic non-fluorine resin, and other materials included as required may be mixed in advance using a mixer such as a tumble mixer or a Henschel mixer, or may be directly introduced into a melt kneader. The temperature of melt kneading is preferably 300 to 330° C. The time of melt kneading is preferably 5 to 15 minutes.

[0033] The present invention also relates to a molded article formed from the composition. The composition can be molded by thermoplastic molding, compression molding such as free-fired molding, injection molding, or transfer molding. The molded article formed from the present composition is excellent in frictional properties such as wear resistance and heat resistance, and can be used as articles requiring these properties, such as sliding parts. Example

[0034] The present invention is described in detail below by way of examples, but the present invention is not limited thereto.

[0035] 《Production and evaluation of resin composition (1)》 [Materials used] Thermoplastic resin A-1: ​​polyamide 9T, produced by Kuraray Co., Ltd., product name: Genestar N1000A, melting point 300°C, specific gravity 1.14. Thermoplastic resin A-2: polyamide 66, produced by Asahi Kasei Corporation, product name: Leona 1500X11, melting point 265° C., specific gravity 1.14. Polymer B-1: a polymer containing 99.5 mol % or more of TFE units, in powder form, manufactured by AGC Corporation, product name: FluonPTFE L169J, average particle size: 18 μm, specific gravity: 2.15. Polymer C-1: A polymer synthesized by a known method containing 97.9 mol % TFE units, 0.1 mol % NAH units and 2.0 mol % PPVE units, with a melting point of 300°C, an average particle size of 3 μm and a specific gravity of 2.13.

[0036] [Examples 1, 4~5] Thermoplastic resin A-1, polymer B-1, and polymer C-1 were added to LABO PLASTOMILL (model: 4C150) manufactured by Toyo Seiki Co., Ltd. at the ratios shown in Table 1, and melt-kneaded at a screw speed of 100 rpm, a set resin temperature of 320° C., and a kneading time of 10 minutes to obtain a resin composition. Among them, polymer B-1 and polymer C-1 were mixed in advance at the mixing ratio shown in Table 1 to prepare a mixed powder, and the mixed powder was added to the above-mentioned LABO PLASTOMILL.

[0037] The obtained resin composition was press-molded using a melt hot press manufactured by TESTER Sangyo Co., Ltd. under the conditions of temperature: 320°C, preheating: 8 minutes, pressure: 5 MPa, and pressing time: 3 minutes to obtain a pressed sheet of 80 mm×80 mm×1 mm in thickness. The mold surface of the melt hot press had an arithmetic mean roughness Ra of 1.6 μm, and a mold release film (UPILEX125S manufactured by Ube Industries, Ltd.) having an arithmetic mean roughness Ra of 1.1 nm was used between the molded body and the mold for molding.

[0038] [Examples 2~3] Thermoplastic resin A-2, polymer B-1, and polymer C-1 were charged into LABO PLASTOMILL (model: 4C150) manufactured by Toyo Seiki Co., Ltd. in the proportions shown in Table 1, and melt-kneaded under the conditions of a screw speed of 50 rpm, a set resin temperature of 300° C., and a kneading time of 5 minutes to obtain a resin composition. The polymer B-1 and the polymer C-1 were mixed in advance at the mixing ratio shown in Table 1 to prepare a mixed powder, and the mixed powder was put into the above-mentioned LABO PLASTOMILL.

[0039] The obtained resin composition was press-molded using a melt hot press manufactured by TESTER Sangyo Co., Ltd. under the conditions of temperature: 300°C, preheating: 8 minutes, pressure: 5 MPa, and pressing time: 3 minutes to obtain a pressed sheet of 80 mm×80 mm×1 mm in thickness.

[0040] [evaluate] The obtained compressed tablets were evaluated as follows. The results are shown in Table 1.

[0041] <Amount of wear and dynamic friction coefficient> The pressed sheet was cut into a size of 40 mm×40 mm to obtain a test piece. The test piece was tested using a friction and wear tester manufactured by Olyentec Co., Ltd. according to the Matsubara friction measurement method (cylindrical flat O-ring type) of JIS K 7218 to measure the wear amount and dynamic friction coefficient of the test piece. In the test, a ring (material: S45Cs (1.5S), contact area: 2 cm) as the target material was placed at room temperature (23°C). 2 ) was contacted with the test piece under the conditions of pressure: 0.7 MPa, rotation speed: 0.5 m / sec, and test time: 30 sec.

[0042] <Average dispersed particle size> The pressed sheet was frozen and cut, and its cross section was observed using SEM (JSM-IT700HR manufactured by JEOL Ltd.). The magnification was 300 times in Examples 1 to 3 and 1000 times in Examples 4 to 5. The maximum diameter (domain size) of the domain (dispersed particles) of polymer B-1 was measured based on the SEM image, and the average value of the 20 values ​​ranked in order from the largest domain size in the image was taken as the average dispersed particle size. The fact that the material constituting each region is a fluorine-containing polymer was confirmed by energy dispersive X-ray spectroscopy (EDS) analysis using JSM-IT700HR manufactured by JEOL Ltd.

[0043] <Arithmetic mean roughness Ra> The arithmetic mean roughness Ra of the pressed tablet surface was measured using a contact surface roughness meter (SURFCOM manufactured by Tokyo Seimitsu Co., Ltd.) in accordance with JIS B0601:1994 under the conditions of measurement length: 4.0 mm, measurement speed: 0.30 mm / s, and cutoff value λc: 0.8 mm.

[0044] <Heat resistance (appearance)> The appearance of the pressed tablet was visually observed, and the heat resistance was evaluated according to the following criteria. ×: The area discolored to dark brown or black accounts for 50% or more of 100% by area of ​​the entire surface of the pressed tablet, and the appearance is uneven. ○: The portion discolored to dark brown or black is less than 50% by area out of 100% by area of ​​the entire surface of the pressed tablet.

[0045] Table 1

[0046] The dynamic friction coefficient and wear loss of Example 1 not containing polymer C-1 were high and the friction characteristics were poor. This is considered to be because the dispersibility of polymer B-1 in thermoplastic resin A-1 was poor and the surface roughness of the pressed tablet was large. In Examples 2 and 3 using the thermoplastic resin A-2 having a melting point of 260° C., more than half of the surface of the pressed tablet changed color to dark brown or black due to thermal degradation, resulting in an appearance of uneven color. Examples 4 and 5 have lower dynamic friction coefficients and wear losses and are excellent in friction characteristics compared to Example 1. In addition, compared to Examples 2 and 3, discoloration due to thermal degradation is suppressed and the heat resistance is excellent.

[0047] 《Manufacturing and evaluation of resin compositions (2)》 [Examples 6~13] The mixed powder obtained by mixing particles 1 and 2 in the proportion shown in Table 2 and the thermoplastic non-fluorine resin in the proportion shown in Table 2 were put into LABO PLASTOMILL (model: 4C150) manufactured by Toyo Seiki Co., Ltd., and melt-kneaded under the conditions of screw speed: 50 rpm, set resin temperature: 300° C., and kneading time: 5 minutes to obtain a resin composition. The details of particles 1, particles 2 and thermoplastic non-fluorine resin used in each example are shown outside the column of Table 2. However, in Example 10, the particles 1 and 2 were not mixed in advance but were separately put into the above-mentioned LABO PLASTOMILL and kneaded under the above-mentioned conditions to obtain a resin composition.

[0048] The obtained resin composition was press-molded using a melt hot press manufactured by TESTER Sangyo Co., Ltd. under the conditions of temperature: 300°C, preheating: 8 minutes, pressure: 5 MPa, and pressing time: 3 minutes to obtain a pressed sheet of 80 mm×80 mm×1 mm in thickness. The wear amount of the obtained pressed tablets was measured in the same manner as in Examples 2 to 3, and the evaluation results of the wear resistance according to the following criteria are shown in Table 2. However, in Example 10, the particles 1 and 2 were not mixed in advance but were separately put into the above-mentioned LABO PLASTOMILL and kneaded under the above-mentioned conditions to obtain a resin composition. <Evaluation criteria for wear resistance> A: Wear loss is 0.003cm 3 the following B: Wear greater than 0.003 cm 3 And within 0.006cm 3 the following C: Wear greater than 0.007 cm 3 And within 0.010cm 3 the following D: Wear greater than 0.010cm 3

[0049] Table 2

Industrial Applicability

[0050] According to the resin composition of the present invention, a molded body excellent in wear characteristics and heat resistance can be obtained. In addition, the entire contents of the specification, claims, and abstract of Japanese Patent Application No. 2022-045241 filed on March 22, 2022 are incorporated herein by reference in their entirety as a disclosure of the present specification.

Claims

1. A resin composition comprising a thermoplastic non-fluorine resin, a first tetrafluoroethylene polymer, and a second tetrafluoroethylene polymer having a melting point of 260° C. or higher and lower than the melting point of the first tetrafluoroethylene polymer, With respect to the total mass of the thermoplastic non-fluorine resin, the first tetrafluoroethylene polymer and the second tetrafluoroethylene polymer, the first tetrafluoroethylene polymer accounts for 4.0 to 32.0 mass %, and the second tetrafluoroethylene polymer accounts for 0.5 to 10.0 mass %, The resin composition is obtained by melt-kneading a mixed powder of first particles of a first tetrafluoroethylene-based polymer and second particles of a second tetrafluoroethylene-based polymer with a powder of a thermoplastic non-fluorine resin.

2. The resin composition according to claim 1, wherein The first tetrafluoroethylene-based polymer is polytetrafluoroethylene.

3. The resin composition according to claim 1, wherein The second tetrafluoroethylene-based polymer contains units based on at least one comonomer selected from the group consisting of perfluoro(alkyl vinyl ether), hexafluoropropylene and fluoroalkylethylene.

4. The resin composition according to claim 1, wherein The second tetrafluoroethylene-based polymer has an oxygen-containing polar group.

5. The resin composition according to claim 1, wherein The melting point of the first tetrafluoroethylene polymer is higher than 320°C and lower than 380°C, and the melting point of the second tetrafluoroethylene polymer is higher than 260°C and lower than 320°C.

6. The resin composition according to claim 1, wherein The difference between the melting point of the first tetrafluoroethylene polymer and the melting point of the second tetrafluoroethylene polymer is 20° C. or more and 60° C. or less.

7. The resin composition according to claim 1, wherein The average particle size of the first particles is 1 to 100 μm.

8. The resin composition according to claim 1, wherein The average particle size of the first particles is larger than the average particle size of the second particles.

9. The resin composition according to claim 8, wherein The ratio of the average particle size of the first particles to the average particle size of the second particles is 2 to 50 as a particle size ratio represented by first particles / second particles.

10. The resin composition according to claim 1, wherein The content of the first particles is greater than the content of the second particles.

11. The resin composition according to claim 1, wherein The content ratio of the first particles to the second particles is 55 / 45 to 99 / 1 in terms of mass ratio expressed as first particles / second particles.

12. The resin composition according to claim 1, wherein The melting point of the thermoplastic non-fluorine resin is not less than the melting point of the second tetrafluoroethylene-based polymer and lower than the melting point of the first tetrafluoroethylene-based polymer.

13. The resin composition according to claim 1, wherein The total content of the thermoplastic non-fluorine resin, the first tetrafluoroethylene polymer and the second tetrafluoroethylene polymer is 60.0% by mass or more based on the total amount of the resin composition.

14. The resin composition according to claim 1, wherein The content of the thermoplastic non-fluorine resin is 65.0 to 95.0% by mass based on the total mass of the resin composition.

15. A molded article formed from the resin composition according to any one of claims 1 to 14.