Use of nickel-iron-chromium alloy with high resistance in carbonization, vulcanization and chlorination environments and at same time good processability and strength

By adjusting the element composition in nickel-iron-chromium alloy, especially the content of nickel, chromium, silicon, aluminum and oxygen affinity elements, the problem of poor corrosion resistance and processability of the alloy in high corrosion environment is solved, and the problem of poor corrosion resistance and processability of the alloy is achieved. High temperature corrosion resistance and weldability in carbonized, vulcanized and chlorinated environments, suitable for component manufacturing in high corrosion environments.

CN118900927APending Publication Date: 2024-11-05VDM METALS INTERNATIONAL GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027115.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In highly corrosive environments, especially in carbonization, vulcanization and chlorination, existing nickel-iron-chromium alloys are difficult to take into account high-temperature corrosion resistance and processability, especially poor weldability, resulting in waste incineration facilities and coal gasification. There are difficulties in applications such as facilities.

Method used

Use nickel content between 35.0 and 38.0%, chromium content between 26.0 and 30.0%, silicon content is greater than 0.7 to 1.50%, aluminum content is 0.40 to 1.30%, and appropriate amounts of magnesium, calcium, carbon, nitrogen and phosphorus are added to the alloy. , oxygen and other elements to meet the specific element concentration relationship, add oxygen affinity elements such as cerium, lanthanum, yttrium, zirconium and hafnium to improve corrosion resistance, and control the content of molybdenum, cobalt, copper, tungsten and other elements to Improve the high-temperature corrosion resistance and weldability of alloys.

Benefits of technology

It realizes high-temperature corrosion resistance in carbonization, vulcanization and chlorination environments, improves the weldability and processability of alloys, and is suitable for component manufacturing in high-corrosion environments, such as waste incineration facilities and coal gasification facilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900927A_ABST
    Figure CN118900927A_ABST
Patent Text Reader

Abstract

Use of a nickel-iron-chromium alloy having excellent resistance to high-temperature corrosion as a semi-finished product in an environment of simultaneous carbonization, vulcanization and chlorination, said nickel-iron-chromium alloy comprising (in mass%): 35.0 to 38% nickel, 26.0 to 30.0% chromium, gt; the invention relates to a steel sheet, in particular a steel sheet, comprising 0.7 to 1.50% of silicon, 0.40 to 1.30% of aluminum, 0.00 to 1.0% of manganese, 0.0001 to 0.05% of magnesium and / or calcium, respectively, 0.015 to 0.12% of carbon, 0.001 to 0.150% of nitrogen, 0.001 to 0.030% of phosphorus, 0.0001 to 0.020% of oxygen, up to 0.010% of sulfur, less than 1.0% of molybdenum, less than 1.0% of cobalt, less than 0.5% of copper, less than 1.0% of tungsten, the balance being iron and common process-induced impurities, the following relationships must be satisfied: Fc =-1.2 + 0.29 * Ni-4.6 * Si-4.4 * Allt; 2.5 (1a), wherein Ni, Si and Al are the relative element concentrations in mass%.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to the use of a nickel-iron-chromium alloy having good high temperature corrosion resistance and improved workability, especially weldability, in highly corrosive environments, for example in simultaneously carburizing, sulfiding and chlorinating environments.

[0002] Austenitic nickel-iron-chromium alloys with different nickel, chromium and iron contents have been used for a long time in furnace construction and in the chemical and petrochemical industries. For such applications, good high-temperature corrosion resistance and good heat resistance even in carburizing, sulfiding environments are required.

[0003] In general, it should be noted that the high-temperature corrosion resistance of the alloys given in Table 1 increases with increasing chromium content. All of these alloys form a chromium oxide layer (Cr2O3) and a more or less closed silicon oxide layer located thereunder. Small additions of elements with a strong affinity for oxygen (e.g. yttrium or cerium) improve the corrosion resistance. During use within the scope of application, the chromium content is slowly consumed in order to form a protective layer. The service life of the material is therefore increased by a higher chromium content, since the higher content of chromium elements forming the protective layer postpones the point in time at which the chromium content falls below a critical limit and oxides other than Cr2O3 (e.g. iron-containing oxides and nickel-containing oxides) are formed. A further increase in the high-temperature corrosion resistance can be achieved by adding silicon or aluminum. Starting from a certain minimum content, these elements form a closed layer below the chromium oxide layer and thus reduce the consumption of chromium.

[0004] In a carburizing environment (CO, H2, CH4, CO2, H2O mixtures), carbon can penetrate into the material, which can form internal carbides. These carbides cause a loss in notched impact strength. Conversion processes may also occur due to chromium depletion in the matrix.

[0005] A high resistance to carburization is achieved by materials with a low carbon solubility and a low carbon diffusion rate. Nickel alloys are therefore generally more resistant to carburization than iron-based alloys, since carbon diffusion and carbon solubility in nickel are lower than in iron. An increase in the chromium content leads to a higher resistance to carburization by forming a chromium oxide protective layer, since the oxygen partial pressure in the gas is insufficient to form this chromium oxide protective layer. At very low oxygen partial pressures, materials can be used that form a silicon dioxide layer or a more stable aluminum oxide layer, both of which can still form an oxide protective layer at significantly lower oxygen contents.

[0006] In a carburizing and sulfiding environment (CO, H2, H2O, CO2, H2S mixture) with a lower oxygen partial pressure, sulfur can penetrate into the material, thereby forming sulfides. The melting point can also be reduced to very low values ​​(635°C for Ni-Ni3S2 eutectic and 988°C for Fe-FeS eutectic). Nickel-iron-chromium alloys with high nickel content are generally more sensitive than nickel-iron-chromium alloys with high iron content in sulfiding environments. Further improvement of high temperature corrosion resistance can also be achieved by adding silicon or aluminum.

[0007] In chlorinated environments with less oxygen partial pressure, volatile metal chlorides with high vapor pressure and / or low melting point can form and thus produce high corrosion rates.High chromium and / or nickel content improves corrosion resistance.

[0008] DE 41 30 139 C1 describes a heat-resistant, hot-forgeable austenitic nickel alloy composed, in % by mass, of 0.05 to 0.15% carbon, 2.5 to 3.0% silicon, 0.2 to 0.5% manganese, up to 0.015% phosphorus, up to 0.005% sulfur, 25 to 30% chromium, 20 to 27% iron, 0.05 to 0.15% aluminum, 0.001 to 0.005% calcium, 0.05 to 0.15% rare earths, 0.05 to 0.20% nitrogen, the remainder being nickel and usual impurities resulting from melting.

[0009] The alloy described in DE 4130139 C1 is known under the names “NiCr28FeSiCe”, Alloy 45™, Nicrofer 45™ or with the material number 2,4889 and is referred to below as “45™”.

[0010] Alloy 45TM is very resistant in carburizing and sulfiding media, so they are suitable for use in waste incineration facilities or coal gasification facilities. Figure 1 The corrosion depths in various alloys measured metallographically as a function of the temperature of the various alloys after aging for 2100 hours in H2S-containing gases in the PRENFLO coal gasification pilot plant in Fürstenhausen are shown. Table 1 shows the composition of the alloys investigated according to the prior art. A higher chromium content and a higher silicon content significantly reduce the corrosion depth. Due to the higher silicon content of ≥2.5%, a silicon oxide layer can be formed below the chromium oxide protective layer, which achieves a high corrosion resistance of the material. 45TM with 26 to 29% chromium and 2.5 to 3% silicon shows the smallest corrosion depth at all temperatures, followed by AC66 with 26 to 28% chromium and a maximum of 0.3% silicon.

[0011] However, alloy 45TM is very difficult to process. This is manifested, for example, in crack formation during hot shaping. During welding, 45TM is also prone to crack formation, which makes intrinsic welding (with welding fillers within the composition range of the materials to be welded) that may make sense for corrosion protection purposes impossible and makes the practical use of this material difficult. For austenitic FeCrNi solders with primary austenite solidification, the formation of low-melting phases (eutectic Fe-Fe2Si: 1212°C; eutectic NiSi-Ni3Si2: 964°C and NiSi: 996°C) and enlarged solidification zones due to silicon enrichment at the austenite grain boundaries can be mentioned as causes of increased thermal crack formation.

[0012] In contrast, alloy AC66 (composition see Table 1) has sufficiently high weldability and machinability, but is not as corrosion resistant in coal gasification facilities, such as Figure 1 shown.

[0013] If, in addition to carbonization and sulfidation conditions, corrosion caused by chlorine is added, such as exists in coal gasification facilities, waste incineration facilities, etc., the requirements for materials are further increased.

[0014] For materials used in carbonized, sulphurized and chlorinated environments, in particular in atmospheres, compromises must be made in terms of composition.

[0015] The heat resistance is improved in particular by a high carbon content. However, high contents of elements for mixed-crystal solidification, such as chromium, aluminum, silicon, molybdenum and tungsten, also improve the heat resistance.

[0016] US 6,623,869 B1 describes a metal material, which contains the following components in mass %: not more than 0.2% carbon, 0.01-4% silicon, 0.05-2% manganese, not more than 0.04% phosphorus, not more than 0.015% sulfur, 10-35% chromium, 30-78% nickel, not less than 0.005% aluminum, less than 4.5% aluminum, 0.005-0.2% nitrogen and 0.015-3% copper and 0.015-3% cobalt or both, wherein the balance is substantially iron. Here, the value of 40Si+Ni+5Al+40N+10(Cu+Co) is not less than 50, wherein the symbol of the element represents the alloy content of the corresponding element. The metal material has excellent corrosion resistance in an environment where the metal may be ashed and can therefore be used in furnace tubes, piping systems, heat exchanger tubes, etc. in petroleum refineries or petrochemical facilities. This can significantly improve the durability and safety of the facility.

[0017] US 3,833,358 A describes an iron-based fireproof alloy which provides high resistance to creep, thermal shock, thermal fatigue and intergranular oxidation as well as good weldability, the alloy consisting essentially of the following elements (in weight proportions):

[0018] C 0.05-0.20

[0019] Ni 30–40

[0020] Cr 20–30

[0021] Nb 0.2–2

[0022] N 0.04-0.2

[0023] Mn 0.6–2

[0024] Si 0.6–2

[0025] Ta 0-0.3

[0026] Ti 0–1

[0027] Mo 0-0.5

[0028] Al 0-0.05

[0029] Pb 0-0.01

[0030] Sn 0-0.01

[0031] Zn 0-0.01

[0032] Cu 0-0.25

[0033] The balance is basically iron. Here, the weight ratio of the above elements satisfies the following formula:

[0034] 30*C%+Ni%+0.5*Mn%+16*N%=

[0035] Cr%+0.5*(Nb+1 / 2Ta)%+3.5*Ti%+1.5*Si%+Mo%+(11+ / -2)%

[0036] A=B+ / -20%

[0037] Wherein A=30*C%B=2*Ti%+6*(Nb+1 / 2Ta)%.

[0038] US 3,865,581 A describes a heat-resistant alloy having heat-shaping properties, comprising 0.01 to 0.5% C, 0.01 to 2.0% Si, 0.01 to 3.0% Mn, 22 to 80% Ni and 10 to 40% Cr as main components, and one or two of 0.0005 to 0.20% B and 0.001 to 6.0% Zr, and also one or more of 0.001 to 0.5% Ce, 0.001 to 0.2% Mg and 0.001 to 1.0% Be, the remainder being iron and unavoidable impurities. It is suitable for furnace construction (burner tips, protective shells, protective tubes for thermal elements, etc.).

[0039] DE 1024719 A describes a method for adding cerium and / or lanthanum to a nickel-iron alloy. This nickel-iron alloy is a heat-formable alloy characterized by the following composition: 0 to 0.5% carbon, 10 to 60% of one or more of the elements chromium, molybdenum and tungsten, wherein the amount of each of these elements does not exceed 30%, 0 to 73% iron, 0.02 to 1.10% cerium or lanthanum or lanthanum or both, and the balance 4 to 70% nickel (including impurities), provided that the content of rare earth metals is adapted to the nickel content in the following manner:

[0040]

[0041] EP 0812926 A1 describes a nickel-based alloy whose strength increases with use, which consists of 0.06-0.14% carbon, 35-46% nickel, 22.5-26.5% chromium, 0-1.5% manganese, 0.5-2% silicon, 0.1-1% titanium, 0.05-2% aluminum, 1-3% molybdenum, 0.2-1% niobium, 0.1-1% tantalum, 0-0.3% tungsten, 0-0.008% boron, 0-0.05% zirconium and the remainder iron and random impurities.

[0042] WO 2007 / 124996 A1 describes a reaction vessel for preparing hydrogen sulfide by reacting sulfur with hydrogen, wherein the reaction vessel and, except for the optional connecting lines and valves and measuring and regulating devices, partly or completely consists of a material that is resistant to the reaction mixture (including aluminum). The material contains, in particular, the following constituents: 0-0.3% C, 0-2.5% Si, 0-2.5% Mn, 0-0.1% P, 0-0.3% S, 15.0-28.0% Cr, 0-1.0% Cu, 0-balance % Fe, 1.0-5.0% Al, 0-2.5% Co, 0-1.5% Ti, 0-0.4% Y and up to 70% Ni (% by weight).

[0043] DE 10 2007 005 605 A1 describes an iron-nickel-chromium-silicon alloy with (in wt. %) 34 to 42% nickel, 18 to 26% chromium, 1.0 to 2.5% silicon and additions of 0.05 to 1% Al, 0.01 to 1% Mn, 0.01 to 0.26% lanthanum, 0.0005 to 0.05% manganese, 0.01 to 0.14% carbon, 0.01 to 0.14% nitrogen, maximum 0.01% sulfur, maximum 0.005% boron, the remainder being iron and usual process-induced impurities. This alloy is used in heating elements.

[0044] US 5,021,215 A discloses a high hardness heat-resistant steel with improved formability, the steel consisting essentially of the following (weight %):

[0045] C: 0.05–0.30%, Si: not more than 3.0%,

[0046] Mn: not more than 10%, Cr: 15–35%,

[0047] Ni:15–50%, Mg:0.001–0.02%,

[0048] B:0.001–0.01%, Zr:0.001–0.10%,

[0049] At least one of the following elements Ti: 0.05-1.0%, Nb: 0.1–2.0%, and

[0050] Al: 0.05–1.0%,

[0051] Mo:0–3.0%, W:0–6.0%,

[0052] (Mo+1 / 2W=3.0% or less)

[0053] The balance is iron and random impurities, wherein the impurities oxygen and nitrogen are limited to 50 ppm or less and 200 ppm or less, and wherein the austenite grain size value is limited to No. 4 or coarser.

[0054] JPS 56163244 A describes improving the heat treatability and oxidation resistance of austenitic steel by adding certain amounts of C, Si, Mn, Ni, Cr, Al, B, rare earth elements and Ca to the steel grade. This is achieved by an austenitic steel containing the following composition in weight %: <0.2% C, 1.5-3.5% Si, <2% Mn, 8-35% Ni, 15-30% Cr, <2% Al, 0.0005-0.005% B, 0.005-0.1% rare earth elements and 0.0005-0.02% Ca or 0.0005-0.03% Mg added additionally when necessary. The austenitic steel thus produced is finished in a conventional steelmaking furnace, and this molten steel is formed into an ingot, which is then hot rolled.

[0055] US 7,118,636 B2 describes a nickel-iron-chromium alloy containing a phase for solidification which is able to maintain a fine grain structure during forging and when the alloy is processed at high temperatures. The alloy contains sufficient amounts of titanium, zirconium, carbon and nitrogen to form fine titanium and zirconium nitrides, but close to their solubility limits in the molten state of the alloy. When articles are prepared from such an alloy by thermomechanical processing, a dispersion of fine titanium carbonitride and zirconium carbonitride precipitates is produced when the melt solidifies, and the dispersion is retained in the alloy during subsequent processing steps (at elevated temperatures) to avoid austenite grain growth. A nickel-iron-chromium alloy comprising less than 0.05 weight percent niobium, at least 0.05 weight percent zirconium, at least 0.05 weight percent carbon, at least 0.05 weight percent nitrogen, the weight ratio of carbon to nitrogen being at least 1 to 2 and less than 1 to 1, sufficient titanium, zirconium and / or aluminum to remove chromium carbides, and sufficient amounts of titanium, zirconium, carbon and nitrogen to form a uniform dispersion free of fine titanium carbonitrides and zirconium carbonitrides, in a molten state of the alloy near the solubility limit of titanium carbonitride and zirconium carbonitride precipitation in sufficient amounts to obtain [(Ti x Zr 1-x )(C y N 1-y )]. In addition, this nickel-iron-chromium alloy consists of about 32% to about 38% by weight iron, about 22% to 28% by weight chromium, about 0.10% to about 0.60% titanium, about 0.05% to about 0.30% zirconium, about 0.05% to about 0.30% carbon, about 0.05% to about 0.30% nitrogen, about 0.05% to about 0.5% aluminum, up to 0.99% molybdenum, up to about 0.01% boron, up to about 1% silicon, up to about 1% manganese, the balance nickel and random impurities.

[0056] JPS 57134544 A describes improving the resistance to stress tearing corrosion by adding a certain amount of Mo, W, etc. to a high Cr-Ni content steel as a pipe material. For this purpose, an alloyed steel having the following composition is used: <0.10% C, <1.0% Si, <2.0% Mn, <0.030% P, <0.005% S, <0.5% Al, 22.5-30% Cr, 25-60% Ni and Mo and / or W, the steel satisfying the following formula

[0057] Cr(%)+10*Mo(%)+5*W(%)≥70%

[0058] 4%≤Mo(%)+1 / 2W(%)<8%

[0059] The steel is used for pipelines of oil wells, which are used in highly corrosive and rough environments of petroleum sources, natural gas sources, etc. <1% Cu and / or <2% Co and / or <0.10% of one or more rare earth elements, <0.20% Y, <0.10% Mg, <0.10% Ca and <0.5% Ti can be added to the alloy. Oil well pipes with strong stress tearing corrosion resistance in highly corrosive environments of petroleum sources containing H2S, CO2 and Cl can be prepared.

[0060] Therefore, the basic object of the present invention is to conceive the use of a nickel-iron-chromium wrought alloy, which

[0061] a) has good high temperature corrosion resistance similar to Alloy 45TM in highly corrosive environments, such as in simultaneously carburizing, sulfiding and chlorinating environments,

[0062] b) have sufficiently high machinability, in particular weldability, as similar as possible to alloy AC66, and

[0063] c) It has sufficiently high heat resistance at 500°C, similar to that of alloy AC66.

[0064] The basic object of the present invention is achieved by the use of a nickel-iron-chromium alloy with excellent high temperature corrosion resistance as a semi-finished product in a simultaneously carburizing, sulfiding and chlorinating environment, the nickel-iron-chromium alloy comprising (in mass %):

[0065] 35.0 to 38% nickel,

[0066] 26.0 to 30.0% chromium,

[0067] >0.7 to 1.50% silicon,

[0068] 0.40 to 1.30% aluminum,

[0069] 0.00 to 1.0% manganese,

[0070] 0.0001 to 0.05% magnesium and / or calcium, respectively,

[0071] 0.015 to 0.12% carbon,

[0072] 0.001 to 0.150% nitrogen,

[0073] 0.001 to 0.030% phosphorus,

[0074] 0.0001 to 0.020% oxygen,

[0075] Maximum 0.010% sulfur,

[0076] Less than 1.0% molybdenum,

[0077] Less than 1.0% cobalt,

[0078] Less than 0.5% copper,

[0079] Less than 1.0% tungsten,

[0080] The balance is iron and common process-related impurities, where the following relationship must be satisfied:

[0081] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5(1a),

[0082] Wherein Ni, Si and Al are the relevant element concentrations in mass %.

[0083] Advantageous developments of the subject matter of the invention can be gathered from the associated dependent claims.

[0084] The nickel content is between 35.0 and 38.0%, wherein the preferred content can be set within the following distribution range:

[0085] -35 or >35.0 to <38.0%

[0086] -35 or >35.0 to 37 or <37.0%.

[0087] The distribution range of the chromium element is between 26.0 and 30.0%, wherein the preferred range can be set as follows:

[0088] ->26.0 to <30.0%

[0089] -27.0 or >27.0 to 30.0 or <30.0%

[0090] -28.0 or >28.0 to 30.0 or <30.0%

[0091] The silicon content is between >0.7 and 1.50%. Preferably, in the alloy, silicon can be set within the following distribution range:

[0092] ->0.70 to <1.50%.

[0093] -0.80 or >0.80 to 1.50 or <1.50%

[0094] -0.90 or >0.90 to 1.50 or <1.50%

[0095] -0.80 or >0.80 to 1.50 or <1.50%

[0096] -0.80 or >0.80 to 1.45 or <1.45%.

[0097] The aluminum content is between 0.40 and 1.30%, wherein the preferred aluminum content can also be set in the following manner:

[0098] ->0.40 to <1.30%

[0099] -0.50 or >0.50 to 1.30 or <1.30%

[0100] -0.50 or >0.50 to 1.20 or <1.20%

[0101] -0.50 or >0.50 to 1.10 or <1.10%

[0102] -0.60 or >0.60 to 1.10 or <1.10%.

[0103] The same applies to the element manganese, which can be contained in the alloy in an amount of 0.0 to 1.0%. Alternatively, the following distribution ranges are also conceivable:

[0104] -> 0.0 to <1.00%

[0105] ->0.0 to 0.50 or <0.50%

[0106] ->0.0 to 0.05 or <0.05%

[0107] -0.005 or >0.005 to 0.20 or <0.20%

[0108] -0.005 or >0.005 to 0.10 or <0.10%.

[0109] Magnesium and / or calcium are also contained in a content of 0.0001 to 0.05%. Preferably, there is the possibility of setting these elements in the alloy as follows:

[0110] -0.0001 to 0.030%

[0111] -0.0001 to 0.020%

[0112] -0.0002 to 0.015%

[0113] -0.0010 to 0.010%.

[0114] The alloy contains 0.015 to 0.12% carbon. Preferably, in the alloy, the carbon can be set within the following distribution range:

[0115] ->0.015 to <0.12%.

[0116] -0.03 or >0.03 to 0.10 or <0.10%

[0117] -0.04 or >0.04 to 0.10 or <0.10%

[0118] -0.05 or >0.05 to 0.10 or <0.10%

[0119] -0.05 or >0.05 to 0.09 or <0.09%.

[0120] The same applies to the nitrogen element contained in a content between 0.001 and 0.150%. Preferred contents may be present as follows:

[0121] ->0.001 to <0.150%

[0122] -0.010 or >0.010 to 0.140 or <0.140%

[0123] -0.020 or >0.020 to 0.140 or <0.140%

[0124] -0.050 or >0.050 to 0.140 or <0.140%.

[0125] The alloy further comprises phosphorus in an amount between 0.001 and 0.030%. Preferred amounts may be present as follows:

[0126] -0.001 to 0.015%.

[0127] The alloy furthermore contains oxygen in a content of between 0.0001 and 0.020%, in particular 0.0001 to 0.010%.

[0128] The sulfur element is present in the alloy at a maximum of 0.010%. Preferred contents may be present as follows:

[0129] - Sulfur 0.008% maximum.

[0130] Molybdenum is contained in the alloy in an amount of less than 1.0%. In addition, the molybdenum content may be limited as follows:

[0131] -Mo max 0.50 or <0.50%

[0132] -Mo max 0.20 or <0.20%

[0133] -Mo max 0.10 or <0.10%

[0134] -Mo max 0.05 or <0.05%

[0135] -Mo maximum 0.02 or <0.02%.

[0136] Furthermore, less than 1.0% cobalt is included in the alloy. In addition, the cobalt content may be limited as follows:

[0137] -Co max 0.50 or <0.50%

[0138] -Co max 0.20 or <0.20%

[0139] -Co max 0.10 or <0.10%

[0140] -Co max 0.05 or <0.05%

[0141] -Co max 0.015 or <0.015%.

[0142] In addition, less than 0.5% copper may be included in the alloy. In addition, the copper content may be limited as follows:

[0143] -Cu max 0.30 or <0.30%

[0144] -Cu max 0.10 or <0.10%

[0145] -Cu max 0.05 or <0.05%

[0146] -Cu max 0.015 or <0.015%.

[0147] Tungsten is contained in the alloy in a content of maximum 1.0%. In addition, the tungsten content can be limited as follows:

[0148] -W < 1.0%

[0149] -W max 0.50 or < 0.50%

[0150] -W max 0.20 or < 0.20%

[0151] -W max 0.10 or < 0.10%

[0152] -W max 0.05 or < 0.05%

[0153] -W 0.02 max or < 0.02%.

[0154] The balance in the alloy consists of iron and common impurities resulting from the production. In addition, the iron content can be limited as follows:

[0155] -28.0 or >28.0 to 38.0%

[0156] -29.0 or >29.0 to 38.0%

[0157] -30.0 or >30.0 to 38.0 or <38.0%.

[0158] The following relationship must be satisfied between nickel, silicon and aluminum so that there is a sufficiently high resistance in a carburizing, sulfiding and chlorinated environment:

[0159] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5(1a),

[0160] Wherein Ni, Si, Al and Si are the relevant element concentrations in mass %.

[0161] The preferred range can be set by the following formula

[0162] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤1.5(1b)

[0163] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤1.0(1c)

[0164] The addition of elements with an affinity for oxygen, such as cerium, lanthanum, yttrium, zirconium and hafnium, improves the corrosion resistance by simultaneously incorporating them into the oxide layer and thereby blocking the diffusion paths of oxygen at the grain boundaries.

[0165] According to the requirements, the alloy may contain 0.001 to 0.20% of one or more of cerium, lanthanum, yttrium, zirconium and hafnium, respectively, wherein the following formula must be satisfied:

[0166] FRE=0.714*Ce+0.720*La+1.124*Y+1.096*Zr+0.560*Hf≤0.10(2a)

[0167] Wherein Ce, La, Y, Zr and Hf are the relevant element concentrations in mass %.

[0168] In the presence of at least one of the elements cerium, lanthanum, yttrium, zirconium and hafnium, the FRE can preferably be set as follows:

[0169] FRE=0.714*Ce+0.720*La+1.124*Y+1.096*Zr+0.560*Hf≤0.075(2b)

[0170] FRE=0.714*Ce+0.720*La+1.124*Y+1.096*Zr+0.560*Hf≤0.065(2c)

[0171] Optionally, cerium mixed metal (abbreviated CeMM) is also used in a content of 0.001 to 0.20% in the presence of cerium and lanthanum, wherein the FRE must be changed as follows:

[0172] FRE=0.716*CeMM+1.124*Y+1.096*Zr+0.560*Hf≤0.10

[0173] (3a)

[0174] Wherein CeMM, Y, Zr and Hf are the concentrations of relevant elements in mass %.

[0175] When adding the cerium mixed metal, the FRE may preferably be set as follows:

[0176] FRE=0.716*CeMM+1.124*Y+1.096*Zr+0.560*Hf≤0.075

[0177] (3b)

[0178] FRE=0.716*CeMM+1.124*Y+1.096*Zr+0.560*Hf≤0.065

[0179] (3c)

[0180] Preferably, in the alloy, cerium, lanthanum, cerium mixed metal, zirconium and hafnium may be included in the following distribution ranges:

[0181] ->0.001 to <0.20%

[0182] -0.001 or >0.001 to 0.15 or <0.15%

[0183] -0.001 or >0.001 to 0.10 or <0.10%

[0184] -0.001 or >0.001 to 0.08 or <0.08%

[0185] -0.001 or >0.001 to 0.05 or <0.05%

[0186] -0.001 or >0.001 to 0.04 or <0.04%.

[0187] -0.01 or >0.01 to 0.04 or <0.04%

[0188] Preferably, in the alloy, yttrium may be contained within the following distribution range:

[0189] ->0.001 to <0.20%

[0190] -0.001 or >0.001 to 0.15 or <0.15%

[0191] -0.001 or >0.001 to 0.10 or <0.10%

[0192] -0.001 or >0.001 to 0.08 or <0.08%

[0193] -0.01 or >0.01 to 0.08 or <0.08%

[0194] -0.01 or >0.01 to <0.045%.

[0195] Optionally, in the alloy, titanium element may be present in an amount of 0.0 to 0.50%. Preferably, in the alloy, titanium may be contained in the following distribution range:

[0196] -> 0.0 to < 0.50%

[0197] ->0.0 to 0.50 or <0.50%

[0198] -0.001 or >0.001 to 0.20 or <0.20%

[0199] -0.001 or >0.001 to 0.15 or <0.15%

[0200] -0.001 or >0.001 to 0.10 or <0.10%

[0201] -0.001 or >0.001 to 0.05 or <0.05%

[0202] -0.001 or >0.001 to 0.04 or <0.04%.

[0203] -0.005 or >0.005 to 0.20 or <0.20%.

[0204] -0.010 or >0.010 to 0.20 or <0.20%.

[0205] Optionally, in the alloy, the niobium element may be set to a content of 0.0 to 0.2%. Preferably, in the alloy, niobium may be contained in the following distribution range:

[0206] -> 0.0 to < 0.20%

[0207] ->0.0 to 0.15 or <0.15%

[0208] ->0.0 to 0.10 or <0.10%

[0209] ->0.0 to 0.05 or <0.05%

[0210] ->0.0 to 0.02 or <0.02%

[0211] -0.001 or >0.001 to 0.20 or <0.20%

[0212] -0.010 or >0.010 to 0.20 or <0.20%.

[0213] Optionally, the alloy may also contain 0.0 to 0.20% tantalum. The preferred content may be as follows:

[0214] -> 0.0 to < 0.20%

[0215] ->0.0 to 0.10 or <0.10%

[0216] ->0.0 to 0.05 or <0.05%.

[0217] Optionally, the alloy may contain boron in an amount of 0.0001-0.008%. Preferred contents may be as follows:

[0218] - Boron 0.0005-0.008%

[0219] - Boron 0.0005-0.005%

[0220] - Boron 0.0005-0.004%.

[0221] Furthermore, up to 0.50% vanadium may be included in the alloy.

[0222] -V<0.50%

[0223] -V max 0.40 or < 0.50%

[0224] -V max 0.20 or < 0.20%

[0225] -V max 0.08 or < 0.10%

[0226] -V max 0.05 or <0.05%

[0227] Finally, the impurities may include lead, zinc and tin in the following amounts:

[0228] Pb max. 0.002%, Zn max. 0.002%, Sn max. 0.002%

[0229] Then, the element beryllium can be present as follows:

[0230] Be is less than 0.001%,

[0231] The alloy of the present invention is preferably melted in an open state and subsequently treated with VOD (vacuum oxygen decarburization) or VLF (vacuum ladle furnace). However, it can also be melted and cast in a vacuum. The alloy is then cast into blocks, electrodes or as a continuous casting for forming a preform. If appropriate, the preform is then annealed at a temperature between 900 and 1270° C. for 0.1 to 70 hours. In addition, the alloy can be additionally remelted once or multiple times with ESU (electroslag remelting) and / or VAR (vacuum arc remelting). The alloy is then made into the desired semi-finished form. For this purpose, annealing is performed at a temperature between 800 and 1290° C. for 0.1 to 70 hours, followed by hot shaping, and, if appropriate, an intermediate annealing is performed between 800 and 1290° C. for 0.05 to 70 hours. If appropriate, the material surface can be (multiple times) occasionally and / or at the end of hot shaping, chemically and / or mechanically ground for cleaning. Then, if appropriate, cold forming can be performed with a degree of shaping of up to 98% into the desired semi-finished product form, if appropriate, and if appropriate, intermediate annealing between 800 and 1250° C. for 0.05 minutes to 70 hours under protective gas (for example argon or hydrogen), followed by cooling in air, in a moving annealing atmosphere or in a water bath. Then, if appropriate, solution annealing is performed in a temperature range of 800 to 1250° C. under protective gas (for example argon or hydrogen) for 0.05 minutes to 70 hours, followed by cooling in air, in a moving annealing atmosphere or in a water bath. If appropriate, the material surface can be chemically and / or mechanically cleaned occasionally and / or after the last annealing.

[0232] The semi-finished product produced by hot rolling and / or cold rolling has a structure with an average grain size of 5 to 600 μm after solution annealing.

[0233] The alloy of the present invention is well prepared or used in the semi-finished forms of bars, plates, castings, longitudinally welded or seamless pipes, pipe fittings, valve parts, flanges. Various semi-finished forms can be converted into the required components or installed into the required parts.

[0234] The alloys of the present invention may also be used for coating and welding onto any type of metal component as desired.

[0235] The alloy of the invention is particularly suitable for use as a component in application areas with carburized, sulfidized and chlorinated environments, in particular atmospheres. Due to the good high-temperature corrosion resistance of the alloy of the invention and its good formability and weldability, the alloy of the invention is suitable for use as a component in waste incineration facilities, pyrolysis facilities, refining furnaces, chemical industry, coal gasification facilities and industrial furnace construction, activated carbon filters, waste pyrolysis and precious metal recovery. Example:

[0236] Tests performed

[0237] High temperature corrosion resistance in a carburizing, sulfiding and chloriding environment was evaluated by the resistance of the material at elevated temperatures in a flowing forming gas atmosphere having carburizing, sulfiding and chloriding characteristics.

[0238] For this purpose, cut the semi-finished products of the corresponding alloy into pieces with the dimensions of 20 x 8 x 4 mm. 3 The specimens are then provided with a bore of 3 mm diameter and subsequently wet-ground with SiC paper of a maximum grit number of 1200 (particle size of about 15 μm). The specimens are degreased and cleaned with isopropanol in an ultrasonic bath. Each specimen is suspended in a reaction vessel by means of a ceramic crucible by means of this bore, so that the corrosion products that flake off in some cases are collected and the mass of the flakes can be determined by weighing the crucible containing the corrosion products. The sum of the mass of the flakes and the mass change of the specimen is the gross weight change of the specimen. The specific mass change is the mass change with respect to the surface area of ​​the specimen. In the following, m 净 Indicates the change in specific net weight, m 毛 Indicates the specific gross weight change, m 剥落 Indicates the specific mass change of the exfoliated oxide.

[0239] A gas mixture formed by 60% CO, 30% H2, 4% CO2, 1% H2S, 0.05% HCl and 3.95% H2O flows through the space of the reaction vessel. This mixture has a carbonizing (60% CO), a sulfiding (1% H2S) and a chlorinating (0.05% HCl) effect. The experiments were carried out at 500°C. The experimental duration was 1056 hours, divided into 11 cycles of 96 hours each. In each experiment, two specimens of each alloy were present. The values ​​given are the average of these two specimens.

[0240] In the following study, the following alloy was described as resistant in a carburizing and sulfiding and chlorinating environment: the alloy showed after 1056 hours

[0241] - ≤ 2.0 mg / cm 2of gross weight increase (4).

[0242] This is the case when the following relationship exists between nickel, silicon and aluminum:

[0243] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5(1a),

[0244] Herein, Ni, Si, Al and Si are the concentrations of the relevant elements in mass %.

[0245] Weldability is assessed by the extent to which hot cracks form during welding. The greater the risk of hot cracks forming, the worse the weldability of the material.

[0246] In order to quantify the hot tearing tendency, various alloys were tested with MVT (Modified Variable Constraint - Transverse Variable Constraint) at the BAM (Federal Institute for Materials Research and Testing). For this purpose, specimens with the dimensions of 100 mm x 40 mm x 10 mm were produced from the alloy. In the MVT test, a WIG weld (WIG: Tungsten Inert Gas) is laid longitudinally on the top surface of this specimen at a constant advance speed in a fully mechanized manner. When the arc passes through the center of the specimen, a defined bending strain is applied to the specimen. The specimen is bent in the welding direction (variable constraint mode). During this phase of bending, hot cracks form in the positionally restricted test area of ​​the MVT specimen.

[0247] The experiment was carried out at a bending strain of 4%, a descending speed of 2 mm / s, and a unit length energy of 7.5 kJ / cm in pure argon gas at 4.8.

[0248] For the analysis, the lengths of all solidification cracks and remelting cracks visible on the specimen in an optical microscope at a magnification of 25 times were determined and summed. These results can then be used to classify the materials given in Table 2 into the categories "safe for thermal cracking" (region 1), "increased tendency to thermal cracking" (region 2) and "at risk of thermal cracking" (region 3).

[0249] In the following studies, it was considered that those alloys can be welded well, which are in the MVT test in zone 1 "safe for hot cracking" and zone 2 "increased tendency to hot cracking", since the weldable alloy AC66 according to the prior art is in zone 2. Alloys in the "risk of hot cracking" (zone 3) are generally difficult to weld. Welding with intrinsic welding fillers (similar in composition to the materials to be welded) is especially difficult or impossible.

[0250] An assessment of the heat resistance is obtained by a hot tensile test. The heat resistance is determined in a tensile test according to DIN EN ISO 6892-2 at the desired temperature. The elongation limit Rp until break is determined.0.2 , tensile strength R m and elongation A. The experiments were carried out on circular specimens with a diameter of 6 mm and an initial measuring length L0 of 30 mm in the test area. The elongation limit Rp at 500 °C 0.2 Or tensile strength R m At least the minimum values ​​for alloy AC66 according to the prior art should be achieved:

[0251] -500℃:R p 0.2≥95MPa or R m ≥115MPa(5a,5b)

[0252] Desirably, they are better than the minimum values ​​for Alloy 45TM according to the prior art.

[0253] -500℃:R p 0.2≥150MPa or R m ≥500MPa. (6a, 6b)

[0254] The particle size was determined by means of the intercept method.

[0255] preparation

[0256] In order to determine the properties of components produced from the alloy, alloys melted in a vacuum furnace were used on a laboratory scale.

[0257] Tables 3a and 3b show the analysis of batches melted at laboratory scale and several batches melted according to the prior art (AC66 (1.4877) and 45TM (2.4889)) for comparison in large-scale production. Batches according to the prior art are marked with T and batches according to the invention are marked with E. Batches melted at laboratory scale are marked with L and batches melted in large-scale production are marked with G.

[0258] Alloy blocks from Tables 3a and 3b melted in vacuum on a laboratory scale were annealed for 8 hours at 900 to 1270° C. and hot rolled to a final thickness of 13 or 6 mm by means of hot rolling and a further intermediate annealing for 0.1 to 1 hour at 900 to 1270° C. The sheets thus produced were solution annealed for 1 hour at 800 to 1250° C. The test specimens required for the measurements were produced from these sheets.

[0259] In the case of large-scale produced molten alloys, samples are taken from large-scale production of plates with matching thickness produced in operation. The test specimens required for the measurement are prepared from these plates.

[0260] All alloy variants typically have a grain size of 50 to 190 μm.

[0261] For the example batches in Table 3a and b), the following properties were compared:

[0262] -High temperature corrosion resistance in carbonized, sulfided and chlorinated environments

[0263] -Weldability by means of MVT testing

[0264] - Creep resistance by means of hot tensile tests

[0265] The results are summarized in Table 4.

[0266] Table 4 shows the results of corrosion tests in the form of gross weight change and spalling after 1056 hours at 500° C. in an atmosphere formed by 60% CO, 30% H2, 4% CO2, 1% H2S, 0.05% HCl and 3.95% H2O. All alloys tested have a chromium content of about 27 to 28%. Alloy AC66 according to the prior art with only 0.2% silicon shows 10.92 mg / cm 2 Alloy 45TM with 2.6% Si according to the prior art and all tested batches melted on a laboratory scale with a Si content greater than 1.0% showed a maximum gross weight increase of 2.0 mg / cm 2 If the aluminum content is additionally greater than 0.40%, a batch with a silicon content of 1.0% or less may also have a silicon content of 2.0 mg / cm or less when Fc≤2.5 is satisfied. 2 This is the case in batches 250084 (Si=0.59% and Al=0.95%), 250085 (Si=0.90% and Al 0.98%), 250106 (Si=0.98% and Al 0.80%) and 250108 (Si=0.70% and Al=0.86%).

[0267] Batches 250084, 250106, 250105, 250108 and 250107 are according to the invention, batch 2209 with a silicon content greater than 1.50% and batch 250098 with a nickel content of 44.0% are not according to the invention. Compared to batches 250106 (Si=0.98% and Al=0.80%) and 250101 (Si=1.01% and Al=0.75%), batch 250098 (Si=1.20% and Al=0.85%) shows a similar or higher gross weight increase despite a significantly increased silicon content of 1.2%. Compared to batches 250106 (Ni=35.6%) and 250101 (Ni=38.2%), batch 250098 (Ni=44.0%) has a significantly increased nickel content. This shows that the higher nickel content makes corrosion more severe. Therefore, the upper limit of nickel is 40% at maximum.

[0268] In the non-inventive 2 Gross weight increase (3.43mg / cm 2 ) of batch 250100 (Ni=38.2%, Si=0.99% and Al=0.43%), the aluminum content is a bit too low, so that, in contrast to batch 250101 (Ni=38.2%, Si=1.01% and Al=0.75%), formula (1a) cannot be satisfied. 2 Gross weight increase (8.01mg / cm 2 and 5.35mg / cm 2 ) in batches 250103 (Ni=38.2%, Si=0.36% and Al=0.82%) and 250099 (Ni=38.4%, Si=1.00% and Al=0.20%), the silicon content and the aluminum content were outside the required limit values ​​and otherwise failed to satisfy formula (1a).

[0269] Alloys 250084, 250106 according to the invention still show spalling. If the formula (1c) Fc≤1.0 is additionally satisfied, these alloys no longer show spalling (250107) and surprisingly have a value of 1.0 mg / cm2 at moderate silicon contents, which is of the order of magnitude of 45TM (with 2.6% silicon and 0.16% aluminum). 2 Very small gross weight change.

[0270] Table 4 shows the classification of the weldability of the alloys by means of the MVT test. The weldable alloy AC66 according to the prior art is in zone 2. Alloy 45TM is classified in zone 3 (risk of hot cracking) and is therefore highly prone to crack formation, which makes welding difficult and makes welding with intrinsic welding fillers in particular difficult or impossible.

[0271] The batches not according to the invention with a silicon content of 1.50% or more (45TM, batches 2091, 2099, 2100, 2200, 2203, 2207, 2208, 2209) are all in zone 3. Of the batches with a silicon content of about 1.4%, the batches with an aluminum content below 0.1% are in zone 2 (batches 2093, 2101), and the batches with a higher aluminum content are already in zone 3 (batches 2103, 2096, 2097, 2098). The batches with a silicon content of less than 1.3% are all in zones 1 or 2 (AC66, batches 2095, 2102, 250084 to 250108). All laboratory batches according to the invention were in zone 1 (batches 250084, 250106, 250105, 250108 and 250107) or zone 2 (batch 250102).

[0272] The results of the hot tensile tests at 500° C. in the table show that in the case of all alloys according to the invention melted on a laboratory scale, the elongation limit R p0.2 153 MPa and thus clearly exceed the minimum value of 95 MPa for AC66. They still exceed the minimum value of 150 MPa for 45TM, although not significantly (see equations 5a and 6a). The tensile strength R of all alloys according to the invention is m It is also greater than or equal to 192 MPa and thus also significantly greater than the minimum value of 115 MPa for AC66 (see formula 5b). All hot stretching tests at 500° C. have an elongation of more than 35%.

[0273] The reasons for the required limit values ​​of alloy "E" according to the invention may therefore specifically be:

[0274] A relatively low nickel content (at a relatively high iron content (remainder)) is conducive to less corrosion in a carburizing, sulfiding and chlorinating environment. Therefore, a content of 40% is the upper limit of nickel. Too low a nickel content (at a relatively high iron content (remainder)) is conducive to the formation of a sigma phase, especially at a relatively high chromium content and silicon content. Therefore, a nickel content of 35% is the lower limit.

[0275] Chromium improves the corrosion resistance in carburizing, sulfiding and chloriding environments. Too low a chromium content means that when the alloy is used in a highly corrosive environment, the chromium concentration drops very quickly below the adjacent limit, so that a closed chromium oxide layer can no longer be formed. Therefore, 26% chromium is the lower limit for chromium when used in carburizing, sulfiding and chloriding environments. Too high a chromium content contributes to the formation of sigma phases of the alloy, especially at high chromium contents. Therefore, 30% chromium is considered to be the upper limit.

[0276] Silicon improves corrosion resistance in carburizing, sulfiding and chlorinated environments. A minimum content of 0.40% is therefore required. Too high a content again affects weldability and contributes to the formation of sigma phases, especially at high chromium contents. Therefore, the silicon content is limited to 1.50%.

[0277] A certain content of aluminum improves the corrosion resistance in carburizing, sulfiding and chloriding environments. Therefore, a minimum content of 0.40% is required. Too high a content again affects the weldability, especially in the case of high chromium and silicon contents. Therefore, the aluminum content is limited to 1.30%.

[0278] Manganese is used to improve the machinability. Manganese is limited to 1.0% because this element reduces the high temperature corrosion resistance. Very low magnesium and / or calcium contents improve the machining already by binding away sulfur, thereby avoiding the occurrence of low-melting NiS eutectics. Therefore, a minimum content of 0.0001% is required for magnesium and / or calcium. In the case of too high a content, intermetallic Ni-Mg phases or Ni-Ca phases may occur, which in turn significantly deteriorate the machinability. Therefore, the magnesium content and / or calcium content is limited to a maximum of 0.05%.

[0279] A minimum carbon content of 0.015% is necessary for good creep resistance. Carbon is limited to a maximum of 0.12% since this element reduces the machinability above this content by forming too many primary carbides.

[0280] A minimum nitrogen content of 0.001% is necessary, thereby improving the machinability and heat resistance of the material. Nitrogen is limited to a maximum of 0.150% because this element reduces machinability by forming coarse-grained carbonitrides.

[0281] The phosphorus content should be 0.030% or less, because this interface active element affects high temperature corrosion resistance. Too low a phosphorus content increases the cost. Therefore, the phosphorus content is ≥ 0.001%.

[0282] The oxygen content must be less than or equal to 0.020% to ensure the manufacturability of the alloy. Too low an oxygen content increases the cost. Therefore, the oxygen content is ≥ 0.0001%.

[0283] The sulfur content should be set as low as possible because this interface-active element affects high-temperature corrosion resistance. Therefore, sulfur is fixed to a maximum of 0.010%.

[0284] Molybdenum is limited to less than 1.0% because this element reduces high temperature corrosion resistance.

[0285] Tungsten is limited to less than 1.0% because this element also reduces high temperature corrosion resistance.

[0286] Less than 1.0% cobalt may be included in this alloy. Higher contents reduce high temperature corrosion resistance.

[0287] Copper is limited to less than 0.5% because this element reduces high temperature corrosion resistance.

[0288] The following relationship must be satisfied between nickel, silicon and aluminum so that there is a sufficiently high resistance in a carburizing, sulfiding and chlorinated environment:

[0289] Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5(1a),

[0290] Wherein Ni, Si, Al and Si are the concentrations of the relevant elements in mass %. The reason for the limit value of Fc has been explained in detail in the previous text.

[0291] If necessary, the high-temperature corrosion resistance can be further improved by adding elements that have an affinity for oxygen, in that they simultaneously become incorporated into the oxide layer and there block the diffusion paths of oxygen at the grain boundaries.

[0292] The minimum content of one or more of cerium, lanthanum, cerium mixed metal, yttrium, zirconium and hafnium elements is required to be 0.001% respectively in order to obtain the effect of increasing high temperature corrosion resistance. For cost reasons, the upper limit of the corresponding element is 0.20%. Here, the following formula must be satisfied:

[0293] FRE=0.714*Ce+0.720*La+1.124*Y+1.096*Zr+0.560*Hf≤0.10(2a)

[0294] Where Ce, La, Y, Zr and Hf are the concentrations of the relevant elements in mass %. The total content of elements such as cerium, lanthanum, yttrium, zirconium and hafnium is defined by this formula. Contents that make FRE>1.0 can again increase the corrosion rate and affect machinability.

[0295] Titanium can be added as needed. Titanium improves high temperature strength. From 0.50%, high temperature corrosion behavior may deteriorate, so the maximum value is 0.50%.

[0296] Niobium can be added as needed, as it also improves high temperature strength. Higher contents increase costs very substantially. Therefore, the upper limit is fixed at 0.20%.

[0297] The alloy may also contain tantalum as required, since it also improves high temperature strength. Higher contents increase the cost very substantially. Therefore, the upper limit is fixed at 0.20%. A minimum content of 0.001% is required to achieve the effect.

[0298] Boron can be added to the alloy as required, since it improves creep resistance. Therefore, a minimum content of 0.0001% should be present. This interface-active element also deteriorates high-temperature corrosion resistance. Therefore, boron is fixed to a maximum of 0.008%.

[0299] Vanadium is desirably limited to a maximum of 0.50% since this element reduces the high temperature corrosion resistance.

[0300] Lead is limited to a maximum of 0.002% as required, since this element reduces the high temperature corrosion resistance. The same applies to zinc and tin.

[0301]

[0302] Table 2: Classification of weldability according to the total length of solidification cracks and remelting cracks in mm (from the MVT (Modified Variable Constraint - Transverse Variable Constraint) hot crack test of the BAM (Bedish Institute for Materials Research and Testing)

[0303]

[0304]

[0305]

[0306]

[0307]

[0308]

[0309]

Claims

1. Use of a nickel-iron-chromium alloy having excellent high temperature corrosion resistance as a semi-finished product in a carburizing, sulfiding and chlorinating environment, the nickel-iron-chromium alloy comprising (in mass %): 35.0 to 38% nickel, 26.0 to 30.0% chromium, >0.7 to 1.50% silicon, 0.40 to 1.30% aluminum, 0.00 to 1.0% manganese, 0.0001 to 0.05% magnesium and / or calcium, respectively, 0.015 to 0.12% carbon, 0.001 to 0.150% nitrogen, 0.001 to 0.030% phosphorus, 0.0001 to 0.020% oxygen, Maximum 0.010% sulfur, Less than 1.0% molybdenum, Less than 1.0% cobalt, Less than 0.5% copper, Less than 1.0% tungsten, The balance is iron and common process-related impurities, where the following relationship must be satisfied: Fc=-1.2+0.29*Ni-4.6*Si-4.4*Al≤2.5(1a), Wherein Ni, Si and Al are the relevant element concentrations in mass %.

2. The method according to claim 1, wherein the nickel content is >35.0 to <38%.

3. Use according to any one of claims 1 to 2, wherein the chromium content is >26.0 to 30.0%.

4. The method according to any one of claims 1 to 3, wherein the aluminum content is ≥ 0.50% or > 0.50% to < 1.30%.

5. Use according to any one of claims 1 to 4, wherein the residual iron content is 28.0 or >28.0 to 38.0%.

6. The use according to any one of claims 1 to 5, wherein 0.001 to 0.20% of one or more elements of cerium, lanthanum, yttrium, zirconium and hafnium are contained respectively, wherein the following formula must be satisfied: FRE = 0.714*Ce + 0.720*La + 1.124*Y + 1.096*Zr + 0.560*Hf ≤ 0.10 (2a) where Ce, La, Y, Zr and Hf are the concentrations of the relevant elements in mass %.

7. The method according to claim 1 , wherein in the presence of cerium and lanthanum, a cerium mixed metal (CeMM) is also used in a content of 0.001 to 0.20%, wherein the FRE must be changed as follows: FRE=0.716*CeMM+1.124*Y+1.096*Zr+0.560*Hf≤0.10(3a) Wherein CeMM, Y, Zr and Hf are the concentrations of relevant elements in mass %.

8. Use according to any one of claims 1 to 7, wherein optionally the titanium content is > 0.0 to 0.50%.

9. Use according to any one of claims 1 to 8, wherein optionally the niobium content and / or the tantalum content is respectively 0.0 to 0.50%.

10. Use according to any one of claims 1 to 9, wherein optionally the boron content is from 0.0001 to 0.008%.

11. Use according to any one of claims 1 to 10, optionally further comprising up to 0.50% vanadium.

12. The use according to any one of claims 1 to 11, wherein the impurities are adjusted to the following contents: lead at most 0.002%, tin at most 0.002%, zinc at most 0.002%.

13. Use according to any one of claims 1 to 12, wherein the semi-finished product is in the form of strips, plates, wires, bars, forgings, longitudinally welded tubes and seamless tubes.

14. The method according to claim 1 as or in a component in the chemical industry.

15. The method according to claim 1, as a semi-finished product in a waste incineration or waste pyrolysis plant or as a semi-finished product in a component of a waste incineration or waste pyrolysis plant.